Electroluminescent device, method of manufacturing the same, and electronic device including the same

By using zinc oxide nanoparticles as an electron transport layer in electroluminescent devices, the problem of harmful heavy metal cadmium has been solved, resulting in cadmium-free electroluminescent devices with high brightness and long lifespan, suitable for display devices and electronic devices.

CN118946218APending Publication Date: 2024-11-12SAMSUNG ELECTRONICS CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410580791.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In existing electroluminescent devices, quantum dot materials containing harmful heavy metals such as cadmium are used in the light-emitting layer, which is environmentally unfriendly and results in limited device lifespan. There is a need to develop electroluminescent devices that do not contain harmful heavy metals to improve lifespan and performance.

Method used

Zinc oxide nanoparticles are used as the electron transport layer material. A light-emitting layer is set on the first electrode, a zinc oxide nanoparticle composition is deposited as the electron transport layer, and a second electrode is set on it. The zinc oxide nanoparticles are formed by the reaction of metal precursor, zinc precursor, alkali and metal carbonate compound in an organic solvent, ensuring cadmium-free electroluminescent devices.

Benefits of technology

A cadmium-free electroluminescent device has been developed, featuring high brightness and long lifespan, with a maximum brightness of 85,000 nits and a lifespan of hundreds of hours. Furthermore, it is manufactured using a solution process, which reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946218A_ABST
    Figure CN118946218A_ABST
Patent Text Reader

Abstract

An electroluminescent device, a method of manufacturing the same, and an electronic apparatus including the same are provided. A method of manufacturing the electroluminescent device includes disposing a light emitting layer including semiconductor nanoparticles on a first electrode; depositing a composition comprising zinc oxide nanoparticles comprising a first metal onto the light emitting layer to provide an electron transport layer; and disposing a second electrode on the electron transport layer to provide the electroluminescent device. The first metal includes an alkaline earth metal, zirconium, tungsten, titanium, yttrium, aluminum, gallium, indium, tin, cobalt, vanadium, or a combination thereof. The zinc oxide nanoparticles have a particle size of 1 nm or more and 50 nm or less. Preparation of the zinc oxide nanoparticles includes contacting a first metal precursor, a zinc precursor, a base, and a metal carbonate in an organic solvent to form the zinc oxide nanoparticles.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to and the benefits of Korean Patent Application No. 10-2023-0061932 filed in the Korean Intellectual Property Office on May 12, 2023, and all rights arising therefrom, the contents of which are incorporated herein by reference in their entirety. Technical Field

[0003] The present disclosure relates to light emitting (eg, electroluminescent) devices, methods of manufacturing the same, and display devices including the electroluminescent devices. Background Art

[0004] Semiconductor nanoparticles (e.g., semiconductor nanocrystal particles) with nanometer size can exhibit luminescent properties. For example, quantum dots comprising semiconductor nanocrystals can exhibit quantum confinement effects. When the electrons in an excited state produced by light excitation or an applied voltage move from the conduction band to the valence band, luminescence from semiconductor nanoparticles can occur. By adjusting the size of the semiconductor nanoparticles, the composition of the semiconductor nanoparticles, or a combination thereof, the semiconductor nanoparticles can be configured to emit light in a desired wavelength region.

[0005] The semiconductor nanoparticles may, for example, be used in a light emitting device (eg, an electroluminescent device) or a display device comprising the electroluminescent device.There remains a need for improved light emitting devices. Summary of the invention

[0006] Embodiments provide methods of making light emitting devices that emit light, for example, by applying a voltage to nanostructures (eg, semiconductor nanoparticles such as quantum dots), for example, with or without a separate illuminating light source.

[0007] The embodiment provides a light emitting device manufactured by the method of the embodiment.

[0008] Embodiments provide display devices (e.g., quantum dot-light emitting diode (QD-LED) display devices) that include semiconductor nanoparticles such as quantum dots as components of a light emitting layer in a pixel configuration (e.g., a blue pixel, a red pixel, a green pixel, or a combination thereof).

[0009] In an embodiment, a method of making an electroluminescent device comprises:

[0010] Disposing a light-emitting layer including semiconductor nanoparticles on the first electrode;

[0011] providing zinc oxide nanoparticles (e.g., a plurality of zinc oxide nanoparticles) comprising a first metal;

[0012] A composition comprising the zinc oxide nanoparticles is deposited on the light-emitting layer to provide an electron transport layer (e.g., on the light-emitting layer); and a second electrode is disposed on the electron transport layer to provide the electroluminescent device. The first metal comprises an alkaline earth metal, zirconium, tungsten, titanium, yttrium, aluminum, gallium, indium, tin, cobalt, vanadium, or a combination thereof. The zinc oxide nanoparticles have a particle size (e.g., an average particle size) greater than or equal to about 1 nanometer and less than or equal to about 50 nanometers. The providing of the zinc oxide nanoparticles comprises contacting a first metal precursor, a zinc precursor, an alkali, and a metal carbonate compound in an organic solvent to form the zinc oxide nanoparticles.

[0013] The first metal may include an alkaline earth metal (eg, magnesium), zirconium, tungsten, titanium, yttrium, aluminum, gallium, indium, tin, cobalt, vanadium, or combinations thereof.

[0014] The first metal may include an alkaline earth metal (eg, magnesium); and optionally zirconium, tungsten, titanium, yttrium, aluminum, Ga, In, Sn, Co, V, or a combination thereof.

[0015] The first metal may include magnesium and gallium.

[0016] The providing of zinc oxide nanoparticles or the contacting may include dissolving the first metal precursor and the zinc precursor in the organic solvent to obtain a first solution. The providing of zinc oxide nanoparticles or the contacting may include adding the base and the metal carbonate compound to the organic solvent before dissolving the first metal precursor and the zinc precursor in the organic solvent, or adding the base and the metal carbonate compound to the first solution. The zinc precursor and the first metal precursor may be allowed to react in the presence of the base and the metal carbonate compound.

[0017] The semiconductor nanoparticles or the light emitting layer may not include cadmium.

[0018] The contact (or the reaction between the zinc precursor and the first metal precursor) may be performed in the absence of ethanolamine (e.g., monoethanolamine). The composition or the organic solvent may or may not include a C1-C12 organic amine, an aromatic amine having a phenyl group, or a combination thereof.

[0019] The zinc oxide nanoparticles may or may not further include lithium, sodium, potassium, rubidium, cesium, francium, or a combination thereof.

[0020] The organic solvent may include a C1-C10 alcohol solvent, dimethyl sulfoxide, a C3-C30 hydrocarbon solvent, or a combination thereof.

[0021] The organic solvent may be a solvent mixture including a first solvent and a second solvent, and the first solvent and the second solvent may have a relative polarity difference of greater than or equal to about 0.3 and less than or equal to about 0.9.

[0022] The first solvent may be a C1-C10 alcohol solvent. The second solvent may be a C3-C30 (eg, C15) hydrocarbon solvent (eg, an aliphatic hydrocarbon solvent, an aromatic hydrocarbon solvent, an alicyclic hydrocarbon solvent, or a solvent having a benzene ring in which one or more double bonds are hydrogenated).

[0023] The ratio between the first solvent and the second solvent (as a volume ratio, first solvent:second solvent) may be about 1:0.3 to about 1:3, or about 1:0.5 to about 1:2, or about 1:1.

[0024] The method may further include stirring the solvent mixture of the first solvent and the second solvent, for example, at a predetermined temperature (eg, at a temperature of greater than or equal to about 40° C. and greater than or equal to about 80° C.).

[0025] The stirring may be performed at about 100 rpm or greater (eg, about 300 rpm to about 700 rpm or about 400 rpm to about 500 rpm, or a combination thereof).

[0026] The electron transport layer may not exhibit a peak attributable to rubidium, cesium, or a combination thereof as determined by X-ray photoelectron spectroscopy (XPS) analysis.

[0027] The base can have a pH greater than about 8, greater than or equal to about 8.5, or greater than or equal to about 9. The base can be a strong base.

[0028] The base may include a first base, a second base, or a combination thereof.

[0029] The first base may include an organic base including a C1-C50 organic group.

[0030] The second base may include an inorganic base including an alkali metal or an alkaline earth metal.

[0031] The first base may include a quaternary ammonium compound (e.g., tetraalkylammonium hydroxide). The second base may include a hydroxide of an alkali metal (lithium, sodium, potassium, rubidium, cesium, or francium) or a combination thereof. The base may not include the second base. The base may not include the first base.

[0032] In an embodiment, the second base is present, and the molar ratio between the second base and the first base (the second base:the first base) may be about 1:0 to about 1:10, about 1:0.1 to about 1:10, about 1:0.05 to about 1:6, about 1:0.1 to about 1:4.5, about 1:0.3 to about 1:3, about 1:0.8 to about 1:1.5, about 1:0.9 to about 1:1.3, about 1:1 to about 1:1.25, or a combination thereof.

[0033] A molar ratio of the sum of the first base and the second base to the sum of the zinc precursor and the first metal precursor may be about 1:0.5 to about 1:5, about 1:0.9 to about 1:2, or a combination thereof.

[0034] The metal carbonate compound may include alkali metal carbonate, alkali metal bicarbonate, alkaline earth metal carbonate, or a combination thereof. The metal carbonate compound may include sodium, potassium, rubidium, cesium, francium, or a combination thereof.

[0035] The metal carbonate compound may include a metal having an atomic radius larger than that of zinc.

[0036] In an embodiment, the base may include C1-C30 alkylammonium hydroxide, an alkali metal hydroxide, or a combination thereof, and the metal carbonate compound may include rubidium carbonate, rubidium bicarbonate, cesium carbonate, cesium bicarbonate, or a combination thereof.

[0037] In the method, the zinc oxide nanoparticles may have a core-shell structure.

[0038] In the method of the embodiment, the preparation of the core-shell structured zinc oxide nanoparticles may further include contacting the prepared zinc oxide nanoparticles, an additional metal precursor and a third base in a third solvent to form a layer containing an additional metal (hereinafter, also referred to as a shell layer) on the zinc oxide nanoparticles. The additional metal may include alkaline earth metals, zirconium, tungsten, titanium, yttrium, aluminum, gallium, indium, tin, cobalt, vanadium, or a combination thereof. The additional metal may be the same as or different from the first metal. The contacting may include adding the zinc oxide nanoparticles, the additional metal precursor, and the third base to the third solvent. The contacting may include or involve a reaction of the additional metal precursor.

[0039] The third solvent may include a C1-C10 alcohol solvent, dimethyl sulfoxide, a C3-C30 (eg, C15) hydrocarbon solvent (eg, an aliphatic hydrocarbon solvent, an aromatic hydrocarbon solvent, an alicyclic hydrocarbon solvent, or a solvent having a benzene ring in which one or more double bonds are hydrogenated).

[0040] The third base used to form the additional metal-containing layer may be the same as described herein for the first base and the second base.

[0041] In ultraviolet-visible (UV-Vis) absorption spectroscopy analysis, the zinc oxide nanoparticles may exhibit a first absorption peak within the following range: greater than or equal to about 285 nanometers (nm), greater than or equal to about 290 nm, or greater than or equal to about 292 nm and less than or equal to about 330 nm, or less than or equal to about 310 nm.

[0042] In the UV-Vis absorption spectrum, the zinc oxide nanoparticles may exhibit a valley adjacent to the first absorption peak, and a valley depth (VD) of the valley defined by Equation 1 may be greater than or equal to about 0.03, or greater than or equal to about 0.05 and less than or equal to about 0.2, or less than or equal to about 0.12:

[0043] 1 - (Abs 谷 / Abs 第一 ) = VD (1)

[0044] Among them Abs 第一 is the absorbance at the wavelength of the first absorption peak and Abs 谷 is the absorbance at the lowest point of the valley.

[0045] In the UV-Vis absorption spectrum, the zinc oxide nanoparticles may exhibit an X-intercept of less than or equal to about 332 nm, for example, less than or equal to about 331 nm and greater than or equal to about 300 nm.

[0046] In thermogravimetric analysis, the zinc oxide nanoparticles or the electron transport layer may exhibit a weight loss of greater than or equal to about 26 weight percent (wt %), for example, greater than or equal to about 30 wt %, based on the total weight of the zinc oxide nanoparticles or the electron transport layer, at a decomposition temperature of greater than or equal to about 500° C. (or about 600° C.).

[0047] In thermogravimetric analysis, the zinc oxide nanoparticles or the electron transport layer may exhibit the following weight loss at a decomposition temperature of greater than or equal to about 500° C. (or about 600° C.): less than or equal to about 55 wt %, for example, less than or equal to about 45 wt %, less than or equal to about 40 wt %, or less than or equal to about 35 wt %, based on the total weight of the zinc oxide nanoparticles or the electron transport layer.

[0048] In a derivative thermogravimetric analysis curve (DTGA), the zinc oxide nanoparticles or the electron transport layer may exhibit a temperature of maximum weight loss (hereinafter, maximum weight loss temperature) of about 200° C. or more, about 250° C. or more, or about 300° C. or more. The maximum weight loss temperature may be about 400° C. or less, or about 380° C. or less.

[0049] The composition may not include cesium carbonate, rubidium carbonate, lithium carbonate, sodium carbonate, potassium carbonate, or a combination thereof.

[0050] In X-ray photoelectron spectroscopy (XPS) analysis, the zinc oxide nanoparticles may exhibit an O1s peak having a full width at half maximum (FWHM) of less than about 4 electron volts (eV), less than or equal to about 3.5 eV, less than or equal to about 3 eV, or less than or equal to about 2.9 eV.

[0051] The O1s peak may have a half width at half maximum (HWHM) of less than or equal to about 2.5 eV, or less than or equal to about 1.9 eV.

[0052] In an embodiment, the electroluminescent device comprises:

[0053] a first electrode and a second electrode spaced apart from each other;

[0054] a light emitting layer disposed between the first electrode and the second electrode; and

[0055] An electron transport layer is provided between the light emitting layer and the second electrode,

[0056] wherein the light-emitting layer comprises semiconductor nanoparticles,

[0057] Wherein the electron transport layer comprises zinc oxide nanoparticles described herein. The zinc oxide nanoparticles further comprise a first metal. The first metal comprises an alkaline earth metal, zirconium, tungsten, titanium, yttrium, aluminum, gallium, indium, tin, cobalt, vanadium, or a combination thereof. The first metal may comprise an alkaline earth metal, and optionally zirconium, tungsten, titanium, yttrium, aluminum, gallium, indium, tin, cobalt, vanadium, or a combination thereof. The zinc oxide nanoparticles have a size greater than or equal to about 1 nanometer and less than or equal to about 50 nanometers. In an X-ray photoelectron spectroscopy (XPS) analysis of the zinc oxide nanoparticles, the O1s XPS intensity spectrum has a full width at half maximum (FWHM) of 3 eV or less. The light emitting layer is configured to emit a first light, and the electroluminescent device is configured to exhibit a light intensity greater than or equal to about 60,000 candela / square meter (cd / m 2 , nits) maximum brightness.

[0058] The zinc oxide nanoparticles can be prepared by the methods described herein.

[0059] The O1s XPS intensity spectrum may have a full width at half maximum (FWHM) of less than or equal to about 2.3 eV, or less than or equal to about 2.1 eV. The O1s XPS intensity spectrum may have a full width at half maximum of greater than or equal to about 1 eV, or greater than or equal to about 1.5 eV.

[0060] The O1s XPS intensity spectrum may have a half width at half maximum (HWHM) of less than or equal to about 2.5 eV, less than or equal to about 1.9 eV, less than or equal to about 1.2 eV, or less than or equal to about 1.1 eV.

[0061] The maximum brightness of the electroluminescent device may be greater than or equal to about 85,000 nits.

[0062] In the O1s XPS intensity spectrum, a ratio of an intensity at 530 eV to a maximum intensity may be less than or equal to about 0.3:1, less than or equal to about 0.25:1, or less than or equal to about 0.22:1.

[0063] The O1s XPS intensity spectrum may present a first peak corresponding to the metal oxide and a second peak corresponding to the oxygen vacancy, wherein the binding energy of the first peak may be greater than the binding energy of the second peak, and the ratio of the maximum intensity of the first peak to the maximum intensity of the second peak (maximum intensity of the first peak: maximum intensity of the second peak) may be less than or equal to about 0.55:1.

[0064] In the O1s XPS intensity spectrum, a binding energy at a maximum intensity of the first peak may be greater than or equal to about 525 eV, greater than or equal to about 530 eV and less than or equal to about 540 eV, or less than or equal to about 535 eV.

[0065] In the O1s XPS intensity spectrum, a binding energy at a maximum intensity of the second peak may be greater than or equal to about 525 eV, greater than or equal to about 530 eV and less than or equal to about 540 eV, or less than or equal to about 535 eV.

[0066] As determined by XPS analysis, the Zn2p XPS intensity spectrum of the zinc oxide nanoparticles may have a maximum intensity of a peak corresponding to Zn2p located at a binding energy in the range of greater than or equal to about 1040 eV and less than or equal to about 1050 eV, greater than or equal to about 1042 eV and less than or equal to about 1047.5 eV, or greater than or equal to about 1042.5 eV and less than or equal to about 1045 eV.

[0067] The electron transport layer of the electroluminescent device may not exhibit a peak attributable to rubidium, cesium, or a combination thereof as determined by X-ray photoelectron spectroscopy (XPS) analysis.

[0068] The electron transport layer or the zinc oxide nanoparticles may or may not include an alkali metal (e.g., rubidium). In an embodiment, the electron transport layer or the zinc oxide nanoparticles may or may not include lithium, potassium, rubidium, cesium, or a combination thereof. In an example, the electron transport layer or the zinc oxide nanoparticles may further include rubidium, and in an XPS analysis, the electron transport layer or the zinc oxide nanoparticles may present a peak of Rb3p in the range of greater than or equal to about 230 eV and less than or equal to about 245 eV or greater than or equal to about 230 eV and less than or equal to about 240 eV.

[0069] The first metal may include magnesium and optionally gallium.

[0070] In the zinc oxide nanoparticles, the molar ratio of magnesium to zinc may be less than or equal to about 0.5: 1, less than or equal to about 0.25: 1, less than or equal to about 0.14: 1, or less than or equal to about 0.13: 1. In the zinc oxide nanoparticles, the molar ratio of magnesium to zinc may be greater than or equal to about 0.01: 1, greater than or equal to about 0.07: 1, greater than or equal to about 0.1: 1, greater than or equal to about 0.12: 1, or greater than or equal to about 0.15: 1.

[0071] In the zinc oxide nanoparticles, the amount of gallium may be greater than or equal to about 3 mol% (mol%), greater than or equal to about 3.5 mol% and less than or equal to about 25 mol%, less than or equal to about 19 mol%, or less than or equal to about 17.5 mol%, based on the total moles of zinc, magnesium, and gallium. In the zinc oxide nanoparticles, the gallium content may be greater than or equal to about 10 mol%, greater than or equal to about 12 mol% and less than or equal to about 16 mol%, based on the total moles of zinc, magnesium, and gallium.

[0072] In the zinc oxide nanoparticles, a molar ratio of gallium to zinc (Ga:Zn) may be greater than or equal to about 0.03:1, greater than or equal to about 0.04:1, greater than or equal to about 0.08:1, greater than or equal to about 0.1:1, greater than or equal to about 0.15:1, greater than or equal to about 0.18:1, greater than or equal to about 0.19:1, or greater than or equal to about 0.2: 1. In the zinc oxide nanoparticles, a molar ratio of gallium to zinc (Ga:Zn) may be less than or equal to about 0.3:1, less than or equal to about 0.25:1, less than or equal to about 0.23:1, or less than or equal to about 0.21:1.

[0073] In the zinc oxide nanoparticles, a molar ratio of gallium to magnesium (Ga:Mg) may be greater than or equal to about 0.3:1, greater than or equal to about 0.32:1, greater than or equal to about 0.5:1, greater than or equal to about 0.7:1, greater than or equal to about 1:1, greater than or equal to about 1.5:1, greater than or equal to about 1.9:1, or greater than or equal to about 2: 1. In the zinc oxide nanoparticles, a molar ratio of gallium to magnesium (Ga:Mg) may be less than or equal to about 2.8:1, less than or equal to about 2.7:1, less than or equal to about 2.5:1, less than or equal to about 2.4:1, less than or equal to about 2:1, less than or equal to about 1.7:1, less than or equal to about 1.4:1, or less than or equal to about 0.9:1.

[0074] In the zinc oxide nanoparticles, a molar ratio of the sum of magnesium and gallium to zinc [(Mg+Ga):Zn] may be greater than or equal to about 0.15:1, greater than or equal to about 0.18:1, greater than or equal to about 0.22:1, greater than or equal to about 0.24:1, greater than or equal to about 0.3:1, or greater than or equal to about 0.35:1. In the zinc oxide nanoparticles, a molar ratio of the sum of magnesium and gallium to zinc [(Mg+Ga):Zn] may be less than or equal to about 0.5:1, less than or equal to about 0.45:1, less than or equal to about 0.4:1, less than or equal to about 0.35:1, less than or equal to about 0.31:1, less than or equal to about 0.29:1, less than or equal to about 0.26:1, less than or equal to about 0.23:1, or less than or equal to about 0.2:1.

[0075] The zinc oxide nanoparticles may include a core comprising Zn 1-x M x O (wherein M is Mg, Ca, Zr, W, Li, Ti, Y, Al, or a combination thereof, and 0≤x≤0.5); and a gallium oxide shell disposed on the core. In the above formula, x may be greater than 0, greater than or equal to about 0.01, greater than or equal to about 0.03, greater than or equal to about 0.05, greater than or equal to about 0.1, or greater than or equal to about 0.15. x may be less than or equal to about 0.45, or less than or equal to about 0.4.

[0076] In the zinc oxide nanoparticles, the gallium oxide shell may have a thickness of less than or equal to about 1 nm, or less than or equal to about 0.5 nm.

[0077] The size or average size (hereinafter referred to as size) of the zinc oxide nanoparticles may be greater than or equal to about 3 nm. The size of the zinc oxide nanoparticles may be less than or equal to about 25 nm, less than or equal to about 10 nm, less than or equal to about 8 nm, less than or equal to about 5 nm, or less than or equal to about 4 nm.

[0078] The thickness of the electron transport layer may be greater than or equal to about 5 nm. The thickness of the electron transport layer may be less than or equal to about 70 nm.

[0079] The electron transport layer may be adjacent to the light emitting layer (e.g., directly disposed on the light emitting layer). The electroluminescent device may further include a hole auxiliary layer between the light emitting layer and the first electrode. The hole auxiliary layer may include a hole transport layer (e.g., including an organic compound), a hole injection layer, or a combination thereof.

[0080] The semiconductor nanoparticles or the light emitting layer may not include cadmium, lead, mercury, or a combination thereof.

[0081] The semiconductor nanoparticles may include: a first semiconductor nanocrystal including (zinc chalcogenide including) zinc, selenium, and tellurium; and a second semiconductor nanocrystal including zinc chalcogenide, the second semiconductor nanocrystal being different from the first semiconductor nanocrystal.

[0082] The semiconductor nanoparticles may include: a first semiconductor nanocrystal including (a Group III-V compound or an indium phosphide compound including) indium, phosphorus, and optionally zinc; and a second semiconductor nanocrystal including zinc chalcogenide and different from the first semiconductor nanocrystal.

[0083] The semiconductor nanoparticles may include zinc chalcogenide, the zinc chalcogenide may include tellurium, and the semiconductor nanoparticles may be configured to emit blue light or green light.

[0084] The electroluminescent device or the light-emitting layer may be configured to emit green light when a voltage is applied. The electroluminescent device or the light-emitting layer may be configured to emit blue light when a voltage is applied. The electroluminescent device or the light-emitting layer may be configured to emit red light when a voltage is applied.

[0085] The electroluminescent device has a maximum external quantum efficiency of about 6% or more, about 7% or more, about 8% or more, about 9% or more, about 10% or more, about 11% or more, about 12% or more, about 13% or more, or about 14% or more. The maximum external quantum efficiency may be about 6% to about 50%, or about 10% to about 40%.

[0086] The electroluminescent device may have a maximum brightness of greater than or equal to about 65,000 candelas per square meter (cd / m 2 ), greater than or equal to about 70,000 cd / m 2 , greater than or equal to about 80,000cd / m 2, greater than or equal to approximately 85,000 cd / m 2 , greater than or equal to about 90,000cd / m 2 , greater than or equal to approximately 100,000 cd / m 2 , or greater than or equal to about 300,000 cd / m 2 The maximum brightness may be less than or equal to about 5,000,000 cd / m 2 , less than or equal to approximately 3,000,000 cd / m 2 , less than or equal to approximately 2,000,000 cd / m 2 , or less than or equal to about 1,000,000 cd / m 2 .

[0087] The electroluminescent device may exhibit a T50 of about 90 hours or more, about 100 hours or more, about 150 hours or more, about 250 hours or more, about 261 hours or more, about 265 hours or more, about 270 hours or more, about 300 hours or more, about 350 hours or more, about 400 hours or more, about 480 hours or more, about 500 hours or more, or about 600 hours or more (e.g., when measured at an initial brightness of 650 nits). The T50 may be about 150 hours to about 2000 hours, about 250 hours to about 1500 hours, about 300 hours to about 1000 hours, or a combination thereof.

[0088] The electroluminescent device may exhibit a T90 of about 10 hours or more, about 20 hours or more, about 30 hours or more, about 40 hours or more, about 50 hours or more, about 60 hours or more, about 70 hours or more, about 80 hours or more, about 90 hours or more, about 100 hours or more, or about 255 hours or more (e.g., when driven at an initial brightness of 650 nits). The T90 of the electroluminescent device may be about 10 hours to about 800 hours, about 50 hours to about 500 hours, about 80 hours to about 300 hours, or a combination thereof.

[0089] In an embodiment, a display device or an electronic apparatus may include the electroluminescent device.

[0090] The display device or electronic apparatus may include (or may be) an augmented reality (AR) device, a virtual reality (VR) device, a handheld terminal (e.g., a device), a monitor, a notebook computer, a television, an electronic display panel, a camera, an electronic display component for an autonomous vehicle or an electric vehicle.

[0091] Disclosed herein are electroluminescent devices that exhibit desired levels of electroluminescent properties and improved lifetimes. The electroluminescent device of an embodiment includes zinc oxide nanoparticles in an electron transport layer, and the zinc oxide nanoparticles may exhibit, for example, an increased weight loss of greater than 25% or greater than 32%, such as the weight of decomposed components such as organic matter, as determined by thermogravimetric analysis (TGA), and zinc defects on the surface of the zinc oxide nanoparticles may be passivated, for example, by carbonate ions to an increased level. The electroluminescent device of an embodiment may exhibit reduced leakage current and reduced hole leakage, and it may maintain an initial drive voltage within a desired range.

[0092] The zinc oxide nanoparticles included in the electron transport layer of the embodiment may also be used to manufacture a panel through an inkjet process.

[0093] In an embodiment, the zinc oxide nanoparticles include a core and a shell disposed on the core. The core of the zinc oxide nanoparticles includes Zn 1-x M x O, wherein M is Mg, Ca, Zr, W, Li, Ti, Y, Al, or a combination thereof, and 0≤x≤0.5, and the shell comprises an oxide layer of an alkaline earth metal, zirconium, tungsten, titanium, yttrium, aluminum, gallium, indium, tin, cobalt, vanadium, or a combination thereof. BRIEF DESCRIPTION OF THE DRAWINGS

[0094] The above and other advantages and features of the present disclosure will become more apparent by further describing in detail exemplary embodiments of the present disclosure with reference to the accompanying drawings, in which:

[0095] Figure 1 To illustrate the full width at half maximum and half width at half maximum of intensity versus binding energy in electron volts (eV),

[0096] Figure 2 A schematic cross-sectional view illustrating one embodiment of a quantum dot light emitting diode ("QD-LED") device;

[0097] Figure 3A A schematic cross-sectional view illustrating another embodiment of a QD-LED device;

[0098] Figure 3B A schematic cross-sectional view illustrating another embodiment of a QD-LED device;

[0099] Figure 3C A schematic plan view for explaining an embodiment of a display panel;

[0100] Figure 3D To illustrate the Figure 3C A cross-sectional view of a display panel;

[0101] Figure 4 A graph illustrating UV-Vis absorbance (arbitrary unit, au) versus wavelength (nanometers, nm) of the zinc oxide nanoparticles prepared in Preparation Example 1 and Preparation Example 2 as a result of UV-Vis absorption spectroscopy analysis thereof;

[0102] Figure 5A A graph illustrating the weight (percent, %) of the zinc oxide nanoparticles manufactured in Comparative Preparation Example 1, Preparation Example 1, and Preparation Example 2 versus temperature (° C.) as a result of thermogravimetric analysis thereof (ie, TGA curve);

[0103] Figure 5B A graph illustrating derivative weight loss (percent / °C, % / °C) versus temperature (°C) of the zinc oxide nanoparticles prepared in Comparative Preparation Example 1, Preparation Example 1, and Preparation Example 2 as a result of thermogravimetric analysis thereof (ie, DTGA curve).

[0104] Figure 6 A graph showing the photoluminescence intensity (arbitrary unit) versus wavelength (nm) of the zinc oxide nanoparticles prepared in Comparative Preparation Example 1 and Preparation Example 1 as a result of photoluminescence analysis (eg, showing a defect emission peak);

[0105] Fig. 7A A graph showing normalized intensity (arbitrary unit) of O1s XPS spectra of zinc oxide nanoparticles prepared in Comparative Preparation Example 1 and Preparation Example 1 versus binding energy (electron volt, eV) as XPS analysis results thereof;

[0106] Figure 7B A graph showing normalized intensity (arbitrary unit) versus binding energy (electron volt, eV) of the Zn2p1 / 2 XPS spectra of the zinc oxide nanoparticles prepared in Comparative Preparation Example 1 and Preparation Example 1 as XPS analysis results thereof;

[0107] Figure 8 To illustrate the logarithmic current (mA / cm 2 ) versus voltage (volts, V); and

[0108] Fig. 9 A graph of photoluminescence intensity (arbitrary unit) versus wavelength (nm) for Experimental Example 1 is provided as a result of a PL quenching experiment as follows: After the zinc oxide nanoparticles of Preparation Example 1 and the zinc oxide nanoparticles of Preparation Comparative Example 1 were each provided on a quantum dot emission layer, photoluminescence characteristics were analyzed. DETAILED DESCRIPTION

[0109] The advantages and characteristics of the present disclosure, and methods for implementing the same will become clear with reference to the following example embodiments and the accompanying drawings attached hereto. However, the present invention can be embodied in many different forms, and the embodiments should not be construed as being limited to the embodiments set forth herein. On the contrary, these embodiments are provided so that the present disclosure will be thorough and complete, and the scope of the present invention will be fully conveyed to those skilled in the art. Similar reference numerals refer to similar elements throughout.

[0110] In order to clearly illustrate the present disclosure, parts that are not related to the description are omitted, and the same reference numerals are always assigned to the same or similar elements in the specification. In the accompanying drawings, for clarity, the thickness of the layer, film, panel, region, etc. is magnified. And in the accompanying drawings, for ease of description, the thickness of some layers and regions is magnified. Therefore, the embodiments described herein should not be interpreted as being limited to the specific shapes of the regions as shown in this article, but include deviations in shape caused by, for example, manufacturing. For example, an area illustrated or described as flat may typically have rough and / or nonlinear features. In addition, the sharp corners illustrated may be rounded. Therefore, the areas shown in the figures are schematic in nature, and their shapes are not intended to illustrate the precise shape of the region and are not intended to limit the scope of the claims.

[0111] In addition, it will be understood that when an element such as a layer, film, region, or substrate is referred to as being "on" another element, it can be directly on the other element or intervening elements may also be present. In contrast, when an element is referred to as being "directly on" another element, there are no intervening elements. In addition, being disposed "on" a reference portion means being disposed above or below the reference portion and does not necessarily mean "over..."

[0112] In addition, relative terms such as "lower" or "bottom" and "upper" or "top" may be used herein to describe the relationship of one element to another element as shown in the figure. It will be understood that in addition to the orientation depicted in the figure, relative terms are also intended to cover different orientations of the device. For example, if the device in one of the figures is turned over, the element described as being on the "lower" side of the other element will be oriented on the "upper" side of the other element. Therefore, depending on the specific orientation of the figure, the term "lower" can cover both "lower" and "upper" orientations. Similarly, if the device in one of the figures is turned over, the element described as "below" or "below" the other element will be oriented "above" the other element. Therefore, the term "below..." or "below..." can cover both "above..." and "below..." orientations.

[0113] It will be understood that although the terms "first", "second", "third", etc. may be used herein to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings herein, the "first element", "component", "region", "layer" or "part" discussed below may be referred to as a second element, component, region, layer or part.

[0114] The terms used herein are only used for the purpose of describing specific embodiments and are not intended to be limiting. As used herein, the singular forms "a, an" and "said" are intended to include plural forms (including "at least one") unless the content clearly indicates otherwise. "At least one" should not be interpreted as limiting "a, an". "Or" means "and / or".

[0115] As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items. It will be further understood that the terms "include" or "comprises" when used in this specification indicate the presence of the stated features, regions, wholes, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more additional features, regions, wholes, steps, operations, elements, components, and / or their collections.

[0116] As used herein, the term "cross-section" means a situation in which a cross section of a given object is cut, for example, in a substantially vertical direction and viewed in a transverse direction.

[0117] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present disclosure belongs. It will be further understood that terms, such as those defined in commonly used (e.g., non-technical) dictionaries, should be interpreted as having a meaning consistent with their meaning in the context of the present disclosure and the relevant art, and will not be interpreted in an idealized or overly formal sense, unless clearly so defined herein.

[0118] As used herein, the value of a work function, conduction band, valence band, lowest unoccupied molecular orbital (LUMO), or highest occupied molecular orbital (HOMO) energy level is expressed as an absolute value from a vacuum energy level. In addition, when a work function or energy level is referred to as "deep," "high," or "large," the work function or energy level has a large absolute value based on a vacuum energy level of "0 electron volts (eV)," and when a work function or HOMO energy level is referred to as "shallow," "low," or "small," the work function or energy level has a small absolute value based on a vacuum energy level of "0 eV." In one aspect, the work function herein refers to the minimum energy required to move an electron from a solid (e.g., a metal surface) to a point in the vacuum exterior of the surface.

[0119] As used herein, average (value) may be a mean or a median. In an embodiment, average (value) may be a mean.

[0120] As used herein, the term "peak emission wavelength" is the wavelength at which a given emission spectrum of light reaches its maximum.

[0121] As used herein, the term "first absorption peak" refers to the main exciton peak that appears first from the longest wavelength region of the UV-vis absorption spectrum (i.e., appears in the lowest energy region of the UV-Vis absorption spectrum), and the term "first absorption peak wavelength" or "wavelength of the first absorption peak" refers to the wavelength at which the first absorption peak reaches maximum intensity.

[0122] As used herein, the term "Group" may refer to a Group of the periodic table.

[0123] As used herein, “Group I” refers to Group IA and Group IB, and examples may include Li, Na, K, Rb, and Cs, but are not limited thereto.

[0124] As used herein, “Group II” refers to Group IIA and Group IIB, and examples of Group II metals may be Cd, Zn, Hg, and Mg, but are not limited thereto.

[0125] As used herein, “Group III” refers to Group IIIA and Group IIIB, and examples of Group IIIA metals may be Al, In, Ga, and Tl, and examples of Group IIIB may be scandium, yttrium, etc., but are not limited thereto.

[0126] As used herein, “Group IV” refers to Group IVA and Group IVB, and examples of Group IVA metals may be Si, Ge, and Sn, and examples of Group IVB metals may be titanium, zirconium, hafnium, etc., but are not limited thereto.

[0127] As used herein, "Group V" includes Group VA and includes nitrogen, phosphorus, arsenic, antimony, and bismuth, but is not limited thereto.

[0128] As used herein, "Group VI" includes Group VIA and includes sulfur, selenium, and tellurium, but is not limited thereto.

[0129] As used herein, "metal" includes semi-metals such as Si.

[0130] As used herein, the number of carbon atoms in a group or molecule may be indicated as a subscript (e.g., C 6-50 ) or as a non-subscript (e.g., C6-C50).

[0131] As used herein, when no definition is otherwise provided, "substituted" refers to a compound or group in which at least one hydrogen is replaced by a C1-C30 alkyl, C2-C30 alkenyl, C2-C30 alkynyl, C6-C30 aryl, C7-C30 alkylaryl, C1-C30 alkoxy, C1-C30 heteroalkyl, C3-C30 heteroaryl, C3-C30 cycloalkyl, C3-C15 cycloalkenyl, C6-C30 cycloalkynyl, C2-C30 heterocycloalkyl, halogen (-F, -Cl, -Br, or -I), hydroxyl (-OH), nitro (-NO), or 2 ), cyano (-CN), amino (-NRR', wherein R and R' are each independently hydrogen or C1-C6 alkyl), azido (-N 3 ), amidino (-C(=NH)NH 2 ), hydrazino (-NHNH 2 ), hydrazone (=N(NH 2 )), aldehyde group (-C(=O)H), carbamoyl group (-C(O)NH 2 ), thiol group (-SH), ester group (-C(=O)OR, wherein R is C1-C6 alkyl or C6-C12 aryl), carboxyl group (-COOH) or its salt (-C(=O)OM, wherein M is an organic or inorganic cation), sulfonic acid group (-SO 3 H) or its salt (-SO 3 M, where M is an organic or inorganic cation), a phosphate group (-PO 3 H 2 ) or its salt (-PO 3 MH or -PO 3 M 2 , wherein M is an organic or inorganic cation), or a combination thereof.

[0132] As used herein, the term "metal carbonate compound" may include or refer to "metal carbonate," "metal bicarbonate," or both.

[0133] As used herein, when no definition is provided in addition, "hydrocarbon" or "hydrocarbon group" refers to a compound or group (e.g., alkyl, alkenyl, alkynyl, or aryl) comprising carbon and hydrogen. The hydrocarbon group may be a monovalent group formed by removing a hydrogen atom (e.g., one or more hydrogen atoms) from an alkane, alkene, alkyne, or aromatic hydrocarbon, or a group having a valence greater than 1. In the hydrocarbon or hydrocarbon group, a methylene group (e.g., at least one methylene group) may be replaced by an oxygen moiety, a carbonyl moiety, an ester moiety, -NH-, or a combination thereof. Unless otherwise indicated to the contrary, the hydrocarbon or hydrocarbon group (alkyl, alkenyl, alkynyl, or aryl) may have 1-60, 2-32, 3-24, or 4-12 carbon atoms.

[0134] As used herein, when no definition is otherwise provided, "alkyl" refers to a linear or branched saturated monovalent hydrocarbon group (methyl, ethyl, hexyl, etc.). In embodiments, the alkyl group may have 1-50 carbon atoms, or 1-18 carbon atoms, or 1-12 carbon atoms.

[0135] As used herein, when no definition is otherwise provided, "alkenyl" refers to a linear or branched monovalent hydrocarbon group having a carbon-carbon double bond. In an embodiment, the alkenyl group may have 2-50 carbon atoms, or 2-18 carbon atoms, or 2-12 carbon atoms.

[0136] As used herein, when no definition is otherwise provided, "alkynyl" refers to a linear or branched monovalent hydrocarbon group having a carbon-carbon triple bond. In embodiments, the alkynyl group may have 2-50 carbon atoms, or 2-18 carbon atoms, or 2-12 carbon atoms.

[0137] As used herein, when no definition is otherwise provided, "aryl" refers to a group (e.g., phenyl or naphthyl) formed by removing hydrogen (e.g., at least one hydrogen) from an aromatic hydrocarbon. In an embodiment, the aryl group may have 6-50 carbon atoms, 6-18 carbon atoms, or 6-12 carbon atoms.

[0138] As used herein, when no definition is otherwise provided, "hetero" is meant to include 1 to 3 heteroatoms such as N, O, S, Si, P, or combinations thereof.

[0139] As used herein, when a definition is not otherwise provided, "alkoxy" refers to an alkyl group attached to an oxygen group (eg, alkyl-O-) such as methoxy, ethoxy, or sec-butoxy.

[0140] As used herein, when no definition is otherwise provided, "amine" is an amine composed of NR 3 A compound represented by wherein each R is independently hydrogen, C1-C12 alkyl, C7-C20 alkylaryl, C7-C20 arylalkyl, or C6-C18 aryl.

[0141] As used herein, the expression "does not include cadmium (or other harmful heavy metals)" may refer to a situation in which the concentration of cadmium (or another heavy metal considered harmful) may be less than or equal to about 100 parts per million by weight (ppmw), less than or equal to about 50 ppmw, less than or equal to about 10 ppmw, less than or equal to about 1 ppmw, less than or equal to about 0.1 ppmw, less than or equal to about 0.01 ppmw, or zero. In embodiments, cadmium (or other toxic heavy metals) may be substantially (essentially) absent, or, if present, the amount of cadmium (or other toxic heavy metals) may be less than or equal to the detection limit of a given analytical tool (e.g., an inductively coupled plasma atomic emission spectrometry instrument) or as an impurity level.

[0142] Unless otherwise stated, the numerical ranges described herein include endpoints. Unless otherwise stated, the numerical ranges described herein include any real number within and including the endpoints of the stated range. In this specification, numerical endpoints or upper or lower limits (e.g., described as "greater than or equal to a value", "at least a value" or "less than or equal to a value" or described with "from" or "to") can be used to form a numerical range for a given feature. In other words, the upper and lower endpoints described for various numerical values ​​can be independently combined to provide a range.

[0143] As used herein, "about" includes the stated value and means within an acceptable range of deviation for the particular value as determined by one of ordinary skill in the art taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" can mean within one or more standard deviations, or within ±5%, relative to the stated value.

[0144] As used herein, nanoparticles are structures with regions or characteristic dimensions (e.g., at least one region or characteristic dimension) having nanoscale dimensions. In an embodiment, the scale (or average scale) of the nanostructure is less than or equal to about 500 nanometers (nm), less than or equal to about 300nm, less than or equal to about 250nm, less than or equal to about 150nm, less than or equal to about 100nm, less than or equal to about 50nm, or less than or equal to about 30nm, and may be greater than about 0.1nm or about 1nm. In an embodiment, nanoparticles may have any suitable shape. Nanoparticles (e.g., semiconductor nanoparticles or metal oxide nanoparticles) may include nanowires, nanorods, nanotubes, branched nanostructures, nano tetrapods, nano tripods, nano bipods, nanodots, multi-foot shapes such as at least two feet, and are not limited thereto. Nanoparticles may be substantially crystalline, substantially monocrystalline, polycrystalline, (e.g., at least partially) amorphous, or a combination thereof.

[0145] In an embodiment, semiconductor nanoparticles such as quantum dots may present quantum confinement or exciton confinement. As used herein, the term "quantum dot" or "semiconductor nanostructure" is not limited in terms of its shape unless otherwise defined. Semiconductor nanoparticles or quantum dots may have a size smaller than the Bohr excitation diameter of a bulk crystalline material with the same composition, and may present a quantum confinement effect. By controlling the size of the nanocrystals acting as emission centers, semiconductor nanoparticles or quantum dots may emit light corresponding to their band gap energy.

[0146] As used herein, the term "T50" is the time (hours, hr) taken for the brightness (e.g., luminance) of a given device to decrease to 50% of the initial brightness (100%) when the given device is initially driven, for example, operated, at a predetermined initial brightness (e.g., 650 nits).

[0147] As used herein, the term "T90" is the time (hours, hrs) taken for the brightness (e.g., luminance) of a given device to decrease to 90% of the initial brightness (100%) when the given device is initially driven at a predetermined initial brightness (e.g., 650 nits).

[0148] As used herein, the phrase "external quantum efficiency (EQE)" is the ratio of the number of photons emitted from a light emitting device (LED), such as an electroluminescent device, to the number of electrons passing through the device, and can be a measure of how efficiently a given device converts electrons into photons and allows photons to escape. EQE can be determined by the following equation:

[0149] EQE = (injection efficiency) x ((solid-state) quantum yield) x (extraction efficiency)

[0150] Where the injection efficiency is the fraction of electrons passing through the device that are injected into the active region, the quantum yield is the fraction of all electron-hole recombination in the active region that are radiative and produce photons, and the extraction efficiency is the fraction of photons generated in the active region that escape from a given device.

[0151] As used herein, maximum EQE is the maximum value of EQE.

[0152] As used herein, maximum brightness is the highest value of brightness for a given device.

[0153] As used herein, the phrase quantum efficiency can be used interchangeably with the phrase quantum yield. In an embodiment, quantum efficiency can be a relative quantum yield or an absolute quantum yield, such as it can be easily measured by any suitable (e.g., commercially available) equipment. Quantum efficiency (or quantum yield) can be measured in a solution state or solid state (with a complex). In an embodiment, "quantum yield (or quantum efficiency)" can be the ratio of photons emitted (e.g., by a group of nanostructures or nanostructures) to photons absorbed. In an embodiment, quantum efficiency can be measured by any suitable method. For example, there can be two methods for measuring fluorescence quantum yield or efficiency: an absolute method and a relative method.

[0154] The absolute method directly obtains the quantum yield by detecting the fluorescence of all samples using an integrating sphere. In the relative method, the fluorescence intensity of a standard sample (e.g., a standard dye) can be compared with the fluorescence intensity of an unknown sample to calculate the quantum yield of the unknown sample. Coumarin 153, coumarin 545, rhodamine 101 inner salt, anthracene, and rhodamine 6G can be used as standard dyes depending on their photoluminescence (PL) wavelength, but are not limited thereto.

[0155] As used herein, the full width at half maximum (FWHM) is the difference between two values ​​of the independent variable at which the dependent variable is equal to half of its maximum value. The FWHM is the width of the spectral curve measured between those points that are half of the maximum amplitude on the y-axis. The half width at half maximum (HWHM) is the right half of the FWHM of a given peak (e.g., a spectral peak). For example, the right half of the FWHM can be measured between the binding energy at the maximum peak intensity (1) and the binding energy at half of the maximum peak intensity in the lower energy region (2) (see Figure 1 ).

[0156] The band gap energy of semiconductor nanoparticles or quantum dots can change with the size and composition of nanocrystals. For example, as the size of semiconductor nanoparticles increases, the band gap energy of semiconductor nanoparticles or quantum dots can be reduced, for example, narrowed, and semiconductor nanoparticles or quantum dots can emit light with increased wavelength. Semiconductor nanocrystals can be used as luminescent materials in various fields, for example, in display devices, energy devices, or bioluminescent devices.

[0157] An electroluminescent device based on semiconductor nanoparticles (hereinafter, also referred to as QD-LED) can emit light by applying a voltage and includes semiconductor nanoparticles or quantum dots as a light-emitting material. QD-LED is different from an organic light-emitting diode (OLED) in terms of a specific light-emitting principle, and can present light emission with more desirable optical properties such as higher color (e.g., red, green, and blue) purity and improved color reproducibility and has attracted attention as a material for next-generation display devices. A method for manufacturing QD-LED may include a solution process, which can reduce manufacturing costs. In addition, the semiconductor nanoparticles in the QD-LED may be based on inorganic materials to promote improved display (luminescence) stability over time. However, it is still desirable to develop technologies that can further improve the device properties and life characteristics of QD-LED.

[0158] In an embodiment, the structure of the QD-LED includes a light-emitting layer (EML) disposed between two electrodes (e.g., an anode and a cathode), and one or more auxiliary layers (including an electron transport layer (ETL) and optionally a hole transport layer (HTL)) provided on the opposite surface of the light-emitting layer, providing charge balance and assisting the operation of the device. In an embodiment, the QD-LED may include an organic or inorganic charge auxiliary layer (e.g., an organic or inorganic hole transport layer). According to an embodiment, the QD-LED may include an inorganic material (e.g., zinc oxide nanoparticles) in an electron auxiliary layer such as an electron transport layer (ETL). In an embodiment of the QD-LED, the electron auxiliary layer containing the inorganic material on the light-emitting layer can be easily formed by a solution process, such as a relatively low temperature (e.g., room temperature) process, and the electron auxiliary layer can provide improved electron mobility. Holes injected from the anode and electrons injected from the cathode can be supplied to the light-emitting layer through the auxiliary layer, and excitons can be formed and light can be emitted therefrom.

[0159] In the light-emitting layer, quantum dots capable of exhibiting electroluminescent properties at practically usable levels may include harmful heavy metals such as cadmium (Cd), lead, mercury, or a combination thereof. Therefore, it is desirable to provide a light-emitting device or display device having a light-emitting layer that is substantially free of harmful heavy metals. In QD-LEDs, currently reported and satisfactory electroluminescent properties are mainly based on LEDs containing cadmium, and there is room for improvement in QD-LED devices that use environmentally friendly quantum dots that do not include cadmium or other harmful heavy metals and, for example, emit blue light.

[0160] In an embodiment of a QD-LED device, zinc oxide nanoparticles prepared by the method of the embodiment and having the characteristics described herein may be included in the electron assist layer, and thus, the QD-LED including cadmium-free semiconductor nanoparticles in the light-emitting layer may exhibit a desired level of electroluminescent properties and improved lifetime.

[0161] In embodiments, an electroluminescent device may be a device configured to emit desired light by application of a voltage (eg, with or without a separate light source).

[0162] In an embodiment, the electroluminescent device includes a first electrode 1 and a second electrode 5 spaced apart from each other (e.g., each having a surface opposite to each other, i.e., each having a surface facing each other); a light-emitting layer 3 disposed between the first electrode 1 and the second electrode 5; and an electron transport layer 4 disposed between the light-emitting layer 3 and the second electrode 5.

[0163] In an embodiment, a method for manufacturing the electroluminescent device comprises:

[0164] Disposing (e.g., forming) a light-emitting layer including semiconductor nanoparticles (e.g., a plurality of semiconductor nanoparticles) on the first electrode;

[0165] providing zinc oxide nanoparticles;

[0166] applying a composition (eg, a coating liquid) including the zinc oxide nanoparticles (eg, a plurality of zinc oxide nanoparticles) onto the light emitting layer to form an electron transport layer, the zinc oxide nanoparticles including a first metal; and

[0167] providing (e.g., forming) a second electrode on the electron transport layer to manufacture the electroluminescent device,

[0168] wherein the first metal comprises an alkaline earth metal, zirconium, tungsten, titanium, yttrium, aluminum, gallium, indium, tin, cobalt, vanadium, or a combination thereof,

[0169] wherein the zinc oxide nanoparticles have a particle size greater than or equal to about 1 nm and less than or equal to about 50 nm,

[0170] wherein providing zinc oxide nanoparticles comprises

[0171] A precursor of the first metal (hereinafter, referred to as a first metal precursor), a zinc precursor, a base, and a metal carbonate compound are contacted in an organic solvent to form the zinc oxide nanoparticles.

[0172] The providing zinc oxide nanoparticles or the contacting may include dissolving the first metal precursor and the zinc precursor in the organic solvent to obtain a first solution.

[0173] The providing zinc oxide nanoparticles or the contacting may include adding the base and the metal carbonate compound to the organic solvent or the first solution.

[0174] The contacting may include a reaction between the zinc precursor and the first metal precursor in the presence of the base and the metal carbonate compound.

[0175] In the method of the embodiment, the composition (e.g., the coating liquid) may be a dispersion in which the zinc oxide nanoparticles are dispersed in an organic solvent. In an embodiment, the dispersion may have a solid dispersed phase and a continuous medium including a liquid. In an embodiment, the dispersion may be a colloidal dispersion in which the dispersed phase has a size of greater than or equal to about 1 nm, such as greater than or equal to about 2 nm, greater than or equal to about 3 nm, greater than or equal to about 4 nm, greater than or equal to about 5 nm, or greater than or equal to about 10 nm and a few micrometers (μm) or less, such as less than or equal to about 2 μm, less than or equal to about 1 μm, less than or equal to about 900 nm, less than or equal to about 800 nm, less than or equal to about 700 nm, less than or equal to about 600 nm, or less than or equal to about 500 nm.

[0176] In an embodiment, the electroluminescent device may further include a hole auxiliary layer 2 (see Figure 2 ). The hole auxiliary layer may include a hole transport layer, a hole injection layer, or a combination thereof. The hole auxiliary layer may include an organic compound.

[0177] In an embodiment, the first electrode or the second electrode comprises an anode or a cathode. In an embodiment, the first electrode may comprise an anode and the second electrode may comprise a cathode. The first electrode may comprise a cathode and the second electrode may comprise an anode. In an embodiment, the second electrode comprises a cathode. In an embodiment of the electroluminescent device, the first electrode 10 or the second electrode 50 may be disposed on a (transparent) substrate 100. The transparent substrate may be a light extraction surface. (See Figure 3A and Figure 3B ). The light-emitting layer may be disposed in a pixel (or sub-pixel) of a display device described herein.

[0178] Reference Figure 3A and 3B In an embodiment of the electroluminescent device, a light emitting layer 30 may be provided between a first electrode (e.g., an anode) 10 and a second electrode (e.g., a cathode) 50. The cathode 50 may include an electron injection conductor. The anode 10 may include a hole injection conductor. The work functions of the electron or hole injection conductors included in the cathode and the anode may be appropriately adjusted and are not particularly limited. For example, the cathode may have a relatively small work function and the anode may have a relatively large work function, or vice versa.

[0179] The electron or hole injection conductor may include a metal-containing material (e.g., a metal, a metal compound, an alloy, or a combination thereof) such as aluminum, magnesium, tungsten, nickel, cobalt, platinum, palladium, calcium, LiF, etc.; a metal oxide such as indium gallium oxide or indium tin oxide (ITO); or a conductive polymer (e.g., having a relatively high work function) such as polyethylenedioxythiophene, but is not limited thereto.

[0180] The first electrode, the second electrode, or a combination thereof may be a light-transmitting electrode or a transparent electrode. In an embodiment, both the first electrode and the second electrode may be light-transmitting electrodes. The first electrode, the second electrode, or a combination thereof may be a patterned electrode.

[0181] The first electrode, the second electrode, or a combination thereof may be disposed on the substrate 100. The substrate 100 may be an insulating substrate. The substrate 100 may be optically transparent (e.g., may have a light transmittance greater than or equal to about 50%, greater than or equal to about 60%, greater than or equal to about 70%, greater than or equal to about 80%, greater than or equal to about 85%, or greater than or equal to about 90% and, for example, less than or equal to about 99%, or less than or equal to about 95%). The substrate may have a transmittance greater than or equal to about 50%, greater than or equal to about 60%, greater than or equal to about 70%, greater than or equal to about 80%, or greater than or equal to about 90% for light emitted from the semiconductor nanoparticles described herein. The substrate 100 may include an area for a blue pixel, an area for a red pixel, an area for a green pixel, or a combination thereof. In an embodiment, a thin film (e.g., film) transistor may be disposed in each area of ​​the substrate, but it is not limited thereto. In an embodiment, a source electrode or a drain electrode of the thin film transistor may be electrically connected to the first electrode or the second electrode.

[0182] The light-transmitting or transparent electrode may be disposed on a (e.g., insulating) transparent substrate. The substrate 100 may be a rigid or flexible substrate. The substrate may include plastic, glass, metal, or a combination thereof. The substrate 100 may be a substrate including an insulating material. The substrate may include: glass; various polymers such as polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycarbonate, and polyacrylate; polysiloxanes (e.g., polydimethylsiloxane (PDMS)); inorganic materials such as Al 2 O 3 or ZnO; or a combination thereof, but not limited thereto. The thickness of the substrate may be appropriately selected in consideration of the substrate material, but is not particularly limited.

[0183] The light-transmitting electrode may include, for example, a transparent conductor such as indium tin oxide (ITO) or indium zinc oxide (IZO), gallium indium tin oxide, zinc indium tin oxide, titanium nitride, polyaniline, LiF / Mg:Ag, etc., or a single-layer or multi-layer metal film, but is not limited thereto. In an embodiment, one of the first electrode or the second electrode may be an opaque electrode, and the opaque electrode may include an opaque conductor such as aluminum (Al), lithium-aluminum (Li:Al) alloy, magnesium-silver (Mg:Ag) alloy, or lithium fluoride-aluminum (LiF:Al).

[0184] The thickness of each electrode (the first electrode, the second electrode, or both) is not particularly limited and can be appropriately selected in consideration of device efficiency. For example, the thickness of the electrode may be greater than or equal to about 5 nm, greater than or equal to about 10 nm, greater than or equal to about 20 nm, greater than or equal to about 30 nm, greater than or equal to about 40 nm, or greater than or equal to about 50 nm. For example, the thickness of the electrode may be less than or equal to about 100 micrometers (μm), less than or equal to about 90 μm, less than or equal to about 80 μm, less than or equal to about 70 μm, less than or equal to about 60 μm, less than or equal to about 50 μm, less than or equal to about 40 μm, less than or equal to about 30 μm, less than or equal to about 20 μm, less than or equal to about 10 μm, less than or equal to about 1 μm, less than or equal to about 900 nm, less than or equal to about 500 nm, or less than or equal to about 100 nm.

[0185] The method of forming the electrode is not particularly limited and may be appropriately selected in consideration of the electrode material. In an embodiment, the electrode may be formed by deposition, coating, or a combination thereof, but is not limited thereto.

[0186] A light-emitting layer 3 or 30 may be provided between the first electrode 1 and the second electrode 5 (e.g., the anode 10 and the cathode 50). The light-emitting layer may include semiconductor nanoparticles (e.g., a plurality of semiconductor nanoparticles) such as blue light-emitting (blue light-emitting) nanoparticles, red light-emitting (red light-emitting) nanoparticles, or green light-emitting (green light-emitting) nanoparticles. The light-emitting layer may include one or more (e.g., 2 or more, or 3 or more and 10 or less) monolayers of the semiconductor nanoparticles.

[0187] The light-emitting layer may be patterned (not shown). In an embodiment, the patterned light-emitting layer may include a blue light-emitting layer disposed in a blue pixel. In an embodiment, the light-emitting layer may further include a red light-emitting layer disposed in a red pixel or a green light-emitting layer disposed in a green pixel. In an embodiment, the light-emitting layer may include a red light-emitting layer disposed in a red pixel and a green light-emitting layer disposed in a green pixel. Each of the (e.g., red, green, or blue) light-emitting layers may be separated from an adjacent light-emitting layer (e.g., optically) by a partition wall. In an embodiment, a partition wall such as a black matrix may be provided between the red light-emitting layer, the green light-emitting layer, and the blue light-emitting layer. The red light-emitting layer, the green light-emitting layer, and the blue light-emitting layer may be optically isolated from each other.

[0188] In an embodiment, the light emitting layer 3, 30, or the semiconductor nanoparticles may not include cadmium. In an embodiment, the light emitting layer 3, 30, or the semiconductor nanoparticles may not include mercury, lead, or a combination thereof.

[0189] In an embodiment, the semiconductor nanoparticle may have a core-shell structure. In an embodiment, the semiconductor nanoparticle or the core-shell structure may include: a core including a first semiconductor nanocrystal, and a shell disposed on the core and including a second semiconductor nanocrystal having a composition different from that of the first semiconductor nanocrystal.

[0190] The semiconductor nanoparticle (or the first semiconductor nanocrystal, the second semiconductor nanocrystal, or a combination thereof) may include a II-VI compound, a III-V compound, an IV-VI compound, an IV element (simple substance) or a compound, an I-III-VI compound, a II-III-VI compound, an I-II-IV-VI compound, or a combination thereof. In an embodiment, the light-emitting layer or the semiconductor nanoparticle (e.g., the first semiconductor nanocrystal or the second semiconductor nanocrystal) may not include cadmium. In an embodiment, the light-emitting layer or the semiconductor nanoparticle (e.g., the first semiconductor nanocrystal or the second semiconductor nanocrystal) may not include lead. In an embodiment, the light-emitting layer or the semiconductor nanoparticle (e.g., the first semiconductor nanocrystal or the second semiconductor nanocrystal) may not include a combination of lead and cadmium.

[0191] The II-VI group compound may be a binary compound such as ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, MgSe, MgS, or a combination thereof; a ternary compound such as ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, HgZnS, HgZnSe, HgZnTe, MgZnSe, MgZnS, or a combination thereof; a quaternary compound such as HgZnTeS, HgZnSeS, HgZnSeTe, HgZnSTe, or a combination thereof; or a combination thereof. The II-VI group compound may further include a group III metal.

[0192] The III-V compound may be a binary compound such as GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, or a combination thereof; a ternary compound such as GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, or a combination thereof; a quaternary compound such as GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, InAlPSb, or a combination thereof; or a combination thereof. The III-V compound may further include a Group II metal (e.g., InZnP).

[0193] The IV-VI Group compound may be a binary compound such as SnS, SnSe, SnTe, PbS, PbSe, PbTe, or a combination thereof; a ternary compound such as SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, or a combination thereof; a quaternary compound such as SnPbSSe, SnPbSeTe, SnPbSTe, or a combination thereof; or a combination thereof.

[0194] An example of the I-III-VI group compound may be CuInSe 2 、CuInS 2 , CuInGaSe, and CuInGaS, but are not limited thereto. Examples of the I-III-VI group compound may include ternary compounds such as AgInS, AgInS 2 、AgInSe 2 、AgGaS、AgGaS 2 、AgGaSe2 、CuInS、CuInS 2 、CuInSe 2 、CuGaS 2 、CuGaSe 2 、CuGaO 2 、AgGaO 2 、AgAlO 2 or a combination thereof; quaternary compounds such as AgInGaS 2 、AgInGaSe 2 or a combination thereof; or a combination thereof.

[0195] Examples of the Group I-II-IV-VI compound may be CuZnSnSe and CuZnSnS, but are not limited thereto.

[0196] The Group IV element (single substance) or compound may include a single element (single substance) such as Si, Ge, or a combination thereof; a binary compound such as SiC, SiGe, or a combination thereof; or a combination thereof.

[0197] Each element included in a multi-component compound such as a binary compound, a ternary compound, or a quaternary compound may exist in a particle at a uniform concentration or at a non-uniform concentration. For example, the chemical formula described above means the type of element included in the compound, and the ratio between the elements in the compound may be different. For example, the chemical formula "AgInGaS 2 " can include AgIn x Ga 1-x S 2 (x is a real number greater than 0 and less than or equal to 1), but is not limited to this.

[0198] In an embodiment, the first semiconductor nanocrystal may include a metal and a non-metal, the metal including indium, zinc, or a combination thereof, and the non-metal including phosphorus, selenium, tellurium, sulfur, or a combination thereof. In an embodiment, the second semiconductor nanocrystal may include a metal and a non-metal element, the metal including indium, zinc, or a combination thereof, and the non-metal element including phosphorus, selenium, tellurium, sulfur, or a combination thereof.

[0199] In an embodiment, the first semiconductor nanocrystal may include InP, InZnP, ZnSe, ZnSeS, ZnSeTe, or a combination thereof; the second semiconductor nanocrystal may include ZnSe, ZnSeS, ZnS, ZnTeSe, or a combination thereof. In an embodiment, the shell may include zinc, sulfur, and optionally selenium, for example in the outermost layer.

[0200] In an embodiment, the semiconductor nanoparticles may emit blue or green light and may include: a core including ZnSeTe, ZnSe, or a combination thereof, and a shell including a zinc chalcogenide (e.g., ZnS, ZnSe, ZnSeS, or a combination thereof). The amount of sulfur in the shell may increase or decrease in a radial direction (from the core toward the surface), for example, the amount of sulfur may have a concentration gradient in which the concentration of sulfur varies in the radial direction (e.g., decreases or increases in a direction toward the core).

[0201] In an embodiment, the semiconductor nanoparticle may emit red or green light, the core may include InP, InZnP, or a combination thereof, and the shell may include a Group II metal and a non-metal, the Group II metal includes zinc, the non-metal includes sulfur, selenium, or a combination thereof. The semiconductor nanoparticle may include: a first semiconductor nanocrystal including zinc, selenium, and tellurium, and a second semiconductor nanocrystal different from the first semiconductor nanocrystal.

[0202] The semiconductor nanoparticle may include: a first semiconductor nanocrystal including indium, phosphorus, and optionally zinc; and a second semiconductor nanocrystal including zinc chalcogenide and different from the first semiconductor nanocrystal. The semiconductor nanoparticle may include zinc chalcogenide. The zinc chalcogenide may include tellurium. The semiconductor nanoparticle may be configured to emit blue light or green light. The semiconductor nanoparticle may include: a core including the first semiconductor nanocrystal, and a shell disposed on the core and including the second semiconductor nanocrystal.

[0203] In an embodiment, the semiconductor nanoparticles may have a core-shell structure, and at the interface between the core and the shell, an alloyed intermediate layer may or may not be present. The alloyed intermediate layer may include a homogeneous alloy or may have a concentration gradient. A gradient alloy may have a concentration gradient in which the concentration of the element of the shell varies radially (e.g., decreases or increases in the direction toward the core).

[0204] In an embodiment, the shell may have a composition that varies in a radial direction. In an embodiment, the shell may be a multilayer shell comprising two or more layers. In a multilayer shell, two adjacent layers may have compositions that are different from each other. In a multilayer shell, a layer (e.g., at least one layer) may independently include semiconductor nanocrystals having a single composition. In a multilayer shell, a layer (e.g., at least one layer) may independently have alloyed semiconductor nanocrystals. In a multilayer shell, a layer (e.g., at least one layer) may have a concentration gradient that varies radially with respect to the composition of semiconductor nanocrystals.

[0205] In an embodiment, in a semiconductor nanoparticle having a core-shell structure, the shell material may have a band gap energy greater than the band gap energy of the core. The material of the shell may have a band gap energy smaller than the band gap energy of the core. In the case of a multilayer shell, the band gap energy of the outermost layer material of the shell may be greater than the band gap energy of the inner layer material (the layer closer to the core) of the core and the shell. In the case of a multilayer shell, the semiconductor nanocrystals of each layer are selected to have an appropriate band gap, thereby effectively presenting a quantum confinement effect.

[0206] The semiconductor nanoparticle according to an embodiment may include, for example, an organic ligand bonded or coordinated to a surface thereof.

[0207] By adjusting the composition, size, or combination thereof of the semiconductor nanoparticles, the absorption or emission wavelength of the semiconductor nanoparticles can be controlled. The semiconductor nanoparticles included in the light-emitting layer 3 or 30 can be configured to emit light of a desired color. The semiconductor nanoparticles can include blue light-emitting semiconductor nanoparticles, green light-emitting semiconductor nanoparticles, or red light-emitting semiconductor nanoparticles.

[0208] In an embodiment, the peak emission wavelength of the semiconductor nanoparticles or the light emitting layer (or the light emitted from the electroluminescent device) may be in the wavelength range from ultraviolet to infrared. In an embodiment, the peak emission wavelength of the semiconductor nanoparticles or the light emitting layer (or the light emitted from the electroluminescent device) may be greater than or equal to about 300nm, greater than or equal to about 500nm, greater than or equal to about 510nm, greater than or equal to about 520nm, greater than or equal to about 530nm, greater than or equal to about 540nm, greater than or equal to about 550nm, greater than or equal to about 560nm, greater than or equal to about 570nm, greater than or equal to about 580nm, greater than or equal to about 590nm, greater than or equal to about 600nm, or greater than or equal to about 610nm. The peak emission wavelength may be less than or equal to about 900 nm, less than or equal to about 800 nm, less than or equal to about 650 nm, less than or equal to about 640 nm, less than or equal to about 630 nm, less than or equal to about 620 nm, less than or equal to about 610 nm, less than or equal to about 600 nm, less than or equal to about 590 nm, less than or equal to about 580 nm, less than or equal to about 570 nm, less than or equal to about 560 nm, less than or equal to about 550 nm, or less than or equal to about 540 nm. The peak emission wavelength may be about 500 nm to about 650 nm.

[0209] The semiconductor nanoparticles, the light-emitting layer, or the electroluminescent device may emit green light (for example, when voltage is applied or irradiated with light), and its peak emission wavelength may be in the following range: greater than or equal to about 500 nm (for example, greater than or equal to about 510 nm, or greater than or equal to about 515 nm) and less than or equal to about 560 nm, for example, less than or equal to about 540 nm, or less than or equal to about 530 nm.

[0210] The semiconductor nanoparticles, the light-emitting layer, or the electroluminescent device may emit red light (for example, when voltage is applied or irradiated with light), and its peak emission wavelength may be in the following range: greater than or equal to about 600 nm, for example, greater than or equal to about 610 nm and less than or equal to about 650 nm, or less than or equal to about 640 nm.

[0211] The semiconductor nanoparticles, the light-emitting layer, or the electroluminescent device may emit blue light (e.g., when voltage is applied or irradiated with light), and its peak emission wavelength may be greater than or equal to about 430 nm (e.g., greater than or equal to about 450 nm, greater than or equal to about 455 nm, greater than or equal to about 460 nm, or greater than or equal to about 465 nm) and less than or equal to about 480 nm (e.g., less than or equal to about 475 nm, less than or equal to about 470 nm, or less than or equal to about 465 nm).

[0212] In an embodiment, the semiconductor nanoparticles, the light-emitting layer, or the electroluminescent device may present a light emission spectrum (e.g., an electroluminescent or photoluminescent spectrum) having a relatively narrow half-maximum full width. In an embodiment, in the electroluminescent or photoluminescent spectrum, the semiconductor nanoparticles, the light-emitting layer, or the electroluminescent device may present a half-maximum full width of less than or equal to about 45 nm, less than or equal to about 44 nm, less than or equal to about 43 nm, less than or equal to about 42 nm, less than or equal to about 41 nm, less than or equal to about 40 nm, less than or equal to about 39 nm, less than or equal to about 38 nm, less than or equal to about 37 nm, less than or equal to about 36 nm, or less than or equal to about 35 nm. The half-maximum full width may be greater than or equal to about 10 nm, greater than or equal to about 15 nm, greater than or equal to about 20 nm, or greater than or equal to about 25 nm.

[0213] The semiconductor nanoparticles may exhibit (or may be configured to exhibit) a quantum efficiency (or quantum yield) of greater than or equal to about 10%, for example, greater than or equal to about 30%, greater than or equal to about 50%, greater than or equal to about 60%, greater than or equal to about 70%, greater than or equal to about 80%, greater than or equal to about 90%, or about 100%.

[0214] The semiconductor nanoparticles may have a size (or average size, hereinafter, may be referred to as "size") greater than or equal to about 1 nm and less than or equal to about 100 nm. The size may be a diameter or an equivalent diameter converted by assuming a spherical shape from an electron microscope image when it is not spherical. The size may be calculated by using the result of inductively coupled plasma atomic emission spectrometry (ICP-AES) analysis. In an embodiment, the semiconductor nanoparticles may have a size of about 1 nm to about 50 nm, for example, about 2 nm (or about 3 nm) to about 35 nm. In an embodiment, the size (or average size) of the semiconductor nanoparticles may be greater than or equal to about 3 nm, greater than or equal to about 4 nm, greater than or equal to about 5 nm, greater than or equal to about 6 nm, greater than or equal to about 7 nm, greater than or equal to about 8 nm, greater than or equal to about 9 nm, greater than or equal to about 10 nm, greater than or equal to about 11 nm, or greater than or equal to about 12 nm. In an embodiment, the size (or average size) of the semiconductor nanoparticles may be less than or equal to about 50 nm, less than or equal to about 40 nm, less than or equal to about 30 nm, less than or equal to about 25 nm, less than or equal to about 20 nm, less than or equal to about 19 nm, less than or equal to about 18 nm, less than or equal to about 17 nm, less than or equal to about 16 nm, less than or equal to about 15 nm, less than or equal to about 14 nm, less than or equal to about 13 nm, or less than or equal to about 12 nm.

[0215] The shape of the semiconductor nanoparticles or semiconductor nanostructures is not particularly limited. For example, the shape of the semiconductor nanoparticles may include, but is not limited to, spheres, polyhedrons, pyramids, multi-foot shapes, hexahedrons, cubes, cuboids, nanotubes, nanorods, nanowires, nanosheets, or combinations thereof.

[0216] The semiconductor nanoparticles can be prepared by suitable methods. The semiconductor nanoparticles can be prepared, for example, by a chemical wet method, wherein in a reaction system comprising an organic solvent and an organic ligand, the reaction between the precursors can grow nanocrystalline particles. The organic ligand or the organic solvent can coordinate with the surface of the semiconductor nanocrystal or be coordinated to the surface of the semiconductor nanocrystal to control its growth.

[0217] In an embodiment, for example, a method for preparing semiconductor nanoparticles having a core / shell structure may include: obtaining the core; reacting a first shell precursor including a metal (e.g., zinc) and a second shell precursor including a non-metallic element (e.g., selenium, sulfur, or a combination thereof) in the presence of the core in a reaction medium including an organic ligand and an organic solvent at a reaction temperature (e.g., greater than or equal to about 180° C., greater than or equal to about 200° C., greater than or equal to about 240° C., or greater than or equal to about 280° C. and less than or equal to about 360° C., less than or equal to about 340° C., or less than or equal to about 320° C.) to form a shell including a second semiconductor nanocrystal on a core including a first semiconductor nanocrystal. The method may further include separating the core from the reaction system in which it is produced and dispersing the core in an organic solvent to obtain a core solution.

[0218] In an embodiment, to form the shell, the solvent and optionally the first shell precursor and the ligand compound may be heated under vacuum at a predetermined temperature (e.g., greater than or equal to about 100° C.) (also referred to herein as vacuum treatment), and then, after an inert gas is introduced into the reaction vessel, the mixture may be heat-treated again at a predetermined temperature (e.g., greater than or equal to 100° C.). Then, the core and the second shell precursor may be added to the mixture and heated at a reaction temperature. The shell precursors may be added simultaneously or sequentially at different ratios during the reaction time.

[0219] In the semiconductor nanoparticles of the embodiment, the core can be prepared in an appropriate manner. In an embodiment, the organic solvent may include a C6-C22 primary amine such as hexadecylamine, a C6-C22 secondary amine such as dioctylamine, a C6-C40 tertiary amine such as trioctylamine, a nitrogen-containing heterocyclic compound such as pyridine, a C6-C40 olefin such as octadecene, a C6-C40 aliphatic hydrocarbon such as hexadecane, octadecane, or squalane, an aromatic hydrocarbon substituted with a C6-C30 alkyl group such as phenyldodecane, phenyltetradecane, or phenylhexadecane, a primary, secondary, or tertiary phosphine (e.g., trioctylphosphine) substituted with a C6-C22 alkyl group (e.g., at least one (e.g., 1, 2, or 3) C6-C22 alkyl group), a phosphine oxide (e.g., trioctylphosphine oxide) substituted with a (e.g., 1, 2, or 3) C6-C22 alkyl group, a C12-C22 aromatic ether such as phenyl ether or benzyl ether, or a combination thereof. Combinations comprising more than one type of organic solvent may be used.

[0220] The organic ligand may include RCOOH, RNH 2 , R 2 NH, R 3 N, RSH, RH 2 PO, R 2 HPO, R 3 PO, RH2 P.R 2 HP, R 3 P, ROH, RCOOR', RPO(OH) 2 , R 2 POOH or a combination thereof. Here, R and R' are each independently a substituted or unsubstituted C3 or greater, C6 or greater, or C10 or greater and C40 or less, C35 or less, or C25 or less aliphatic hydrocarbon group (e.g., alkyl, alkenyl, alkynyl, etc.), a substituted or unsubstituted C6-C40 aromatic hydrocarbon group (e.g., aryl), or a combination thereof. In an embodiment, at least two different organic ligands may be used.

[0221] Examples of the organic ligands may be thiol compounds such as methyl mercaptan, ethyl mercaptan, propyl mercaptan, butyl mercaptan, pentyl mercaptan, hexyl mercaptan, octyl mercaptan, dodecanethiol, hexadecyl mercaptan, octadecyl mercaptan, benzyl mercaptan, etc.; amines such as methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, octylamine, nonylamine, decylamine, dodecylamine, hexadecylamine, octadecylamine, dimethylamine, diethylamine, dipropylamine, tributylamine, trioctylamine, etc.; carboxylic acid compounds such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, hexanoic acid, heptanoic acid, octanoic acid, dodecanoic acid, hexadecanoic acid, octadecanoic acid, oleic acid, myristic acid, stearic acid, lauric acid, benzoic acid, etc.; phosphine compounds such as Phosphine compounds such as methyl phosphine, ethyl phosphine, propyl phosphine, butyl phosphine, pentyl phosphine, octyl phosphine, dioctyl phosphine, tributyl phosphine, trioctyl phosphine, etc.; phosphine oxide compounds such as methyl phosphine oxide, ethyl phosphine oxide, propyl phosphine oxide, butyl phosphine oxide, pentyl phosphine oxide, tributyl phosphine oxide, octyl phosphine oxide, dioctyl phosphine oxide, trioctyl phosphine oxide, etc.; diphenylphosphine (DPP), triphenylphosphine compounds or their oxide compounds; C5-C20 alkyl phosphinic acids such as hexyl phosphinic acid, octyl phosphinic acid, dodecane phosphinic acid, tetradecane phosphinic acid, hexadecane phosphinic acid, octadecane phosphinic acid; C5-C20 alkyl phosphinic acids; etc., but are not limited thereto.

[0222] The semiconductor nanoparticles can be collected by the following process: pouring a non-solvent into a mixture including the semiconductor nanoparticles and subjecting the mixture to centrifugation to remove excess organic matter not coordinated on the surface. For example, in an embodiment, after completing the reaction (for forming the core or for forming the shell), a non-solvent can be added to the reaction mixture and the semiconductor nanoparticles coordinated with the ligand compound can be separated therefrom. The non-solvent can be a polar solvent: it is miscible with the solvent used in the core forming reaction, the shell forming reaction, or a combination thereof, and the prepared semiconductor nanoparticles cannot be dispersed. The non-solvent can be selected depending on the solvent used in the reaction, and can include, for example, acetone, ethanol, butanol, isopropanol, ethylene glycol, water, tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), diethyl ether, formaldehyde, acetaldehyde, a solvent with a solubility parameter similar to the aforementioned non-solvent, or a combination thereof. The semiconductor nanoparticles can be separated by centrifugation, sedimentation, or chromatography. If desired, the separated semiconductor nanoparticles can be washed with a washing solvent. The washing solvent is not particularly limited, and may have a solubility parameter similar to that of the ligand, and may include, for example, hexane, heptane, octane, chloroform, toluene, benzene, and the like.

[0223] The semiconductor nanoparticles of the embodiment may be non-dispersible or insoluble in water, the aforementioned non-solvent, or a combination thereof. The semiconductor nanoparticles of the embodiment may be dispersed in the aforementioned organic solvent. In an embodiment, the aforementioned semiconductor nanoparticles may be dispersed in substituted or unsubstituted C6-C40 aliphatic hydrocarbons, substituted or unsubstituted C6-C40 aromatic hydrocarbons, or a combination thereof.

[0224] In an embodiment of an electroluminescent device or a display device, the thickness of the light-emitting layer may be appropriately selected. In an embodiment, the light-emitting layer may include a monolayer of nanoparticles. In an embodiment, the light-emitting layer may include one or more, for example, two or more, three or more, or four or more and 20 or less, 10 or less, 9 or less, 8 or less, 7 or less, or 6 or less monolayers of semiconductor nanoparticles. The light-emitting layer may have a thickness of greater than or equal to about 5 nm, for example, greater than or equal to about 10 nm, greater than or equal to about 20 nm, or greater than or equal to about 30 nm and less than or equal to about 200 nm, less than or equal to about 150 nm, less than or equal to about 100 nm, less than or equal to about 90 nm, less than or equal to about 80 nm, less than or equal to about 70 nm, less than or equal to about 60 nm, or less than or equal to about 50 nm. The light emitting layer may have a thickness of, for example, about 10 nm to about 150 nm, about 20 nm to about 100 nm, or about 30 nm to about 50 nm.

[0225] In an embodiment, setting (e.g., forming) a light-emitting layer 3 including the semiconductor nanoparticles can be performed as follows: providing a composition including semiconductor nanoparticles and an organic solvent, and applying or depositing it on a substrate (e.g., an electrode) or a charge auxiliary layer (e.g., a hole auxiliary layer or an electron auxiliary layer) in an appropriate manner (e.g., by spin coating, inkjet printing, etc.).

[0226] The formed film of the semiconductor nanoparticles may further be subjected to contact with an organic solution / eg, a metal halide (eg, zinc chloride) organic solution (eg, alcohol solution).

[0227] Forming the light-emitting layer may further include heat treating the coated or deposited semiconductor nanoparticle layer. The heat treatment temperature is not particularly limited, and it may be appropriately selected in consideration of the boiling point of the organic solvent. For example, the heat treatment temperature may be greater than or equal to about 60° C. The type of organic solvent used to disperse the semiconductor nanoparticles is not particularly limited and may be appropriately selected. In an embodiment, the organic solvent may include a substituted or unsubstituted aliphatic hydrocarbon organic solvent, a substituted or unsubstituted aromatic hydrocarbon solvent, a substituted or unsubstituted alicyclic hydrocarbon solvent, an acetate solvent, or a combination thereof.

[0228] In an embodiment, the light-emitting layer may be a single layer or a multilayer structure having at least two layers. In the multilayer structure, adjacent layers (e.g., a first light-emitting layer and a second light-emitting layer) may be configured to emit a first light (e.g., green light, blue light, or red light). In the multilayer structure, adjacent layers (e.g., a first light-emitting layer and a second light-emitting layer) may have the same or different compositions, ligands, or a combination thereof. In an embodiment, the (multilayer) light-emitting layer may have a halogen amount that varies (increases or decreases) in the thickness direction. In an embodiment, in the (multilayer) light-emitting layer, the amount of halogen may increase in the direction toward the electron-assisted layer. In the (multilayer) light-emitting layer, the amount or content of organic ligands may decrease in the direction toward the electron-assisted layer. In the (multilayer) light-emitting layer, the amount or content of organic ligands may increase in the direction toward the electron-assisted layer.

[0229] In an embodiment, the light-emitting layer may include: a first light-emitting layer including first semiconductor nanoparticles and a second light-emitting layer including second semiconductor nanoparticles, wherein the first semiconductor nanoparticles have a surface exchanged with halogen (e.g., chlorine) and the second light-emitting layer has an amount of organic ligands greater than that of the first light-emitting layer. The amount of halogen (e.g., chlorine) and the amount of organic ligands of the light-emitting layer can be controlled in an appropriate manner (e.g., post-treatment of the formed layer). In an embodiment, a film of the semiconductor nanoparticles having organic ligands (e.g., having carboxylic acid groups) is formed, and then treated with a solution including a metal halide (e.g., zinc halide such as zinc chloride in an alcohol solvent) to control (reduce) the amount of organic ligands of the semiconductor nanoparticles in the film. The treated film may have an increased amount of halogen, exhibiting a changed property (e.g., solubility) for an organic solvent, and the following may be possible: a layer of semiconductor nanoparticles having different amounts of organic ligands (e.g., halogen-treated semiconductor nanoparticles or semiconductor nanoparticles having ligands having carboxylic acid groups) is subsequently formed on the treated film.

[0230] An electron auxiliary layer 4 or 40 may be provided on the light-emitting layer 3 or 30, for example, between the light-emitting layer and the second electrode 5 or 50. In the electron auxiliary layer 4 or 40, electron transport, injection, or transport and injection may occur. The electron auxiliary layer 4 or 40 includes an electron transport layer (ETL). The electron auxiliary layer 4 or 40 may further include an electron injection layer, a hole blocking layer, or a combination thereof. The electron injection layer may be provided between the electron transport layer and the second electrode, and the hole blocking layer may be provided between the electron transport layer and the light-emitting layer, but they are not limited thereto. The electron transport layer may be adjacent to the light-emitting layer (for example, directly adjacent to the light-emitting layer, or directly provided on the light-emitting layer). In an embodiment, the light-emitting layer 3 or 30 may contact the electron transport layer.

[0231] The electron transport layer may include zinc oxide nanoparticles (e.g., a plurality of zinc oxide nanoparticles). The zinc oxide nanoparticles may further include a first metal different from zinc. The zinc oxide nanoparticles may have a size or average size (hereinafter referred to as "size") greater than or equal to about 1 nm and less than or equal to about 50 nm. The first metal may include an alkaline earth metal (e.g., magnesium, calcium, barium, strontium, or a combination thereof), zirconium (Zr), tungsten (W), titanium (Ti), yttrium (Y), aluminum (Al), gallium (Ga), indium (In), tin (Sn), cobalt (Co), vanadium (V), or a combination thereof. The first metal may include an alkaline earth metal, and the first metal may further include or may not include zirconium (Zr), tungsten (W), titanium (Ti), yttrium (Y), aluminum (Al), gallium (Ga), indium (In), tin (Sn), cobalt (Co), vanadium (V), or a combination thereof. The zinc oxide nanoparticles may further include or may not include an alkali metal. The zinc oxide nanoparticles or the alkali metal may include sodium, potassium, rubidium, cesium, francium, or a combination thereof. The zinc oxide nanoparticles or the alkali metal may or may not include lithium.

[0232] An electron assist layer based on zinc oxide nanoparticles may be provided for QD-LEDs containing cadmium. However, the inventors have found that despite the use of an electron assist layer based on zinc oxide nanoparticles, in the case of an electroluminescent device including cadmium-free semiconductor nanoparticles configured to emit light of a desired wavelength (e.g., blue light) in a light-emitting layer, there may be technical limitations for simultaneously improving both electroluminescent properties and lifetime.

[0233] Without wishing to be bound by theory, it is believed that in a QD-LED having a light-emitting layer containing semiconductor nanoparticles that do not contain cadmium (e.g., blue light-emitting semiconductor nanoparticles containing zinc chalcogenide cores), a charge imbalance between holes moving through a hole-assisting layer (e.g., HTL) and electrons moving through an ETL containing zinc oxide nanoparticles may occur, and the charge imbalance may result in a reduction in the electroluminescent properties of the light-emitting device (e.g., maximum external quantum efficiency or maximum brightness) or deterioration of the device.

[0234] The QD-LED may include zinc oxide nanoparticles in the electron transport layer, and the zinc oxide nanoparticles may be synthesized by a bottom-up process or a solution-precipitation process. The inventors have found that the method of making the zinc oxide nanoparticles may affect the particle size, the amount of surface organic matter, and the surface defect passivation, which can ultimately affect the characteristics of an electroluminescent device (e.g., a QD-LED) including such an ETL. The inventors have found that in an ETL material containing zinc oxide, defects include various types, such as Zn interstitial (ZnI) and oxygen vacancies (V O), and using currently known methods, it is difficult to control them in a desired manner. In this regard, attempts have been made to provide an electron transport layer by adding an alkali metal carbonate to an original solution containing a precursor and a stabilizer to form a zinc oxide layer according to a sol-gel method. The inventors have found that in this type of technology, the formation of zinc oxide nanoparticles of a desired size cannot be guaranteed, and there are limitations on the performance improvement of QD-LEDs including the ETL prepared in this way. The zinc oxide nanoparticles prepared by known methods can only exhibit dispersibility for a limited type of solvent (e.g., ethanol). In order to form an electron transport layer on the emission layer by an inkjet printing method, the following may be desired: the composition for providing the ETL exhibits physical properties suitable for the inkjet printing method. The inventors have also found that compositions containing zinc oxide nanoparticles manufactured according to conventional techniques tend to clog ink nozzles. Without wishing to be bound by theory, it is believed that under inkjet printing conditions, solvents such as ethanol may evaporate relatively quickly, and therefore, ethanol compositions containing zinc oxide nanoparticles according to conventional techniques have lower stability over time, and this may limit their use in manufacturing light-emitting devices via inkjet printing.

[0235] The inventors have also found that zinc metal oxide nanoparticles produced by bottom-up processes can have organic materials derived from reagents such as precursors contained in the reaction system as ligands for particle surface stabilization, but can still include considerable levels of various surface defects. Using methods known to date, it can be difficult to achieve additional surface passivation in the prepared zinc oxide nanoparticles. Without wishing to be bound by theory, it is believed that the surface properties of the zinc oxide nanoparticles can affect the physical properties of the electroluminescent device, resulting in, for example, reduced efficiency and deterioration of the electron transport layer.

[0236] The inventors have found that the methods of the embodiments described herein can achieve passivation in a manner different from conventional techniques. Without wishing to be bound by theory, it is believed that, according to the methods of the embodiments, in addition to the surface passivation provided by the ligands derived from the organic acid and the hydroxyl ligands derived from the precursor, direct surface passivation caused by the binding of carbonate groups can also be provided. Without wishing to be bound by theory, it is believed that due to the surface passivation occurring in the zinc oxide nanoparticles by the methods of the embodiments, the features described herein (e.g., in terms of the spectrum confirmed by XPS) can be confirmed. The zinc oxide nanoparticles of the embodiments or the electron transport layer containing them may present a component spectrum as determined by XPS analysis (e.g., O1s spectrum, etc.) and TGA analysis results as described herein (e.g., differential thermogravimetric analysis curves, etc.).

[0237] Surprisingly, the present inventors have discovered that electroluminescent devices comprising an electron transport layer including embodiment zinc oxide nanoparticles can exhibit extended lifetime as well as improved optical properties.

[0238] In an embodiment, providing zinc oxide nanoparticles includes contacting a first metal precursor, a zinc precursor, a base, and a metal carbonate compound in an organic solvent to form the zinc oxide nanoparticles. In an embodiment, providing zinc oxide nanoparticles may include: dissolving the first metal precursor and the zinc precursor in an organic solvent, and adding a base and a metal carbonate compound to the organic solvent and allowing the zinc precursor and the first metal precursor to react (e.g., at a first temperature) to form the zinc oxide nanoparticles.

[0239] The first metal may include an alkaline earth metal (e.g., magnesium). The first metal may include zirconium, tungsten, titanium, yttrium, aluminum, gallium, indium, tin, cobalt, vanadium, or a combination thereof. The first metal may include: magnesium; and optionally zirconium, tungsten, titanium, yttrium, aluminum, gallium, indium, tin, cobalt, vanadium, or a combination thereof. The first metal may include magnesium and gallium. The zinc oxide nanoparticles may further include or may not include an alkali metal. The zinc oxide nanoparticles or the alkali metal may or may not include lithium, sodium, potassium, rubidium, cesium, francium, or a combination thereof.

[0240] The organic solvent may include a C1-C10 alcohol solvent, dimethyl sulfoxide, a substituted or unsubstituted C1-C30 or C3-C15 hydrocarbon solvent (e.g., a substituted or unsubstituted aliphatic hydrocarbon, a substituted or unsubstituted aromatic hydrocarbon, a substituted or unsubstituted alicyclic hydrocarbon, or a combination thereof), or a combination thereof. The organic solvent may include a C1-C10 alcohol solvent (e.g., methanol, ethanol, propanol, isopropanol, butanol, isobutanol, amyl alcohol, isopentanol, or a combination thereof), a sulfoxide solvent (e.g., dimethyl sulfoxide), a C3-C15 hydrocarbon solvent (e.g., an aliphatic, aromatic, alicyclic solvent, or an alicyclic compound obtained by hydrogenation of an aromatic hydrocarbon), or a combination thereof.

[0241] The organic solvent may include a first solvent, a second solvent, or a mixture thereof. In an embodiment, the organic solvent may be a solvent mixture including a first solvent and a second solvent, and the relative polarity difference between the first solvent and the second solvent may be greater than or equal to about 0.3 and less than or equal to about 0.9. The method may further include stirring the mixture of the first solvent and the second solvent, for example, at a predetermined temperature (e.g., at a temperature greater than or equal to about 40° C. and less than or equal to about 80° C.).

[0242] By using the mixed solvent, the synthesis of the zinc oxide nanoparticles may involve phase transition and separation mechanisms occurring at the interface of liquid, solid, and solution phases during synthesis (e.g., liquid-solid-solution synthesis, LSS synthesis). Without wishing to be bound by theory, it is believed that in the method of the embodiment, due to the polarity difference between the first solvent and the second solvent, nanobubbles (e.g., solution bubbles or liquid bubbles) may be easily formed in the solvent mixture including the first solvent and the second solvent, and the movement (e.g., phase transfer and / or phase separation) and reaction of the precursor (solid) may occur at the interface between the solvent mixture and the formed nanobubbles to form oxide nanoparticles (e.g., first nanoparticles) including magnesium and zinc. The zinc oxide nanoparticles thus formed may further react with additional metal precursors (e.g., gallium precursors) as described below, and zinc oxide nanoparticles having a core-shell structure may be more easily formed.

[0243] The difference (difference) between the relative polarities of the first solvent and the second solvent may be greater than or equal to about 0.35, greater than or equal to about 0.4, greater than or equal to about 0.45, greater than or equal to about 0.5, or greater than or equal to about 0.55. The difference between the relative polarities may be less than or equal to about 3, less than or equal to about 2, less than or equal to about 1, less than or equal to about 0.85, less than or equal to about 0.8, less than or equal to about 0.75, less than or equal to about 0.7, less than or equal to about 0.65, less than or equal to about 0.6, less than or equal to about 0.55, less than or equal to about 0.5, or less than or equal to about 0.45. The relative polarities of the solvents may be obtained from the literature (e.g., Solvents and solvent effects in organic chemistry, Wiley VCH publisher, 3rd edition (3 rd For example, water has a relative polarity of about 1.

[0244] The first solvent may include a C1-C10 alcohol solvent, for example, methanol, ethanol, propanol, isopropanol, butanol, isobutanol, amyl alcohol, isopentanol, or a combination thereof. The first solvent may have a relative polarity of greater than or equal to about 0.4, greater than or equal to about 0.45, greater than or equal to about 0.5, greater than or equal to about 0.55, greater than or equal to about 0.6, greater than or equal to about 0.65, greater than or equal to about 0.7, or greater than or equal to about 0.75. The relative polarity of the first solvent may be less than or equal to about 2, less than or equal to about 1, or less than or equal to about 0.9.

[0245] The second solvent may include a C3-C15 hydrocarbon solvent (aliphatic, aromatic, alicyclic, or a hydrocarbon solvent including a hydrogenated benzene ring, for example, cyclohexane, hexane, heptane, nonane, octane, etc.). The second solvent may have a relative polarity of greater than or equal to about 0.001, greater than or equal to about 0.003, greater than or equal to about 0.006, greater than or equal to about 0.009, greater than or equal to about 0.01, or greater than or equal to about 0.012. The relative polarity of the second solvent may be less than or equal to about 4, less than or equal to about 3.5, less than or equal to about 3, less than or equal to about 2.5, less than or equal to about 2, less than or equal to about 1.5, less than or equal to about 1, less than or equal to about 0.5, less than or equal to about 0.1, less than or equal to about 0.05, or less than or equal to about 0.01.

[0246] In an embodiment, the second solvent may form nanobubbles in the first solvent. In an embodiment, the first solvent may form nanobubbles in the second solvent. The volume ratio of the second solvent to the first solvent (second solvent: first solvent) may be about 1:0.2-about 1:5, about 1:0.3-about 1:3, about 1:0.5-about 1:2, about 1:0.8 or about 1:1.25, about 1:1-about 1:1.5, or a combination thereof. In an embodiment, the amount of the first solvent may be greater than the amount of the second solvent. In an embodiment, the amount of the first solvent may be less than the amount of the second solvent.

[0247] The stirring of the solvent mixture may be performed at a speed of about 100 revolutions per minute (rpm), about 150 rpm, about 200 rpm, about 250 rpm, about 300 rpm, about 350 rpm, about 400 rpm, about 450 rpm, or about 500 rpm. The stirring may be performed at a speed of about 800 rpm or less, about 700 rpm or less, or about 600 rpm or less. The predetermined temperature may be about 40° C. or greater, for example, about 50° C. or greater, or about 55° C. or greater. The predetermined temperature may be about or less than the boiling point of the first solvent (or about or less than the boiling point of the second solvent), about 78° C. or less, about 70° C. or less, about 65° C. or less, or about 60° C. or less.

[0248] The organic solvent (or the composition for forming the ETL described herein) may not contain butylamine, ethylamine, ethanolamine, hexylamine, aniline, hexamethylamine, or a combination thereof. The organic solvent (or the composition for forming the ETL described below) may not contain C1-C12 organic amine, aromatic amine having a phenyl group, or a combination thereof. The organic amine may be ethylamine, butylamine, hexamethylenediamine, aniline, or ethanolamine.

[0249] The zinc precursor may include an organic compound including zinc, and the first metal precursor may include an organic compound including a first metal. The first metal precursor may further include or may not include an alkali metal. The details of the first metal and the alkali metal are the same as described herein. In an embodiment, the first metal may include magnesium. In an embodiment, the first metal may be magnesium.

[0250] The zinc precursor and the first metal precursor may include a carboxylate moiety (eg, an acetate moiety).

[0251] The zinc precursor may include a zinc carboxylate such as zinc acetylacetonate, zinc acetate, a zinc halide (zinc chloride, zinc bromide, zinc iodide, zinc fluoride, etc.), zinc nitrate, zinc oxide, or a combination thereof.

[0252] The first metal precursor (e.g., which may include magnesium, gallium, etc.) may include a compound (e.g., an organic compound), such as a carboxylate compound (acetate), an acetylacetonate compound, a halide, a nitrogen compound such as a nitride or a nitrate, an oxide, or a combination thereof. In an embodiment, the first metal precursor may include a magnesium carboxylate (e.g., magnesium acetate), magnesium acetylacetonate, a magnesium halide (magnesium chloride, magnesium bromide, magnesium fluoride, magnesium iodide), magnesium nitrate, magnesium oxide, or a combination thereof. In an embodiment, a precursor for the first metal (or another metal described below) may include gallium acetate, gallium acetylacetonate, gallium carboxylate, gallium halide, gallium nitride, gallium oxide, or a combination thereof. In an embodiment, the halide may include chloride, fluoride, bromide, or iodide.

[0253] The zinc oxide nanoparticles obtained by the method may include a first metal and an alkali metal, and may exhibit the optical properties described herein. The molar ratio between the zinc precursor and the first metal precursor may be appropriately selected in consideration of the desired composition of the zinc oxide nanoparticles. In an embodiment, the molar ratio of the first metal precursor may be about 0.1-1.5 moles, about 0.2-1 moles, about 0.3-0.9 moles, about 0.4-0.8 moles, about 0.5 moles, or a combination thereof, per 1 mole of the zinc precursor.

[0254] In an embodiment, a metal carbonate compound and a base may be added to the organic solvent (or a solution obtained by dissolving the first metal precursor and the zinc precursor in the organic solvent), and the zinc precursor and the first metal precursor may be allowed to react together.

[0255] The metal carbonate compound may include alkali metal carbonate, alkali metal bicarbonate, alkaline earth metal carbonate or a combination thereof. The metal carbonate compound may include sodium, potassium, rubidium, cesium, francium or a combination thereof. The metal carbonate compound may be an alkali metal carbonate compound. The metal carbonate compound may include lithium carbonate, sodium carbonate, potassium carbonate, rubidium carbonate, cesium carbonate or a combination thereof. In an embodiment, the metal carbonate compound may include a metal (e.g., cesium or rubidium) having an atomic radius larger than the atomic radius of zinc.

[0256] In the method of the embodiment, based on the Zn content supplied to the reaction system (e.g., the total Zn molar content), the amount of metal carbonate added or the amount of carbonate ions provided therefrom may be less than or equal to about 25%, less than or equal to about 20%, less than or equal to about 15%, less than or equal to about 10%, less than or equal to about 9%, less than or equal to about 8%, less than or equal to about 7%, less than or equal to about 6%. In the method of the embodiment, based on the Zn content supplied to the reaction system, the amount of metal carbonate added or the amount of carbonate ions provided therefrom may be greater than or equal to about 0.5%, greater than or equal to about 1%, greater than or equal to about 3%, greater than or equal to about 6%, greater than or equal to about 9%.

[0257] The layer including the zinc oxide nanoparticles can be used as an electron transport layer in an electroluminescent device including a light-emitting layer containing quantum dots. The inventors have found that zinc oxide nanoparticles manufactured by a method according to a conventional method can generate a significant amount of leakage current when applied to an electron transport layer. Without wishing to be bound by theory, it is believed that current leakage can occur due to various trap energy levels present in zinc oxide nanoparticles prepared by conventional methods. Without wishing to be bound by theory, it is believed that these various trap energy levels can be generated by defects on the surface and in the interior of the zinc oxide nanoparticles. In the prior art, the composition for forming an electron transport layer containing zinc oxide may further include additional additives or dopants, and such a composition may not provide a desired level of dispersibility and may be difficult to use in an inkjet printing process in which the composition needs to be ejected from an inkjet nozzle and deposited in a pixel.

[0258] Surprisingly, the inventors have discovered that zinc oxide nanoparticles prepared by the methods described herein (i.e., which involve a metal carbonate compound and a base, as described) can exhibit different properties or surface characteristics (e.g., as determined by XPS analysis, TGA, or a combination thereof) than zinc oxide nanoparticles synthesized using conventional techniques. Without wishing to be bound by theory, it is believed that zinc oxide nanoparticles according to embodiments can have not only surface passivation provided by carboxylate and hydroxyl moieties, but also additional passivation provided by carbonate ions on the surface of the particles. Without wishing to be bound by theory, it is believed that in methods according to embodiments, carbonate moieties provided to the synthesis reaction system can effectively passivate zinc dangling bonds that may otherwise be present on the particle surface.

[0259] It is believed that, in an embodiment, the zinc oxide nanoparticles may have a surface ligand composition different from that of conventional technologies, and therefore, through trap passivation of the zinc oxide nanoparticles, the leakage current of the device may be reduced, and the balance of holes and electrons may be matched, thereby increasing the efficiency of the device and improving the life of the device. In an embodiment, an alkali metal or an alkaline earth metal may have an atomic radius larger than that of zinc, and therefore, in the zinc oxide nanoparticles prepared in the presence of such a metal carbonate compound, the content of the metal element derived from the metal carbonate compound may be limited or controlled.

[0260] The base may contain a strong base. The base or the base solution may have a pH of about 8 or more, about 8.5 or more, about 9 or more, about 9.5 or more, about 10 or more, about 10.5 or more, or about 11 or more.

[0261] The base may include a first base, a second base, or a combination thereof. The first base may include an organic base containing a C1-C50 organic group (e.g., an aliphatic hydrocarbon group such as an alkyl group). The second base may include an inorganic base containing an alkali metal or an alkaline earth metal.

[0262] The first base may include a substituted or unsubstituted C1-C50 (e.g., C2-C40, C3-C30, C4-C25, C5-C20, C6-C15, C7-C14, C8-C12, C9-C11, or a combination thereof) aliphatic hydrocarbon group. The number of aliphatic hydrocarbon groups may be 1, 2, 3, or 4. The first base may include a quaternary ammonium salt compound. The first base may include a tetraalkylammonium hydroxide (e.g., tetra(C1-C6 alkyl)ammonium hydroxide, such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, diethyldimethylammonium hydroxide, dimethyldipropylammonium hydroxide, or a combination thereof).

[0263] The second base may include an alkali metal hydroxide (eg, lithium hydroxide, sodium hydroxide, potassium hydroxide, cesium hydroxide, rubidium hydroxide, francium hydroxide, or a combination thereof).

[0264] The second alkali may include at least one or at least two alkali metal hydroxides. The second alkali may include or may not include lithium hydroxide. In an embodiment, the second alkali may include sodium hydroxide, potassium hydroxide, cesium hydroxide, rubidium hydroxide, or a combination thereof. The second alkali may include or may not include lithium hydroxide, sodium hydroxide, or a combination thereof. In an embodiment, the second alkali may include potassium hydroxide, cesium hydroxide, rubidium hydroxide, or a combination thereof. In an embodiment, the second alkali may be used alone or may be used together with the first alkali.

[0265] In embodiments, the base may include a second base, and the zinc oxide nanoparticles may further contain an alkali metal (eg, lithium, potassium, rubidium, cesium, or a combination thereof).

[0266] In an embodiment, the first base may be used, and the molar ratio between the first base and the second base (i.e., first base:second base) may be about 1:0-about 1:10, about 1:0.1-about 1:3, about 1:0.3-about 1:2.7, about 1:0.5-about 1:1.5, about 1:0.7-about 1:1.2, about 1:0.8-about 1:1.3, about 1:0.9-about 1:1.25, about 1:1-about 1:1.2, or a combination thereof.

[0267] In an embodiment, the molar ratio of the second base to the first base (second base:first base) may be about 1:0 to about 1:10, about 1:0.01 to about 1:10, about 1:0.1 to about 1:3, about 1:0.5 to about 1:2.7, about 1:0.8 to about 1:1.5, about 1:0.8 to about 1:1.2, about 1:0.9 to about 1:1.3, about 1:1 to about 1:1.25, or a combination thereof.

[0268] In an embodiment, the molar ratio of the sum of the zinc precursor and the first metal precursor relative to the sum of the first base and the second base (sum of metal precursors:sum of bases) may be about 1:0.5 to about 1:5, about 1:0.6 to about 1:4, about 1:0.7 to about 1:3, about 1:0.8 to about 1:2.5, about 1:0.9 to about 1:2, about 1:1 to about 1:1.5, about 1:1.1 to about 1:1.48, about 1:1.21 to about 1:1.45, about 1:1.2 to about 1:1.35, or a combination thereof.

[0269] The molar ratio between the zinc precursor and the first metal precursor may be appropriately selected in consideration of the desired composition of the zinc oxide nanoparticles. In an embodiment, the molar amount of the first metal precursor may be about 0.1 mol to about 1.5 mol, about 0.2 mol to about 1 mol, about 0.3 mol to about 0.9 mol, about 0.4 mol to about 0.8 mol, about 0.5 mol to about 0.7 mol, or a combination thereof, based on 1 mol of the zinc precursor.

[0270] In the method of the embodiment, the first base and the second base may be dissolved in the solvent (eg, an alcohol solvent) and added. The first base and the second base may be added separately or may be added as a mixture.

[0271] In an embodiment, the base may include a C1-C30 alkylammonium hydroxide compound, an alkali metal hydroxide, or a combination thereof, and the metal carbonate compound may include rubidium carbonate, rubidium bicarbonate, cesium bicarbonate, or a combination thereof.

[0272] The first temperature and time of the reaction can be appropriately adjusted. The first temperature of the reaction can be greater than or equal to about 0°C, for example, greater than or equal to about 10°C, greater than or equal to about 20°C, greater than or equal to about 25°C, greater than or equal to about 30°C, greater than or equal to about 35°C, greater than or equal to about 40°C, or greater than or equal to about 45°C. The temperature can be less than or equal to about 100°C, less than or equal to about 80°C, less than or equal to about 70°C, less than or equal to about 65°C, less than or equal to about 60°C, less than or equal to about 55°C, less than or equal to about 50°C, or less than or equal to about 42°C. The reaction time can be about 10 minutes-300 minutes. The reaction time may be greater than or equal to about 20 minutes, greater than or equal to about 40 minutes, greater than or equal to about 50 minutes, greater than or equal to about 70 minutes, greater than or equal to about 90 minutes, greater than or equal to about 110 minutes, greater than or equal to about 120 minutes, greater than or equal to about 130 minutes, or greater than or equal to about 140 minutes. The reaction time may be less than or equal to about 280 minutes, less than or equal to about 250 minutes, or less than or equal to about 150 minutes.

[0273] In the method of the embodiment, for example, in order to improve the dispersibility of the prepared nanoparticles, the addition of the base can be carried out at a predetermined temperature, for example, at room temperature, or at a temperature of about 20° C. to about 40° C., or at a temperature of about 25° C. to about 30° C. In the method of the embodiment, for example, in order to improve the dispersibility of the prepared particles, the reaction can be carried out at a temperature of less than or equal to about 60° C., for example, about 20 to about 35° C.

[0274] In an embodiment, the zinc oxide nanoparticles may have a core-shell structure including a core and an outer layer (eg, a shell or a layer containing another metal) disposed on the core, and the core may include Zn 1-x M x O (herein, M includes magnesium, calcium, zirconium, tungsten, titanium, yttrium, aluminum, or a combination thereof, and x is greater than or equal to 0 and less than or equal to about 0.5). 1-x M x In O, x can be greater than or equal to about 0.01, greater than or equal to about 0.03, greater than or equal to about 0.05, greater than or equal to about 0.07, greater than or equal to about 0.1, greater than or equal to about 0.13, greater than or equal to about 0.15, greater than or equal to about 0.17, greater than or equal to about 0.2, greater than or equal to about 0.23, or greater than or equal to about 0.25. 1-x M x In O, x may be less than or equal to about 0.47, less than or equal to about 0.45, less than or equal to about 0.43, less than or equal to about 0.4, less than or equal to about 0.37, less than or equal to about 0.35, or less than or equal to about 0.3. In an embodiment, M may be magnesium; and calcium, zirconium, tungsten, titanium, yttrium, aluminum, or a combination thereof.

[0275] The outer layer may include a metal oxide, the metal oxide including the first metal and optionally zinc. The metal oxide included in the outer layer may have a composition different from the composition of the core. The metal oxide included in the outer layer may include gallium oxide. The outer layer of the zinc oxide nanoparticle may include an alkali metal (e.g., provided by the base) and optionally an organic material. In an embodiment, the alkali metal may be bonded or adsorbed in the zinc oxide nanoparticle or on the surface of the zinc oxide nanoparticle (or on a hydroxyl group on the particle surface).

[0276] In the method of the embodiment, providing zinc oxide nanoparticles having a core-shell structure may further include, for example: dispersing the zinc oxide nanoparticles in a third solvent; and forming a layer containing another metal (e.g., an oxide layer of the other metal) on the zinc oxide nanoparticles by adding a precursor for the other metal and a base to the third solvent for reaction. The other metal may include alkaline earth metals, zirconium, tungsten, titanium, yttrium, gallium, indium, tin, cobalt, vanadium, or a combination thereof. The third solvent may include a C1-C10 alcohol solvent, dimethyl sulfoxide, a C3-C30 (C15) hydrocarbon solvent (e.g., an aliphatic hydrocarbon solvent, an aromatic hydrocarbon solvent, an alicyclic hydrocarbon solvent, or a solvent having a benzene ring in which one or more double bonds are hydrogenated).

[0277] The zinc oxide nanoparticles prepared by the method of the embodiment or the electron transport layer including the same may exhibit the molar ratio or properties as described herein (X-ray photoelectron spectroscopy properties, UV-Vis absorption spectroscopy analysis properties, quenching properties in the case where the light-emitting layer includes quantum dots, trapped light emission, dispersion properties, etc.). The characteristics such as the presence of each component in the zinc oxide nanoparticles or the molar ratio therebetween can be determined or measured by appropriate analytical means (X-ray photoelectron spectroscopy, inductively coupled plasma atomic emission spectroscopy, scanning or transmission electron microscope energy dispersive spectroscopy, etc.).

[0278] In the zinc oxide nanoparticles, the molar ratio of the first metal (e.g., magnesium) to zinc may be less than or equal to about 0.5:1, less than or equal to about 0.45:1, less than or equal to about 0.35:1, less than or equal to about 0.3:1, less than or equal to about 0.25:1, less than or equal to about 0.2:1, less than or equal to about 0.14:1, or less than or equal to about 0.13:1. In the zinc oxide nanoparticles, the molar ratio of the first metal (e.g., magnesium) to zinc may be greater than or equal to about 0.01:1, greater than or equal to about 0.03:1, greater than or equal to about 0.05:1, greater than or equal to about 0.07:1, greater than or equal to about 0.09:1, greater than or equal to about 0.1:1, greater than or equal to about 0.12:1, greater than or equal to about 0.14:1, greater than or equal to about 0.16:1, greater than or equal to about 0.18:1, or greater than or equal to about 0.24:1.

[0279] In the zinc oxide nanoparticles of the embodiment, the first metal may include two or more types of metals. In an embodiment, the zinc oxide nanoparticles may further include a Group 13 metal (e.g., gallium, aluminum, or a combination thereof) together with magnesium, and the amount of the Group 13 metal (e.g., gallium or aluminum) in the zinc oxide nanoparticles may be greater than or equal to about 1 mol% (i.e., greater than or equal to about 0.01:1 as a molar ratio), greater than or equal to about 5 mol%, 10 mol% or more, or 15 mol% or more to 30 mol% or less (i.e., less than or equal to about 0.3:1 as a molar ratio), 12 mol% or less, 8 mol% or less, or 6 mol% or less, based on the total moles of zinc, magnesium, and gallium.

[0280] In the zinc oxide nanoparticles of the embodiments, the molar ratio of the Group 13 metal to zinc (Group 13 metal:Zn) may be greater than or equal to about 0.04:1, greater than or equal to about 0.042:1, greater than or equal to about 0.044:1, greater than or equal to about 0.048:1, greater than or equal to about 0.05:1, greater than or equal to about 0.06:1, greater than or equal to about 0.07:1, greater than or equal to about 0.08:1, greater than or equal to about 0.085:1, greater than or equal to about 0.09:1, greater than or equal to about 10. about 0.09:1, greater than or equal to about 0.1:1, greater than or equal to about 0.11:1, greater than or equal to about 0.115:1, greater than or equal to about 0.12:1, greater than or equal to about 0.13:1, greater than or equal to about 0.15:1, greater than or equal to about 0.17:1, greater than or equal to about 0.18:1, greater than or equal to about 0.19:1, greater than or equal to about 0.2:1, greater than or equal to about 0.21:1, or greater than or equal to about 0.25:1. In the zinc oxide nanoparticles of the embodiment, the molar ratio of the Group 13 metal to zinc (Group 13 metal:Zn) may be less than or equal to about 0.7:1, less than or equal to about 0.5:1, less than or equal to about 0.4:1, less than or equal to about 0.35:1, less than or equal to about 0.3:1, less than or equal to about 0.25:1, less than or equal to about 0.23:1, less than or equal to about 0.21:1, less than or equal to about 0.2:1, less than or equal to about 0.16:1, or less than or equal to about 0.15:1.

[0281] In the zinc oxide nanoparticles of the embodiment, the molar ratio of the Group 13 metal to magnesium (Group 13 metal:Mg) may be greater than or equal to about 0.05:1, greater than or equal to about 0.1:1, greater than or equal to about 0.15:1, greater than or equal to about 0.2:1, greater than or equal to about 0.25:1, greater than or equal to about 0.3:1, greater than or equal to about 0.32:1, greater than or equal to about 0.35:1, greater than or equal to about 0.4:1, greater than or equal to about 0.45:1, greater than or equal to about 0.5:1, greater than or equal to about 0.5 5:1, greater than or equal to about 0.6:1, greater than or equal to about 0.65:1, greater than or equal to about 0.7:1, greater than or equal to about 0.75:1, greater than or equal to about 0.8:1, greater than or equal to about 0.85:1, greater than or equal to about 0.9:1, greater than or equal to about 0.95:1, greater than or equal to about 1:1, greater than or equal to about 1.3:1, greater than or equal to about 1.5:1, greater than or equal to about 1.7:1, greater than or equal to about 1.9:1, greater than or equal to about 2:1, or greater than or equal to about 2.1:1. In the zinc oxide nanoparticles of the embodiment, the molar ratio of the Group 13 metal to magnesium (Group 13 metal:Mg) may be less than or equal to about 3.2:1, less than or equal to about 3.1:1, less than or equal to about 3:1, less than or equal to about 2.9:1, less than or equal to about 2.8:1, less than or equal to about 2.7:1, less than or equal to about 2.6:1, less than or equal to about 2.5:1, less than or equal to about 2.4:1, less than or equal to about 2.35:1, less than or equal to about 2.3:1, less than or equal to about 2.2:1, less than or equal to about 2.1:1, less than or equal to about 2:1, less than or equal to about 1.8:1, less than or equal to about 1.6:1, less than or equal to about 1.4:1, less than or equal to about 1.2:1, less than or equal to about 1.1:1, less than or equal to about 1:1, less than or equal to about 0.9:1, or less than or equal to about 0.85:1.

[0282] In the zinc oxide nanoparticles of the embodiment, the molar ratio of the sum of magnesium and the Group 13 metal to zinc [(Mg+Group 13 metal):Zn] may be greater than or equal to about 0.15:1, greater than or equal to about 0.155:1, greater than or equal to about 0.16:1, greater than or equal to about 0.165:1, greater than or equal to about 0.17:1, greater than or equal to about 0.175:1, greater than or equal to about 0.18:1, greater than or equal to about 0.19:1, greater than or equal to about 0.20:1, greater than or equal to about 0.21:1, greater than or equal to about 0.23:1, greater than or equal to about 0.24:1, greater than or equal to about 0.25:1, greater than or equal to about 0.26:1, greater than or equal to about 0.27:1, greater than or equal to about 0.28:1, greater than or equal to about 0.29:1, greater than or equal to about 0.30:1, greater than or equal to about 0.31:1, greater than or equal to about 0.32:1, greater than or equal to about 0.33:1, greater than or equal to about 0.34:1, greater than or equal to about 0.35:1, greater than or equal to about 0.36:1, greater than or equal to about 0.37:1, greater than or equal to about 0.38:1, greater than or equal to about 0.39:1, greater than or equal to about 0. greater than or equal to about 0.2:1, greater than or equal to about 0.21:1, greater than or equal to about 0.22:1, greater than or equal to about 0.23:1, greater than or equal to about 0.24:1, greater than or equal to about 0.25:1, greater than or equal to about 0.26:1, greater than or equal to about 0.27:1, greater than or equal to about 0.28:1, greater than or equal to about 0.29:1, greater than or equal to about 0.3:1, or greater than or equal to about 0.35:1. In the zinc oxide nanoparticles of the embodiment, the molar ratio of the sum of magnesium and the Group 13 metal to zinc [(Mg+Group 13 metal):Zn] may be less than or equal to about 0.7:1, less than or equal to about 0.6:1, less than or equal to about 0.5:1, less than or equal to about 0.45:1, less than or equal to about 0.4:1, less than or equal to about 0.35:1, less than or equal to about 0.33:1, less than or equal to about 0.31:1, less than or equal to about 0.29:1, less than or equal to about 0.26:1, less than or equal to about 0.23:1, or less than or equal to about 0.2:1.

[0283] The zinc oxide nanoparticles according to the embodiment may or may not include an alkali metal in addition to the first metal (eg, it may be provided by a base containing an alkali metal).

[0284] The molar ratio of the alkali metal (e.g., sodium, potassium, cesium, rubidium, or the total molar amount thereof) to the first metal (e.g., magnesium or the total molar amount when two or more first metals are present) may be greater than or equal to about 0.005:1, greater than or equal to about 0.01:1, greater than or equal to about 0.015:1, greater than or equal to about 0.02:1, greater than or equal to about 0.025:1, greater than or equal to about 0.03:1, greater than or equal to about 0.04:1, greater than or equal to about 0.05:1, greater than or equal to about 0.06:1, greater than or equal to about 0.07:1, greater than or equal to about 0.08:1, greater than or equal to about 0.09:1, greater than or equal to about 0.1:1, greater than or equal to about 0.11:1, greater than or equal to about 0.12:1, greater than or equal to about 0.13:1, greater than or equal to about 0.14:1, greater than or equal to about 0.15:1, greater than or equal to about 0.16:1, greater than or equal to about 0.17:1, greater than or equal to about 0.18:1, greater than or equal to about 0.19:1, greater than or equal to about 0.20:1, greater than or equal to about 0.21:1, greater than or equal to about 0.22:1, greater than or equal to about 0.23:1, greater than or equal to about 0.24:1, greater than or equal to about 0.25:1, greater than or equal to about 0. or greater than about 0.14:1, about 0.15:1 or greater, about 0.16:1 or greater, about 0.17:1 or greater, about 0.18:1 or greater, about 0.19:1 or greater, about 0.2:1 or greater, about 0.22:1 or greater, about 0.24:1 or greater, about 0.26:1 or greater, about 0.28:1 or greater, about 0.3:1 or greater, about 0.32:1 or greater, about 0.34:1 or greater, about 0.36:1 or greater, about 0.38:1 or greater, about 0.4:1 or greater, about 0.42:1 or greater, about 0.44:1 or greater, about 0.46:1 or greater, about 0.48:1 or greater, or about 0.5:1 or greater. In the zinc oxide nanoparticles of the embodiment, the molar ratio of the alkali metal to the first metal may be less than or equal to about 2:1, less than or equal to about 1.7:1, less than or equal to about 1.5:1, less than or equal to about 1.3:1, less than or equal to about 1.1:1, less than or equal to about 1:1, less than or equal to about 0.9:1, less than or equal to about 0.7:1, less than or equal to about 0.65:1, or less than or equal to about 0.6:1.

[0285] In the zinc oxide nanoparticles of the embodiment, the molar ratio of the alkali metal (e.g., sodium, potassium, cesium, rubidium, or the sum thereof) to zinc may be greater than or equal to about 0.01:1, greater than or equal to about 0.02:1, greater than or equal to about 0.03:1, greater than or equal to about 0.035:1, greater than or equal to about 0.04:1, greater than or equal to about 0.05:1, greater than or equal to about 0.07:1, greater than or equal to about 0.09:1, greater than or equal to about 0.1:1, greater than or equal to about 0.13:1, or greater than or equal to about 0.15:1. In the zinc oxide nanoparticles of the embodiment, the molar ratio of the alkali metal (e.g., sodium, potassium, cesium, rubidium, or the sum thereof) to zinc may be less than or equal to about 0.5:1, less than or equal to about 0.4:1, less than or equal to about 0.3:1, less than or equal to about 0.2:1, less than or equal to about 0.1:1, less than or equal to about 0.08:1, less than or equal to about 0.06:1, or less than or equal to about 0.045:1.

[0286] In the zinc oxide nanoparticles of the embodiment, the molar ratio of the sum of the first metal and the alkali metal to zinc may be [(first metal+alkali metal):zinc)] and may be greater than or equal to about 0.1:1, greater than or equal to about 0.15:1, greater than or equal to about 0.17:1, greater than or equal to about 0.19:1, greater than or equal to about 0.2:1, greater than or equal to about 0.21:1, greater than or equal to about 0.23:1, greater than or equal to about 0.25 ... less than or equal to about 0.27:1, greater than or equal to about 0.29:1, or greater than or equal to about 0.3 and less than or equal to about 1:1, less than or equal to about 0.9:1, less than or equal to about 0.8:1, less than or equal to about 0.7:1, less than or equal to about 0.6:1, less than or equal to about 0.5:1, less than or equal to about 0.4:1, less than or equal to about 0.35:1, less than or equal to about 0.34:1, or less than or equal to about 0.31:1.

[0287] In XPS analysis of zinc oxide nanoparticles of embodiments, the zinc spectrum (e.g., Zn2p spectrum) may exhibit a peak (e.g., maximum intensity) at a binding energy of less than or equal to about 1047 eV (e.g., less than or equal to about 1045 eV) and greater than or equal to about 1042 eV.

[0288] In the XPS analysis of the zinc oxide nanoparticles of the embodiment, the oxygen (e.g., O1s) spectrum may have a full width at half maximum (FWHM) of less than 4 eV, less than or equal to about 3.9 eV, less than or equal to about 3.8 eV, less than or equal to about 3.7 eV, less than or equal to about 3.6 eV, less than or equal to about 3.5 eV, less than or equal to about 3.4 eV, less than or equal to about 3.3 eV, less than or equal to about 3.2 eV, less than or equal to about 3.6 eV, less than or equal to about 3.7 eV, less than or equal to about 3.8 eV, less than or equal to about 3.9 eV, less than or equal to about 3.8 eV, less than or equal to about 3.7 eV, less than or equal to about 3.6 eV, less than or equal to about 3.7 eV, less than or equal to about 3.8 eV, less than or equal to about 3.9 ... less than or equal to about 3.1 eV, less than or equal to about 3 eV, less than or equal to about 2.9 eV, less than or equal to about 2.8 eV, less than or equal to about 2.7 eV, less than or equal to about 2.6 eV, less than or equal to about 2.5 eV, less than or equal to about 2.4 eV, less than or equal to about 2.3 eV, less than or equal to about 2.25 eV, less than or equal to about 2.2 eV, less than or equal to about 2.1 eV, or less than or equal to about 2 eV. In the XPS analysis of the zinc oxide nanoparticles of the embodiment, the oxygen (e.g., O1s) spectrum may have a FWHM of about 1 eV or more, about 1.2 eV or more, about 1.5 eV or more, about 1.8 eV or more, about 1.9 eV or more, about 2.eV or more, about 2.3 eV or more, about 2.5 eV or more, or about 2.7 eV or more.

[0289] In an embodiment, the oxygen (e.g., O1s) intensity spectrum of the XPS analysis may have a half width at half maximum (HWHM) of less than or equal to about 3.5 eV, less than or equal to about 3.3 eV, less than or equal to about 3.1 eV, less than or equal to about 3 eV, less than or equal to about 2.9 eV, less than or equal to about 2.7 eV, less than or equal to about 2.5 eV, less than or equal to about 2.3 eV, less than or equal to about 2.2 eV, less than or equal to about 3.6 eV, less than or equal to about 3.9 eV, less than or equal to about 3.8 ... The intensity spectrum of oxygen (e.g., O1s) analyzed by XPS may have a half width at half maximum (HWHM) of greater than or equal to about 0.5 eV, greater than or equal to about 0.7 eV, or greater than or equal to about 0.8 eV.

[0290] In the XPS analysis of the zinc oxide nanoparticles of the embodiment, the O1s XPS intensity spectrum may include (e.g., may be resolved) a peak representing a metal-oxygen bond (hereinafter referred to as the first oxygen peak), a peak representing a hydroxyl moiety (hereinafter referred to as the third oxygen peak), or other peaks (e.g., a peak representing passivation by a ligand, e.g., the second oxygen peak), and the sum of the peaks may be understood as the O1s XPS intensity spectrum. The second oxygen peak may appear at a higher binding energy than the first oxygen peak, and the third oxygen peak may appear at a higher binding energy than the second oxygen peak. The first oxygen peak, the second oxygen peak, and the third oxygen peak may each independently be, for example, greater than or equal to about 525 eV, greater than or equal to about 527 eV, greater than or equal to about 528 eV, greater than or equal to about 530 eV, or greater than or equal to about 531 eV and less than or equal to about 535 eV, less than or equal to about 533 eV, less than or equal to about 531 eV, less than or equal to about 530 eV, less than or equal to about 529 eV, less than or equal to about 528 eV, less than or equal to about 526 eV, or a combination thereof.

[0291] The inventors have found that the zinc oxide nanoparticles of the embodiment can present an O1sXPS intensity spectrum as described herein, which can represent the surface aspects of the zinc oxide nanoparticles described herein. The zinc oxide nanoparticles of the embodiment can present improved passivation, and therefore, the ratio of the maximum intensity of the first oxygen peak to the maximum intensity of the second oxygen peak can be significantly reduced.

[0292] In the O1s XPS intensity spectrum of the zinc oxide nanoparticles of the embodiment, the intensity ratio of the first oxygen peak to the second oxygen peak (first oxygen peak: second oxygen peak) may be less than or equal to about 0.8: 1, less than or equal to about 0.7: 1, less than or equal to about 0.65: 1, less than or equal to about 0.6: 1, less than or equal to about 0.55: 1, less than or equal to about 0.5: 1, or less than or equal to about 0.45: 1. The intensity ratio of the first oxygen peak to the second oxygen peak may be greater than or equal to about 0.05: 1, greater than or equal to about 0.1: 1, greater than or equal to about 0.3: 1, greater than or equal to about 0.35: 1, greater than or equal to about 0.4: 1, greater than or equal to about 0.45: 1, greater than or equal to about 0.5: 1, or greater than or equal to about 0.55: 1. In the O1s XPS spectrum of the zinc oxide nanoparticles of one embodiment, the ratio of the intensity at a binding energy of 530 eV to the maximum intensity may be less than or equal to about 0.4:1, less than or equal to about 0.35:1, less than or equal to about 0.32:1, less than or equal to about 0.3:1, or less than or equal to about 0.25:1.

[0293] The zinc oxide nanoparticles may further include an alkali metal. In this case, in the zinc oxide nanoparticles, for example, a peak related to an alkali metal (e.g., an Rb3p peak) may be exhibited within a predetermined range (for Rb, within the following ranges: greater than or equal to about 230 eV to less than or equal to about 250 eV, greater than or equal to about 235 eV to less than or equal to about 245 eV, less than or equal to about 237 eV to less than or equal to about 240 eV, less than or equal to about 245 eV to less than or equal to about 250 eV, or a combination thereof). The peaks of the alkali metal may be at least two peaks.

[0294] The zinc oxide nanoparticles prepared according to the method of the embodiment may exhibit different decomposition patterns in thermogravimetric analysis.

[0295] As measured by differential thermogravimetric analysis (DTGA), the zinc oxide nanoparticles of the embodiment or the electron transport layer including the zinc oxide nanoparticles of the embodiment may show the following temperature representing the maximum weight reduction (maximum weight reduction temperature): greater than or equal to about 200° C., greater than or equal to about 250° C., greater than or equal to about 290° C., or greater than or equal to about 300° C. The maximum weight reduction temperature of the zinc oxide nanoparticles or the electron transport layer may be less than or equal to about 400° C., or less than or equal to about 380° C. In embodiments, the zinc oxide nanoparticles or the electron transport layer may exhibit a maximum peak temperature in a DTGA curve obtained by differentiating the TGA curve, for example, in a relatively high temperature range of 200°C or more, about 250°C or more, about 280°C or more, about 290°C or more, about 295°C or more, about 300°C or more, about 305°C or more, about 310°C or more, about 315°C or more, about 320°C or more, about 325°C or more, about 330°C or more to 350°C, about 345°C or less, about 340°C or less, about 335°C or less, about 330°C or less, or about 327°C or less.

[0296] As measured in thermogravimetric analysis at a decomposition temperature of 500° C. or higher (e.g., 600° C.), the zinc oxide nanoparticles or electron transport layer prepared according to the method of the embodiment may exhibit a total weight loss of about 22 weight percent or more (wt%), about 23 wt% or more, about 24 wt% or more, about 25 wt% or more, about 26 wt% or more, about 27 wt% or more, about 29 wt% or more, about 30 wt% or more, about 31 wt% or more, or about 32 wt% or more. In an embodiment, the total weight loss may be less than or equal to about 50 wt%, less than or equal to about 45 wt%, less than or equal to about 40 wt%, less than or equal to about 39 wt%, less than or equal to about 37 wt%, less than or equal to about 36 wt%, or less than or equal to about 35 wt%. In embodiments, the zinc oxide nanoparticles or electron transport layer as prepared may exhibit a weight residue of about 50 wt % or more, about 55 wt % or more, about 60 wt % or more, or about 65 wt % or more, as measured in thermogravimetric analysis at a decomposition temperature of about 500° C. or more (e.g., 550° C. or 600° C.).

[0297] Without wishing to be bound by theory, in embodiments, the zinc oxide nanoparticles may include carboxylate moieties (e.g., acetate moieties) and hydroxyl moieties as well as carbonate moieties on the surface, and these moieties are believed to be able to further passivate the zinc oxide nanoparticles (e.g., passivate zinc dangling bonds located on the surface of the particles), such that the resulting particles may exhibit a relatively increased amount of organic matter.

[0298] In the electroluminescent device of an embodiment, the zinc oxide nanoparticles exhibit a first absorption peak wavelength of greater than or equal to about 285 nm, greater than or equal to about 289 nm, greater than or equal to about 292 nm, or greater than or equal to about 295 nm and less than or equal to about 330 nm, less than or equal to about 315 nm, less than or equal to about 302 nm, less than or equal to about 300 nm, less than or equal to about 299 nm, less than or equal to about 298 nm, or less than or equal to about 297 nm, as analyzed by UV-Vis absorption spectroscopy. When the zinc oxide nanoparticles are analyzed by UV-Vis absorption spectroscopy, the zinc oxide nanoparticles exhibit a first absorption peak wavelength of less than or equal to about 320 nm, less than or equal to about 319 nm, less than or equal to about 318 nm, less than or equal to about 317 nm, less than or equal to about 316 nm, less than or equal to about 315 nm, less than or equal to about 314 nm, less than or equal to about 313 nm, less than or equal to about 312 nm, or less than or equal to about 311 nm. The first absorption peak wavelength may be greater than or equal to about 290 nm. The first absorption peak wavelength may be greater than or equal to about 295 nm, greater than or equal to about 300 nm, greater than or equal to about 301 nm, greater than or equal to about 302 nm, or greater than or equal to about 303 nm.

[0299] When the zinc oxide nanoparticles are analyzed by UV-Vis absorption spectroscopy, the UV-Vis absorption spectrum has a valley adjacent to the first absorption peak, and the valley depth of the valley defined by Equation 1 may be greater than or equal to about 0.01, greater than or equal to about 0.02, greater than or equal to about 0.027, greater than or equal to about 0.03, greater than or equal to about 0.035, greater than or equal to about 0.04, greater than or equal to about 0.045, greater than or equal to about 0.05, greater than or equal to about 0.055, or greater than or equal to about 0.06:

[0300] 1 - (Abs 谷 / Abs 第一 ) = VD (1)

[0301] Among them Abs 第一 is the absorbance at the wavelength of the first absorption peak and Abs 谷 is the absorbance at the lowest point of the valley, and VD is the valley depth.

[0302] The valley depth (VD) may be less than or equal to about 0.2, less than or equal to about 0.15, less than or equal to about 0.12, less than or equal to about 0.1, less than or equal to about 0.08, less than or equal to about 0.07, or less than or equal to about 0.06.

[0303] In an embodiment, the zinc oxide nanoparticles may have a band gap energy of about 3.6 eV or more, about 3.65 eV or more, about 3.7 eV or more, about 3.75 eV or more, about 3.77 eV or more, about 3.78 eV or more, or about 3.79 eV or more and about 3.95 eV or less, about 3.94 eV or less, about 3.9 eV or less, about 3.85 eV or less, about 3.8 eV or less, about 3.78 eV or less, about 3.77 eV or less, about 3.75 eV or less, or about 3.7 eV or less. The band gap energy may be determined by UV-Vis absorption spectroscopy analysis, for example, by the X-intercept value of the tangent line of the UV-Vis absorption curve.

[0304] In a photoluminescence spectrum obtained by irradiating light having a wavelength of 300 nm, the zinc oxide nanoparticles may exhibit a defect emission peak having an intensity ratio of about 10:1 or less, about 9:1 or less, about 8:1 or less, about 7:1 or less, about 6:1 or less, about 5:1 or less, about 4:1 or less, about 3:1 or less, about 2:1 or less, or about 1:1 or less relative to a band edge emission peak. In a photoluminescence spectrum obtained by irradiating light having a wavelength of 300 nm, the zinc oxide nanoparticles may exhibit a defect emission peak having an intensity ratio of about 0.1:1 or more, about 0.5:1 or more, about 0.9:1 or more, or about 1:1 or more relative to a band edge emission peak. The band edge emission peak wavelength may be about 350 nm or more and about 400 nm or less. The defect emission peak wavelength may be greater than or equal to about 450 nm and less than or equal to about 550 nm.

[0305] When zinc oxide nanoparticles prepared by conventional techniques are disposed on a quantum dot emission layer, the photoluminescence properties (e.g., photoluminescence quantum yield) of the quantum dot emission layer may be significantly reduced (hereinafter referred to as PL quenching phenomenon). Without wishing to be bound by any theory, it is believed that the PL quenching phenomenon may be due to traps present in the emission layer or the electron transport layer and the Forster resonance energy transfer (FRET) of the quantum dots. The inventors have found that, surprisingly, a layer including zinc oxide nanoparticles according to an embodiment may not cause such a PL quenching phenomenon when disposed on the quantum dot emission layer. In an embodiment, a stacked structure including an emission layer containing semiconductor nanocrystal particles and an electron transport layer based on the zinc oxide nanoparticles disposed on the emission layer may present the same or greater luminous efficiency of the emission layer.

[0306] In an embodiment, the zinc oxide nanoparticles may have, for example, desired dispersibility in a solution process of the method for manufacturing the electroluminescent device. In an embodiment, when dispersed in an alcohol solvent and measured by dynamic light scattering analysis, the zinc oxide nanoparticles may exhibit an average particle diameter (also referred to as a DLS average particle diameter) of about 4.5 nm or more, about 5 nm or more, about 5.5 nm or more, about 6 nm or more, about 6.5 nm or more, about 7 nm or more, or about 7.5 nm or more. The zinc oxide nanoparticles may have a DLS average particle diameter of about 500 nm or less, about 300 nm or less, about 150 nm or less, about 100 nm or less, about 50 nm or less, about 40 nm or less, about 30 nm or less, about 20 nm or less, about 10 nm or less, about 9 nm or less, about 8.5 nm or less, about 8 nm or less, about 7.5 nm or less, or about 7 nm or less. In one aspect, when dispersed in an alcohol solvent and the average particle diameter is measured by dynamic light scattering analysis, the zinc oxide nanoparticles may have an average particle diameter of about 5 nm or more and about 20 nm or less.

[0307] In an embodiment, the zinc oxide nanoparticles may have a size or average size (hereinafter referred to as "size") greater than or equal to about 1 nm, greater than or equal to about 3 nm, greater than or equal to about 5 nm, or greater than or equal to about 7 nm. The zinc oxide nanoparticles may have a size less than or equal to about 50 nm, for example, less than or equal to about 10 nm, less than or equal to about 8 nm, less than or equal to about 7.2 nm, or less than or equal to about 6.2 nm. The size of the zinc oxide nanoparticles may be a diameter or an equivalent diameter converted by assuming a spherical shape when not spherical. The size of the zinc oxide nanoparticles may be measured by electron microscopy [e.g., transmission electron microscopy (TEM)] analysis (e.g., a two-dimensional TEM image).

[0308] In an embodiment, an electron auxiliary layer (e.g., an electron transport layer) including the zinc oxide nanoparticles may be prepared by a solution process. In an embodiment, the electron transport layer may be formed by dispersing the zinc oxide nanoparticles in an organic solvent (e.g., a polar organic solvent, a non-polar organic solvent, or a combination thereof) to obtain a dispersion for forming an electron transport layer, and applying the dispersion to form a film. In an embodiment, the dispersion for forming an electron transport layer may be applied to the light-emitting layer. The solution process may further include removing the organic solvent from the formed film (e.g., by evaporation or heat treatment). The heat treatment (i.e., heat treatment) may be performed at a temperature greater than or equal to about 50°C, greater than or equal to about 60°C, greater than or equal to about 70°C, or greater than or equal to about 85°C and less than or equal to about 100°C.

[0309] In an embodiment, the thickness of the electron transport layer may be greater than or equal to about 5 nm, greater than or equal to about 6 nm, greater than or equal to about 7 nm, greater than or equal to about 8 nm, greater than or equal to about 9 nm, greater than or equal to about 10 nm, greater than or equal to about 11 nm, greater than or equal to about 12 nm, greater than or equal to about 13 nm, greater than or equal to about 14 nm, greater than or equal to about 15 nm, greater than or equal to about 16 nm, greater than or equal to about 17 nm, greater than or equal to about 18 nm, greater than or equal to about 19 nm, or greater than or equal to about 20 nm and less than or equal to about 120 nm, less than or equal to about 110 nm, less than or equal to about 100 nm, less than or equal to about 90 nm, less than or equal to about 80 nm, less than or equal to about 70 nm, less than or equal to about 60 nm, less than or equal to about 50 nm, less than or equal to about 40 nm, less than or equal to about 30 nm, or less than or equal to about 25 nm, but is not limited thereto.

[0310] In an embodiment, an electron injection layer may be further provided between the electron transport layer and the second electrode. The material of the electron injection layer is not particularly limited and may be appropriately selected.

[0311] In an embodiment, the electroluminescent device may further include a hole auxiliary layer 2 or 20 between the first electrode 1 or 10 and the light emitting layer 3 or 30. The hole auxiliary layer 2 or 20 may include a hole injection layer, a hole transport layer, an electron blocking layer, or a combination thereof. Figure 2-3B As shown in FIG. 1 , the hole assisting layer 2 or 20 may be a single layer or a multilayer structure in which adjacent layers include different components.

[0312] The hole auxiliary layer 2 or 20 may have a HOMO energy level that can match the HOMO energy level of the light-emitting layer 3 or 30 to improve the mobility of holes migrating from the hole auxiliary layer 2 or 20 to the light-emitting layer 3 or 30. In an embodiment, the hole auxiliary layer 2 or 20 may include a hole injection layer close to, for example, the first electrode 1 or 10, and a hole transport layer close to, for example, the light-emitting layer 3 or 30.

[0313] In an embodiment, the material included in the hole auxiliary layer 2 or 20 (e.g., a hole transport layer, a hole injection layer, or an electron blocking layer) is not particularly limited, and may include, for example, poly(9,9-dioctyl-fluorene-co-N-(4)-butylphenyl)-diphenylamine) (TFB), polyarylamine (polyarylamine), poly(N-vinylcarbazole), poly(3,4-ethylenedioxythiophene) (PEDOT), poly(3,4-ethylenedioxythiophene):polystyrene sulfonate (PEDOT:PSS), polyaniline, polypyrrole, N,N,N',N'-tetrakis(4-methoxyphenyl)-benzidine (TPD), 4,4'-bis[N-(1-naphthyl)-N-phenyl-amino]biphenyl (α-NPD), m-MTDATA (4,4',4"-tris[phenyl(m-tolyl)amino]triphenylamine), 4,4',4"-tris(N-carbazolyl)-triphenylamine (TCTA), 1,1-bis[(di-4-tolylamino)phenyl]cyclohexane (TAPC), p-type metal oxides (e.g., NiO, WO 3 、MoO 3 etc.), carbon-containing materials such as graphene oxide, or a combination thereof, but not limited thereto.

[0314] In the hole auxiliary layer, the thickness of each layer can be appropriately selected. For example, the thickness of each layer can be greater than or equal to about 5nm, greater than or equal to about 10nm, greater than or equal to about 15nm, or greater than or equal to about 20nm and less than or equal to about 100nm, less than or equal to about 90nm, less than or equal to about 80nm, less than or equal to about 70nm, less than or equal to about 60nm, less than or equal to about 50nm, less than or equal to about 40nm, less than or equal to about 35nm, or less than or equal to about 30nm, but is not limited thereto.

[0315] According to one embodiment, the device may have, for example, Figure 3A In the embodiment, and with reference to Figure 2In the device, the anode 10 disposed on the transparent substrate 100 may include a transparent electrode containing a metal oxide (e.g., an ITO electrode), and the cathode 50 facing the anode 10 may include a conductive metal. The conductive metal may have a relatively low work function, such as Mg, Al, etc. A hole auxiliary layer 20 may be provided between the transparent electrode and the light-emitting layer 30. The hole auxiliary layer 20 may be a hole injection layer such as PEDOT:PSS or a p-type metal oxide, or a hole transport layer such as TFB or polyvinylcarbazole (PVK). The hole injection layer may be disposed close to the transparent electrode, and the hole transport layer may be disposed close to the light-emitting layer. An electron auxiliary layer 40 including an electron transport layer and optionally an electron injection layer may be disposed between the light-emitting layer 30 and the cathode 50. The details of the electron transport layer may be as described above.

[0316] A device according to another embodiment may have an inverted structure. Here, the second electrode 50 provided on the transparent substrate 100 may include a transparent electrode containing a metal oxide, and the anode 10 facing the cathode 50 may include a metal. For example, the metal oxide of the transparent electrode containing a metal oxide may be ITO, and the anode may be a metal having a relatively high work function, such as Au, Ag, etc. For example, an electron auxiliary layer 40 (including an electron transport layer and optionally an electron injection layer) may be provided between the transparent electrode and the light emitting layer 30. The details of the electron transport layer may be as described above. As Figure 3B As shown in FIG. 1 , MoO may be provided between the metal anode 10 and the light emitting layer 30. 3 or other p-type metal oxides as the hole auxiliary layer 20. For example, the hole auxiliary layer 20 may be a hole transport layer including TFB or PVK, or a hole transport layer including MoO 3 Or a hole injection layer of other p-type metal oxide.

[0317] The above devices can be manufactured by appropriate methods. For example, the electroluminescent device can be manufactured as follows: a hole auxiliary layer is optionally formed on a substrate on which a first electrode is formed, a light-emitting layer including semiconductor nanoparticles is formed, an electron auxiliary layer (including an electron transport layer) is formed on the light-emitting layer, and a second electrode is formed on the electron auxiliary layer. The method for forming the electrode / hole auxiliary layer / light-emitting layer can be appropriately selected and is not particularly limited. The formation of the hole auxiliary layer can be carried out by deposition or coating. Forming a light-emitting layer including semiconductor nanoparticles may include forming a pattern of the semiconductor nanoparticles. The formation of the electron auxiliary layer may be carried out by vapor deposition or coating.

[0318] As described above, the electroluminescent device of the embodiment may exhibit an improved level of electroluminescent properties together with a prolonged lifespan.

[0319] In an embodiment, the electroluminescent device may have a maximum external quantum efficiency (EQE) of about 5%, about 5.5%, about 6%, about 6.5%, about 7%, about 7.5%, about 7.7%, about 8%, about 8.5%, about 9%, about 9.5%, about 10%, about 10.5%, about 11%, about 11.5%, about 12%, about 12.5%, about 13%, about 13.5%, or about 14%. The maximum external quantum efficiency (EQE) may be about 40%, about 30%, or about 20%.

[0320] The electroluminescent device of the embodiment may have a maximum brightness of greater than or equal to about 50,000 candelas / square meter (cd / m 2 ), greater than or equal to about 60,000 cd / m 2 , greater than or equal to approximately 70,000 cd / m 2 , greater than or equal to about 80,000cd / m 2 , greater than or equal to about 90,000cd / m 2 , greater than or equal to approximately 100,000 cd / m 2 , greater than or equal to approximately 150,000 cd / m 2 , greater than or equal to approximately 200,000 cd / m 2 , greater than or equal to approximately 250,000 cd / m 2 , greater than or equal to approximately 300,000 cd / m 2 , greater than or equal to approximately 310,000 cd / m 2 , greater than or equal to approximately 320,000 cd / m 2 , greater than or equal to approximately 330,000 cd / m 2 , greater than or equal to approximately 340,000 cd / m 2 , greater than or equal to approximately 350,000 cd / m 2 , greater than or equal to approximately 360,000 cd / m 2 , greater than or equal to approximately 370,000 cd / m 2 , greater than or equal to approximately 380,000 cd / m 2 , greater than or equal to approximately 390,000 cd / m 2 , greater than or equal to approximately 400,000 cd / m 2 , greater than or equal to approximately 440,000 cd / m 2, greater than or equal to approximately 500,000 cd / m 2 , or greater than or equal to approximately 550,000 cd / m 2 The maximum brightness may be about 50,000 cd / m 2 -Approx. 1,000,000cd / m 2 、About 70,000cd / m 2 -About 600,000cd / m 2 , or about 90,000cd / m 2 -About 500,000cd / m 2 .

[0321] The electroluminescent device of the embodiment may be configured to emit blue light, green light, or red light. The peak emission wavelength of the blue light, the peak emission wavelength of the green light, or the peak emission wavelength of the red light is the same as described herein.

[0322] In an embodiment, as measured by driving the electroluminescent device at a predetermined initial brightness (e.g., about 650 nits), the electroluminescent device may exhibit a T50 of about 200 hours or more, about 250 hours or more, about 300 hours or more, about 350 hours or more, about 400 hours or more, about 450 hours or more, about 500 hours or more, about 550 hours or more, about 600 hours or more, about 650 hours or more, or about 700 hours or more. The T50 may be about 275 hours to about 4000 hours, about 330 hours to about 2000 hours, about 350 hours to about 1500 hours, about 420 hours to about 1000 hours, or about 430 hours to about 900 hours.

[0323] In embodiments, the electroluminescent device may have a T90 of about 5 hours or more, for example, a T90 of about 10 hours or more, about 20 hours or more, about 30 hours or more, about 40 hours or more, about 50 hours or more, about 60 hours or more, about 70 hours or more, about 80 hours or more, about 90 hours or more, about 100 hours or more, about 110 hours or more, about 120 hours or more, about 130 hours or more, about 140 hours or more, about 150 hours or more, about 160 hours or more, about 170 hours or more, about 180 hours or more, about 190 hours or more, or about 200 hours or more, as measured by driving the device at a predetermined initial brightness (e.g., about 650 nits). The T90 may be about 35 hours to about 1500 hours, about 55 hours to about 1200 hours, about 85 hours to about 1000 hours, about 105 hours to about 900 hours, about 115 hours to about 800 hours, or about 145 hours to about 500 hours.

[0324] The electroluminescent device (when driven at a predetermined brightness, such as 650 nits) may have an initial voltage of less than or equal to about 3 volts, for example, less than or equal to about 2.9 volts, or less than or equal to about 2.88 volts. The initial voltage may be greater than or equal to about 2.5 volts, greater than or equal to about 2.6 volts, or greater than or equal to about 2.7 volts.

[0325] Under an applied voltage of 1 volt, the electroluminescent device may have a leakage current density of 0.1 mA / cm2. 2 ) or less, 0.05mA / cm 2 Or smaller, 0.01mA / cm 2 or less, or 0.005mA / cm 2 or less. The leakage current density may be 0.0001 mA / cm 2 or greater, 0.0005mA / cm 2 or greater, or 0.001mA / cm 2 or larger.

[0326] In an embodiment, a display device or an electronic apparatus may include the electroluminescent device.

[0327] The display device may include a first pixel and a second pixel configured to emit light of a color different from the color of the first pixel. In the first pixel, the second pixel, or both, an electroluminescent device according to an embodiment may be provided. In an embodiment, the display device may further include a blue pixel, a red pixel, a green pixel, or a combination thereof. In the display device, the red pixel may include a red light-emitting layer including a plurality of red light-emitting semiconductor nanoparticles, the green pixel may include a green light-emitting layer including a plurality of green light-emitting semiconductor nanoparticles, and the blue pixel may include a blue light-emitting layer including a plurality of blue light-emitting semiconductor nanoparticles. The electroluminescent device according to an embodiment may be provided in the blue pixel, the red pixel, or the green pixel, for example, in the blue pixel.

[0328] Reference Figure 3C , the display panel 1000 according to the embodiment includes a display area 1000D for displaying an image and a non-display area 1000P disposed around the display area 1000D in which a bonding element may be located.

[0329] The display area 1000D may include a plurality of pixels PX arranged along rows (eg, X direction) and / or columns (eg, Y direction), and each pixel PX may include a plurality of sub-pixels PX displaying different colors. 1 , PX 2 , and PX 3 As an example, Figure 3C The three sub-pixels PX are shown in FIG. 1 , PX 2 , and PX 3 The configuration of a pixel PX is constituted, but the configuration is not limited thereto. It may further include additional sub-pixels such as white sub-pixels, and may include one or more sub-pixels displaying the same color. The plurality of pixels PX may be arranged, for example, in a Bayer matrix, a PenTile matrix, and / or a diamond matrix, but is not limited thereto.

[0330] Sub-pixel PX 1 , PX 2 , and PX 3 Each may be configured to display one of the three primary colors or a combination of the three primary colors, for example, red, green, blue, or a combination thereof (for example, white light). 1 Can be configured to display red, the second sub-pixel PX 2 can be configured to display green, and the third sub-pixel PX 3 Can be configured to display blue.

[0331] exist Figure 3CIn the embodiment, the sub-pixels are each depicted as having the same size, but the present disclosure is not limited thereto. For example, at least one of the sub-pixels may be larger or smaller than another sub-pixel, or have a different shape.

[0332] In an embodiment, the display panel of the embodiment may include a light emitting panel, which may include a lower substrate 110, a buffer layer 111, a thin film transistor TFT, and a light emitting element 180. The display panel may further include circuit elements for switching and / or driving each of the light emitting elements.

[0333] Reference Figure 3D In the light emitting panel of the embodiment, for each sub-pixel PX 1 , PX 2 , and PX 3 A light emitting element 180 is provided. 1 , PX 2 , and PX 3 The light emitting elements 180 in the embodiment may be driven independently. The sub-pixels may include a blue sub-pixel, a red sub-pixel, or a green sub-pixel. At least one of the light emitting elements 180 may be an electroluminescent element according to the embodiments described herein.

[0334] The details of the substrate are the same as described herein. The buffer layer 111 may include an organic material, an inorganic material, or an organic-inorganic material. The buffer layer 111 may include, for example, an oxide, a nitride, or an oxynitride, and may include, for example, silicon oxide, silicon nitride, silicon oxynitride, or a combination thereof, but is not limited thereto. The buffer layer 111 may be one layer or two or more layers, and may cover a portion or the entire surface of the lower substrate 110. The buffer layer 111 may be omitted.

[0335] The thin film transistor TFT may be a three-terminal element for switching and / or driving the light emitting element 180, and may include one or two or more for each sub-pixel. The thin film transistor TFT may include a gate electrode 124, a semiconductor layer 154 overlapping the gate electrode 124, a gate insulating layer 140 between the gate electrode 124 and the semiconductor layer 154, and a source electrode 173 and a drain electrode 175 electrically connected to the semiconductor layer 154. A coplanar top gate structure is shown as an example, but the structure is not limited thereto and may have a different structure.

[0336] The gate electrode 124 is electrically connected to a gate line (not shown) and may include, for example, a low resistance metal such as aluminum (Al), molybdenum (Mo), copper (Cu), titanium (Ti), silver (Ag), gold (Au), alloys thereof, or combinations thereof, but is not limited thereto.

[0337] The semiconductor layer 154 may be an inorganic semiconductor such as amorphous silicon, polycrystalline silicon, or an oxide semiconductor; an organic semiconductor; an organic-inorganic semiconductor; or a combination thereof. For example, the semiconductor layer 154 may include an oxide semiconductor including at least one of indium (In), zinc (Zn), tin (Sn), and gallium (Ga), and the oxide semiconductor may include, for example, indium gallium zinc oxide, zinc tin oxide, or a combination thereof, but they are not limited thereto. The semiconductor layer 154 may include a channel region and doped regions disposed on both sides of the channel region and electrically connected to the source electrode 173 and the drain electrode 175, respectively.

[0338] The gate insulating layer 140 may include an organic material, an inorganic material, or an organic-inorganic material, and may include, for example, an oxide, a nitride, or a nitride oxide, and may include, for example, silicon oxide, silicon nitride, silicon oxynitride, or a combination thereof, but is not limited thereto. In the drawings, an example is illustrated in which the gate insulating layer 140 is formed on the entire surface of the lower substrate 110, but the present disclosure is not limited thereto and may be selectively formed between the gate electrode 124 and the semiconductor 154. The gate insulating layer 140 may be formed of one or two or more layers.

[0339] The source electrode 173 and the drain electrode 175 may include, for example, a low resistance metal such as aluminum (Al), molybdenum (Mo), copper (Cu), titanium (Ti), silver (Ag), gold (Au), an alloy thereof, or a combination thereof, but are not limited thereto. The source electrode 173 and the drain electrode 175 may be electrically connected to the doped regions of the semiconductor layer 154, respectively. The source electrode 173 is electrically connected to a data line (not shown), and the drain electrode 175 is electrically connected to the light emitting element 180.

[0340] In addition, an interlayer insulating layer 145 is formed between the gate electrode 124 and the source / drain electrodes 173 and 175. The interlayer insulating layer 145 may include an organic material, an inorganic material, or an organic-inorganic material, for example, an oxide, a nitride, or a nitride oxide, for example, silicon oxide, silicon nitride, silicon oxynitride, or a combination thereof, but is not limited thereto. The interlayer insulating layer 145 may be formed of one or two or more layers.

[0341] A protective layer 160 is formed on the thin film transistor TFT. The protective layer 160 may be, for example, a passivation layer. The protective layer 160 may include an organic material, an inorganic material, or an organic-inorganic material, for example, a (meth) acrylic polymer, polyimide, polyamide, poly(amide-imide), or a combination thereof, but is not limited thereto. The protective layer 160 may be formed of one or two or three or more layers.

[0342] In an embodiment, one of the first electrode 1 , 10 and the second electrode 5 , 50 may be a pixel electrode connected to a TFT, and the other one thereof may be a common electrode.

[0343] In an embodiment, the electroluminescent device or a display apparatus including the same may be used in a top emission type, a bottom emission type, a dual emission type, or a combination thereof.

[0344] In an embodiment, the first electrodes 1, 10 may be light-transmitting electrodes, and the second electrodes 5, 50 may be reflective electrodes, and the display panel may be a bottom-emission display panel that emits light toward the first electrode 10 and, if present, the substrate 100. In an embodiment, the first electrodes 1, 10 may be reflective electrodes, and the second electrodes 5, 50 may be light-transmitting electrodes, and the display panel may be a top-emission display panel that emits light to the opposite side of the first electrode 10 and, if present, the substrate 100. In an embodiment, both the first electrode and the second electrode may be semi-transparent electrodes, and the display panel 1000 may be a double-side emission display panel that emits light on a substrate side and on an opposite side of the substrate.

[0345] The display device or electronic apparatus may include (or may be) an augmented reality (AR) device, a virtual reality (VR) device, a handheld terminal (e.g., a device), a monitor, a notebook computer, a television, an electronic display panel, a camera, an electronic display component for an autonomous vehicle or an electric vehicle.

[0346] Hereinafter, the embodiments are described in more detail with reference to examples. However, these examples are exemplary, and the present scope is not limited thereto.

[0347] Example

[0348] Analytical methods

[0349] 1. Electroluminescence Measurement

[0350] The current according to the applied voltage was measured with a Keithley 2635B source meter, and the electroluminescent properties (eg, brightness and EQE) of the light-emitting device were measured using a CS2000 spectrometer.

[0351] 2. Lifespan characteristics

[0352] (1) T50: A device is initially driven at a predetermined brightness (eg, 650 nits) and the time taken for the brightness of a given device to decrease to 50% of its initial brightness is measured.

[0353] (2) T90: A device is initially driven at a predetermined brightness (eg, 650 nits) and the time taken for the brightness of a given device to decrease to 90% of its initial brightness is measured.

[0354] (3) The initial voltage is the first voltage of a device measured when the device is operated at a predetermined luminance for measurement of its lifetime.

[0355] 3.XPS analysis

[0356] XPS analysis was performed using an X-ray photoelectron spectrometer (manufacturer: Physical Electronics, model name: Quantum2000).

[0357] 4.ICP-AES analysis

[0358] Inductively coupled plasma atomic emission spectrometry (ICP-AES) analysis was performed using Shimadzu ICPS-8100.

[0359] 5.TEM analysis

[0360] Transmission electron microscopy analysis of the prepared nanoparticles was performed using a UT F30 Tecnai electron microscope.

[0361] 6. Photoluminescence Analysis

[0362] Photoluminescence (PL) analysis was performed using a Hitachi F-7100 spectrophotometer.

[0363] 7. UV-Vis spectroscopy

[0364] UV-visible absorption spectrum analysis was performed using Shimadzu UV-2600 spectrophotometer and provided UV-visible absorption spectrum. Band gap energy was obtained based on the following equation from the X-intercept value of the UV-visible absorption spectrum:

[0365] Bandgap energy (eV) = 1240 (nm) / X intercept value (nm)

[0366] 8.TGA analysis

[0367] The Trios V3.2 system (TA Instruments) was used to 2 Thermogravimetric analysis was performed from 20°C to 600°C at a heating rate of 10°C / min under a 37°C atmosphere.

[0368] 9. Dynamic Light Scattering (DLS) Analysis

[0369] DLS analysis was performed using Otsuka, ELSZ-2000.

[0370] Unless otherwise stated, the following syntheses were performed under an inert atmosphere (eg, under nitrogen). Unless otherwise stated, precursor amounts are provided as molar amounts.

[0371] Synthesis Example 1:

[0372] Se / trioctylphosphine (TOP) stock solution [2 mol / L (M)], S / TOP stock solution (1M), and Te / TOP stock solution (0.1M) were prepared by dispersing selenium (Se), sulfur (S), and tellurium (Te) in trioctylphosphine (TOP), respectively. In a reactor containing trioctylamine, 0.125 millimoles (mmol) of zinc acetate were added to the reactor together with oleic acid and heated at 120° C. under reduced pressure (e.g., under vacuum). After 1 hour, nitrogen was introduced into the reactor.

[0373] The reactor was heated to 240°C and a Se / TOP stock solution and a Te / TOP stock solution at a Te:Se molar ratio of 1:15 were quickly added to the reactor. When the reaction was complete, the reaction mixture was quickly cooled to room temperature and acetone was added to promote the formation of a precipitate. The mixture (suspension) was centrifuged to separate the solids, which were then dispersed in toluene to provide ZnSeTe cores (dispersion in toluene).

[0374] Zinc acetate [1.8 millimoles (mmol)] was added to the flask containing trioctylamine together with oleic acid, and the mixture was heated at 120° C. under reduced pressure for 10 minutes. Nitrogen (N 2 ) was introduced into a reactor, and the reactor was heated to 220° C. The prepared ZnTeSe core particle dispersion was quickly added to the reactor, and Se / TOP stock solution and S / TOP stock solution at a Se:S molar ratio of 1:2 were also added to the reactor, and the reactor temperature was raised to about 280° C. After 2 hours, the reactor was cooled to room temperature, and ethanol was added to precipitate semiconductor nanoparticles, which were separated by centrifugation.

[0375] The prepared semiconductor nanoparticles emit blue light at about 460 nanometers (nm).

[0376] Preparation Example 1 (ZnMgO:Rb 2 CO 3 5%):

[0377] Rubidium carbonate (Cas No. 584-09-8) was dissolved in ethanol to provide a 0.1 M metal carbonate solution.Tetramethylammonium hydroxide (first base) was dissolved in ethanol to provide a 0.55 M base solution.

[0378] In a flask containing dimethyl sulfoxide, zinc acetate dihydrate (powder) and magnesium acetate tetrahydrate (powder) were added and dissolved, and the alkali solution and the metal carbonate solution were added thereto and stirred at room temperature for 60 minutes.

[0379] Ethyl acetate is added to precipitate the particles, and the formed precipitate is centrifuged. The obtained particles are washed two or more times with ethyl acetate to provide zinc oxide nanoparticles including magnesium (i.e., zinc oxide magnesium nanoparticles, also referred to as ZnMgO). The obtained nanoparticles are redispersed in ethanol and subjected to transmission electron microscopy analysis. The size of the zinc oxide magnesium nanoparticles is calculated to be about 3nm-4.5nm.

[0380] The molar ratio between the magnesium precursor and the zinc precursor was 0.15:0.85. The metal carbonate content was 5 mol% based on the Zn content (5 mol per 100 mol of Zn).

[0381] The obtained nanoparticles were subjected to UV-Vis absorption spectroscopy analysis, DLS analysis, and TGA analysis, and the results are shown in Figure 4 , 5A , and 5B.

[0382] The obtained zinc oxide nanoparticles were subjected to photoluminescence analysis (e.g., defect emission peak), and the results are shown in Figure 6 middle.

[0383] The obtained zinc oxide nanoparticles were subjected to XPS analysis, and the results are shown in FIG. 7 and Table 2.

[0384] The obtained zinc oxide nanoparticles were subjected to ICP-AES analysis, and the results are summarized in Table 3.

[0385] Preparation Comparative Example 1:

[0386] Zinc oxide nanoparticles (raw ZnMgO) were produced in the same manner as in Preparation Example 1, except that the rubidium carbonate solution was not used.

[0387] Preparation Example 2 (ZnMgO:Ga+Rb 2 CO 3 5%):

[0388] Potassium hydroxide (second base) was dissolved in ethanol to provide a 0.4 M base solution. Rubidium carbonate was dissolved in ethanol to provide a metal carbonate solution.

[0389] A mixed solvent obtained by mixing ethanol (relative polarity: 0.654) and cyclohexane (relative polarity: 0.006) at a ratio (volume) of 1:1 was added to the flask and stirred. Zinc acetate dihydrate (powder) and magnesium acetate tetrahydrate (powder) were added to the flask and dissolved by heating to 55° C. in a nitrogen atmosphere, and then the alkali solution and the metal carbonate solution were added to the flask and stirred at 30° C. for 60 minutes.

[0390] Ethyl acetate is added to the reaction solution to precipitate particles, and the formed precipitate is centrifuged. The particles obtained are washed twice or more with ethyl acetate to provide ZnMgO nanoparticles (i.e., prepared by the LSS method, hereinafter, the first nanoparticles). The nanoparticles obtained are redispersed in ethanol and analyzed by transmission electron microscopy. The average size of the particles is calculated to be about 3nm.

[0391] Gallium chloride is dissolved in ethanol to provide a gallium precursor solution. Tetramethylammonium hydroxide (first base) is dissolved in ethanol to provide a 0.55M base solution. Ethanol and the first nanoparticles synthesized above are added to the flask and dispersed, and the temperature is maintained at 30°C. The gallium precursor solution and the base solution are added to the flask, and the reaction is allowed to proceed for 60 minutes. Based on the zinc used in the preparation of the first nanoparticles, the gallium content used is 5 mol%. After the reaction is complete, ethyl acetate (EA) is added to precipitate nanoparticles, and the nanoparticles are separated and washed twice or more to provide zinc oxide nanoparticles including magnesium and gallium.

[0392] The obtained nanoparticles were subjected to UV-Vis absorption spectroscopy analysis, DLS analysis, and TGA analysis, and the results are shown in Figure 4 , 5A , and 5B.

[0393] Preparation Example 3 (ZMO:Rb 2 CO 3 8%):

[0394] Zinc oxide nanoparticles were prepared in the same manner as in Preparation Example 1, except that the content of rubidium carbonate was changed to 8 mol % based on the Zn content.

[0395] Preparation Example 4 (ZMO:Rb 2 CO 3 10%):

[0396] Zinc oxide nanoparticles were prepared in the same manner as in Preparation Example 1, except that the content of rubidium carbonate was changed to 10 mol % based on the Zn content.

[0397] Table 1

[0398]

[0399] like Figure 4 As shown in Table 1, the zinc oxide nanoparticles prepared in Preparation Example 1 and Preparation Example 2 have a first absorption peak of 305 nm or less and a clear valley.

[0400] From Table 1, Figure 5A and5B The results of the present invention confirm that the zinc oxide nanoparticles of Preparation Example 1 and Preparation Example 2 exhibit a decomposition mode different from the decomposition mode of the zinc oxide nanoparticles of Preparation Comparative Example 1 prepared without using a metal carbonate, and also have a relatively high TGA residual content. The results show that the zinc oxide nanoparticles prepared in Preparation Example 1 and Preparation Example 2 may have an increased amount of surface ligands compared to the zinc oxide particles of Preparation Comparative Example 1. Without wishing to be bound by theory, it is believed that this is because, in the zinc oxide nanoparticles of Preparation Example 1 and Preparation Example 2, not only -OH and CH 3 COO - The carbonate ions serve to passivate Zn dangling bonds on the surface of the particles. Figure 5B The DTG data shown in the table indicate that the decomposition pattern (or degree of decomposition) of the carbon-containing functional groups in the zinc oxide nanoparticles of Preparation Example 1 and Preparation Example 2 is different from that of the zinc oxide nanoparticles of Preparation Comparative Example 1. Without wishing to be bound by theory, Figure 5B The difference in the DTG data shown in may be due to the incorporation of carbonate ions into the zinc oxide nanoparticles prepared in Preparation Example 1 and Preparation Example 2.

[0401] like Figure 6 As shown in the photoluminescence analysis results, the zinc oxide nanoparticles prepared in Preparation Example 1 exhibited a significantly lower level of trap emission intensity than the zinc oxide nanoparticles prepared in Preparation Comparative Example 1. Without wishing to be bound by theory, it is believed that the reduction in trap emission may be caused by the binding of carbonate ions on the surface of the metal oxide nanoparticles.

[0402] Fig. 7A The O1s XPS spectrum of the zinc oxide nanoparticles prepared in Example 1 and the 2 CO 3 O1s XPS spectrum of the sample obtained by simply blending into the zinc oxide nanoparticles of Preparation Comparative Example 1 (ie, O1s peak). Figure 7B The Zn2p XPS spectrum of the zinc oxide nanoparticles prepared in Example 1 and the Rb 2 CO 3 Zn2p XPS spectrum of the sample obtained by simply blending into the zinc oxide nanoparticles of Preparation Comparative Example 1 (ie, Zn2p peak).

[0403] like Fig. 7A As shown in the example 1, the zinc oxide nanoparticles were prepared by 2 CO 3The sample obtained by simply blending into the zinc oxide nanoparticles of Preparation Comparative Example 1 has a peak (first peak) in the range of about 532eV-533eV, and exhibits a lattice oxygen peak (second peak) of the metal oxide at 531eV. However, the zinc oxide nanoparticles of Preparation Example 1 show that the intensity of the first peak is significantly reduced compared to the intensity of the second peak, and thus the full width at half maximum (FWHM) and half width at half maximum (HWHM) of the Os1 peak are less than 3.0eV and less than 2.0eV, respectively. In contrast, in the case of the sample containing the zinc oxide nanoparticles of Preparation Comparative Example 1, the intensity of the second peak is significantly increased, and the ratio of the second peak intensity to the intensity of the first peak is high, and it is confirmed that the full width at half maximum (FWHM) and half width at half maximum (HWHM) of the Os1 peak are greater than 3.0eV and greater than 2.0eV, respectively. Without wishing to be bound by theory, it is believed that when carbonate ions are provided in the synthesis step under the conditions detailed in the preparation of zinc oxide nanoparticles prepared in Example 1, the particle surface metal oxide lattice oxygen may be reduced and the provided carbonate ions may be bonded to the Zn—OH surface via hydrogen bonds.

[0404] like Figure 7B As shown in FIG. 1 , in the case of the zinc oxide nanoparticles of Preparation Example 1, the Zn2p peak shifts toward lower binding energy and is thus shown in a range below 1045 eV. Without wishing to be bound by theory, the results may indicate that, in the case of the zinc oxide nanoparticles of Preparation Example 1, carbonate ions provide passivation for Zn dangling bonds on the surface of the particles in the form of bridging, chelating, or monodentate adsorption.

[0405] Table 2

[0406]

[0407] Without wishing to be bound by theory, it is believed that when an alkali metal carbonate precursor is added during the synthesis of the ZnMgO of the preparation examples, the adsorption of carbonates to the surface of the ZnMgO may change the composition / aspect (orientation) of the surface ligands compared to the original ZnMgO, and therefore, the binding of peripheral carbon-containing functional groups on the resulting particles may also change.

[0408] Table 3

[0409] Zn Mg Preparation Example 1 About 0.88 About 0.12 Preparation Comparative Example 1 About 0.88 About 0.12

[0410] As shown in Table 3, there is no significant difference between the molar compositions of zinc and magnesium in the particles of Preparation Example 1 and Comparative Preparation Example 1.

[0411] Fabrication of electroluminescent devices

[0412] Example 1

[0413] A semiconductor nanoparticle solution was prepared by dispersing in octane the semiconductor nanoparticles prepared in Synthesis Example 1. An ETL dispersion was prepared by dispersing in ethanol the zinc oxide nanoparticles prepared in Preparation Example 1.

[0414] An electroluminescent device (ITO / PEDOT:PSS (35 nm) / TFB (25 nm) / QD light emitting layer (20 nm) / ETL (20 nm) / Al (100 nm)) was fabricated according to the following method.

[0415] After the glass substrate deposited with ITO was surface treated with UV-ozone for 15 minutes, a PEDOT:PSS solution (HC Starks, Inc.) was spin-coated thereon and heat-treated at 150° C. for 10 minutes in an air atmosphere and then in N 2 The resulting mixture was heat treated at 150° C. for 20-30 minutes in an atmosphere to form a 35 nm thick hole injection layer.

[0416] On the hole injection layer, poly[(9,9-dioctylfluorene-2,7-diyl-co-(4,4'-(N-4-butylphenyl)diphenylamine] solution (TFB) (Sumitomo Corp.) was spin-coated and heat-treated at 150° C. for 30 minutes to form a 25 nm thick hole transport layer.

[0417] On the hole transport layer, the semiconductor nanoparticle solution was spin-coated to form a 20 nm thick light emitting layer.

[0418] On the light emitting layer, the ETL dispersion was spin-coated and heat-treated for 30 minutes to form an electron transport layer (thickness: 20 nm).

[0419] On the obtained electron transport layer, aluminum (Al) (thickness: 100 nm) was vacuum deposited to form a second electrode and thereby manufacture an electroluminescent device.

[0420] The electroluminescent properties and lifetime of the fabricated electroluminescent device were measured, and the results are summarized in Table 4. The maximum external quantum efficiency (Max EQE) of the fabricated electroluminescent device was 9.4%.

[0421] Example 2

[0422] An electroluminescent device was manufactured in the same manner as in Example 1, except that the zinc oxide nanoparticles prepared in Preparation Example 2 were used.

[0423] The electroluminescent properties and lifetime of the fabricated electroluminescent device were measured, and the results are summarized in Table 4. The maximum external quantum efficiency (Max EQE) of the fabricated electroluminescent device was 10.3%.

[0424] Example 3

[0425] An electroluminescent device was manufactured in the same manner as in Example 1, except that the zinc oxide nanoparticles prepared in Preparation Example 3 were used.

[0426] The electroluminescent properties and lifetime of the fabricated electroluminescent devices were measured, and the results are summarized in Table 4.

[0427] Example 4

[0428] An electroluminescent device was manufactured in the same manner as in Example 1, except that the zinc oxide nanoparticles prepared in Preparation Example 4 were used.

[0429] The electroluminescent properties and lifetime of the fabricated electroluminescent devices were measured, and the results are summarized in Table 4.

[0430] Comparative Example 1

[0431] An electroluminescent device was manufactured according to the same method as in Example 1, except that the nanoparticles manufactured in Comparative Preparation Example 1 were used. The electroluminescent properties and lifetime of the electroluminescent device were measured, and the results are summarized in Table 4.

[0432] The maximum external quantum efficiency (Max EQE) of the fabricated electroluminescent device was 8.1%.

[0433] Table 4

[0434]

[0435] As shown in Table 4, the electroluminescent device of the example exhibits improved electroluminescent properties and extended life characteristics compared to the electroluminescent device of Comparative Example 1. For the electroluminescent device of Comparative Example 1, the electroluminescent device of Example 1, and the electroluminescent device of Example 2, the leakage current was determined by measuring the current density according to the applied voltage. The results are shown in Figure 8 In. Figure 8 As shown in , the leakage current in the electroluminescent device of the embodiment is significantly smaller than that in the electroluminescent device of the comparative example.

[0436] Experimental Example 1

[0437] A semiconductor nanoparticle solution prepared by dispersing the semiconductor nanoparticles prepared in Synthesis Example 1 in octane was prepared. The zinc oxide nanoparticles prepared in Preparation Example 1 were dispersed in ethanol to provide ETL Dispersion 1. The zinc oxide nanoparticles prepared in Comparative Preparation Example 1 were dispersed in ethanol to provide ETL Dispersion 2.

[0438] In the same manner as in Example 1, on a glass substrate, a light-emitting layer was formed using a semiconductor nanoparticle solution, and on the formed light-emitting layer, an electron transport layer was provided using ETL dispersion 1 to provide a stacked structure 1. Similarly, in the same manner as in Example 1, on a glass substrate, a light-emitting layer was formed using a semiconductor nanoparticle solution, and on the formed light-emitting layer, an electron transport layer was formed using ETL dispersion 2 to provide a stacked structure 2. In the same manner as in Example 1, on a glass substrate, a light-emitting layer was formed using a semiconductor nanoparticle solution to provide a stacked structure 3.

[0439] Photoluminescence analysis was performed on each of stacked structure 1 (glass / QD / manufacturing example 1 ZnMgO), stacked structure 2 (glass / QD / manufacturing comparative example 1 ZnMgO), and stacked structure 3 (glass / QD), and the results are shown in FIG. Fig. 9 middle.

[0440] like Fig. 9 As shown in , stacked structure 2 exhibits significant PL quenching compared to stacked structure 3, which, without wishing to be bound by any theory, is believed to be due to trapping and FRET effects. In contrast, stacked structure 1 exhibits increased PL emission compared to stacked structure 3.

[0441] While the disclosure has been described in conjunction with what are presently considered to be practical example embodiments, it is to be understood that the invention is not limited to the disclosed embodiments, but, on the contrary, is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.

Claims

1. A method for producing an electroluminescent device, wherein include: Disposing a light-emitting layer including semiconductor nanoparticles on the first electrode; providing zinc oxide nanoparticles; depositing a composition including the zinc oxide nanoparticles onto the light emitting layer to provide an electron transport layer, the zinc oxide nanoparticles including a first metal; and A second electrode is provided on the electron transport layer to provide the electroluminescent device, wherein the first metal comprises an alkaline earth metal, zirconium, tungsten, titanium, yttrium, aluminum, gallium, indium, tin, cobalt, vanadium, or a combination thereof, wherein the zinc oxide nanoparticles have a particle size greater than or equal to 1 nanometer and less than or equal to 50 nanometers, wherein providing zinc oxide nanoparticles comprises A first metal precursor, a zinc precursor, a base, and a metal carbonate compound are contacted in an organic solvent to form the zinc oxide nanoparticles.

2. The method of claim 1, wherein the first metal comprises magnesium, zirconium, tungsten, titanium, yttrium, aluminum, gallium, indium, tin, cobalt, vanadium, or a combination thereof.

3. The method of claim 1, wherein the providing zinc oxide nanoparticles comprises dissolving the first metal precursor and the zinc precursor in the organic solvent to provide a first solution; adding the base and the metal carbonate compound to the organic solvent before dissolving the first metal precursor and the zinc precursor in the organic solvent, or adding the base and the metal carbonate compound to the first solution; and The zinc precursor and the first metal precursor are allowed to react in the presence of the base and the metal carbonate compound.

4. The method of claim 1, wherein the electron transport layer does not exhibit a peak attributable to rubidium, cesium, or a combination thereof as determined by X-ray photoelectron spectroscopy analysis. 5 . The method of claim 1 , wherein the organic solvent is a solvent mixture including a first solvent and a second solvent, and a relative polarity difference between the first solvent and the second solvent is greater than or equal to 0.3 and less than or equal to 0.

9.

6. The method of claim 1, wherein the base comprises a first base, a second base, or a combination thereof, The first base includes an organic base containing a C1-C50 organic group, and The second base includes an inorganic base containing an alkali metal or an alkaline earth metal.

7. The method of claim 6, wherein the base comprises the second base, The second base comprises an alkali metal hydroxide, and The molar ratio between the second base and the first base (second base: first base) is 1:0-1:

10.

8. The method of claim 1, wherein the metal carbonate compound comprises an alkali metal carbonate, an alkali metal bicarbonate, an alkaline earth metal carbonate, or a combination thereof.

9. The method of claim 1, wherein the base comprises a C1-C30 alkylammonium hydroxide compound, an alkali metal hydroxide, or a combination thereof, and the metal carbonate compound comprises rubidium carbonate, rubidium bicarbonate, cesium carbonate, cesium bicarbonate, or a combination thereof.

10. The method of claim 1, wherein the zinc oxide nanoparticles have a core-shell structure, and providing the zinc oxide nanoparticles having a core-shell structure further comprises: include: dispersing the formed zinc oxide nanoparticles in a third solvent; adding an additional metal precursor and a third base to the third solvent; and reacting the additional metal precursor and the third base to form a layer containing an additional metal on the formed zinc oxide nanoparticles, and Wherein the additional metal is different from the first metal and comprises an alkaline earth metal, zirconium, tungsten, titanium, yttrium, aluminum, gallium, indium, tin, cobalt, vanadium, or a combination thereof.

11. The method of claim 1, wherein the composition does not include cesium carbonate, rubidium carbonate, lithium carbonate, sodium carbonate, potassium carbonate, or a combination thereof.

12. Electroluminescent devices, include: a first electrode and a second electrode spaced apart from each other; and a light-emitting layer disposed between the first electrode and the second electrode; as well as An electron transport layer is provided between the light emitting layer and the second electrode, wherein the light-emitting layer comprises semiconductor nanoparticles, wherein the electron transport layer comprises zinc oxide nanoparticles, wherein the zinc oxide nanoparticles comprise a first metal, and the first metal comprises an alkaline earth metal; and optionally zirconium, tungsten, titanium, yttrium, aluminum, gallium, indium, tin, cobalt, vanadium, or a combination thereof, wherein the zinc oxide nanoparticles have a size greater than or equal to 1 nanometer and less than or equal to 50 nanometers, wherein in the X-ray photoelectron spectroscopy analysis of the zinc oxide nanoparticles, the O1s peak has a half-maximum width less than or equal to 3 electron volts, wherein the light emitting layer is configured to emit blue light, Wherein the electroluminescent device is configured to exhibit a maximum brightness greater than or equal to 60,000 candelas per square meter.

13. The electroluminescent device of claim 12, wherein the O1s peak has a half width at half maximum (HWHM) less than or equal to 2.5 electron volts.

14. The electroluminescent device of claim 12, wherein the O1s peak has a ratio of intensity at 530 electron volts to maximum intensity of less than or equal to 0.3:

1.

15. The electroluminescent device of claim 12, wherein the electron transport layer does not exhibit a peak attributable to rubidium, cesium, or a combination thereof as determined by X-ray photoelectron spectroscopy analysis.

16. The electroluminescent device of claim 12, wherein the zinc oxide nanoparticles comprise magnesium and gallium, Wherein in the zinc oxide nanoparticles, the amount of gallium is greater than or equal to 3 mol % and less than or equal to 25 mol % based on the total moles of zinc, magnesium, and gallium.

17. The electroluminescent device of claim 12, wherein in an X-ray photoelectron spectroscopy analysis of the zinc oxide nanoparticles, an O1s X-ray photoelectron spectroscopy intensity spectrum has a full width at half maximum of less than or equal to 2.5 electron volts and a half width at half maximum of less than or equal to 1.9 electron volts.

18. The electroluminescent device of claim 12, wherein The electroluminescent device has a maximum external quantum efficiency greater than or equal to 6%, or The electroluminescent device exhibits a T90 greater than or equal to 255 hours, as measured at an initial brightness of 650 nits.

19. The electroluminescent device of claim 12, wherein the electroluminescent device is manufactured by the method of any one of claims 1-11.

20. An electronic device comprising the electroluminescent device according to any one of claims 12 to 19.

21. The electronic device of claim 20, wherein the display device comprises a handheld terminal device, a monitor, a notebook computer, a television, an electronic display board, a camera, or an electronic component for an electric vehicle.

Citation Information

Patent Citations

  • Apparatus for detecting 5g edge network intrusion using multiple learning models and method using the same

    KR1020230061932A