Rotary dresser and manufacturing method thereof

By forming a super abrasive grain layer on the rotary trimmer and adjusting the ratio of super abrasive grain action surfaces of different particle sizes, the problems of short life and sharpness deviation of the rotary trimmer are solved, and higher wear resistance and stable rotation are achieved Temperature performance.

CN118946432APending Publication Date: 2024-11-12A L M T CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380030247.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2023-03-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing rotary trimmer has a short life, and the sharpness and life deviations are large, making it difficult to effectively extend its service life in forming rotary trimmers.

Method used

The super abrasive grain layer is formed on the base metal, combined with the metal material, and the first and second super abrasive grains with different average particle sizes are used to form multiple action surfaces to increase the concentration and action area ratio of the super abrasive grain layer to ensure that The total area of ​​the working surface is 30% or more than 60%, and the wear resistance and sharpness of the rotary trimmer are improved by adjusting the grinding amount.

Benefits of technology

By increasing the working area ratio of the super abrasive grain layer, extending the life of the rotary trimmer, improving its sharpness and wear resistance, ensuring stable performance, and increasing the working area of ​​diamond to improve dressing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946432A_ABST
    Figure CN118946432A_ABST
Patent Text Reader

Abstract

A rotary dresser having a super abrasive grain layer in which super abrasive grains are bonded into one layer via a plating layer on a base metal, the super abrasive grains including first super abrasive grains having a first average particle diameter and second super abrasive grains having a second average particle diameter smaller than the first average particle diameter, the first super abrasive grains having a first average particle diameter, and the second super abrasive grains having a second average particle diameter smaller than the first average particle diameter, among the first super abrasive grains and the second super abrasive grains, a plurality of super abrasive grains exposed on the surface of the super abrasive grain layer form active surfaces, and the total area ratio of the plurality of active surfaces to the area of an imaginary plane that gently connects the plurality of active surfaces in a region where the concentration of the super abrasive grains is the highest is 30-60%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a rotary dresser. This application claims priority based on Japanese patent application No. 2022-052113 filed on March 28, 2022. All the contents described in the Japanese patent application are incorporated herein by reference. Background Art

[0002] International Publication No. 2017 / 145491 (Patent Document 1) describes reducing the variation in sharpness and life while extending the life of a rotary dresser.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: International Publication No. 2017 / 145491 Summary of the invention

[0006] The rotary dresser disclosed in the present invention has a superabrasive layer on a base metal in which superabrasives are bonded into one layer by a metal bonding material, and the superabrasives have: a first superabrasive having a first average particle size, and a second superabrasive having a second average particle size smaller than the first average particle size, and a plurality of superabrasives exposed on the surface of the superabrasive layer among the first superabrasives and the second superabrasives form an active surface, and in an area where the concentration of the superabrasives is the highest, the total area ratio of the plurality of active surfaces relative to the area of ​​an imaginary surface smoothly connecting the active surfaces is greater than 30% and less than 60%. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] [ Figure 1 ] Figure 1 is a photograph of a diamond rotary dresser 100 according to an embodiment of the present disclosure.

[0008] [ Figure 2 ] Figure 2 This is a photograph of the grooves 102 provided in the superabrasive grain layer 101 of the diamond rotary dresser 100 according to the embodiment.

[0009] [ Figure 3 ] Figure 3 This is a photograph of the superabrasive layer 101 including the grooves 102 shown to explain the method of measuring the effective area.

[0010] [ Figure 4 ] Figure 4 This is a photograph of the superabrasive layer 101 before trimming so as to include the grooves 102 , which is shown to explain the method of measuring the effective area.

[0011] [ Figure 5 ] Figure 5 This is a photograph showing the surface of the cut groove 102 for explaining the method of measuring the active area.

[0012] [ Figure 6 ] Figure 6 It is a graph showing the height (horizontal axis) of each action surface 205 from the measurement start point and the frequency (vertical axis) obtained from the photograph of the groove 102 subjected to planarization.

[0013] [ Figure 7 ] Figure 7 1 is a diagram showing a cross-sectional structure of the superabrasive grain layer 101 along a direction from the center toward the outer periphery of the diamond rotary dresser 100 .

[0014] [ Figure 8 ] Figure 8 Graph showing the grain size and frequency of the superabrasive grains 204 constituting the grooves 102 whose area ratios were measured.

[0015] [ Fig. 9 ] Fig. 9 This is a diagram for explaining a grinding method of the superabrasive grains 204 for forming the action surface 205 . DETAILED DESCRIPTION

[0016] [Problems to be Solved by the Present Disclosure]

[0017] Conventional rotary dressers have a problem of short life.

[0018] A rotary dresser is a dresser that shapes (truing or dressing) the grinding surface of a grindstone. As one of the representative rotary dressers, there is a disc-shaped rotary dresser used for shaping or dressing a grindstone for gear processing. The rotary dresser forms an action surface on a plurality of abrasive grains, and the total area ratio of the action surfaces of the plurality of abrasive grains is set to 5 to 30% relative to the area of ​​an imaginary surface smoothly connecting the plurality of action surfaces, thereby achieving the effect of reducing the deviation of sharpness and life while extending the life of the rotary dresser.

[0019] The rotary dresser having the above-mentioned structure can obtain the above-mentioned effects as a disc-shaped rotary dresser for a gear, but even if the above-mentioned features are applied to a molded rotary dresser or the like, there is still a problem of short life.

[0020] In order to solve the above problems, it is conceivable to increase the effective area of ​​diamond and, for this purpose, to increase the amount of processing for forming the effective surface of diamond or to fill fine particles between coarse grains to make the abrasive grains dense.

[0021] To achieve this, the present disclosure relates to a rotary dresser having the following features.

[0022] A rotary dresser has a superabrasive layer formed by superabrasive grains bonded to a single layer by a metal bonding material on a base metal, wherein the superabrasive grains include: first superabrasive grains having a first average grain size, and second superabrasive grains having a second average grain size smaller than the first average grain size, and a plurality of superabrasive grains exposed on the surface of the superabrasive layer among the first superabrasive grains and the second superabrasive grains form an active surface, and in an area where the concentration of the superabrasive grains is the highest, the total area ratio of the plurality of active surfaces is 30 to 60% relative to the area of ​​an imaginary surface smoothly connecting the active surfaces.

[0023] If the total area ratio is less than 30%, the effective surface is too small and the life is shortened. If the total area ratio exceeds 60%, the effective surface is too large and the sharpness is deteriorated.

[0024] In order to make the total area ratio be between 30% and 60%, it is easy to achieve by using superabrasive grains with a small average particle size. In order to improve the sharpness and life of the rotary dresser, for example, it is necessary to use superabrasive grains with an average particle size of about 0.3 to 0.8 mm. When large superabrasive grains are used, the total area ratio of multiple action surfaces relative to the area of ​​the imaginary surface tends to become smaller. In order to increase the total area ratio, the amount of grinding used to form the action surface on the superabrasive grains increases. By combining a second superabrasive grain with a small diameter, even if the amount of grinding used to form the action surface is reduced, the total area ratio of multiple action surfaces relative to the area of ​​the imaginary surface can be increased to 30 to 60%. As a result, the life of the rotary dresser is also improved.

[0025] By adopting the rotary dresser having such a configuration, it is possible to realize a rotary dresser having improved wear resistance and stable sharpness and life.

[0026] Since diamonds play a role during processing, the life span increases as the number of diamonds increases.

[0027] The concentration (number of abrasive grains) of a grinding wheel has a great influence on performance such as sharpness, but in the case of a rotary dresser, the effective area of ​​the diamond part that acts has a great influence on performance, especially since abrasive grains with an average grain size of about 300 to 800 μm are mostly used, so the influence on performance is significant. In the present disclosure, since the effective area ratio of superabrasive grains is high, the sharpness of the dresser is good and the life is also improved.

[0028] Preferably, the second average particle size is 30% to 80% of the first average particle size. If the average particle size of the second superabrasive grains is 30 to 80% of the average particle size of the first superabrasive grains, the second superabrasive grains are easy to enter between the first superabrasive grains, the abrasive grain density becomes higher, and the effective area ratio of the abrasive grains is easy to increase.

[0029] When synthetic diamond is used as superabrasive grains, since the crystal face of diamond is a clearly visible shape, the crystal face is nearly parallel to the bonding surface of the base metal. As a result, the superabrasive grains are closely bonded in a stable form, and even if the amount of grinding used to form the active surface on the superabrasive grains is reduced, the active area ratio can be increased. As a result, the active surface is easily formed, and since the thickness of the superabrasive grain layer becomes thicker, the life is also improved.

[0030] Preferably, the ratio of the maximum grain size to the minimum grain size of the first superabrasive grains and the second superabrasive grains (maximum grain size D1 of the first superabrasive grains / minimum grain size D3 of the second superabrasive grains) is 1.3 to 4.

[0031] Preferably, the first average particle size is 300 μm or more and 800 μm or less. In order to dress the grindstone with a rotary dresser, the particle size of the abrasive grains of the grindstone is about 100 μm to 200 μm. When the abrasive grain diameter of the rotary dresser is not larger than the particle size of the abrasive grains of the grindstone, the dressing performance of the rotary dresser is reduced, so it is set to be 300 μm or more. In addition, as the forming shape of the superabrasive layer of the rotary dresser, R is about 400 μm. In order to correspond to this shape, the average particle size of the first abrasive grain is preferably 800 μm or less.

[0032] Preferably, the superabrasive grains are synthetic diamonds.

[0033] Preferably, when observing a cross section of the superabrasive grain layer, within a certain range, the average value of the distance between each first superabrasive grain and the base metal is smaller than the average value of the distance between each second superabrasive grain and the base metal.

[0034] Preferably, the rotary dresser of the present disclosure is manufactured through a process including the following steps.

[0035] The step (1) is to prepare a reverse mold having a predetermined shape formed on the inner surface of the mold, and to attach superabrasive grains to the inner surface of the mold by a plating method.

[0036] Step (2) is to further perform build-up plating to embed the superabrasive grains with the plating metal and completely fix them.

[0037] Step (3) is a step of placing a core metal at the center of the inverted mold and bonding the superabrasive grains to the core metal.

[0038] The step (4) is a step of removing the outer inverted mold.

[0039] As described above, the production is performed by the reverse method (or reverse plating method).

[0040] As described above, if the rotary dresser of the present invention is made by the inversion method, both the first superabrasive grains and the second superabrasive grains exist on the surface side of the abrasive layer of the rotary dresser, and the total area ratio of the action surfaces formed on the plurality of superabrasive grains is easily increased, and the life is also increased. In addition, when the rotary dresser of the present invention is used for dressing, the second superabrasive grains with a small average particle size can also effectively act on the dressing, so even if the number of superabrasive grains as a whole is reduced, the total area ratio of the action surfaces formed on the plurality of superabrasive grains can be increased.

[0041] In the rotary dresser made by this method, the distance from the bottom end of the first superabrasive grain and the second superabrasive grain to the base metal is inconsistent due to the random deviation of each superabrasive grain. The core metal may be the base metal or may not be the base metal. In the case where the core metal is not the base metal, the core metal is also provided with a structure for joining the core metal to the base metal.

[0042] The method of measuring the action surface is described. Figure 1 is a photograph of a diamond rotary dresser 100 according to an embodiment of the present disclosure. Figure 1 As shown, the diamond rotary dresser 100 includes a base metal 103 and a super abrasive grain layer provided on the surface of the base metal 103 .

[0043] The base metal 103 is made of, for example, stainless steel. The base metal 103 is cylindrical, and a superabrasive layer 101 is provided on the outer peripheral surface of the base metal 103. Diamond as a superabrasive is fixed in the superabrasive layer 101. It should be noted that CBN (cubic boron nitride) can also be used instead of diamond. In addition, diamond and cubic boron nitride can also exist in a mixed state.

[0044] Grooves 102 extending in the circumferential direction are formed in the superabrasive grain layer 101. The grooves 102 are formed along the shape of the workpiece. Such a diamond rotary dresser 100 dresses a so-called shaped grindstone.

[0045] Figure 2 FIG. 1 is a photograph of the groove 102 provided in the superabrasive grain layer 101 of the diamond rotary dresser 100 according to the embodiment. Figure 2 As shown, in the groove 102 , the action surface 205 of the superabrasive grain 204 is exposed. The action surface 205 is a surface that contacts with the target material (grindstone) and performs dressing. The superabrasive grain 204 is held by the plating layer 203 . Figure 2The two digits in are numbers for identifying each superabrasive grain 204. The concentration of superabrasive grains 204 is the highest in the groove 102. As for the region with the highest concentration, when measuring the active surface in the region divided along the axial direction (direction orthogonal to the circumferential direction) in the superabrasive layer 101 with a circumferential length of more than 10 mm and containing more than 50 abrasive grains, the portion with the highest concentration is selected. The area ratio of the active surface 205 in such superabrasive grains 204 is measured by the following method.

[0046] Measuring instrument: VR5000 manufactured by KEYENCE. The measuring principle is the "light section method". The analysis steps are: (1) Three-dimensional measurement. (2) Planarize the shape by using either or both of the following A and B. A: Fluctuation removal (cutoff processing). Planarize fluctuations above a certain wavelength. B: Secondary curve correction. Planarize the arc shape obtained by fitting the entire shape with a secondary curve. (3) Set a threshold and calculate the effective area.

[0047] Figure 3 This is a photograph of a superabrasive layer 101 including grooves 102 for explaining the method of measuring the effective area. Figure 3 As shown, the focus is set at the deepest part of the groove 102, and the superabrasive layer including the groove 102 is photographed. The X direction is a direction that crosses the groove 102. The Y direction is a circumferential direction along the direction in which the groove 102 extends. Figure 3 , the height of the superabrasive grain layer 101 along the X direction and the Y direction is shown.

[0048] Figure 4 This is a photograph of the superabrasive layer 101 before cutting to include the groove 102, which is shown to illustrate the method of measuring the effective area. Three locations with the highest concentration (the parts with high concentration of abrasive particles visually) are selected as measurement locations. Cutting is performed to include these locations. The size of the measurement range is set to a length of 10 mm or more in the Y direction and a range of about 50 to 200 abrasive particles.

[0049] Figure 5 1 is a photograph showing the surface of the cut groove 102 for explaining the method of measuring the effective area. Figure 5 As shown, the cropping area 105 is set to perform cropping in such a way that only the groove 102 is photographed. Then, the image of the cropping area 105 is subjected to plane correction. The plane correction includes fluctuation correction and quadratic curve correction. Thus, the photograph of the groove 102 as a curved surface can be replaced with a flat photograph.

[0050] Figure 6This is a graph showing the height (horizontal axis) and frequency (vertical axis) of each action surface 205 from the measurement start point obtained from a photograph of the groove 102 processed by planarization. There is a deviation in the height of the action surface 205 (diamond top) of each superabrasive grain 204 from the measurement start point. The height with the highest frequency is set as the reference height. Figure 6 In the example, 1.320 mm is the reference height, and a height 0.02 mm lower than this height is used as the threshold.

[0051] Set the unnecessary area removal. In the micro area removal setting, set the lower limit of noise removal to [0.01mm 2 ], and remove areas smaller than this area from the total area.

[0052] Using the threshold value and the lower limit value of noise removal, the total area of ​​the active surface 205 and the area ratio (55.2%) of the active surface 205 to the area of ​​the cutout region are calculated.

[0053] Figure 7 1 is a diagram showing a cross-sectional structure of a superabrasive grain layer 101 along a direction from the center toward the periphery of a diamond rotary dresser 100. In the superabrasive grain layer 101, a low melting point alloy 202 is stacked on a base metal 103. A plating layer 203 is stacked on the low melting point alloy 202. Superabrasive grains 204 are fixed by the plating layer.

[0054] That is, in Figure 6 In the process of calculating: in the region where the concentration of the superabrasive grains 204 is the highest, the total area ratio of the plurality of action surfaces 205 relative to the area of ​​the imaginary surface 206 smoothly connected to the action surfaces 205 is calculated.

[0055] The action surface 205 of the superabrasive grains 204 is formed by grinding or polishing the superabrasive grains 204. The area of ​​the action surface 205 can be adjusted by changing the time for grinding or polishing the superabrasive grains 204.

[0056] Figure 8 Graph showing the particle size and frequency of the superabrasive grains 204 constituting the grooves 102 whose area ratios were measured. In order to measure the particle size of the superabrasive grains 204, the superabrasive grains 204 are removed from the grooves 102. Specifically, the superabrasive grains 204 are removed by etching or electrolytic polishing using a chemical suitable for the metal bonding material holding the superabrasive grains 204. For example, when the metal holding the superabrasive grains 204 is nickel, the active surface 205 is immersed in a nickel etching solution.

[0057] The particle size of the superabrasive grains 204 was measured by a Malvern imaging particle size distribution device Morphologi. The measurement result showed that there were at least two peaks P1 and P2. A boundary line 401 was drawn in the valley between the peaks P1 and P2, and the diameter side larger than the boundary line 401 was defined as the first superabrasive grain, and the diameter side smaller than the boundary line 401 was defined as the second superabrasive grain.

[0058] The maximum particle size of the first superabrasive grains is D1, the minimum particle size of the first superabrasive grains is D2, the maximum particle size of the second superabrasive grains is D2, and the minimum particle size of the second superabrasive grains is D3.

[0059] The average particle diameters of the first superabrasive grains and the second superabrasive grains can be measured by a Malvern-made imaging particle size distribution apparatus, Morphologi.

[0060] When the protrusion of the super abrasive grains 204 is small, Figure 6 The mountain of the load curve shown becomes wider. Therefore, it is difficult to determine the height of the maximum frequency. In this case, the plating layer 203 holding the superabrasive grains 204 is dissolved by etching to make the superabrasive grains 204 protrude, thereby enabling measurement.

[0061] In this embodiment, the area ratio of the superabrasive grains 204 in the grooves 102 is measured. However, in the diamond rotary dresser 100, there are cases where the grooves 102 are not present but Figure 2 There are rotary dressers with a constant height in the X direction, and there are rotary dressers with a convex shape toward the periphery in the X direction. In these cases, the area ratio of the portion with the highest concentration is also measured by the above method.

[0062] Fig. 9 2 is a diagram for explaining a grinding method of superabrasive grains 204 for forming an action surface 205. Fig. 9 As shown, the first superabrasive grains 1204 of coarse grains and the second superabrasive grains 2204 of fine grains constituting the superabrasive grains are fixed on the base metal 103. The top surface of the first superabrasive grain 1204 is used as the reference surface 280, and the cutting depth H is cut therefrom to form the action surface 205. By increasing the cutting depth H, the proportion of the action surface 205 can be increased.

[0063] When observing the cross section of the superabrasive grain layer 101 , within a certain range, the average value of the distance between each first superabrasive grain 1204 and the base metal 103 is smaller than the average value of the distance between each second superabrasive grain 2204 and the base metal 103 .

[0064] (Example 1)

[0065] In order to confirm the performance difference caused by the difference in the effective area ratio, a rotary dresser of the specifications shown in Table 1 was made and a dressing test of a grindstone was carried out. The unit of the average particle size of coarse and fine particles is μm, which is the same as in other tables. The grindstone diameter is 300 mm, the grindstone peripheral speed is 19.1 m / s, the grindstone rotation speed is 1216 rpm, the rotary dresser diameter is 70 mm, the rotary dresser peripheral speed is 8.8 m / s, the rotary dresser rotation speed is 2400 rpm, the peripheral speed ratio is 0.46, the cutting speed is 0.3 um / rev, the dressing time (dress out) is 3 sec, and the grindstone is a vitrified bond grinding wheel using CBN abrasives.

[0066] [Table 1]

[0067]

[0068] Life index ※Comparison based on 5μm wear as life

[0069] In Table 1, the life index and dressing resistance index represent the ratio of the life and dressing resistance of each sample number when the life and dressing resistance of sample number 3 are set to 1. The unit of "the amount of cutting into the surface of the superabrasive layer" is μm, which is equivalent to Fig. 9 The amount of H. In the samples with an active area ratio of less than 30%, the life was significantly shortened compared to the samples with an active area ratio of 30% or more.

[0070] In addition, when the effective area ratio exceeds 60%, it is very troublesome to manufacture a sample with such an effective area ratio, and the yield rate is also deteriorated. That is, although a sample with a large amount of cutting into the surface of the superabrasive layer and an effective area ratio of 65% was manufactured and tested, due to the high resistance during dressing, chattering occurred.

[0071] In addition, in order to compare with the conventional rotary dresser, a sample with an average particle size of 650 μm of abrasive grains was prepared. As shown in sample numbers 10 to 16, samples with different effective area ratios were prepared. Compared with sample numbers 1 to 9, there was no significant difference in life and resistance during dressing. However, in the production of rotary dressers, it is very troublesome to adjust the effective area ratio, and it is difficult to mass produce.

[0072] (Example 2)

[0073] Next, an experiment was conducted to investigate the difference caused by the difference in the grain size ratio between the first abrasive grains and the second abrasive grains and the difference in the ratio between the maximum and minimum abrasive grain diameters.

[0074] The preferred ranges of the particle diameter ratios are set because the main issue is the production of a high-quality rotary dresser, rather than the performance of the rotary dresser.

[0075] In this test, the average particle size of the first abrasive was set to 650 μm, and by changing the average particle size of the second abrasive, the difference caused by the difference in particle size ratio and the difference in the ratio of the maximum to the minimum abrasive diameter was confirmed. In addition, the obtained rotary dresser was used to evaluate the life and dressing resistance.

[0076] Tables 2 and 3 show sample numbers 21 to 50 manufactured in this Example 2.

[0077] [Table 2]

[0078]

[0079] [Table 3]

[0080]

[0081] In this test, a rotary dresser was made, and the surface of the superabrasive layer was cut into with a grindstone to form an action surface on the abrasive grains. The unit of "the amount of cutting into the surface of the superabrasive layer" is μm, which is equivalent to Fig. 9 The amount of H is increased in stages, and the change behavior of the effective area ratio at this time is observed. In addition, the effective area ratio of the first superabrasive grain and the effective area ratio of the second superabrasive grain are also measured at each stage, and the extent to which the second abrasive grain is in a state of acting on dressing is also confirmed. Fig. 9 The following is a process for cutting into the surface of the superabrasive layer.

[0082] As a result, for samples whose average particle size ratio deviated from the range of 30 to 80%, the effective area of ​​the second superabrasive grains was 0% or very small at any stage. In contrast, it was confirmed that the proportion of the effective surface formed in the second superabrasive grains increased when the average particle size ratio fell within the range of 30 to 80%. Therefore, it can be seen that by adding the second superabrasive grains, it is easy to control the increase in the effective area ratio, and it is easy to make a high-quality rotary dresser.

[0083] In addition, from the difference in the ratio of the maximum to the minimum abrasive grain diameter, the samples whose maximum grain diameter / minimum grain diameter value deviates from 1.3 to 4 have an active area of ​​the second abrasive grain of 0% at any stage. The abrasive grains whose maximum grain diameter / minimum grain diameter value falls within 1.3 to 4 also form an active surface on the second abrasive grain. Therefore, it can be seen that by adding the second superabrasive grain, it is easy to control the increase in the active area ratio, and it is easy to produce a high-quality rotary dresser.

[0084] Then, under the same conditions as in Example 1, a grinding stone dressing test was carried out using Sample Nos. 21 to 50. The results are shown in Tables 4 and 5.

[0085] [Table 4]

[0086] Sample No. Life expectancy index Resistance index during trimming 21 0.7 0.8 22 1.1 1.1 23 1.7 1.2 24 1.5 1.4 25 1.6 1.2 26 0.7 0.8 27 1.1 1.1 28 1.5 1.2 29 1.7 1.3 30 2.2 1.4 31 0.7 0.8 32 1.4 1.1 33 2.1 1.5 34 2.3 1.6 35 2.2 1.5

[0087] Life index ※Comparison based on 5μm wear as life

[0088] [Table 5]

[0089] Sample No. Life expectancy index Resistance index during trimming 36 0.7 0.8 37 1.2 1.1 38 1.8 1.4 39 2.0 1.3 40 1.8 1.3 41 0.8 0.8 42 1.2 1.1 43 1.5 1.2 44 1.7 1.3 45 1.6 1.3 46 0.8 0.8 47 1.1 1.1 48 1.5 1.3 49 1.4 1.3 50 1.6 1.2

[0090] Life index ※Comparison based on 5μm wear as life

[0091] In Tables 4 and 5, the life index and dressing resistance index represent the ratio of the life and dressing resistance of each sample number when the life and dressing resistance of sample number 3 are set to 1. Tables 4 and 5 show the same tendency as Table 1 of Example 1.

[0092] It should be understood that the embodiments and examples disclosed this time are illustrative in all aspects and not restrictive. The scope of the present invention is indicated by the claims rather than the above description, and is intended to include all changes within the meaning and scope equivalent to the claims.

[0093] Explanation of symbols

[0094] 100 diamond rotary dresser, 101 superabrasive grain layer, 102 groove, 103 base metal, 105 dressing area, 202 low melting point alloy, 203 coating, 204 superabrasive grain, 205 top surface, 280 reference surface, 401 boundary line, 1204 first superabrasive grain, 2204 second superabrasive grain.

Claims

1. A rotary dresser having a superabrasive layer formed by superabrasive grains bonded to a base metal by a metal bonding material, The superabrasive grains include first superabrasive grains having a first average grain size and second superabrasive grains having a second average grain size smaller than the first average grain size. A plurality of the superabrasive grains exposed on the surface of the superabrasive grain layer among the first superabrasive grains and the second superabrasive grains form an active surface. In the region where the concentration of the superabrasive grains is the highest, the total area ratio of the plurality of action surfaces relative to the area of ​​a virtual surface smoothly connecting the action surfaces is 30% to 60%.

2. The rotary dresser according to claim 1, in, The second average particle size is not less than 30% and not more than 80% of the first average particle size.

3. The rotary dresser according to claim 1 or 2, in, The ratio of the maximum particle size to the minimum particle size of the first superabrasive grains and the second superabrasive grains (maximum particle size D1 of the first superabrasive grains / minimum particle size D3 of the second superabrasive grains) is 1.3 to 4.

4. The rotary dresser according to any one of claims 1 to 3, in, The first average particle size is greater than or equal to 300 μm and less than or equal to 800 μm.

5. The rotary dresser according to any one of claims 1 to 4, in, The superabrasive grains are artificial synthetic diamonds.

6. The rotary dresser according to any one of claims 1 to 5, in, When observing a cross section of the superabrasive grain layer, within a certain range, an average value of distances between each of the first superabrasive grains and the base metal is smaller than an average value of distances between each of the second superabrasive grains and the base metal.

7. A method for manufacturing a rotary dresser, which is a method for manufacturing the rotary dresser according to any one of claims 1 to 6, comprising the following steps: Step (1): a step of preparing a reverse mold having a predetermined shape formed on the inner surface of the mold, and attaching the first and second superabrasive grains to the inner surface by a plating method; Step (2): further performing build-up plating to embed and fix the first and second superabrasive grains by plating metal; Step (3): a step of setting a core bar at the center of the reverse mold and bonding the first and second superabrasive grains to the core bar; and Step (4): a step of removing the outer side of the inverted mold.

Citation Information

Patent Citations

  • Abrasive tool

    WO2017145491A1