Preparation method of three-dimensional micro-gap lithium ion battery diaphragm and lithium ion battery
By inlaid inorganic particles on the lithium-ion battery separator and cleaning and extraction of pores, a three-dimensional microgap structure is formed, which solves the thermal stability and coating peeling problems of the lithium-ion battery separator at high temperatures, and improves the battery's Tensile lift strength and electrochemical properties.
Patent Information
- Application Number
- CN202410988650.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The existing lithium-ion battery separators have poor thermal stability at high temperatures, which can easily lead to short circuits and fires. The use of a large number of adhesives in the ceramic coating process leads to the coating peeling and the increase in the interface resistance of the electrolyte, which affects battery performance and safety.
The preparation method of three-dimensional microgap lithium-ion battery separator is adopted. By spraying or rolling inlaid inorganic particles, cleaning and extraction of pores is formed by cleaning and extraction of the wash solution to form a rough three-dimensional structure and pore structure, which enhances the tensile lift strength and wettability of the separator.
It effectively solves the problems of coating shedding and large interface resistance of electrolyte, improves the tensile strength and electrochemical performance of lithium-ion batteries, and improves the charging, discharge and cycling performance of the battery.
Smart Images

Figure CN118943641A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of lithium-ion battery separators, and in particular, relates to a method for preparing a three-dimensional microgap lithium-ion battery separator and a lithium-ion battery. Background Art
[0002] At present, polyolefin separators are the mainstream separators, but the thermal stability of this separator is poor. Among them, the melting points of polypropylene (PP) and polyethylene (PE) are 165℃ and 135℃ respectively. At high temperatures, this separator will shrink or melt, causing internal short circuits, leading to fires and even explosions, so there are potential safety issues. In response to this situation, the technical field has adopted a variety of methods to improve the thermal stability of the separator. Coating a layer of inorganic ceramic particles on the PP separator or PE separator is considered to be the most effective and economical method. The ceramic material provides high heat resistance, while the adhesive provides adhesion to maintain the structural integrity of the coating and the entire composite separator. On the one hand, due to the improved thermal stability, this ceramic coated separator can effectively improve the safety of lithium-ion batteries by preventing short circuits at high temperatures; on the other hand, the ceramic coated separator has good infiltration and liquid absorption and retention capabilities with the electrolyte and the positive and negative electrode materials, which greatly improves the performance and service life of the battery.
[0003] However, when conventional polymer diaphragms such as PE and PP are coated with inorganic ceramics, a large amount of high-strength adhesives and special coating equipment are required to evenly coat the ceramics on the diaphragm surface due to the poor compatibility between the inorganic ceramics and the polymer surface. As a result, there are several defects: (1) A large amount of adhesive increases the contact resistance between the diaphragm and the electrolyte; (2) In high temperature and organic solvent environments, the adhesive is easy to fall off, causing the ceramic coating to fall off at the same time, thereby blocking the ion channel of the diaphragm, causing the positive and negative electrodes of the lithium-ion battery to be short-circuited and causing quality problems such as bloating, which not only seriously reduces the energy density of the lithium-ion battery, but also seriously affects the safety of the lithium-ion battery; (3) Aluminum-containing materials such as aluminum oxide or aluminum hydroxide (boehmite) contain a large amount of free aluminum ions or elemental aluminum, which can easily cause aluminum ions to migrate between the positive and negative electrodes during the electrochemical reaction of the lithium-ion battery, seriously affecting the capacity of the lithium-ion battery.
[0004] In view of this, the present application provides a method for preparing a three-dimensional microgap lithium-ion battery separator and a lithium-ion battery. Summary of the invention
[0005] This application is made in view of the above technical problems and aims to provide a method for preparing a three-dimensional micro-gap lithium-ion battery separator and a lithium-ion battery, which can solve the technical problems existing in the existing lithium-ion battery separators and thus improve the performance of the lithium-ion battery separators and lithium-ion batteries.
[0006] In order to solve the above technical problems, the present application provides a method for preparing a three-dimensional microgap lithium-ion battery separator and a lithium-ion battery, the method comprising the following steps:
[0007] S1, preparing a composite eutectic matrix based on a high molecular polymer and an organic solvent in a preset mass ratio;
[0008] S2, preparing a first composite film according to the prepared composite eutectic matrix;
[0009] S3, embedding inorganic particles of a preset particle size onto the first composite film by spraying or rolling, so that both ends of the inorganic particles pass through the first composite film, thereby obtaining a second composite film;
[0010] S4, washing the second composite film with a washing liquid, and then immersing the washed second composite film in circulating pure water;
[0011] S5, extracting and forming pores in the washed second composite film by using an extractant to obtain a third composite film having a porous structure;
[0012] S6. Thermally radiate the third composite film to obtain a three-dimensional microgap lithium-ion battery separator.
[0013] In some embodiments, step S1 is specifically as follows: a high molecular polymer and an organic solvent are mixed in a preset mass ratio, and after the reaction and precipitation, the high molecular polymer is uniformly stirred to obtain a composite eutectic matrix, wherein the high molecular polymer is at least one of polyethylene, polypropylene, and polyimide, and the organic solvent is one of paraffin oil and methyl silicone oil, and the preset mass ratio is 1:2-5.
[0014] In some embodiments, the step S2 is specifically as follows: at 200-300° C., the prepared composite eutectic matrix is stirred and extruded using a twin-screw extruder, then flows out through a mold of a casting machine, and is cooled on a cooling roller to form a film, thereby obtaining a first composite film.
[0015] In some embodiments, the inorganic substance is at least one of aluminum oxide, aluminum oxyhydroxide, zirconium oxide, and magnesium oxide, and the preset particle size of the inorganic particles is 500-1000 nm.
[0016] In some embodiments, the spraying or rolling is double-sided spraying or double-sided rolling, wherein the spraying is one of thermal spraying, cold spraying, ultrasonic spraying and supersonic spraying.
[0017] In some embodiments, the spraying is cold spraying, and the spraying amount of cold spraying is 200-800g / m 2, the spraying power is 1-5KW, the spraying speed is 100-500mm / s, the powder feeding rate is 10-30g / min, and the spraying pressure is 0.5-1.5MPa.
[0018] In some embodiments, in step S4, the second composite film is cleaned by a washing liquid by obtaining an alkaline washing liquid or an inorganic acid washing liquid with a mass concentration of 10-30%, and soaking the second composite film in the alkaline washing liquid or the inorganic acid washing liquid for 10-30 minutes, wherein the temperature of the washing liquid is controlled at 20-50°C.
[0019] In some embodiments, the alkaline washing solution is at least one of sodium hydroxide and potassium hydroxide solutions.
[0020] In some embodiments, the extractant is a dichloromethane aqueous solution, and the concentration of the extractant is 500-1000 mL / L.
[0021] The present application also provides a lithium-ion battery, which comprises a three-dimensional microgap lithium-ion battery separator prepared by the above-mentioned method for preparing the three-dimensional microgap lithium-ion battery separator.
[0022] In the lithium-ion battery diaphragm preparation method provided in the present application, inorganic particles are embedded in the first composite film by spraying or rolling, so that the surface of the prepared diaphragm has a rough three-dimensional structure, while retaining the smoothness and structural integrity of the pores inside the diaphragm, effectively solving the technical problems of coating shedding caused by the use of a large amount of adhesive in the existing diaphragm coating process and the large electrolyte interface resistance caused by the adhesive. Moreover, since the rough inorganic particles are combined with the polymer matrix in a hot melt state, a more stable structural state can be formed, so that the tensile strength of the lithium-ion battery diaphragm matrix is effectively improved; at the same time, the second composite film is cleaned with a lotion, which can effectively remove the residual metal aluminum or free aluminum ions in the ceramic coating, thereby purifying the interface contact between the lithium-ion battery diaphragm and the electrolyte, and increasing the wettability of the lithium-ion battery diaphragm and the electrolyte, thereby correspondingly improving the battery charging and discharging and cycle performance. Therefore, the lithium-ion battery separator prepared by the method for preparing the lithium-ion battery separator provided in the present application effectively solves the technical problems existing in the prior art, and the lithium-ion battery separator has better tensile strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a flow chart of a method for preparing a three-dimensional microgap lithium-ion battery separator in this application.
[0024] Figure 2 is a schematic diagram of the structure of the second composite film in this application,
[0025] Figure 3: is a contact angle test result diagram of the lithium ion battery separator prepared by the preparation method provided in this application and the conventional coating method,
[0026] Figure 4 is a tensile strength test result diagram of the lithium-ion battery separator prepared by the preparation method provided in this application and the conventional coating method,
[0027] Figure 5 The figure is a test result diagram of the charge and discharge performance of lithium-ion batteries corresponding to the lithium-ion battery separators prepared by the preparation method provided in this application and the conventional coating method.
[0028] Figure 6 The graph of the cycle performance test results of lithium-ion batteries corresponding to the lithium-ion battery separators prepared by the preparation method provided in this application and the conventional coating method. DETAILED DESCRIPTION
[0029] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0030] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0031] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0032] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0033] In order to more clearly understand the above-mentioned purposes, features and advantages of the present application, the present application is further described in detail below in conjunction with the accompanying drawings and specific embodiments. The additional embodiments and advantages of the present application will be partially given in the following description, and some will become obvious from the following description, or will be understood through practice. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.
[0034] like Figure 1 , Figure 2 As shown, the embodiment of the present application provides a method for preparing a three-dimensional microgap lithium-ion battery separator and a lithium-ion battery, the method comprising the following steps:
[0035] S1, preparing a composite eutectic matrix based on a high molecular polymer and an organic solvent in a preset mass ratio;
[0036] S2, preparing a first composite film according to the prepared composite eutectic matrix;
[0037] The specific steps are:
[0038] At a temperature of 200-300°C, the prepared composite eutectic matrix is stirred and extruded by a twin-screw extruder, then flows out through the mold of a casting machine, and is cooled on a cooling roller to form a film to obtain a first composite film. Generally, the extrusion rate is 100-300g / min, and the cooling time is 1-5min. After film formation, the composite film is simultaneously biaxially stretched by a transverse and longitudinal stretching mechanism to obtain a first composite film of any desired width and thickness.
[0039] S3, embedding inorganic particles of a preset particle size onto the first composite film by spraying or rolling, so that both ends of the inorganic particles pass through the first composite film, thereby obtaining a second composite film;
[0040] In this step, the spraying or rolling is double-sided spraying or double-sided rolling, wherein the spraying is one of thermal spraying, cold spraying, ultrasonic spraying and supersonic spraying;
[0041] In the above embodiment, double-sided cold spraying is preferred, and the spraying amount of cold spraying is 200-800g / m 2 , spraying power is 1-5KW, spraying speed is 100-500mm / s, powder feeding rate is 10-30g / min, spraying pressure is 0.5-1.5MPa;
[0042] like Figure 2 As shown, one third of the inorganic particles are embedded in the first composite film, and two thirds of the inorganic particles are protruding from the two side surfaces of the first composite film.
[0043] S4, washing the second composite film with a washing liquid, and then immersing the washed second composite film in circulating pure water;
[0044] The steps are as follows:
[0045] Obtain an alkaline washing solution or an inorganic acid washing solution with a mass concentration of 10-30%, and soak the second composite film in the alkaline washing solution or the inorganic acid washing solution for 10-30 minutes, wherein the temperature of the washing solution is controlled to be 20-50° C.;
[0046] In the above embodiment, the washing liquid is selected from at least one of sodium hydroxide solution and potassium hydroxide solution, and the mixing ratio is not limited, and the mass ratio of hydroxide can be maintained at 10-30%.
[0047] It should be noted that, since aluminum-containing inorganic particles are selected in the above embodiment, aluminum can fully react with acids and alkalis, so conventional inorganic acids can also be selected as the washing liquid. However, the reaction between inorganic acids and aluminum is more violent than the reaction between alkalis and aluminum, and the impact on the environment is more serious. Therefore, alkaline washing liquid is preferred in the above embodiment.
[0048] The second composite film after immersion cleaning is placed in flowing circulating pure water for immersion for 60-120 minutes until the pH value of the surface of the second composite film is detected to be 6-7.5 after immersion. The immersion process can effectively remove the residual alkali on the surface of the second composite film and the free alkali in the gaps of the second composite film.
[0049] S5, extracting and forming pores in the washed second composite film by using an extractant to obtain a third composite film having a porous structure;
[0050] In this step, the extractant is a dichloromethane aqueous solution, and the concentration of the extractant is 500-1000mL / L, and its concentration values include 500mL, 600mL, 700mL, 800mL, 900mL, and 1000mL, that is, the extractant concentration value can be all real numbers within the limited interval, and the above interval is just an abbreviation of these numerical combinations.
[0051] S6, subjecting the third composite film to thermal radiation, thereby obtaining a three-dimensional microgap lithium-ion battery separator;
[0052] In this step, due to the problem of thermal expansion and contraction when combining inorganic particles (i.e., inorganic ceramic particles) with plastic, in order to strengthen the adhesion between the third composite film and the inorganic ceramic particles, reduce the gap between the inorganic ceramic particles and the third composite film, and make the third composite film firmly adhere to the inorganic ceramic particles, the above-mentioned embodiment uses thermal radiation to treat the third composite film, thereby forming a lithium-ion battery separator with a three-dimensional microgap structure.
[0053] In the above embodiment, inorganic particles are embedded in the first composite film by spraying or rolling, so that the surface of the prepared diaphragm has a rough three-dimensional structure, and the smoothness and structural integrity of the pores inside the diaphragm are retained, which effectively solves the technical problems of coating shedding caused by the use of a large amount of adhesive in the existing diaphragm coating process and the large electrolyte interface resistance caused by the adhesive. Moreover, since the rough inorganic particles are combined with the polymer matrix in a hot melt state, a more stable structural state can be formed, so that the tensile strength of the lithium ion battery diaphragm matrix is effectively improved; at the same time, the second composite film is cleaned based on the lotion, which can effectively remove the residual metal aluminum element or free aluminum ions in the ceramic coating, thereby purifying the interface contact between the lithium ion battery diaphragm and the electrolyte, and increasing the wettability of the lithium ion battery diaphragm and the electrolyte, thereby correspondingly improving the battery charging and discharging and cycle performance. Therefore, the lithium ion battery diaphragm prepared by the preparation method of the lithium ion battery diaphragm provided in the present application effectively solves the technical problems existing in the prior art, and the lithium ion battery diaphragm has better tensile strength.
[0054] In some embodiments, step S1 is specifically as follows: a high molecular polymer and an organic solvent are mixed in a preset mass ratio, and after the reaction and precipitation, the high molecular polymer is uniformly stirred to obtain a composite eutectic matrix, wherein the high molecular polymer is at least one of polyethylene, polypropylene, and polyimide, and the organic solvent is one of paraffin oil and methyl silicone oil, and the preset mass ratio is 1:2-5.
[0055] In the above embodiment, the preset mass ratio of the high molecular weight polymer to the organic solvent is 1:2-5, and its values include but are not limited to 1:2, 1:3, 1:4, and 1:5. It should be noted that the value of the preset mass ratio can be all real numbers within the limited interval, and the above interval is just an abbreviation of these numerical combinations; the molecular weight of the high molecular weight polymer is controlled between 1 million and 3 million, and its values include but are not limited to 1 million, 1.2 million, 1.4 million, 1.6 million, 1.8 million, 2 million, 2.2 million, 2.4 million, 2.6 million, 2.8 million, and 3 million. The molecular weight of the high molecular weight polymer can be all real numbers within the limited interval, and the above interval is just an abbreviation of these numerical combinations.
[0056] In some embodiments, the inorganic substance is at least one of aluminum oxide, aluminum oxyhydroxide, zirconium oxide, and magnesium oxide, and the preset particle size of the inorganic particles is 500-1000 nm.
[0057] In the above embodiment, the inorganic material is preferably aluminum oxide, and the preset particle size values of the inorganic particles include but are not limited to 500nm, 600nm, 700nm, 800nm, 900nm, and 1000nm. The preset particle size values can be all real numbers within a limited interval, and the above interval is only an abbreviation of these numerical combinations. The above parameter range can ensure that the inorganic particles are embedded and protrudingly set on the first composite film.
[0058] The present application also provides a lithium-ion battery, which includes a three-dimensional microgap lithium-ion battery separator prepared by the method for preparing a three-dimensional microgap lithium-ion battery separator in the above embodiment.
[0059] Based on the description of the beneficial technical effects of the above-mentioned method for preparing the three-dimensional micro-gap lithium-ion battery separator, the lithium-ion battery has the same beneficial technical effects, which will not be repeated here.
[0060] In order to better illustrate the working principle and technical effect of the present application, a performance comparison test is performed on the lithium-ion battery separator prepared according to the implementation method of the present application and the separator prepared by the conventional coating method. The performance comparison includes wettability comparison, tensile strength comparison and electrochemical performance test comparison. During the test, the separator sample refers to the lithium-ion battery separator prepared by the implementation method of the present application and the conventional coating method.
[0061] Wettability comparison test: Since the contact angle is the most effective means to characterize the wettability of a material, the wettability comparison test in this embodiment selects a contact angle comparison test of two lithium-ion batteries. The contact angle test process is as follows:
[0062] The membrane sample was cut into small discs with a diameter of 20 mm, and the sample was placed flat on a glass slide. The glass slide was then placed on the stage of the contact angle meter. The organic electrolyte of the button cell was used as a reagent to test the contact angle of the membrane sample. The test volume was 10 μL. Data was recorded 5 seconds after the organic liquid was dropped, and photos were taken for record.
[0063] like Figure 3 As shown, Figure 3 a is a contact angle test result diagram of the lithium-ion battery separator prepared in this application, Figure 3 b is the contact angle test result of the lithium-ion battery separator prepared by the conventional coating method.
[0064] from Figure 3 It can be seen that the contact angle test result of the lithium-ion battery separator prepared by the present application is 5.9°, while the contact angle test result of the lithium-ion battery separator prepared by the conventional coating method is 47.2°. The smaller the angle formed by the droplet on the surface of the material, the larger the diffusion area of the droplet on the surface of the material, that is, the better its corresponding wettability. Therefore, compared with the lithium-ion battery separator prepared by the conventional coating method, the contact angle test result of the lithium-ion battery separator prepared by the embodiment of the present application is smaller, that is, the lithium-ion battery separator prepared by the embodiment of the present application has better wettability.
[0065] The tensile strength comparison test process is as follows:
[0066] The membrane samples were cut into strips of 10 cm × 2 cm (length × width) using a cutter, and the tensile strength and elongation of the strip membrane samples were tested using a PT-301A electronic tensile testing machine. The samples were stretched at a rate of 300 mm / min with a gauge length of 20 mm.
[0067] like Figure 4 As shown, Figure 4 The tensile strength comparison results of lithium ion battery separators prepared by the present application and conventional coating methods are shown. Figure 4 It can be seen that the tensile strength of the lithium-ion battery separator prepared by the conventional coating method is 300MPa in the transverse test and 220MPa in the longitudinal test, while the tensile strength of the lithium-ion battery separator prepared by the embodiment of the present application is 350MPa in the transverse test and 265MPa in the longitudinal test. It can be seen that compared with the lithium-ion battery prepared by the conventional coating method, the lithium-ion battery separator prepared by the embodiment of the present application has a better tensile strength.
[0068] The electrochemical performance comparison test process is as follows:
[0069] Different ceramic-coated PE diaphragms were used as diaphragm samples, and the positive electrode active material NCM811, the conductive agent and the binder PVDF were mixed into a slurry in a mass ratio of 8:1:1, and then evenly coated on the aluminum foil with a medical scraper, placed in an electric hot air drying oven, and dried at 120°C for 12 hours. After cooling, the aluminum foil was taken out and punched into electrode sheets with a diameter of 12 mm using a tablet press (the active material content of each electrode sheet was about 3 mg). The metal lithium sheet was used as the negative electrode, and LiPF6 (lithium hexafluorophosphate) / EC (ethylene carbonate) + DMC (ethyl methyl carbonate) + EMC (dimethyl carbonate) with a volume ratio of 1:1:1 of 1 mol / L was used as the electrolyte. CR2032 button batteries were assembled in a glove box filled with argon. The test was carried out at 25°C and the test voltage was 2.0-4.5V.
[0070] like Figure 5 As shown, Figure 5 The comparative results of charge and discharge performance tests of lithium-ion batteries corresponding to lithium-ion battery separators prepared by the present application and conventional coating methods are shown. In the figure, line ① represents the charging performance test curve of the lithium-ion battery prepared by the present application, line ② represents the charging performance test curve of the lithium-ion battery prepared by the conventional coating method, line ③ represents the discharge performance test curve of the lithium-ion battery prepared by the present application, and line ④ represents the discharge performance test curve of the lithium-ion battery prepared by the conventional coating method.
[0071] from Figure 5 It can be seen that, whether it is a charging test or a discharging test, under the same battery capacity conditions, the voltage of the lithium-ion battery prepared by the present application is higher than that of the conventional coating method. Therefore, compared with the lithium-ion battery separator prepared by the conventional coating method, the lithium-ion battery corresponding to the lithium-ion battery separator prepared by the present application has a better charging and discharging performance.
[0072] Figure 6 The cycle performance test results of lithium-ion batteries corresponding to the lithium-ion battery separators prepared by the present application and the conventional coating method are shown. In the figure, line ① represents the cycle performance test curve of the lithium-ion battery prepared by the present application, and line ② represents the cycle performance test curve of the lithium-ion battery prepared by the conventional coating method.
[0073] from Figure 6It can be seen that the lithium-ion battery separator prepared by the embodiment of the present application has a first discharge capacity of 198.8mAh / g at a rate of 0.2C corresponding to the button battery, and after 100 cycles, the button battery capacity retention rate is 95.8%; while the lithium-ion battery separator prepared by the conventional coating method has a first discharge capacity of 192.5mAh / g at a rate of 0.2C corresponding to the button battery, and after 100 cycles, the button battery capacity retention rate is 91.4%. Therefore, compared with the lithium-ion battery separator prepared by the conventional coating method, the lithium-ion battery corresponding to the lithium-ion battery separator prepared by the present application has a better cycle performance.
[0074] In summary, compared with the lithium-ion battery separator prepared by the conventional coating method, the lithium-ion battery separator prepared by the embodiment of the present application has better performance, which effectively solves the technical problems of coating shedding caused by the use of a large amount of adhesive in the conventional coating method and the large electrolyte interface resistance caused by the adhesive. Moreover, in the embodiment of the present application, since the rough inorganic particles are combined with the polymer matrix in a hot melt state, a more stable structural state can be formed, so that the tensile strength of the lithium-ion battery separator matrix is effectively improved; at the same time, the second composite film is cleaned with a lotion, which can effectively remove the residual metal aluminum or free aluminum ions in the ceramic coating, thereby purifying the interface contact between the lithium-ion battery separator and the electrolyte, and increasing the wettability of the lithium-ion battery separator and the electrolyte, thereby correspondingly improving the battery charging and discharging and cycle performance.
[0075] The above is a detailed introduction to the preparation method of a three-dimensional microgap lithium-ion battery separator and a lithium-ion battery provided by the present application. This article uses specific examples to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the core idea of the present application. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present application, several improvements and modifications can be made to the present application, and these improvements and modifications also fall within the scope of protection of the claims of the present application.
Claims
1. A method for preparing a three-dimensional microgap lithium-ion battery separator, characterized in that: The method comprises the following steps: S1, preparing a composite eutectic matrix based on a high molecular polymer and an organic solvent in a preset mass ratio; S2, preparing a first composite film according to the prepared composite eutectic matrix; S3, embedding inorganic particles of a preset particle size onto the first composite film by spraying or rolling, so that both ends of the inorganic particles pass through the first composite film, thereby obtaining a second composite film; S4, washing the second composite film with a washing liquid, and then immersing the washed second composite film in circulating pure water; S5, extracting and forming pores in the washed second composite film by using an extractant to obtain a third composite film having a porous structure; S6. Thermally radiate the third composite film to obtain a three-dimensional microgap lithium-ion battery separator.
2. The method for preparing a three-dimensional microgap lithium-ion battery separator according to claim 1, characterized in that: The step S1 specifically comprises: mixing a high molecular polymer and an organic solvent in a preset mass ratio, and uniformly stirring after reaction and precipitation to obtain a composite eutectic matrix, wherein the high molecular polymer is at least one of polyethylene, polypropylene, and polyimide, and the organic solvent is one of paraffin oil and methyl silicone oil, and the preset mass ratio is 1:2-5.
3. The method for preparing a three-dimensional microgap lithium-ion battery separator according to claim 2, characterized in that: The step S2 is specifically as follows: at 200-300° C., the prepared composite eutectic matrix is stirred and extruded by a twin-screw extruder, then flows out through a mold of a casting machine, and is cooled on a cooling roller to form a film, thereby obtaining a first composite film.
4. The method for preparing a three-dimensional microgap lithium-ion battery separator according to claim 3, characterized in that: The inorganic substance is at least one of aluminum oxide, aluminum hydroxide, zirconium oxide, and magnesium oxide, and the preset particle size of the inorganic particles is 500-1000 nm.
5. The method for preparing a three-dimensional microgap lithium-ion battery separator according to claim 4, characterized in that: The spraying or rolling is double-sided spraying or double-sided rolling, wherein the spraying is one of thermal spraying, cold spraying, ultrasonic spraying and supersonic spraying.
6. The method for preparing a three-dimensional microgap lithium-ion battery separator according to claim 5, characterized in that: The spraying is cold spraying, and the spraying amount of cold spraying is 200-800g / m 2 , the spraying power is 1-5KW, the spraying speed is 100-500mm / s, the powder feeding rate is 10-30g / min, and the spraying pressure is 0.5-1.5MPa.
7. The method for preparing a three-dimensional microgap lithium-ion battery separator according to claim 6, characterized in that: In step S4, the second composite film is cleaned by a cleaning solution. Specifically, an alkaline cleaning solution or an inorganic acid cleaning solution with a mass concentration of 10-30% is obtained, and the second composite film is immersed in the alkaline cleaning solution or the inorganic acid cleaning solution for 10-30 minutes, wherein the temperature of the cleaning solution is controlled to be 20-50°C.
8. The method for preparing a three-dimensional microgap lithium-ion battery separator according to claim 7, characterized in that: The alkaline washing solution is at least one of sodium hydroxide and potassium hydroxide solutions.
9. The method for preparing a three-dimensional microgap lithium-ion battery separator according to claim 8, characterized in that: The extractant is a dichloromethane aqueous solution, and the concentration of the extractant is 500-1000mL / L.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises a three-dimensional microgap lithium-ion battery separator prepared by the method for preparing a three-dimensional microgap lithium-ion battery separator according to any one of claims 1 to 9.
Citation Information
Patent Citations
Lithium battery diaphragm and preparation method thereof
CN106159161A
Diaphragm, preparation method of diaphragm and battery
CN112864531A
Ceramic composite diaphragm and lithium ion battery
CN114374052A
Separator and preparation method therefor, secondary battery using separator, battery module, battery pack, and electrical device
WO2024031652A1