Lithium supplement agent, preparation method thereof, lithium ion battery diaphragm and lithium ion battery

By using lithium supplement agent with naphthyl complex lithium ion structure in lithium-ion batteries, uniform prelithiation of lithium-ion batteries is achieved, and the problem of poor prelithiation of lithium-ion battery electrodes is solved, which significantly improves the The battery's first charge and discharge efficiency and cycle performance.

CN118943529APending Publication Date: 2024-11-12HEFEI GUOXUAN HIGH TECH POWER ENERGY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411206088.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prelithiation effect of existing lithium-ion battery electrodes is poor, resulting in low first-term efficiency and poor circulation performance of lithium-ion batteries.

Method used

A lithium supplement agent with a naphthyl complex lithium ion structure is provided, and the first charge and discharge efficiency and cycle stability of the battery are improved by achieving uniform prelithiation on the negative electrode sheet of the lithium ion battery. The lithium supplement agent is complexed by polyimide and lithium ions. When the naphthalene group is brought into contact with the negative electrode active material, it is reduced and embedded in the negative electrode, avoiding direct contact of lithium metal and potential chemical reactions.

Benefits of technology

It significantly improves the first charge and discharge efficiency and cycling performance of lithium-ion batteries, avoids excessive prelithiation of lithium metal and structural damage, and ensures the safety and stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943529A_ABST
    Figure CN118943529A_ABST
Patent Text Reader

Abstract

The invention provides a lithium supplement agent, a preparation method thereof, a lithium ion battery diaphragm and a lithium ion battery. The lithium supplement agent has the structure: # imgabs0 #, wherein L is one or a combination of more of a single bond, an ether bond, a thioether bond, substituted or unsubstituted C1-C8 alkylene, carbonyl and phenylene; r1 and R2 are respectively and independently selected from empty, halogen and substituted or unsubstituted C1-C5 alkyl, n1 and n2 are respectively and independently any integer in a range of 0 to 4, and n is 100 to 150; and when each group carries a substituent group, the substituent group is halogen or C1-C5 alkyl substituted by halogen. The invention provides a polymer lithium supplement agent with a polyimide structure, and naphthyl free radicals in the structure are in a reduction state and are complexed with lithium ions. The lithium supplement agent can realize a uniform pre-lithiation effect of the negative pole piece, so that the first effect and the cycle life of the lithium ion battery are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion batteries, and more specifically, to a lithium replenishing agent, its preparation method, a lithium-ion battery separator, and a lithium-ion battery. Background Technology

[0002] During the first charge and discharge cycle of a lithium-ion battery, the negative electrode material consumes some active lithium due to the formation of an SEI film, resulting in irreversible capacity loss. Furthermore, novel high-specific-capacity negative electrode materials, such as silicon-based materials, exhibit significant volume changes during charge and discharge, leading to poor cycle performance. To address these issues, researchers have employed pre-lithiation techniques, which involve adding additional active lithium to the negative electrode or adding additional active lithium to the positive electrode and releasing it to the negative electrode during the first charge to compensate for the insufficient cycle performance.

[0003] However, directly using lithium metal for pre-lithiation of the negative electrode presents several problems. For instance, the pre-lithiation rate and degree are difficult to control when lithium foil or stabilized lithium metal powder reacts chemically with the negative electrode, easily leading to over-lithiation and lithium deposition on the negative electrode, posing a safety hazard. Furthermore, introducing lithium metal as an additional electrode to form a temporary battery for electrochemical pre-lithiation is incompatible with existing lithium-ion battery manufacturing processes. Moreover, lithium metal is chemically reactive and easily reacts with air and moisture, making industrialization of lithium metal pre-lithiation difficult. On the other hand, pre-lithiation of the positive electrode, such as adding lithium-rich additives, can lead to the formation of poorly conductive residues or defects in the positive electrode after decomposition, increasing charge transfer resistance or damaging the electrode structure. Over-lithiation of the positive electrode active material can also easily lead to structural instability or even destruction.

[0004] Therefore, developing a suitable lithium replenishing agent for lithium-ion batteries to achieve effective pre-lithiation of their negative electrode and improve the first-efficiency and cycle performance of the final lithium-ion battery is one of the technical challenges that needs to be solved in this field. Summary of the Invention

[0005] The main objective of this invention is to provide a lithium replenishing agent, its preparation method, a lithium-ion battery separator, and a lithium-ion battery, in order to solve the problem that the pre-lithiation effect of the lithium-ion battery electrode in the prior art is not good, resulting in low initial efficiency and poor cycle performance of the lithium-ion battery.

[0006] To achieve the above objectives, a first aspect of the present invention provides a lithium replenishing agent having the structure shown in Formula I:

[0007]

[0008] Wherein, L is a combination of one or more of the following: single bond, ether bond, thioether bond, substituted or unsubstituted C1-C8 alkylene group, carbonyl group, and phenylene group; R1 and R2 are each independently selected from empty, halogenated, substituted or unsubstituted C1-C5 alkyl groups; n1 and n2 are each independently any integer from 0 to 4; and n is 100-150. When the above groups carry substituents, the substituents are halogenated or halogenated C1-C5 alkyl groups. The lithium replenishing agent provided by this invention has a unique structural design, wherein the naphthyl group in the polymer repeating unit exists in a reduced state and forms a complex with lithium ions. When the special lithium-naphthalene complex group comes into direct contact with the negative electrode active material of the lithium-ion battery, the naphthyl group can reduce the negative electrode active material, and at the same time, the complexed lithium ions will be embedded in the negative electrode, realizing uniform pre-lithiation of the negative electrode sheet, thereby improving the initial efficiency and cycle performance of the final lithium-ion battery.

[0009] Furthermore, L can be a single bond, an ether bond, or a combination of one or more of substituted or unsubstituted C1-C3 alkylene groups, carbonyl groups, and phenylene groups; when the above groups carry substituents, the substituents are fluorinated C1-C3 alkyl groups. Through extensive experimentation, the inventors further designed the molecular structure of the lithium replenisher and found that the above structure provides better lithium replenishment and exhibits higher cycle stability in batteries.

[0010] Furthermore, L can be a single bond, ether bond, methylene, ethylene, monofluoromethylene, difluoromethylene, 1,1-difluoroethylene, tetrafluoroethylene, hexafluoroisopropylene, and... One or more of the following combinations, wherein R' is methylene, ethylene, isopropylene, -O-, or -S-. To further improve the lithium replenishment effect and thus enhance the cycle performance of the corresponding lithium-ion battery, the inventors optimized the above structure again through extensive experiments.

[0011] Furthermore, R1 and R2 are each independently selected from H, F, Cl, methyl, or ethyl, and n1 and n2 are each independently 0, 1, or 2; preferably, R1 and R2 are both ortho-substituted. The resulting lithium replenishing agent exhibits superior lithium replenishment performance in the battery, has a more stable structure, and results in a battery with higher overall performance.

[0012] To improve the lithium replenishment effect and thus enhance the cycle performance of lithium-ion batteries, the inventors, through extensive experiments, further optimized the lithium replenishment agent by selecting one or more of the following structures:

[0013]

[0014]

[0015] A second aspect of the present invention provides a method for preparing the above-mentioned lithium supplement, comprising: step S1, preparing polyimide; step S2, preparing a lithium-containing organic solution; and step S3, adding the polyimide to the lithium-containing organic solution to react and obtain the lithium supplement; the polyimide having the structure shown in Formula II:

[0016]

[0017] Wherein, L, R1, R2, n1, n2, and n have the same definitions as above. Accordingly, this invention provides a preparation method compatible with various lithium-ion processes for the aforementioned lithium-ion supplement, thereby obtaining the aforementioned lithium-ion supplement with good lithium-ion supplementation effect and electrochemical stability.

[0018] Furthermore, the molar ratio of lithium to polyimide in the lithium-containing organic solution is (2-3):1; preferably, the solvent of the lithium-containing organic solution is tetrahydrofuran. The inventors optimized the above conditions through numerous experiments and obtained a lithium replenishing agent that significantly improves the initial efficiency and cycle performance of lithium-ion batteries.

[0019] Furthermore, in several typical embodiments, in order to improve the complexation effect of lithium ions and naphthalene groups, and to prevent the structure of the obtained lithium replenishing agent from being destroyed, thereby improving the stability of its lithium replenishment effect and the cycle performance of the corresponding battery, the inventors have optimized the reaction time to be 3h to 4h and the temperature to be 25±10℃ through a large number of experiments; preferably, the reaction is carried out under nitrogen and / or argon protection.

[0020] A third aspect of the present invention provides a lithium-ion battery separator, comprising a base film and a coating disposed on one surface of the base film. The coating includes the aforementioned lithium replenishing agent and binder. The base film is a polyolefin film, and the binder is selected from one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, and polymethyl methacrylate. The resulting separator with the coating formed by the lithium replenishing agent can prevent short circuits while tightly bonding to the lithium-ion negative electrode sheet and achieving stable lithium replenishment of the negative electrode active material, ultimately effectively improving its first-efficiency and cycle performance.

[0021] Furthermore, based on the total weight of the coating (100%), the weight percentage of the lithium replenishing agent is 20%–45%; preferably, the coating thickness is 2μm–5μm. The inventors have conducted extensive experiments to optimize the amount of lithium replenishing agent in the coating and the thickness of the coating itself, in order to better coordinate the coating's adhesion, insulation, ion transport capacity, mechanical properties, and pre-lithiation function, thereby improving the overall electrical performance of the lithium-ion battery.

[0022] Furthermore, in order to improve the isolation performance and wettability of the separator, the coating preferably also includes inorganic particles; preferably, the inorganic particles are selected from one or more of Al2O3, SiO2, B2O3, Ga2O3, TiO2 and SnO2, thereby further improving the safety and electrical performance of the battery.

[0023] A fourth aspect of the present invention provides a lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, and a separator. The negative electrode sheet includes a negative current collector and a negative active layer disposed on at least one side surface of the negative current collector. The positive electrode sheet includes a positive current collector and a positive active layer disposed on at least one side surface of the positive current collector. The separator is disposed between the negative active layer of the negative electrode sheet and the positive active layer of the positive electrode sheet. The separator is the aforementioned lithium-ion battery separator, and the coating of the lithium-ion battery separator is disposed in contact with the negative active layer. In the separator structure of the aforementioned lithium-ion battery, since it contains a lithium replenishing agent capable of uniformly providing lithium ions, it exhibits higher initial charge-discharge efficiency and more durable cycle stability.

[0024] The present invention provides a polymer lithium replenisher with a polyimide structure, wherein the naphthyl radical in the structure is in a reduced state and complexed with lithium ions. After lithium-ion battery electrolyte filling, the naphthyl group reduces the negative electrode and lithium ions are simultaneously inserted into the negative electrode, achieving pre-lithiation of the negative electrode. The lithium replenisher provided by the present invention can achieve a uniform pre-lithiation effect on the negative electrode sheet, thereby significantly improving the initial efficiency and cycle life of lithium-ion batteries. Detailed Implementation

[0025] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the embodiments.

[0026] As described in the background section, existing lithium-ion battery electrodes suffer from poor pre-lithiation effects, resulting in low initial efficiency and poor cycle performance in the resulting lithium-ion batteries. To address these technical problems, a first aspect of the present invention provides a lithium replenishing agent having the structure shown in Formula I:

[0027]

[0028] Wherein, L is a combination of one or more of a single bond, ether bond, thioether bond, substituted or unsubstituted C1-C8 alkylene group, carbonyl group, and phenylene group; R1 and R2 are each independently selected from empty, halogenated, substituted or unsubstituted C1-C5 alkyl groups; n1 and n2 are each independently any integer from 0 to 4; and n is 100-150. When the above groups carry substituents, the substituents are halogenated or halogenated C1-C5 alkyl groups.

[0029] The lithium replenishing agent provided by this invention has a unique structural design, in which the naphthyl groups in the polymer repeating units exist in a reduced state and form complexes with lithium ions. When the special lithium-naphthalene complex group comes into direct contact with the negative electrode active material of the lithium-ion battery, the naphthyl group can reduce the negative electrode active material, and at the same time, the complexed lithium ions will be inserted into the negative electrode, realizing uniform pre-lithiation of the negative electrode sheet, thereby improving the initial efficiency and cycle performance of the final lithium-ion battery.

[0030] Of particular note is that, compared to other lithium-naphthalene pre-lithiation reagents used in the art, i.e., organic solvent systems containing naphthalene radical anions and lithium-ion complexes, the polymer containing naphthalene radical anions and lithium-ion complexes provided by this invention, when used for separator coatings, can achieve more stable in-situ pre-lithiation treatment after lithium-ion battery assembly. This eliminates the need for non-in-situ pre-lithiation treatment of the negative electrode active material before battery assembly, and avoids increased reactivity of the pre-lithiated negative electrode active material, as well as side reactions caused by air or moisture that may occur during subsequent assembly. Ultimately, the lithium replenishing agent provided by this invention can effectively improve battery performance and ensure its safe operation.

[0031] The inventors further designed the molecular structure of the lithium replenisher through extensive experiments. In several preferred embodiments, L is a single bond, an ether bond, or a combination of one or more of substituted or unsubstituted C1-C3 alkylene groups, carbonyl groups, and phenylene groups. When the above groups carry substituents, the substituents are fluorinated C1-C3 alkyl groups. The above structure provides better lithium replenishment and exhibits higher cycle stability in batteries.

[0032] In several more preferred embodiments, L represents a single bond, an ether bond, a methylene group, an ethylene group, a monofluoromethylene group, a difluoromethylene group, a 1,1-difluoroethylene group, a tetrafluoroethylene group, a hexafluoroisopropylene group, and... One or more of the following combinations, wherein R' is methylene, ethylene, isopropylene, -O-, or -S-. To further improve the lithium replenishment effect and thus enhance the cycle performance of the corresponding lithium-ion battery, the inventors optimized the above structure again through extensive experiments.

[0033] Furthermore, R1 and R2 are each independently selected from H, F, Cl, methyl, or ethyl, and n1 and n2 are each independently 0, 1, or 2. The resulting lithium replenisher exhibits superior lithium replenishment performance in the battery, and its structure is more stable. Through extensive experimentation, the inventors designed the molecular structure of the lithium replenisher and discovered that when both R1 and R2 are ortho-substituted, the lithium replenisher with the above structure exhibits better lithium replenishment performance, resulting in a battery with higher overall performance.

[0034] To improve the lithium replenishment effect and thus enhance the cycle performance of lithium-ion batteries, the inventors, through extensive experiments, further optimized the lithium replenishment agent by selecting one or more of the following structures:

[0035]

[0036]

[0037] A second aspect of the present invention provides a method for preparing the above-mentioned lithium supplement, comprising: step S1, preparing polyimide; step S2, preparing a lithium-containing organic solution; and step S3, adding the polyimide to the lithium-containing organic solution to react and obtain the lithium supplement; the polyimide having the structure shown in Formula II:

[0038]

[0039] L, R1, R2, n1, n2, and n have the same definitions as above.

[0040] Regarding the aforementioned lithium replenishing agent, this invention correspondingly provides a preparation method compatible with various lithium-ion processes, thereby obtaining the aforementioned lithium replenishing agent with good lithium replenishment effect and electrochemical stability. The preparation of polyimide further includes:

[0041] Step S1-1: Dissolve naphthaldehyde in hydrochloric acid solution to obtain the first reaction solution; Step S1-2: Add the first reaction solution to an aniline compound to carry out the first reaction to obtain the second reaction solution. The reaction temperature of the first reaction is 120-130℃, and the reaction time is 6-8h; Step S1-3: Add sodium hydroxide aqueous solution to the second reaction solution to obtain the third reaction solution. Then pour the third reaction solution into methanol and filter to obtain the first product; Step S1-4: Wash the obtained first product with methanol and dry it to obtain the diamine monomer. Step S1-5: Carry the obtained diamine monomer and dianhydride monomer in a polar aprotic solvent to carry out the second reaction to obtain the fourth reaction solution. The reaction temperature of the second reaction is 0℃, and the reaction time is 10-15h; Step S1-6: Electrospin the obtained fourth reaction solution and dry it to obtain the second product; Step S1-7: Calcine the second product at 300-350℃ for 10-30min to finally obtain polyimide.

[0042] Among them, aniline compounds are The structure of the obtained diamine monomer is as follows: The structure of the dianhydride monomer is as follows: L, R1, R2, n1, n2, and n have the same definitions as above.

[0043] In several typical implementations, the dianhydride monomer is selected from...

[0044] To improve the yield and purity of the polyimide with the above structure, the preferred molar ratio of hydrogen chloride, aniline, and naphthaldehyde in steps S1-1 and S1-2 is (0.03–0.05):(3.5–5.0):1; and the preferred molar ratio of hydrogen chloride and sodium hydroxide in step S1-3 is 1:1. Furthermore, through extensive experimentation, the inventors have optimized the molar ratio of diamine monomer to dianhydride monomer in step S1-5 to be 1:1, thereby significantly improving the structural stability of the obtained polyimide and enhancing its affinity for Li. + The lithium replenishment effect of the lithium replenishing agent obtained after complexation.

[0045] Furthermore, the molar ratio of lithium to polyimide in the lithium-containing organic solution is (2-3):1, and the solvent of the lithium-containing organic solution is preferably tetrahydrofuran, thereby obtaining a lithium replenishing agent that significantly improves the first efficiency and cycle performance of lithium-ion batteries.

[0046] Furthermore, in several typical embodiments, in order to enhance the complexation effect of lithium ions and naphthalene groups, and to prevent the structure of the obtained lithium replenishing agent from being destroyed, thereby improving the stability of its lithium replenishment effect and the cycle performance of the corresponding battery, the inventors have optimized the reaction time to be 3h to 4h and the temperature to be 25±10℃ through a large number of experiments; and more preferably, the reaction is carried out under nitrogen and / or argon protection.

[0047] Specifically, in lithium-containing organic solutions, lithium exists as elemental lithium metal.

[0048] A third aspect of the present invention provides a lithium-ion battery separator, comprising a base film and a coating disposed on one side surface of the base film, the coating comprising the aforementioned lithium replenishing agent and binder, the base film being a polyolefin film, and the binder being selected from one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, and polymethyl methacrylate.

[0049] The separator with a coating formed by the lithium replenishing agent provided by the present invention can prevent short circuits, bond tightly with the lithium-ion negative electrode sheet, and achieve stable lithium replenishment of the negative electrode active material, thereby effectively improving its first-efficiency and cycle performance.

[0050] In several preferred embodiments, the lithium replenishing agent accounts for 20% to 45% of the total weight of the coating (100%); preferably, the coating thickness is 2 μm to 5 μm. The inventors have conducted extensive experiments to optimize the amount of lithium replenishing agent in the coating and the thickness of the coating itself, in order to better coordinate the coating's adhesion, insulation, ion transport capacity, mechanical properties, and pre-lithiation function, thereby improving the electrical performance of the lithium-ion battery in various aspects.

[0051] Furthermore, to improve the separator's isolation performance and wettability, the coating preferably also includes inorganic particles. In several preferred embodiments, to better complement the aforementioned lithium replenishing agent, the inorganic particles are selected from one or more of Al2O3, SiO2, B2O3, Ga2O3, TiO2, and SnO2, thereby further enhancing the battery's safety and electrical performance.

[0052] A fourth aspect of the present invention provides a lithium-ion battery, including a positive electrode sheet, a negative electrode sheet, and a separator. The negative electrode sheet includes a negative current collector and a negative active layer disposed on at least one side surface of the negative current collector. The positive electrode sheet includes a positive current collector and a positive active layer disposed on at least one side surface of the positive current collector. The separator is disposed between the negative active layer of the negative electrode sheet and the positive active layer of the positive electrode sheet. The separator is the aforementioned lithium-ion battery separator, and the coating of the lithium-ion battery separator is disposed in contact with the negative active layer.

[0053] The separator structure of the aforementioned lithium-ion battery contains a lithium replenishing agent that can uniformly provide lithium ions, thus exhibiting higher initial charge-discharge efficiency and more durable cycle stability.

[0054] The present application will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed in the present application.

[0055] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.

[0056] Example 1

[0057] 1. Preparation of lithium supplement: Naphthalene formaldehyde (CAS No.: 66-77-3) dissolved in hydrochloric acid was added dropwise to aniline (CAS No.: 62-53-3) and reacted at 125℃ for 7 hours. Sodium hydroxide aqueous solution was added to the resulting solution, and the reaction mixture was then poured into methanol and filtered to obtain a precipitate. The molar ratio of hydrogen chloride, sodium hydroxide, aniline, and naphthaldehyde was 0.04:0.04:4.5:1. The precipitate was washed repeatedly with methanol and dried to obtain a diamine monomer. The diamine monomer and biphenyltetracarboxylic dianhydride (CAS No.: 2420-87-3) were reacted in N,N-dimethylformamide. The reaction was carried out in amide with a molar ratio of 1:1 at 0°C for 12 hours. The resulting solution was electrospun. The collected solid was subjected to high-temperature treatment at 300°C for 30 minutes to obtain polyimide. Lithium metal was dissolved in tetrahydrofuran under a nitrogen atmosphere to obtain a lithium metal solution. Polyimide was added to the lithium metal solution with a molar ratio of 2:1 at room temperature for 4 hours. After the reaction, the solution was filtered, washed with methanol, and dried to obtain a lithium replenishing agent, where n is 130–150. The reaction formula is as follows.

[0058]

[0059] 2. Preparation of pre-lithiated separator: Polyvinylidene fluoride, the above-mentioned polyimide lithium supplementer, and Al2O3 were dispersed in acetone at mass percentages of 10%, 12%, and 18%, respectively, to obtain three dispersions; the polyvinylidene fluoride dispersion, polyimide dispersion, Al2O3 dispersion, and acetone were mixed and dispersed evenly at a mass ratio of 1:1:1:7 to obtain a coating slurry, which was coated on a 9μm polyethylene base film with a coating thickness of 2μm. After drying, a pre-lithiated separator with a lithium supplementer content of 30wt% in the coating was obtained.

[0060] Example 2

[0061] 1. Preparation of lithium supplement: Naphthaldehyde (CAS No.: 66-77-3) dissolved in hydrochloric acid was added dropwise to 3-fluoroaniline (CAS No.: 372-19-0) and reacted at 130℃ for 8 hours. Sodium hydroxide aqueous solution was added to the resulting solution, and the reaction mixture was then poured into methanol and filtered to obtain a precipitate. The molar ratio of hydrogen chloride, sodium hydroxide, 3-fluoroaniline, and naphthaldehyde was 0.05:0.05:5.0:1. The precipitate was washed repeatedly with methanol and dried to obtain a diamine monomer. The diamine monomer and hexafluorodianhydride (CAS No.: 1107-00-2) were reacted in N,N-dimethylformamide. The reaction was carried out in amide with a molar ratio of 1:1 at 0°C for 15 hours. The resulting solution was electrospun. The collected solid was then subjected to high-temperature treatment at 330°C for 20 minutes to obtain polyimide. Lithium metal was dissolved in tetrahydrofuran under a nitrogen atmosphere to obtain a lithium metal solution. Polyimide was added to the lithium metal solution at a molar ratio of 2.5:1 at room temperature for 3.5 hours. After the reaction, the solution was filtered, washed with methanol, and dried to obtain a lithium replenishing agent, where n is 120–140. The reaction formula is as follows.

[0062]

[0063] 2. Preparation of pre-lithiated separator: Polyvinylidene fluoride, the above-mentioned polyimide lithium supplementer, and Al2O3 were dispersed in acetone at mass percentages of 10%, 8%, and 22%, respectively, to obtain three dispersions; the polyvinylidene fluoride dispersion, polyimide dispersion, Al2O3 dispersion, and acetone were mixed and dispersed evenly at a mass ratio of 1:1:1:7 to obtain a coating slurry, which was coated on a 9μm polyethylene base film with a coating thickness of 3μm. After drying, a pre-lithiated separator with a lithium supplementer content of 20wt% in the coating was obtained.

[0064] Example 3

[0065] 1. Preparation of lithium supplement: Naphthaldehyde (CAS No.: 66-77-3) dissolved in hydrochloric acid was added dropwise to 2-chloroaniline (CAS No.: 95-51-2) and reacted at 130℃ for 8 hours. Sodium hydroxide aqueous solution was added to the resulting solution, and the reaction mixture was then poured into methanol and filtered to obtain a precipitate. The molar ratio of hydrogen chloride, sodium hydroxide, 2-chloroaniline, and naphthaldehyde was 0.05:0.05:5.0:1. The precipitate was washed repeatedly with methanol and dried to obtain a diamine monomer. The diamine monomer and benzophenone tetracarboxylic dianhydride (CAS No.: 2421-28-5) were reacted in an N,N... The reaction was carried out in dimethylformamide at a molar ratio of 1:1, at 0°C, and for 15 hours. The resulting solution was electrospun. The collected solid was then subjected to high-temperature treatment at 350°C for 10 minutes to obtain polyimide. Lithium metal was dissolved in tetrahydrofuran under a nitrogen atmosphere to obtain a lithium metal solution. Polyimide was added to the lithium metal solution at a molar ratio of 3:1, at room temperature, and for 3 hours. After the reaction, the solution was filtered, washed with methanol, and dried to obtain a lithium supplement, where n is 120–140. The reaction formula is as follows.

[0066]

[0067] 2. Preparation of pre-lithiated separator: Polyvinylidene fluoride, the above-mentioned polyimide lithium supplementer, and Al2O3 were dispersed in acetone at mass percentages of 10%, 10%, and 20%, respectively, to obtain three dispersions; the polyvinylidene fluoride dispersion, polyimide dispersion, Al2O3 dispersion, and acetone were mixed and dispersed evenly at a mass ratio of 1:1:1:7 to obtain a coating slurry, which was coated on a 9μm polyethylene base film with a coating thickness of 3μm. After drying, a pre-lithiated separator with a lithium supplementer content of 25wt% in the coating was obtained.

[0068] Example 4

[0069] 1. Preparation of lithium supplement: Naphthaldehyde (CAS No.: 66-77-3) dissolved in hydrochloric acid was added dropwise to 2-ethylaniline (CAS No.: 578-54-1) and reacted at 120℃ for 6 hours. Sodium hydroxide aqueous solution was added to the resulting solution, and the reaction mixture was then poured into methanol and filtered to obtain a precipitate. The molar ratio of hydrogen chloride, sodium hydroxide, 2-ethylaniline, and naphthaldehyde was 0.03:0.03:3.5:1. The precipitate was washed repeatedly with methanol and dried to obtain a diamine monomer. The diamine monomer and diphenyl ether tetracarboxylic dianhydride (CAS No.: 50662-95-8) were reacted in an N, The reaction was carried out in N-dimethylformamide at a molar ratio of 1:1, at a reaction temperature of 0℃, and for a reaction time of 10h. The resulting solution was electrospun. The collected solid was subjected to high-temperature treatment at a reaction temperature of 350℃ for a reaction time of 10min to obtain polyimide. Lithium metal was dissolved in tetrahydrofuran under a nitrogen atmosphere to obtain a lithium metal solution. Polyimide was added to the lithium metal solution at a molar ratio of lithium metal to polyimide of 3:1 at a reaction temperature of room temperature for a reaction time of 3h. After the reaction was completed, the solution was filtered, washed with methanol, and dried to obtain a lithium replenishing agent, where n is 110-130. The reaction formula is as follows.

[0070]

[0071] 2. Preparation of pre-lithiated separator: Polyvinylidene fluoride, the above-mentioned polyimide lithium supplementer, and Al2O3 were dispersed in acetone at mass percentages of 8%, 15%, and 17%, respectively, to obtain three dispersions; the polyvinylidene fluoride dispersion, polyimide dispersion, Al2O3 dispersion, and acetone were mixed and dispersed evenly at a mass ratio of 1:1:1:7 to obtain a coating slurry, which was coated on a 9μm polyethylene base film with a coating thickness of 3μm. After drying, a pre-lithiated separator with a lithium supplementer content of 37.5wt% in the coating was obtained.

[0072] Example 5

[0073] 1. Preparation of lithium supplement: Naphthaldehyde (CAS No.: 66-77-3) dissolved in hydrochloric acid was added dropwise to 2,6-dimethylaniline (CAS No.: 87-62-7) and reacted at 120℃ for 6 hours. Sodium hydroxide aqueous solution was added to the resulting solution, and the reaction mixture was then poured into methanol and filtered to obtain a precipitate. The molar ratio of hydrogen chloride, sodium hydroxide, 2,6-dimethylaniline, and naphthaldehyde was 0.03:0.03:3.5:1. The precipitate was washed repeatedly with methanol and dried to obtain a diamine monomer. The diamine monomer was then reacted with bisphenol A type diether dianhydride (CAS No.: 38103-06-9). The reaction was carried out in N,N-dimethylformamide at a molar ratio of 1:1 at 0°C for 10 h. The resulting solution was electrospun. The collected solid was subjected to high-temperature treatment at 350°C for 10 min to obtain polyimide. Lithium metal was dissolved in tetrahydrofuran under a nitrogen atmosphere to obtain a lithium metal solution. Polyimide was added to the lithium metal solution at a molar ratio of 3:1 at room temperature for 3 h. After the reaction, the solution was filtered, washed with methanol, and dried to obtain a lithium supplement, where n is 100–130. The reaction formula is as follows.

[0074]

[0075] 2. Preparation of pre-lithiated separator: Polyvinylidene fluoride, the above-mentioned polyimide lithium supplementer, and Al2O3 were dispersed in acetone at mass percentages of 7%, 18%, and 15%, respectively, to obtain three dispersions; the polyvinylidene fluoride dispersion, polyimide dispersion, Al2O3 dispersion, and acetone were mixed and dispersed evenly at a mass ratio of 1:1:1:7 to obtain a coating slurry, which was coated on a 9μm polyethylene base film with a coating thickness of 5μm. After drying, a pre-lithiated separator with a lithium supplementer content of 45wt% in the coating was obtained.

[0076] Example 6

[0077] The only difference between this embodiment and Example 1 is that, in the process of preparing the pre-lithiated separator, the mass ratio of polyvinylidene fluoride dispersion, polyimide dispersion, Al2O3 dispersion, and acetone is changed to 0.6:1.8:0.6:7. After drying, a pre-lithiated separator with a lithium replenishing agent content of 56.3 wt% in the coating is obtained.

[0078] Example 7

[0079] The only difference between this embodiment and Example 1 is that, in the process of preparing the pre-lithiated separator, the mass ratio of polyvinylidene fluoride dispersion, polyimide dispersion, Al2O3 dispersion, and acetone is changed to 1.3:0.4:1.3:7. After drying, a pre-lithiated separator with a lithium supplement content of 11.7wt% is obtained.

[0080] Example 8

[0081] The only difference between this example and Example 1 is that the molar ratio of lithium metal to polyimide is 4:1 and the reaction time is 5 hours.

[0082] Example 9

[0083] The only difference between this example and Example 1 is that the molar ratio of lithium metal to polyimide is 1:1 and the reaction time is 2 hours.

[0084] Application Comparative Example 1

[0085] The only difference between this comparative example and Example 1 is that, in the membrane preparation process, polyvinylidene fluoride and Al2O3 are dispersed in acetone at mass percentages of 10% and 18%, respectively, to obtain two dispersions; the polyvinylidene fluoride dispersion, Al2O3 dispersion, and acetone are mixed and dispersed evenly at a mass ratio of 1.5:1.5:7 to obtain the coating slurry, that is, the membrane coating does not contain lithium supplementation agent.

[0086] Test methods

[0087] Battery assembly: The coating of the separator obtained in each embodiment is placed face to the graphite negative electrode sheet, and a lithium iron phosphate positive electrode sheet is used. After stacking, aluminum-plastic film encapsulation, electrolyte injection and impregnation, a pre-lithiated soft pack battery is obtained.

[0088] Battery performance testing: The soft-pack battery samples obtained above were formed and capacity tested at 45℃ and 25℃ respectively, and the initial coulombic efficiency of the battery was calculated. The soft-pack battery samples obtained above were subjected to 1000-cycle performance testing at 25℃ and 1C rate, and their capacity retention rate was calculated. The results are shown in Table 1.

[0089] Table 1

[0090] First-time coulomb efficiency (%) Capacity retention rate (%) after 1000 cycles Example 1 93.4 99.8 Example 2 93.6 99.5 Example 3 94.1 100.2 Example 4 94.7 100.5 Example 5 95.2 101.2 Example 6 94.3 91.5 Example 7 91.5 94.2 Example 8 92.8 92.7 Example 9 91.7 94.0 Application Comparative Example 1 91.3 93.8

[0091] As can be seen from the above description, the embodiments of the present invention achieve a significant improvement in both the initial coulombic efficiency and the capacity retention rate after 1000 cycles compared to the control group of soft-pack batteries without added lithium replenishment, and can achieve a capacity retention rate of not less than 100% under long-cycle conditions, that is, no capacity decay.

[0092] Specifically, as in Examples 1-5, the higher the lithium replenishment content (20%–45%) in the separator coating, the thicker the separator coating, meaning a higher total amount of lithium replenishment added, resulting in a more significant improvement in the initial coulombic efficiency and capacity retention of the lithium-ion battery. If the lithium replenishment content in the separator coating exceeds 45%, the coating is prone to detachment, which deteriorates the cycle performance of the lithium-ion battery. If the lithium replenishment content in the separator coating is below 20%, the pre-lithiation effect is not significant, resulting in insufficient improvement in the initial coulombic efficiency and capacity retention of the lithium-ion battery. It is worth noting that during the preparation of the lithium replenishment, if the molar ratio of lithium metal to polyimide is greater than 3:1 and the reaction time is greater than 4 hours, the lithium replenishment structure is destroyed, the coating is prone to detachment, and its chemical stability deteriorates, thus worsening the cycle performance of the lithium-ion battery. If the molar ratio of lithium metal to polyimide is less than 2:1 and the reaction time is less than 3 hours, the naphthalene groups are not sufficiently reduced and lithium ions are not fully complexed, reducing the pre-lithiation effect, resulting in insufficient improvement in the initial coulombic efficiency and capacity retention of the lithium-ion battery.

[0093] It should be noted that the terms "first," "second," etc., used in the specification and claims of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such terms can be used interchangeably where appropriate so that the embodiments of this application described herein can be implemented, for example, in a sequence other than those described herein.

[0094] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A lithium supplement, characterized in that: The lithium supplement has a structure shown in Formula I: Wherein, L is a combination of one or more of a single bond, an ether bond, a thioether bond, a substituted or unsubstituted C1-C8 alkylene group, a carbonyl group and a phenylene group; R1 and R2 are each independently selected from null, halogen, substituted or unsubstituted C1-C5 alkyl, n1 and n2 are each independently any integer from 0 to 4, and n is 100 to 150; When the above groups have a substituent, the substituent is a halogen or a C1-C5 alkyl group substituted by a halogen.

2. The lithium supplement according to claim 1, characterized in that: L is a single bond, an ether bond, a substituted or unsubstituted C1-C3 alkylene group, a carbonyl group, and a phenylene group, or a combination of one or more thereof; When the above groups have a substituent, the substituent is a fluorinated C1-C3 alkyl group.

3. The lithium supplement according to claim 2, characterized in that: The L is a single bond, an ether bond, a methylene group, an ethylene group, a monofluoromethylene group, a difluoromethylene group, a 1,1-difluoroethylene group, a tetrafluoroethylene group, a hexafluoroisopropylidene group, and A combination of one or more of the following, wherein R' is methylene, ethylene, isopropylene, -O- or -S-.

4. The lithium supplement according to any one of claims 1 to 3, characterized in that: R1 and R2 are each independently selected from H, F, Cl, methyl or ethyl, n1 and n2 are each independently 0, 1 or 2; Preferably, R1 and R2 are both ortho-substituted.

5. The lithium supplement according to any one of claims 1 to 4, characterized in that: The lithium supplement agent is selected from one or more of the following structures:

6. A method for preparing the lithium supplement according to any one of claims 1 to 5, characterized in that: The preparation method comprises: Step S1, preparing polyimide; Step S2, preparing a lithium-containing organic solution; Step S3, adding the polyimide into the lithium-containing organic solution to react to obtain the lithium supplement agent; The polyimide has a structure shown in Formula II: Wherein, L, R1, R2, n1, n2 and n have the same definitions as described in any one of claims 1 to 5.

7. The preparation method according to claim 6, characterized in that: The molar ratio of lithium in the lithium-containing organic solution to the polyimide is (2-3):1; Preferably, the solvent of the lithium-containing organic solution is tetrahydrofuran.

8. The preparation method according to claim 6 or 7, characterized in that: The reaction time is 3h to 4h, and the temperature is 25±10°C; Preferably, the reaction is carried out under the protection of nitrogen and / or argon.

9. A lithium-ion battery separator, comprising a base film and a coating disposed on one surface of the base film, characterized in that: The coating comprises the lithium supplement agent and a binder according to any one of claims 1 to 5, the base film is a polyolefin film, and the binder is selected from one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer and polymethyl methacrylate.

10. The diaphragm according to claim 9, characterized in that Based on the total weight of the coating being 100%, the weight of the lithium supplement agent accounts for 20% to 45%; Preferably, the coating has a thickness of 2 μm to 5 μm.

11. The diaphragm according to claim 9 or 10, characterized in that: The coating also includes inorganic particles; Preferably, the inorganic particles are selected from one or more of Al2O3, SiO2, B2O3, Ga2O3, TiO2 and SnO2.

12. A lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet and a separator, wherein the negative electrode sheet comprises a negative electrode current collector and a negative electrode active layer disposed on at least one side surface of the negative electrode current collector, the positive electrode sheet comprises a positive electrode current collector and a positive electrode active layer disposed on at least one side surface of the positive electrode current collector, the separator is disposed between the negative electrode active layer of the negative electrode sheet and the positive electrode active layer of the positive electrode sheet, characterized in that: The separator is the lithium-ion battery separator according to any one of claims 9 to 11, and the coating layer of the lithium-ion battery separator is arranged in contact with the negative electrode active layer.

Citation Information

Patent Citations

  • Electrolytic solution and lithium ion battery containing electrolytic solution

    CN112670570A

  • Lithium supplement additive for positive electrode and lithium ion battery

    CN115832466A

  • Lithium supplement agent and preparation method thereof, diaphragm and preparation method thereof, and battery

    CN116813499A

  • Chemical pre-lithiation agent, lithium ion battery and preparation method of lithium ion battery

    CN117059804A

  • Polyimide compound, negative electrode material for lithium ion secondary batteries that uses said polyimide compound, negative electrode for lithium ion secondary batteries, and lithium ion secondary battery

    EP4318676A1