Compound as well as preparation method and application thereof
By adding silicon-based compounds to the cup[4] aromatic structure to the lithium-ion battery electrolyte solution, the problem of poor stability of LiPF6 electrolyte salt is solved, the internal impedance of the battery cell is reduced, and the first effect and magnification of the battery are improved. Retention rate improves cell performance.
Patent Information
- Application Number
- CN202411154195.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The stability of LiPF6 electrolyte salt in organic solvents is poor, resulting in an increase in the internal impedance of lithium-ion batteries and a dip in the battery cell. The existing additives have limited effect on improving battery performance.
Add a specific compound to the lithium-ion battery electrolyte. This compound is a compound that introduces a silicon-based structure on the cup[4] aromatic structure. As an additive, it quickly compatible with the electrode-electrolyte interface, balances the internal characteristics of the battery cell, and reduces electricity. The inner impedance of the core improves the performance of the battery cell.
It significantly reduces the SEI interface resistance, improves the first-effect and rate retention rate of the battery, and improves the stability and performance of the battery cell.
Smart Images

Figure CN119039341A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a compound, a preparation method thereof and an application thereof. Background Art
[0002] As electrochemical devices, such as lithium-ion batteries, are widely used in various electronic products, users have placed increasingly higher demands on the cycle performance of batteries.
[0003] LiPF6 electrolyte salt is widely used in commercial lithium-ion batteries due to its high ionic conductivity and excellent electrochemical stability. However, its stability in organic solvents is poor. The highly active acidic substances such as POF3, PF5, and HF produced by hydrolysis will cause irreversible damage to the solid electrolyte interface (SEI) / positive electrode electrolyte interface (CEI), causing a sharp increase in the internal impedance of the battery and a drop in the battery cell. The existing technology generally improves the interface stability by adding additives to the electrolyte, but its effect on improving battery performance is limited. Summary of the invention
[0004] In view of this, the present invention provides a compound, a preparation method and an application thereof. The compound provided in the present application is added to the electrolyte of a lithium-ion battery as an additive, which can quickly become compatible with the electrode-electrolyte interface, balance various characteristics inside the battery cell, amplify the water and acid removal effects, and promote its stable CEI / SEI properties, thereby reducing and stabilizing the internal impedance changes of the battery cell and improving the performance of the battery cell.
[0005] The present application provides a compound represented by formula (I):
[0006]
[0007] wherein R1, R2 and R3 are independently selected from alkyl or an alkyl substituted with at least one substituent, alkenyl or an alkenyl substituted with at least one substituent, alkynyl or an alkynyl substituted with at least one substituent, ester or an ester substituted with at least one substituent, alkylamino or an alkylamino substituted with at least one substituent, nitrogen-containing heterocyclic group or at least one substituent-substituted nitrogen-containing heterocyclic group, phosphate or a phosphate substituted with at least one substituent, borate or a borate substituted with at least one substituent, sulfonate or a sulfonate substituted with at least one substituent, alkylaminocarbonyl or an alkylaminocarbonyl substituted with at least one substituent, alkyl or a keto substituted with at least one substituent;
[0008] The substituents are independently selected from halogen, alkyl, alkenyl, alkynyl, alkylsilyl or alkylsiloxy.
[0009] In some specific implementations, R1, R2 and R3 are not alkyl groups at the same time.
[0010] In some specific implementations, R1, R2 and R3 are independently selected from alkyl, alkynyl, halogen-substituted alkyl, alkylsilyloxy-substituted alkyl, alkylsilyl-substituted phosphate, alkylsilyl-substituted borate or oxazolidinone.
[0011] In some specific implementations, the compound has R C-1 ~R C-9 The structure described:
[0012]
[0013] The present application also provides an electrolyte additive, comprising the compound described in the above technical solution.
[0014] In some specific implementations, the electrolyte additive further includes one or more of vinylene carbonate, fluoroethylene carbonate, 1,3-propane sultone, vinyl sulfate, diphenyl carbonate, toluene carbonate, acrylic nitrile, succinic anhydride, succinonitrile and adiponitrile.
[0015] In some specific implementations, the electrolyte additive includes fluoroethylene carbonate and vinylene carbonate;
[0016] The mass ratio of the compound, vinylene carbonate and fluoroethylene carbonate is 0.1-3:0.5-1.5:0.5-1.5.
[0017] The present application also provides an electrolyte, comprising an electrolyte, a solvent and the additive described in the above technical solution.
[0018] In some specific implementations, the mass concentration of the electrolyte is 5wt% to 20wt%;
[0019] The additive is added in an amount of 0.5 wt % to 5 wt % of the total amount of the electrolyte and the solvent.
[0020] The present application also provides a battery, comprising the electrolyte described in the above technical solution.
[0021] The compound provided in this application introduces a silicon-based structure into the calix[4]arene structure, and uses the characteristics of its amphiphilic compound to quickly become compatible with the electrode-electrolyte interface, balance various characteristics inside the battery cell, amplify the water and acid removal effects, promote its stable CEI / SEI properties, stabilize the positive electrode material structure, thereby reducing and stabilizing the internal impedance changes of the battery cell and improving the performance of the battery cell. Experimental results show that after the compound provided in this application is added to the electrolyte, compared with calix[4]arene and silicon-based compounds as additives, the first efficiency of the battery is improved, the SEI interface resistance is significantly reduced, and the rate retention rate is improved. DETAILED DESCRIPTION
[0022] It should be understood that the expression "one or more of..." includes each of the items recited after the expression individually and in various different combinations of two or more of the recited items, unless otherwise understood from the context and usage. The expression "and / or" in combination with three or more recited items should be understood to have the same meaning, unless otherwise understood from the context.
[0023] The use of the terms "comprising", "having" or "containing", including their grammatical synonyms, should generally be understood as open and non-restrictive, for example not excluding other unrecited elements or steps, unless otherwise specifically stated or otherwise understood from the context.
[0024] The term "halogen" refers to fluorine, chlorine, bromine and iodine;
[0025] The term "alkyl" represents a saturated straight or branched hydrocarbon group having 1 to 6 carbon atoms, such as methyl, ethyl, propyl, 1-methylethyl, butyl, 1-methylpropyl, 2-methylpropyl, 1,1-dimethylethyl, pentyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, 2,2-dimethylethyl, 1-ethylpropyl, hexyl, 1,1-dimethylpropyl, 1,2-dimethylpropyl, 1-methylpentyl, 2-methylpentyl, 3-methylpentyl, 4-methylpentyl, 1,1-dimethylbutyl, 1,2-dimethylbutyl, 1,3-dimethylbutyl, 2,2-dimethylbutyl, 2,3-dimethylbutyl, 3,3-dimethylbutyl, 1-ethylbutyl, 2-ethylbutyl, 1,1,2-trimethylpropyl, 1,2,2-trimethylpropyl, 1-ethyl-1-methylpropyl and 1-ethyl-2-methylpropyl;
[0026] The term "alkenyl" represents an unsaturated straight-chain or branched hydrocarbon radical having 2 or 3 to 6 carbon atoms and having a double bond in any desired position, for example, C2-C6-alkenyl such as ethenyl, 1-propenyl, 2-propenyl, 1-methylethenyl, 1-butenyl, 2-butenyl, 3-butenyl, 1-methyl-1-propenyl, 2-methyl-1-propenyl, 1-methyl-2-propenyl, 2-methyl-2-propenyl, 1-pentenyl, 2-pentenyl, 3-pentenyl, 4-pentenyl, 1-methyl-1-butenyl, 2-methyl-1-butenyl, 3-methyl-1-butenyl, 1-methyl-2-butenyl, 2-methyl-2 -butenyl, 3-methyl-2-butenyl, 1-methyl-3-butenyl, 2-methyl-3-butenyl, 3-methyl-3-butenyl, 1,1-dimethyl-2-propenyl, 1,2-dimethyl-1-propenyl, 1,2-dimethyl-2-propenyl, 1-ethyl-1-propenyl, 1-ethyl-2-propenyl, 1-hexenyl, 2-hexenyl, 3-hexenyl, 4-hexenyl, 5-hexenyl, 1-methyl-1-pentenyl, 2-methyl-1-pentenyl, 3-methyl-1-pentenyl, 4-methyl-1-pentenyl, 1-methyl-2-pentenyl, 2-methyl-2-pentenyl, 3-methyl-2 4-methyl-2-pentenyl, 1-methyl-3-pentenyl, 2-methyl-3-pentenyl, 3-methyl-3-pentenyl, 4-methyl-3-pentenyl, 1-methyl-4-pentenyl, 2-methyl-4-pentenyl, 3-methyl-4-pentenyl, 4-methyl-4-pentenyl, 1,1-dimethyl-2-butenyl, 1,1-dimethyl-3-butenyl, 1,2-dimethyl-1-butenyl, 1,2-dimethyl-2-butenyl, 1,2-dimethyl-3-butenyl, 1,3-dimethyl-1-butenyl, 1,3-dimethyl-2-butenyl, 1,3-dimethyl-3-butenyl , 2,2-dimethyl-3-butenyl, 2,3-dimethyl-1-butenyl, 2,3-dimethyl-2-butenyl, 2,3-dimethyl-3-butenyl, 3,3-dimethyl-1-butenyl, 3,3-dimethyl-2-butenyl, 1-ethyl-1-butenyl, 1-ethyl-2-butenyl, 1-ethyl-3-butenyl, 2-ethyl-1-butenyl, 2-ethyl-2-butenyl, 2-ethyl-3-butenyl, 1,1,2-trimethyl-2-propenyl, 1-ethyl-1-methyl-2-propenyl, 1-ethyl-2-methyl-1-propenyl or 1-ethyl-2-methyl-2-propenyl;
[0027] The term "alkynyl" represents a straight-chain or branched hydrocarbon radical having 2 to 6 carbon atoms and having a triple bond at any desired position, such as ethynyl, 1-propynyl, 2-propynyl, 1-butynyl, 2-butynyl, 3-butynyl, 1-methyl-2-propynyl, 1-pentynyl, 2-pentynyl, 3-pentynyl, 4-pentynyl, 1-methyl-2-butynyl, 1-methyl-3-butynyl, 2-methyl-3-butynyl, 3-methyl-1-butynyl, 1,1-dimethyl-2-propynyl, 1-ethyl-2-propynyl, 1-hexynyl, 2-hexynyl, 3-hexynyl, 4-hexynyl, 5-hexynyl, 1-methyl- 2-pentynyl, 1-methyl-3-pentynyl, 1-methyl-4-pentynyl, 2-methyl-3-pentynyl, 2-methyl-4-pentynyl, 3-methyl-1-pentynyl, 3-methyl-4-pentynyl, 4-methyl-1-pentynyl, 4-methyl-2-pentynyl, 1,1-dimethyl-2-butynyl, 1,1-dimethyl-3-butynyl, 1,2-dimethyl-3-butynyl, 2,2-dimethyl-3-butynyl, 3,3-dimethyl-1-butynyl, 1-ethyl-2-butynyl, 1-ethyl-3-butynyl, 2-ethyl-3-butynyl and 1-ethyl-1-methyl-2-propynyl;
[0028] The term "alkylamino" represents (as defined above) a straight-chain or branched alkyl group having 1 to 6 carbon atoms, which is bonded to the main structure via an amino group (-NH-);
[0029] The term "alkylaminocarbonyl" represents an alkylamino group (as defined above) which is bonded to the main structure via a carbonyl group (-CO-);
[0030] The term "alkylcarbonyl" represents (as defined above) a straight-chain or branched alkyl group having 1 to 6 carbon atoms, which is bonded to the main structure via a carbonyl group (-CO-);
[0031] The term "ester group" represents a straight-chain or branched alkyl group (as described above) having 1 to 6 carbon atoms, which is bonded to the main structure via a carbonyl group (-CO-) and an oxygen atom (-O-);
[0032] The term "phosphate" means bonded to the main structure via a phosphate group (PO4-);
[0033] The term "borate" means bonded to the main structure via a borate group (BO3-);
[0034] The term "sulfonate group" means that the bond to the main structure is through a sulfonate group (SO2-);
[0035] The term "nitrogen-containing heterocyclic group" represents a nitrogen-containing heterocyclic group, which is bonded to the main structure through -N-, and in addition to C and N, may also contain the group consisting of oxygen and sulfur as ring members, for example, it may be a 5-membered nitrogen-containing heterocyclic group containing one to four nitrogen atoms or one to three nitrogen atoms and one sulfur or oxygen atom; the nitrogen-containing heterocyclic group may be a nitrogen-containing six-membered heterocyclic group, including carbon atoms and one to five nitrogen atoms, and in addition, may contain a sulfur atom or an oxygen atom as a ring member, etc.;
[0036] The term "alkylsilyloxy" represents (as described above) a straight-chain or branched alkyl group having 1 to 6 carbon atoms, which is bonded to the main structure via a siloxy group (-Si-O-);
[0037] The term "alkylsilyl" represents (as defined above) a straight-chain or branched alkyl group having 1 to 6 carbon atoms, which is bonded to the main structure via a silicon group (-Si-).
[0038] It should be understood that the order of steps or the order in which certain actions are performed is not important as long as the present invention remains operable. In addition, two or more steps or actions may be performed simultaneously.
[0039] The use of any and all examples or exemplary language, such as "for example" or "including", herein is intended only to better illustrate the invention and does not limit the scope of the invention unless otherwise claimed. No language in this specification should be construed as indicating that any non-claimed element is essential to the practice of the invention.
[0040] In addition, the numerical ranges and parameters used to define the present invention are approximate values, and the relevant values in the specific embodiments have been presented as accurately as possible. However, any numerical value inherently inevitably contains standard deviations due to individual test methods. Therefore, unless otherwise expressly stated, it should be understood that all ranges, quantities, values and percentages used in this disclosure are modified by "about". Here, "about" generally means that the actual value is within plus or minus 10%, 5%, 1% or 0.5% of a specific value or range.
[0041] The present application provides a compound represented by formula (I):
[0042]
[0043] wherein R1, R2 and R3 are independently selected from alkyl or alkyl substituted with at least one substituent, alkenyl or alkenyl substituted with at least one substituent, alkynyl or alkynyl substituted with at least one substituent, ester or ester substituted with at least one substituent, alkylamino or alkylamino substituted with at least one substituent, nitrogen-containing heterocyclic group or nitrogen-containing heterocyclic group substituted with at least one substituent, phosphate or phosphate substituted with at least one substituent, borate or borate substituted with at least one substituent, sulfonate or sulfonate substituted with at least one substituent, alkylaminocarbonyl or alkylaminocarbonyl substituted with at least one substituent, alkylcarbonyl or alkylcarbonyl substituted with at least one substituent;
[0044] The substituents are independently selected from halogen, alkyl, alkenyl, alkynyl, alkylsiloxy or alkylsilyl.
[0045] The present application introduces a silicon-based structure into the calix[4]arene structure to form a compound represented by formula (I), which has both a calix[4]arene structure and a silicon-based structure. When added to the electrolyte of a lithium-ion battery as an additive, the compound can quickly become compatible with the electrode-electrolyte interface, balance various characteristics inside the battery cell, amplify the water and acid removal effects, and promote the stabilization of the CEI / SEI properties, thereby reducing and stabilizing the internal impedance changes of the battery cell and improving the performance of the battery cell.
[0046] In some specific implementations, R1, R2 and R3 are not alkyl at the same time. In some specific implementations, at least one of R1, R2 and R3 is selected from alkynyl or at least one substituted alkynyl, ester or at least one substituted ester, alkylamino or at least one substituted alkylamino, nitrogen-containing heterocyclic group or at least one substituted nitrogen-containing heterocyclic group, phosphate or at least one substituted phosphate, borate or at least one substituted borate.
[0047] In some specific implementations, R1, R2 and R3 are independently selected from alkyl, alkynyl, halogen-substituted alkyl, alkylsilyloxy-substituted phosphate, alkylsilyl-substituted phosphate, alkylsilyl-substituted borate or oxazolidinone, preferably methyl, ethyl, acetate, trimethylsiloxyacetate, ethynyl, trifluoromethyl, oxazolidin-2-one, trimethylsilyl phosphate, trimethylsilyl borate, etc.
[0048] In some specific implementations, the compound has R C-1 ~R C-9 The structure described:
[0049]
[0050] The present application has no particular restrictions on the preparation method of the compound represented by formula (I), and the compound can be prepared according to the following method:
[0051] The compound represented by formula A reacts with the calix[4]arene represented by formula B to obtain the compound represented by formula (I), and the reaction process is as follows:
[0052]
[0053] The present application uses the compound shown in formula A as a raw material to prepare the compound shown in formula (I). The present application has no special restrictions on its source, and it can be purchased on the market and can be prepared according to the following method:
[0054] The compound shown in formula C is reacted with a chlorinating agent to obtain the compound shown in formula A, and the reaction process is as follows:
[0055]
[0056] The compound shown in formula C is a silane containing substituents R1, R2 and R3, wherein R1, R2 and R3 have the same definitions as above, and are not described in detail in this application. The source of the compound shown in formula C is not particularly limited in this application, and it can be purchased on the market.
[0057] The compound shown in formula C reacts under the action of hydrochloric acid and a chlorinating agent to obtain a compound shown in formula A. The present application has no special restrictions on the chlorinating agent, which may be zinc chloride, thionyl chloride, phosphorus chloride, etc. The present application has no special restrictions on the steps, parameters, conditions, etc. of the reaction, and methods familiar to those skilled in the art may be used. The applicant has found that although trimethylsilyl additives can form a film on the negative electrode in secondary batteries, they cannot truly protect the negative electrode. They can reduce internal resistance in the early stage but affect the life in the later stage. They are effective in removing water and acid, but the performance effect on the battery cell is not significantly improved. Therefore, they are introduced into the molecular structure of calix[4]arene in order to improve the performance of the battery cell.
[0058] After obtaining the compound shown in formula A, it is reacted with the calix[4]arene shown in formula B to obtain the compound shown in formula (I). Specifically, the calix[4]arene shown in formula B is p-tert-butylcalix[4]arene, which can be purchased on the market. As the third generation supramolecular host after crown ethers and cyclodextrins, calixarene has the characteristics of easy modification (simple synthesis), adjustable cavity size, and the ability to recognize ions or molecular guests, and has been widely used in various fields. The electrolyte, as the only fluid in the battery core, has an interface with the positive and negative electrodes and the diaphragm. One side of the electrode interface film is tightly combined with the electrode, and the other side is well mixed with the solvated lithium ions. Its properties change gradually from polarity to non-polarity, so that it can achieve amphiphilicity with the electrode and the electrolyte and complete the screening of lithium ions and solvents. The calix[4]arene structure has the characteristics of an amphiphilic compound and can be used to improve the compatibility of electrolytes and electrode materials. Its repellent groups form a new surface on one side, coordinate and include ions, and polymerize to form a continuous thin layer, which is in line with the formation mechanism of the electrode interface film. Its hydrophilic end can capture a small amount of H2O and HF and isolate them from the interface film. However, the resulting battery cell performance interface resistance is relatively high. The present application introduces a silicon-based structure into the calix[4]arene structure, which can further reduce the interface resistance and thus improve the battery cell performance.
[0059] In some specific implementations, the compound shown in formula B and the alkaline compound are first dissolved in a reaction medium, and then the compound shown in formula A and the catalyst are added to react. In some specific implementations, the alkaline compound includes but is not limited to potassium carbonate, sodium carbonate, sodium sulfite, sodium acetate, potassium acetate, etc., preferably potassium carbonate. In some specific implementations, the catalyst includes but is not limited to KI, Al2O3, Al2O3-SiO2, ZnS, etc., preferably KI. In some specific implementations, the reaction medium includes but is not limited to acetone, benzene, toluene, dichloromethane, etc., preferably acetone. In some specific implementations, the molar ratio of the compound represented by formula B to the compound represented by formula A is preferably 1:4-5, the mass ratio of the compound represented by formula B to the alkaline compound is preferably 1-10:10, preferably 3-9:10; the mass volume ratio of the compound represented by formula B to the reaction medium is preferably 1g-10g:200mL-500mL, more preferably 2g-8g:250mL-450mL; the mass ratio of the compound represented by formula B to the catalyst is preferably 1g-10g:0.1g-0.5g, more preferably 1g-10g:0.2g-0.4g.
[0060] After uniform mixing, the reaction system is heated to react. In some specific implementations, the reaction temperature is preferably 70°C to 100°C, more preferably 80°C to 90°C; the reaction time is preferably 30h to 60h, more preferably 35h to 55h. After the reaction is completed, the obtained reaction system is cooled to room temperature, and an aging machine is added to the obtained solid after filtration for aging. After filtering again, the obtained filter residue is recrystallized to obtain a compound shown in formula (I). In some specific implementations, the aging agent is selected from methanol, ethanol, isopropanol, acetone or acetonitrile, preferably methanol. In some specific implementations, the aging time is preferably 10h to 30h, more preferably 15h to 25h. In some specific implementations, the solvent for the recrystallization includes but is not limited to anhydrous ethanol, methanol, isopropanol, acetone, acetonitrile, etc., preferably anhydrous ethanol.
[0061] The present application also provides an electrolyte additive, comprising the compound described in the above technical solution.
[0062] In some specific implementations, the electrolyte additive also includes one or more of vinyl carbonate, fluoroethylene carbonate, 1,3-propane sultone, vinyl sulfate, diphenyl carbonate, toluene carbonate, acrylic nitrile, succinic anhydride, butanediol and adiponitrile, preferably including fluoroethylene carbonate (FEC) and vinyl carbonate (VC). In some specific implementations, the mass ratio of the compound, vinyl carbonate and fluoroethylene carbonate is 0.1-3:0.5-1.5:0.5-1.5, preferably 0.5-2.5:1:1.
[0063] The present application also provides an electrolyte, including an electrolyte, a solvent and the additives described in the above technical solution. In some specific implementations, the electrolyte can be a lithium-ion battery electrolyte, in which case the electrolyte includes a lithium salt electrolyte, an organic solvent and the additives described in the above scheme. In some specific implementations, the lithium salt electrolyte includes but is not limited to lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalate borate (LiDFOB), lithium dioxalate borate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalate phosphate) (LiDFOP) and lithium tetrafluorooxalate phosphate (LiTFOP) One or more, preferably lithium hexafluorophosphate. In some specific implementations, the concentration of the lithium salt electrolyte is 10wt% to 20wt%, preferably 12wt% to 15wt%. In some specific implementations, the organic solvent includes but is not limited to one or more of ethylene carbonate, ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethylene carbonate, ethyl propionate, ethyl acetate, methyl acetate, dimethyl acetate, methyl butyrate, and n-propyl acetate, preferably a mixture of ethylene carbonate (EC) and ethyl methyl carbonate (EMC), and the mass ratio of EC to EMC is preferably 20-40:40-60, more preferably 25-35:45:55. In some specific implementations, the additive is added in an amount of 0.5wt% to 5wt% of the total amount of the electrolyte and the solvent, preferably 1wt% to 4wt%, and more preferably 2wt% to 3wt%.
[0064] In some specific implementations, in the electrolyte, the electrolyte is sodium hexafluorophosphate, the solvent is a mixture of ethylene carbonate (EC) and ethyl methyl carbonate (EMC), the mass ratio of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) is preferably 20-40:40-60, more preferably 25-35:45:55, the concentration of the electrolyte is 10wt%-20wt%, preferably 12wt%-15wt%. The additive includes the compound described in the above technical solution, vinylene carbonate and fluoroethylene carbonate, and the mass ratio thereof is 0.1-3:0.5-1.5:0.5-1.5, preferably 0.5-2.5:1:1; the amount of the additive added is 0.5wt%-5wt% of the total amount of the electrolyte and the solvent, preferably 1wt%-4wt%, more preferably 2wt%-3wt%.
[0065] In some specific implementations, the electrolyte may be a sodium ion battery electrolyte, in which case the electrolyte includes a sodium salt electrolyte, an organic solvent, and the additives described in the above scheme. Similar to the lithium ion battery electrolyte, the difference in the sodium ion battery electrolyte is that the electrolyte is a sodium salt, which may be selected from sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium hexafluoroarsenate (NaAsF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium trifluoromethanesulfonate (NaTFS), sodium difluorooxalate borate (NaDFOB), sodium dioxalate borate (NaBOB), sodium difluorophosphate (NaPO2F2), sodium difluorobis(oxalate phosphate) (NaDFOP), and sodium tetrafluorooxalate phosphate (NaTFOP), etc., and the present application has no particular restrictions on this.
[0066] The present application has no particular restrictions on the preparation method of the electrolyte, and the electrolyte can be prepared by the following method:
[0067] The solvent, electrolyte and additives are mixed to obtain an electrode solution.
[0068] Specifically, the present application can firstly mix the solvent and the electrolyte evenly, and then add the additives and mix them evenly. The present application has no special restrictions on the process parameters of each step, as long as each substance can be fully dissolved and mixed evenly.
[0069] The present application also provides a battery, comprising the electrolyte described in the above technical solution. Specifically, the battery can be a lithium-ion battery, which comprises a positive electrode sheet, a negative electrode sheet, a separator separating the positive electrode sheet and the negative electrode sheet, and the electrolyte described in the above technical solution.
[0070] The lithium-ion battery includes a positive electrode plate, and the positive electrode plate includes a positive electrode collector and a positive electrode active material layer formed on the positive electrode collector. In some specific implementations, the positive electrode collector can be a metal foil, including but not limited to aluminum foil, nickel foil, stainless steel, etc. For example, the positive electrode collector can be aluminum foil. A positive electrode active material layer is provided on the surface of the positive electrode collector, which includes a positive electrode material, an optional conductive agent and an optional binder. In some specific implementations, the mass ratio of the positive electrode material, the conductive agent and the binder is 90-98:1-5:1-5, preferably 92-95:2-4:1.5-2. In some specific implementations, the positive electrode material includes but is not limited to LiFePO4, LiCoO2, LiNi x Co y Mn 1-x-y O2, LiMn2O4, Na(Ni 0.5 Mn 0.5 ) x Fe 1-xO2, Na3V2(PO4)3, Na2FeFe(CN)6, etc., can be one or more of them. When the positive electrode material is a mixture of multiple specific substances, the present application does not make too many restrictions on the ratio between the specific substances. In some specific implementations, the conductive agent includes but is not limited to carbon black, hard carbon, graphite, carbon nanotubes, graphene, silver powder, nickel powder, tin oxide, conductive titanium dioxide, etc., can be one or more of them. When the conductive agent is a mixture of multiple specific substances, the present application does not make too many restrictions on the ratio between each specific substance. The binder includes but is not limited to polyvinylidene fluoride, polytetrafluoroethylene, polyacrylic acid, polyamide, lithium polyacrylate, methacrylate, sodium polymethylcellulose, aluminum dihydrogen phosphate, etc., can be one or more of them. When the binder is a mixture of multiple specific substances, the present application does not make too many restrictions on the ratio between each specific substance.
[0071] The present application has no special restrictions on the preparation method of the positive electrode sheet. The positive electrode material, the optional conductive agent and the optional binder are uniformly mixed in a solvent, such as N-methylpyrrolidone (NMP), coated on the positive electrode collector in an optional manner, and dried to obtain the positive electrode sheet. Furthermore, after drying, rolling, slicing, etc. are also included, and the present application has no special restrictions on them.
[0072] The lithium-ion battery includes a negative electrode plate, and the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector. In some specific implementations, the negative electrode current collector can be a metal foil, including but not limited to aluminum foil, nickel foil, stainless steel, etc. For example, the negative electrode current collector can be aluminum foil. A negative electrode active material layer is provided on the surface of the negative electrode current collector, which includes a negative electrode material, an optional conductive agent, an optional binder, and an optional thickener. In some specific implementations, the mass ratio of the negative electrode material, the conductive agent, the binder, and the thickener is 90-98:0.5-2:0.5-3:1-5, preferably 92-97:0.7-1.5:0.8-1.5:1-2. In some specific implementations, the negative electrode material includes but is not limited to graphite, hard carbon, soft carbon, lithium titanate, silicon-based composite materials, tin-based composite materials, and can be one or more thereof. When the negative electrode material is a mixture of multiple specific substances, the present application does not make too many restrictions on the ratio between the specific substances. In some specific implementations, the conductive agent includes but is not limited to carbon black, hard carbon, graphite, carbon nanotubes, graphene, silver powder, nickel powder, tin oxide, conductive titanium dioxide, etc., which can be one or more thereof, and when the conductive agent is a mixture of multiple specific substances, the application does not make too many restrictions on the ratio between each specific substance. The binder includes but is not limited to styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polyvinylidene fluoride (PVDF), sodium carboxymethyl cellulose (CMC-Na), polyacrylic acid (PAA), polytetrafluoroethylene (PTFE), polyimide (PI), etc., which can be one or more thereof, and when the binder is a mixture of multiple specific substances, the application does not make too many restrictions on the ratio between each specific substance. The thickener includes but is not limited to sodium carboxymethyl cellulose (CMC), polyvinylidene fluoride (PVDF), sodium carboxymethyl cellulose (CMC-Na), polyacrylic acid (PAA), polytetrafluoroethylene (PTFE), polyimide (PI), etc., which can be one or more thereof, and when the thickener is a mixture of multiple specific substances, the application does not make too many restrictions on the ratio between each specific substance.
[0073] The present application has no special restrictions on the preparation method of the negative electrode sheet. The negative electrode material, the optional conductive agent, the optional binder and the optional thickener are uniformly mixed in a solvent, such as deionized water, and coated on the negative electrode current collector in an optional manner, and then dried to obtain the negative electrode sheet. Furthermore, after drying, rolling, slicing, etc. are also included, and the present application has no special restrictions on them.
[0074] In some specific implementations, the diaphragm includes but is not limited to glass fiber microporous membrane, polyester microporous membrane, polyethylene microporous membrane, polypropylene microporous membrane, polytetrafluoroethylene microporous, ceramic coated diaphragm, etc.
[0075] In some specific implementations, the electrode liquid is as described above, and is added with a compound additive of formula (I), which can quickly become compatible with the electrode-electrolyte interface, balance various characteristics inside the battery cell, amplify the water and acid removal effects, promote its stable CEI / SEI properties, and stabilize the positive electrode material structure, thereby reducing and stabilizing the internal impedance changes of the battery cell and improving the battery cell performance.
[0076] In the present application, a positive electrode sheet, a separator and a negative electrode sheet are stacked in sequence to obtain a battery cell assembly, which is sealed in an aluminum-plastic bag, and an electrolyte is injected. After packaging, standing, formation and other processes, a lithium-ion battery is obtained.
[0077] The compounds provided by the present invention, their preparation methods and applications are further described below in conjunction with the examples.
[0078] Example 1
[0079] 7 g (7.7 mmol) of p-tert-butylcalix[4]arene and 10 g of potassium carbonate dissolved in a small amount of water were added to 300 mL of acetone solution, and then 5.18 g (30.8 mmol) of dimethylchlorosilyl acetate and 0.2 g of KI were added. After mixing evenly, the temperature was quickly raised to 80° C. and refluxed for 48 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. An appropriate amount of methanol was added to the obtained solid and the mixture was aged for 24 h. After filtering again, the residue was recrystallized using anhydrous ethanol to obtain a product of formula R c-1 The compound shown is 7.25 g (6.15 mmol), with a yield of 80% and a purity of 98.5%.
[0080]
[0081] Example 2
[0082] 7 g (7.7 mmol) of p-tert-butylcalix[4]arene and 10 g of potassium carbonate dissolved in a small amount of water were added to 300 mL of acetone solution, and then 7.41 g (30.8 mmol) of 2-((trimethylsilyl)oxy)chlorodimethylsilyl acetate and 0.2 g of KI were added. After mixing evenly, the temperature was quickly raised to 80° C. and refluxed for 48 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. An appropriate amount of methanol was added to the obtained solid and aged for 24 h. After filtering again, the filter residue was recrystallized using anhydrous ethanol to obtain a product of formula R c-2 The compound shown is 7.58 g (6.15 mmol), with a yield of 80% and a purity of 98%.
[0083]
[0084] Example 3
[0085] 5 g (7.7 mmol) of p-tert-butylcalix[4]arene and a small amount of 10 g of anhydrous potassium carbonate dissolved in water were added to 300 mL of acetone solution, and then 4.52 g (30.8 mmol) of diethylchloro(ethynyl)silane and 0.2 g of KI were added. After mixing evenly, the temperature was quickly raised to 60°C and refluxed for 36 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. An appropriate amount of methanol was added to the obtained solid and aged for 20 h. After filtering again, the residue was recrystallized using anhydrous ethanol to obtain a product of formula R c-3 The compound shown is 7.17 g (5.93 mmol), with a yield of 77% and a purity of 98%.
[0086]
[0087] Example 4
[0088] 7 g (7.7 mmol) of p-tert-butylcalix[4]arene and 10 g of potassium carbonate dissolved in a small amount of water were added to 300 mL of acetone solution, and then 4.39 g (30.8 mmol) of chlorotriethynylsilane and 0.2 g of KI were added. After mixing evenly, the temperature was quickly raised to 80° C. and refluxed for 48 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. An appropriate amount of methanol was added to the obtained solid and the mixture was aged for 24 h. After filtering again, the residue was recrystallized using anhydrous ethanol to obtain a product of formula R c-4 The compound shown is 7.33 g (6.15 mmol), with a yield of 80% and a purity of 99%.
[0089]
[0090] Example 5
[0091] 7 g (7.7 mmol) of p-tert-butylcalix[4]arene and 10 g of potassium carbonate dissolved in a small amount of water were added to 300 mL of acetone solution, and then 6.98 g (30.8 mmol) of chloro(ethynyl)bis(trifluoromethyl)silane and 0.2 g of KI were added. After mixing evenly, the temperature was quickly raised to 80° C. and refluxed for 48 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. An appropriate amount of methanol was added to the obtained solid and the mixture was aged for 24 h. After filtering again, the residue was recrystallized using anhydrous ethanol to obtain a product of formula R c-5 The compound shown is 8.96 g (5.86 mmol), with a yield of 76% and a purity of 98%.
[0092]
[0093] Example 6
[0094] 7 g (7.7 mmol) of p-tert-butylcalix[4]arene and 10 g of potassium carbonate dissolved in a small amount of water were added to 300 mL of acetone solution, and then 5.16 g (30.8 mmol) of 3-(chlorodimethylsilyl)oxazolidin-2-one and 0.2 g of KI were added. After mixing evenly, the temperature was quickly raised to 80° C. and refluxed for 48 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. An appropriate amount of methanol was added to the obtained solid and the mixture was aged for 24 h. After filtering again, the residue was recrystallized using anhydrous ethanol to obtain a compound of formula R c-6 The compound shown is 8.06 g (6.24 mmol), with a yield of 81% and a purity of 99%.
[0095]
[0096] Example 7
[0097] 7 g (7.7 mmol) of p-tert-butylcalix[4]arene and 10 g of potassium carbonate dissolved in a small amount of water were added to 300 mL of acetone solution, and then 10.31 g (30.8 mmol) of chlorodimethylsilylbis(trimethylsilyl)phosphate and 0.25 g of KI were added. After mixing evenly, the temperature was quickly raised to 80°C and refluxed for 48 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. An appropriate amount of methanol was added to the obtained solid and the mixture was aged for 24 h. After filtering again, the residue was recrystallized using anhydrous ethanol to obtain a product of formula R c-7 The compound shown is 12.85 g (6.55 mmol), with a yield of 85% and a purity of 98%.
[0098]
[0099] Example 8
[0100] 7 g (7.7 mmol) of p-tert-butylcalix[4]arene and 10 g of potassium carbonate dissolved in a small amount of water were added to 300 mL of acetone solution, and then 9.20 g (30.8 mmol) of chlorodimethylsilylbis(trimethylsilyl)borate and 0.2 g of KI were added. After mixing evenly, the temperature was quickly raised to 80° C. and refluxed for 48 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. An appropriate amount of methanol was added to the obtained solid and the mixture was aged for 24 h. After filtering again, the residue was recrystallized using anhydrous ethanol to obtain a product of formula R c-8 The compound shown is 11.61 g (6.39 mmol), with a yield of 83% and a purity of 99%.
[0101]
[0102] Example 9
[0103] 7 g (7.7 mmol) of p-tert-butylcalix[4]arene and 10 g of potassium carbonate dissolved in a small amount of water were added to 300 mL of acetone solution, and then 4.48 g (30.8 mmol) of 1-chloro-N,N-diethyl-1,1-dimethylsilylamine and 0.2 g of KI were added. After mixing evenly, the temperature was quickly raised to 80°C and refluxed for 48 h. After the reaction was completed, the mixture was cooled to room temperature and filtered. An appropriate amount of methanol was added to the obtained solid and the mixture was aged for 24 h. After filtering again, the residue was recrystallized using anhydrous ethanol to obtain a compound of formula R c-9 The compound shown is 7.41 g (6.15 mmol), with a yield of 80% and a purity of 98.5%.
[0104]
[0105] Embodiments 10 to 19
[0106] Additives were prepared using the compounds prepared in Examples 1 to 9, FEC and VC in a mass ratio of 0.5:1:1.
[0107] Comparative Examples 1 to 9
[0108] Additives were prepared with the silicon compounds used in Examples 1 to 9, FEC and VC in a mass ratio of 0.5:1:1.
[0109] Comparative Example 10
[0110] The additive was prepared by mixing p-tert-butylcalix[4]arene with FEC and VC in a mass ratio of 0.5:1:1.
[0111] Comparative Example 11
[0112] The additive was prepared with FEC and VC in a mass ratio of 1:1.
[0113] Test example
[0114] In a dry room environment with a dew point of -50°C, the positive electrode active material polyanion LiFePO4, conductive carbon black SP, and binder polyvinylidene fluoride PVDF were mixed in a mass ratio of 95:2.5:2.5, and N-methylpyrrolidone (NMP) was added as a solvent to adjust the slurry to a solid content of 63%. After coating, rolling, and die-cutting, a 56*63mm positive electrode sheet was prepared for standby use;
[0115] The negative electrode active material graphite, conductive carbon black (SP), thickener sodium carboxymethyl cellulose (CMC), binder PAA and styrene-butadiene rubber (SBR) are mixed in a mass ratio of 95:1.0:1.0:1.2:1.8, deionized water is added as a solvent, and the mixture is adjusted to a slurry with a solid content of 52%, and a 58*65mm negative electrode sheet is prepared by coating, rolling and die-cutting for standby use;
[0116] The negative electrode sheet, the separator, and the positive electrode sheet are stacked in 13+12 layers, and the tabs are welded to prepare a soft-pack battery, which is then placed in a vacuum dryer for 24 hours to remove moisture;
[0117] In an argon atmosphere glove box with a water content of less than 10ppm, non-aqueous organic solvents EC and EMC were mixed in a mass ratio of 30:53.5, and then 14% LiPF6 was added to the non-aqueous organic solvent, dissolved and mixed evenly, and then 2.5% of the additives prepared in Examples 10 to 19 and Comparative Examples 1 to 11 were added, and stirred evenly to obtain an electrolyte. The above-configured electrolyte was injected into the above-mentioned soft-pack battery cell, and a lithium-ion battery was obtained after vacuum packaging, standing, hot pressing, volume separation, and secondary sealing.
[0118] The lithium-ion battery was tested, and the test method was as follows: the battery after injection was immersed at 45°C, left to stand for 24 hours, and formed at a small rate of 0.05C. After charging for 3 hours, the rate was increased to 0.2C and charged to an upper limit voltage of 3.65V. After two seals and exhaust, an EIS test was performed, and the capacity was divided three times at 0.5C, and the first cycle discharge capacity was recorded to calculate the first efficiency. The divided capacity was recorded, and the divided battery cell was tested at a rate, 0.5C constant current and constant voltage charging to 3.65V, constant current discharge to 2.0V, 2C constant current and constant voltage charging to 3.65V, and constant current discharge to 2.0V. See Table 1 for the results. Table 1 is the performance test results of the lithium-ion battery provided in this application.
[0119] Table 1 Performance test results of lithium-ion batteries provided in this application
[0120]
[0121]
[0122] By comparing Examples 11-19, it is found that the first effect, membrane impedance, and rate capacity retention rate of different target products basically show a positive correlation trend. The effect is related to the energy level window and solvation structure caused by the physicochemical structure of the substituent group. The relatively optimal target product R C-3 , followed by R C-7 , R C-8 , the number of trimethylsilyl groups may have a greater effect.
[0123] By comparing the comparative examples 1-11, it is found that there are certain differences between the target products corresponding to the different chlorotrimethylsilyl derivatives and the examples 11-19, and the relatively optimal one is R C-7 , followed by R C-4 , R C-8As for the performances of Comparative Examples 10 and 11 containing only p-tert-butylcalix[4]arene, all three have been improved to a certain extent, and p-tert-butylcalix[4]arene itself has certain advantages.
[0124] The first effect and membrane impedance R of Examples 11 to 19 and Comparative Examples 1 to 11 were compared. SEI From the capacity retention rate at 2C / 0.5C, it can be seen that the introduction of supramolecular p-tert-butyl cup[4] structure on the matrix of trimethylsilyl derivatives can effectively reduce the loss of active lithium during the formation process, effectively stabilize the dynamic balance of SEI / CEI, achieve lower membrane impedance, fundamentally improve the compatibility inside the battery cell, and improve the rate performance.
[0125] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. Compound represented by formula (I): in, R1, R2 and R3 are independently selected from alkyl or alkyl substituted by at least one substituent, alkenyl or alkenyl substituted by at least one substituent, alkynyl or alkynyl substituted by at least one substituent, ester or ester substituted by at least one substituent, alkylamino or alkylamino substituted by at least one substituent, nitrogen-containing heterocyclic group or nitrogen-containing heterocyclic group substituted by at least one substituent, phosphate or phosphate substituted by at least one substituent, borate or borate substituted by at least one substituent, sulfonate or sulfonate substituted by at least one substituent, alkylaminocarbonyl or alkylaminocarbonyl substituted by at least one substituent, alkylcarbonyl or alkylcarbonyl substituted by at least one substituent; The substituents are independently selected from halogen, alkyl, alkenyl, alkynyl, alkylsiloxy or alkylsilyl.
2. The compound according to claim 1, characterized in that R1, R2 and R3 are not alkyl groups at the same time.
3. The compound according to claim 1, characterized in that R1, R2 and R3 are independently selected from alkyl, alkynyl, halogen-substituted alkyl, alkylsilyloxy-substituted phosphate, alkylsilyl-substituted phosphate, alkylsilyl-substituted borate or oxazolidinone.
4. The compound according to claim 1, characterized in that With R C-1 ~R C-9 The structure described:
5. An electrolyte additive, characterized in that: The invention comprises the compound according to any one of claims 1 to 4.
6. The electrolyte additive according to claim 5, characterized in that: It also includes one or more of vinylene carbonate, fluoroethylene carbonate, 1,3-propane sultone, vinyl sulfate, diphenyl carbonate, toluene carbonate, acrylic nitrile, succinic anhydride, succinonitrile and adiponitrile.
7. The electrolyte additive according to claim 6, characterized in that: including fluoroethylene carbonate and vinylene carbonate; The mass ratio of the compound, vinylene carbonate and fluoroethylene carbonate is (0.1-3):(0.5-1.5):(0.5-1.5).
8. An electrolyte comprising an electrolyte, a solvent and the additive according to any one of claims 5 to 7.
9. The electrolyte according to claim 8, characterized in that The mass concentration of the electrolyte is 5wt% to 20wt%; The additive is added in an amount of 0.5 wt % to 5 wt % of the total amount of the electrolyte and the solvent.
10. A battery comprising the electrolyte according to claim 8 or 9.
Citation Information
Patent Citations
Electrolyte solution, electrochemical device, and electronic device
CN113067032A
Binder, adhesive tape, preparation method of adhesive tape and electrochemical device
CN115820169A
Copper foil composite additive and method for preparing electrolytic copper foil with highly oriented crystal face
CN118028918A
Positive active material composition for rechargeable lithium battery and rechargeable lithium battery
US20140141322A1
All-solid-state secondary cell, cell electrode sheet and solid electrolyte composition used in said cell, method for manufacturing cell electrode sheet, and method for manufacturing all-solid-state secondary cell
WO2015147282A1
Cited By
Positive pole piece, electrochemical device and electronic device
CN119833560A
Positive electrode sheet, electrochemical device, and electronic device
WO2026149258A1