Large manufacturing mold

By using poly(etherimide), poly(biphenylsulfone) and reinforced carbon filler composition materials, combined with melt deposition and additive manufacturing technology, the problem of deformation and dimensional changes of plastic molds at high temperatures is solved, and the problem of deformation and dimensional change of plastic molds is achieved. The high heat resistance and mechanical properties of the mold ensure stable molding of large-sized plastic items.

CN118946447APending Publication Date: 2024-11-12SOLVAY SPECIALTY POLYMERS USA LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028843.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-06
Filing Date
2023-03-15
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing plastic molds for manufacturing large-sized items are prone to deform during heating and cooling, resulting in dimensional changes and reproducibility of molded products, and lack good heat and mechanical resistance.

Method used

The mold is prepared by melt deposition additive manufacturing technology using a composition material containing poly(etherimide), poly(biphenylsulfone) and reinforced carbon filler to ensure that the mold does not deform at high temperatures and has good mechanical characteristics.

Benefits of technology

It has achieved a significant improvement in the warping resistance and thermal deformation temperature of the mold, ensured the stability of the mold under high temperature conditions and the reproducibility of the molded products, and was suitable for the manufacture of plastic items with large sizes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005051053400000061
    Figure BDA0005051053400000061
  • Figure BDA0005051053400000071
    Figure BDA0005051053400000071
  • Figure BDA0005051053400000072
    Figure BDA0005051053400000072
Patent Text Reader

Abstract

There is provided a mold for molding a large article, the mold comprising at least one molding surface for receiving a material to be molded and the mold comprising at least one polyarylsulfone polymer selected from the group consisting of poly (ether sulfone) and poly (biphenyl sulfone), at least one poly (ether imide) and a reinforcing carbon filler. The mold has the characteristics of good mechanical resistance and heat resistance.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Citation of Related Applications

[0002] This application claims priority to U.S. Provisional Patent Application No. 63 / 322,727, filed on March 23, 2022, and European Patent Application No. 22171948.7, filed on May 6, 2022, the entire contents of each of which are incorporated by reference into this application for all purposes. Technical Field

[0004] The present invention relates to a mould for moulding large sized articles from plastics material, including composite materials having continuous fibres. Background Art

[0005] The present invention relates to a mould for moulding large-sized objects from plastic material.

[0006] Moulds used to manufacture large-sized objects are usually made of metal. Replacing metal with lighter plastic materials would bring several advantages in terms of overall cost and ease of manufacturing. However, there are still several obstacles, such as the thermal and mechanical resistance of the mould itself. In fact, the moulding of plastics or composite materials involves exposing the mould to heating and cooling cycles, either by heating the mould itself or by bringing it into contact with molten plastic material. This has the disadvantage that, during the subsequent cooling process, the mould shape is deformed and its dimensions change, which jeopardizes the reproducibility of the moulded article.

[0007] Therefore, there is still a need for a mold made of a plastic material suitable for molding large-sized objects having good thermal and mechanical resistance and low warpage. Summary of the invention

[0009] It has now been found that certain compositions comprising at least one polyaryl sulfone chosen from poly(ether sulfone) or poly(biphenyl sulfone), at least one poly(etherimide) and a reinforcing carbon filler allow to obtain moulds having large dimensions which are remarkably resistant to warping.

[0010] Therefore, a first object of the present invention is a mold for molding an article, said mold comprising at least one molding surface for receiving the material to be molded and comprising at least one polyarylsulfone polymer chosen from poly(ethersulfone) and poly(biphenylsulfone), at least one poly(etherimide) and a reinforcing carbon filler.

[0011] The mold of the present invention has mechanical properties such as impact strength, tensile strength and tensile modulus that can meet application requirements, as well as a high heat deformation temperature.

[0012] The second object of the present invention is a method for manufacturing a mold using a melt manufacturing technique (including injection molding, compression molding) and a fused deposition additive manufacturing technique. The fused deposition additive manufacturing techniques that can be employed include both filament-based methods (fused filament manufacturing, FFF) and large-format fused deposition by direct extrusion.

[0013] Another object of the invention is a method for producing a molded article using the mold of the invention. DETAILED DESCRIPTION

[0015] In this application:

[0016] - even any description related to a specific embodiment is applicable to and interchangeable with other embodiments of the present disclosure;

[0017] - When an element or component is said to be included in and / or selected from a list of listed elements or components, it should be understood that in the relevant embodiments explicitly considered herein, the element or component may also be any of these listed independent elements or components, or may also be selected from a group consisting of any two or more of the explicitly listed elements or components; any element or component listed in the list of elements or components may be omitted from this list; and

[0018] - Any recitation of numerical ranges by endpoints herein includes all numbers subsumed within the recited range as well as the endpoints of that range and equivalents thereof.

[0019] A first object of the present invention is a mold for molding an article, said mold comprising at least one molding surface for receiving a material to be molded, said molding surface having a length of at least 1.0 m in at least one direction, wherein the mold comprises a composition (C) comprising:

[0020] - 0.5 wt % to 40.0 wt % of at least one poly(etherimide) polymer;

[0021] - 0.0 wt % to 70.0 wt % of at least one poly(biphenyl sulfone) polymer;

[0022] - 0.0 wt% to 70.0 wt% of at least one poly(ethersulfone) polymer; and

[0023] - 5.0 wt% to 50.0 wt% of at least one reinforcing carbon filler, preferably a carbon fiber filler,

[0024] The composition is characterized in that 10.0≤(X PPSU +X PES )≤94.5 and X PPSU and XPES are not zero at the same time, where X PPSU is the weight percentage of the at least one poly(biphenyl sulfone) polymer in composition (C), and X PES is the weight percent of the at least one poly(ethersulfone) polymer in composition (C).

[0025] In the present specification, unless expressly stated otherwise, all weight percentages (wt %) are based on the total weight of the composition.

[0026] The molding surface of the mold of the present invention typically has a length of at least 1.5 m, even at least 2.0 m and / or up to 30 m or even up to 50 m in at least one direction. The molding surface may have a length of 1.0 m to 30.0 m, even 1.5 m to 25.0 m, also 3.0 m to 20.0 m in at least one direction.

[0027] The molding surface of the mold of the present invention may have a length in at least two directions of at least 1.0 m, even at least 1.5 m, also at least 2.0 m or more.

[0028] In certain embodiments, the molding surface has a length in both directions of 1.0 m to 30.0 m, or even 1.5 m to 20.0 m.

[0029] The contour of the molding surface is generally designed to be the same shape as the article to be molded. It can have a convex or concave shape. The mold can include inserts as required by the article to be molded therein. In some embodiments, the mold can include more than one molding surface, for example more than one molding surface arranged to form a closed continuous surface.

[0030] The mould of the present invention comprises a composition (C) as described in detail below. Typically, the moulding surface of the mould of the present invention comprises composition (C). Preferably, the mould is made of composition (C).

[0031] Composition (C)

[0032] The composition (C) comprises:

[0033] - 0.5 wt% to 40.0 wt% of at least one poly(etherimide) polymer, hereinafter [polymer PEI];

[0034] - 0.0 wt% to 70.0 wt% of at least one poly(biphenyl sulfone) polymer, hereinafter [polymer PPSU];

[0035] - 0.0 wt% to 70.0 wt% of at least one poly(ethersulfone) polymer, hereinafter [Polymer PES]; and

[0036] - 5.0 wt. % to 50.0 wt. % of at least one reinforcing carbon filler,

[0037] The composition is characterized in that 10.0≤(X PPSU +X PES )≤94.5 and X PPSU and X PES are not zero at the same time, where X PPSU is the weight percentage of the at least one poly(biphenyl sulfone) polymer in composition (C), and X PES is the weight percent of the at least one poly(ethersulfone) polymer in composition (C).

[0038] For the avoidance of doubt, when X PPSU = 0, then X PES ≠0, and when X PES = 0, then X PPSU ≠0.

[0039] The present invention also relates to a composition (C) comprising:

[0040] - 0.5 to 40.0 wt% of at least one polymer PEI;

[0041] - 0.0 wt% to 70.0 wt% of at least one polymer PPSU;

[0042] - 30.0 wt% to 70.0 wt% of at least one polymer PES; and

[0043] - 5.0 to 50.0 wt.% of at least one reinforcing carbon filler.

[0044] In the first embodiment of the present invention, the composition (C) does not contain any polymer PPSU, that is, 0.0 wt% of polymer PPSU or X PPSU =0. In this embodiment, composition (C) comprises:

[0045] - 0.5 to 40.0 wt% of at least one polymer PEI;

[0046] - 40.0 wt% to 70.0 wt% of at least one polymer PES; and

[0047] - 5.0 to 50.0 wt.% of at least one reinforcing carbon filler.

[0048] In such embodiments, the amount of polymer PES may be at least 45.0 wt%, or even 50.0 wt%, based on the total weight of the composition.

[0049] Favorable results were obtained with a composition (C) comprising: 3.0 to 15.0 wt% of at least one polymer PEI; 50.0 to 70.0 wt% of at least one polymer PES; and 15.0 to 50.0 wt.% of at least one reinforcing carbon filler.

[0050] In another embodiment of the present invention, the composition (C) does not contain any polymer PES, i.e., 0.0 wt% of polymer PES or X PES =0. In this embodiment, composition (C) comprises:

[0051] - 0.5 to 40.0 wt% of at least one polymer PEI;

[0052] - 30.0 wt% to 65.0 wt% of at least one polymer PPSU; and

[0053] - 5.0 to 50.0 wt.% of at least one reinforcing carbon filler.

[0054] In such an embodiment, the amount of polymer PPSU may be at least 35.0 wt % based on the total weight of the composition.

[0055] Favorable results were obtained with a composition (C) comprising: 5.0 to 40.0 wt% of at least one polymer PEI; 35.0 to 65.0 wt% of at least one polymer PPSU; and 15.0 to 50.0 wt.% of at least one reinforcing carbon filler.

[0056] In another embodiment, composition (C) comprises:

[0057] - 0.5 to 40.0 wt% of at least one polymer PEI;

[0058] - 5.0 to 70.0 wt% of at least one polymer PPSU;

[0059] - 30.0 wt% to 70.0 wt% of at least one polymer PES; and

[0060] - 5.0 to 50.0 wt.% of at least one reinforcing carbon filler.

[0061] Favorable results were obtained with a composition (C) comprising: 5.0 wt% to 20.0 wt% of at least one polymer PEI; 30.0 wt% to 70.0 wt% of at least one polymer PES; 5.0 wt% to 20.0 wt% of at least one polymer PPSU; and 15.0 wt% to 50.0 wt% of at least one reinforcing carbon filler, based on the total weight of the composition.

[0062] Composition (C) typically comprises at least 2.0 wt%, preferably at least 5.0 wt% of polymer PEI. The amount of polymer PEI is usually not more than 35.0 wt%, based on the total weight of the composition.

[0063] Composition (C) typically comprises at least 10.0 wt%, preferably at least 15.0 wt% of at least one reinforcing carbon filler. The amount of reinforcing carbon filler usually does not exceed 45.0 wt%. Good results in terms of reinforcing properties are usually obtained with reinforcing carbon fillers in an amount ranging from 15.0 wt% to 45.0 wt%, even from 20.0 wt% to 45.0 wt%.

[0064] PEI polymer

[0065] For the purposes of the present invention, a poly(etherimide) polymer (ie, a polymer PEI) is intended to mean a polymer in which the repeating unit (R PEI ) containing more than 50 mol % of at least one aromatic ring, at least one imide group (as such and / or in its amide acid form), and at least one ether group [repeating unit (A)].

[0066] The repeating unit (A) may optionally further comprise at least one amide group which is not included in the amic acid form of the imide group.

[0067] The repeating unit (A) is advantageously selected from the group consisting of the following formulae (I), (II), (III), (IV) and (V), and mixtures thereof:

[0068]

[0069] wherein: Ar is a tetravalent aromatic moiety and is selected from the group consisting of substituted or unsubstituted, saturated, unsaturated or aromatic monocyclic and polycyclic groups having 5 to 50 carbon atoms;

[0070] Ar"' is a trivalent aromatic moiety and is selected from the group consisting of substituted or unsubstituted, saturated, unsaturated or aromatic monocyclic and polycyclic groups having 5 to 50 carbon atoms; and

[0071] R is selected from the group consisting of substituted or unsubstituted divalent organic groups, and more particularly selected from the group consisting of (a) aromatic hydrocarbon groups having 6 to 20 carbon atoms and halogenated derivatives thereof; (b) straight-chain or branched alkylene groups having 2 to 20 carbon atoms; (c) cycloalkylene groups having 3 to 20 carbon atoms, and (d) divalent groups having the general formula (VI):

[0072]

[0073] wherein Y is selected from the group consisting of: an alkylene group having 1 to 6 carbon atoms, specifically -C(CH3)2 and -C n H 2n – (n is an integer from 1 to 6); a perfluoroalkylene group having 1 to 6 carbon atoms, specifically –C(CF3)2 and –C n F 2n – (n is an integer from 1 to 6); a cycloalkylene group having 4 to 8 carbon atoms; an alkylene group having 1 to 6 carbon atoms; a cycloalkylene group having 4 to 8 carbon atoms; –O–; –S–; –C(O)–; -SO2-; –SO–, and R′ is selected from the group consisting of hydrogen, halogen, alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali metal or alkaline earth metal sulfonate, alkyl sulfonate, alkali metal or alkaline earth metal phosphonate, alkyl phosphonate, amine and quaternary ammonium, and i and j are the same or different from each other and are independently 0, 1, 2, 3 or 4.

[0074] The proviso is that at least one of Ar, Ar'" and R comprises at least one ether group, wherein the ether group is present in the polymer chain backbone.

[0075] Preferably, Ar is selected from the group consisting of those conforming to the following formula:

[0076]

[0077] wherein X is a divalent moiety having a divalent bond at the 3,3', 3,4', 4,3" or 4,4' position and is selected from the group consisting of an alkylene group having 1 to 6 carbon atoms, specifically -C(CH3)2 and -C n H 2n – (n is an integer from 1 to 6); a perfluoroalkylene group having 1 to 6 carbon atoms, specifically –C(CF3)2 and –C n F 2n – (n is an integer from 1 to 6); a cycloalkylene group having 4 to 8 carbon atoms; an alkylene group having 1 to 6 carbon atoms; a cycloalkylene group having 4 to 8 carbon atoms; -O–; –S–; –C(O)–; -SO2-; –SO–, or X is a group having the formula O-Ar”-O; and wherein Ar” is selected from the group consisting of those conforming to the following formulae (VII) to (XIII), and mixtures thereof:

[0078]

[0079] wherein R and R', which are the same or different from each other, are independently selected from the group consisting of hydrogen, halogen, alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali metal or alkaline earth metal sulfonate, alkyl sulfonate, alkali metal or alkaline earth metal phosphonate, alkyl phosphonate, amine and quaternary ammonium, and j, k, l, n and m, which are the same or different from each other, are independently 0, 1, 2, 3 or 4, and W is selected from the group consisting of alkylene having 1 to 6 carbon atoms, specifically -C(CH3)2 and -C n H 2n - (wherein n is an integer from 1 to 6); a perfluoroalkylene group having 1 to 6 carbon atoms, specifically -C(CF3)2 and -C n F 2n – (wherein n is an integer from 1 to 6); a cycloalkylene group having 4 to 8 carbon atoms; an alkylene group having 1 to 6 carbon atoms; a cycloalkylene group having 4 to 8 carbon atoms; -O–; –S–; –C(O)–; -SO2-; and –SO–.

[0080] Preferably, Ar"' is selected from the group consisting of those conforming to the following formula:

[0081]

[0082] wherein X has the same meaning as defined above.

[0083] In a preferred embodiment, the repeating unit (A) is selected from the group consisting of units in the imide form of formula (XIV), corresponding units in the amic acid form of formula (XV) and (XVI), and mixtures thereof:

[0084]

[0085] in:

[0086] → represents isomerism, such that in any repeating unit the groups to which these arrows point may exist as shown or in interchanged positions;

[0087] -Ar" is selected from the group consisting of: those conforming to the following formulae (VII) to (XIII)

[0088]

[0089] wherein R and R', which are the same or different from each other, are independently selected from the group consisting of hydrogen, halogen, alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali metal or alkaline earth metal sulfonate, alkyl sulfonate, alkali metal or alkaline earth metal phosphonate, alkyl phosphonate, amine and quaternary ammonium, and j, k, l, n and m, which are the same or different from each other, are independently 0, 1, 2, 3 or 4, and W is selected from the group consisting of alkylene having 1 to 6 carbon atoms, specifically C(CH3)2 and -C n H 2n -(n is an integer from 1 to 6); a perfluoroalkylene group having 1 to 6 carbon atoms, specifically -C(CF3)2 and -C n F 2n – (n is an integer from 1 to 6); a cycloalkylene group having 4 to 8 carbon atoms; an alkylene group having 1 to 6 carbon atoms; a cycloalkylene group having 4 to 8 carbon atoms; -O–; –S–; –C(O)–; -SO2-; and –SO–;

[0090] -E Select from the group consisting of: -C n H 2n - (n is an integer from 1 to 6), a divalent group having the general formula (VI) as defined above, and those conforming to the following formulas (XVII) to (XXII)

[0091]

[0092] wherein R' is selected from the group consisting of hydrogen, halogen, alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali metal or alkaline earth metal sulfonate, alkyl sulfonate, alkali metal or alkaline earth metal phosphonate, alkyl phosphonate, amine and quaternary ammonium, and o, p and q are the same or different from each other and are independently 0, 1, 2, 3 or 4.

[0093] Preferably, E is selected from the group consisting of those conforming to formulae (XVII) to (XIX) as defined above, more preferably, E is selected from the group consisting of unsubstituted m-phenylene and unsubstituted p-phenylene, and mixtures thereof.

[0094] Preferably, Ar" has the general formula (XIII) as described in detail above; more preferably, Ar" is

[0095]

[0096] The polymer PEI wherein the repeating unit (A) is a repeating unit of formula (XIV) as defined above (as such, in the form of an imide), and / or in the form of an amic acid [formula (XV) and (XVI)] can be prepared by any method known to those skilled in the art, including any aromatic bis(ether anhydride) of the formula

[0097]

[0098] wherein Ar" is as defined above, with a diamino compound having the formula: H2N-E-NH2 (XXIV)

[0099] where E is as defined before.

[0100] Alternatively, the poly(etherimide) polymers can be prepared by melt polymerization of any dianhydride having formula (XXIII) with any diamino compound having formula (XXIV) while heating the mixture of these ingredients at elevated temperature and while mixing.

[0101] Aromatic bis(ether anhydrides) having formula (XXIII) include, for example:

[0102] 2,2-Bis[4-(2,3-dicarboxyphenoxy)phenyl]propane dianhydride; 4,4'-bis(2,3-dicarboxyphenoxy)diphenyl ether dianhydride; 1,3-bis(2,3-dicarboxyphenoxy)phthalic anhydride; 4,4'-bis(2,3-dicarboxyphenoxy)diphenyl sulfide dianhydride; 1,4-bis(2,3-dicarboxyphenoxy)phthalic anhydride; 4,4'-bis(2,3-dicarboxyphenoxy)benzophenone dianhydride; 4,4'-bis(2,3-dicarboxyphenoxy)diphenyl sulfone dianhydride; 2,2-bis[4(3,4-dicarboxyphenoxy)phenyl]propane dianhydride; 4,4'-bis(2,3-dicarboxyphenoxy)diphenyl sulfone ...

[0013] dianhydride; 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl]propane dianhydride; 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl ether dianhydride; 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride; 1,3-bis(3,4-dicarboxyphenoxy)phthalic dianhydride; 1,4-bis(3,4-dicarboxyphenoxy)phthalic dianhydride; 4,4'-bis(3,4-dicarboxyphenoxy)benzophenone dianhydride; 4-(2,3-dicarboxyphenoxy)-4'-(3,4-dicarboxyphenoxy)diphenyl-2,2-propane dianhydride; etc., and mixtures of such dianhydrides.

[0103] Organic diamines having formula (XXIV) include, for example, m-phenylenediamine, p-phenylenediamine, 2,2-bis(p-aminophenyl)propane, 4,4′-diaminodiphenyl-methane, 4,4′-diaminodiphenyl sulfide, 4,4′-diaminodiphenyl sulfone, 4,4′-diaminodiphenyl ether, 1,5-diaminonaphthalene, 3,3′-dimethylbenzidine, 3,3′-dimethoxybenzidine, and mixtures thereof.

[0104] In a preferred embodiment, the organic diamine having formula (XXIV) is selected from the group consisting of meta-phenylenediamine and para-phenylenediamine and mixtures thereof.

[0105] In the most preferred embodiment, the repeating unit (A) is a repeating unit selected from the group consisting of those in imide form having formula (XXV), their corresponding amido acid forms having formula (XXVI) and (XXVII), and mixtures thereof:

[0106]

[0107] Wherein in formulae (XXVI) and (XXVII), the → represents isomerism, such that in any repeating unit two groups pointed by an arrow from the same aromatic ring may be present as shown or in interchanged positions.

[0108] In another most preferred embodiment, the repeating unit (A) is a repeating unit selected from the group consisting of those in imide form having formula (XXVIII), their corresponding amido acid forms having formula (XXIX) and (XXX), and mixtures thereof:

[0109]

[0110]

[0111] Wherein in formulae (XXIX) and (XXX), the → represents isomerism, such that in any repeating unit two groups pointed by an arrow from the same aromatic ring may be present as shown or in interchanged positions.

[0112] Preferably more than 75 mol% and more preferably more than 90 mol% of the repeating units of the polymer PEI are repeating units (A). Still more preferably, substantially all, if not all, of the repeating units of PEI are repeating units (A).

[0113] In a preferred embodiment of the present invention, greater than 75 mol%, more preferably greater than 90 mol%, more preferably greater than 99 mol%, even more preferably all of the repeating units of the PEI are repeating units selected from the group consisting of those in the imide form having formula (XXV), their corresponding amide acid forms having formula (XXVI) and (XXVII), and mixtures thereof.

[0114] In another preferred embodiment of the present invention, greater than 75 mol%, more preferably greater than 90 mol%, more preferably greater than 99 mol%, even more preferably all of the repeating units of the polymer PEI are repeating units selected from the group consisting of those in the imide form having formula (XXVIII), their corresponding amide acid forms having formula (XXIX) and (XXX), and mixtures thereof.

[0115] A suitable polymer, PEI, is available from Sabic Innovative Plastics as Poly(etherimide) polymers are commercially available.

[0116] The composition may comprise one and only one polymer PEI or a mixture of more than one polymer PEI.

[0117] Typically, the polymer PEI useful in the present invention has a melt flow rate (MFR) in the range of 0.1 to 40.0 g / 10 min as measured according to ASTM D1238 at 337° C. and under a load of 6.6 kg, preferably in the range of 4 to 25 g / 10 min as measured according to ASTM D1238 at 337° C. and under a load of 6.6 kg.

[0118] In a specific embodiment, the polymer PEI advantageously has a weight average molecular weight (Mw) of 10,000 to 150,000 grams per mole (g / mol) as measured by gel permeation chromatography using polystyrene standards. Such polymers PEI typically have an intrinsic viscosity greater than 0.2 deciliters per gram (dl / g), advantageously 0.35 dl / g to 0.7 dl / g, measured in m-cresol at 25°C.

[0119] Polymer PPSU

[0120] The composition comprises at least one polymer PPSU. As used herein, a polymer PPSU refers to a polymer comprising at least 50 mol % of repeating units (R) of formula (B) PPSU ), mol % is based on the total moles of repeating units in the polymer:

[0121]

[0122] According to embodiments of the present disclosure, at least 60 mol%, at least 70 mol%, at least 80 mol%, at least 90 mol%, at least 95 mol%, at least 99 mol%, or all of the repeating units in the PPSU are repeating units (R) having formula (B): PPSU ).

[0123] PPSU can be prepared by known methods and is available in particular from Solvay Specialty Polymers USA, Inc. PPSU available.

[0124] The PPSU polymer advantageously has a melt flow rate (MFR) equal to or higher than 5 g / 10 min at 365° C. and under a load of 5.0 kg, preferably equal to or higher than 10 g / 10 min at 365° C. and under a load of 5.0 kg, more preferably equal to or higher than 14 g / 10 min at 365° C. and under a load of 5.0 kg, as measured according to ASTM method D1238.

[0125] The upper limit of the melt flow rate of the PPSU polymer will generally be at most 100 g / 10 min, preferably at most 60 g / 10 min, more preferably at most 40 g / 10 min.

[0126] The weight average molecular weight of the PPSU polymer may be 20,000 to 100,000 grams per mole (g / mol) as determined by gel permeation chromatography according to ASTM D5296 using dichloromethane as the mobile phase and using polystyrene standards. In some embodiments, the weight average molecular weight of the PPSU polymer may be 40,000 to 80,000 grams per mole (g / mol). In other embodiments, the PPSU polymer has a weight average molecular weight (Mw) ranging from 48,000 g / mol to 52,000 g / mol.

[0127] Polymer PES

[0128] As used herein, poly(ethersulfone), polymer PES, means any polymer wherein at least 50 mol % of the repeating units are repeating units having formula (D):

[0129]

[0130] Preferably at least 60 mol%, 70 mol%, 80 mol%, 90 mol%, 95 mol%, 99 mol% and most preferably all of the repeating units in the PES are repeating units having formula (D).

[0131] PES can be prepared by known methods and is notably available from Solvay Specialty Polymers USA, Inc. as Available from PESU.

[0132] The PES polymer advantageously has a melt flow rate (MFR) of at least 10 g / 10 min as measured according to ASTM D1238 using a temperature of 380° C. and a weight of 2.17 kg. The MFR is more preferably greater than 15 g / 10 min, and most preferably greater than 20 g / 10 min. The MFR will typically be at most 100 g / 10 min, preferably at most 80 g / 10 min, and most preferably at most 60 g / 10 min.

[0133] Reinforced carbon filler

[0134] Composition (C) comprises at least one reinforcing carbon filler, preferably a carbon fiber filler.

[0135] For the purposes of the present invention, the term "carbon fiber filler" is intended to include graphitized, partially graphitized, and non-graphitized carbon reinforcing fibers or mixtures thereof.

[0136] The term "graphitized" is intended to mean carbon fibers obtained by high temperature pyrolysis (above 2000°C) of carbon fibers, wherein the carbon atoms are arranged in a manner similar to the graphite structure.

[0137] Carbon fibers useful in the present invention can be advantageously obtained by heat treatment and pyrolysis of different polymer precursors such as, for example, rayon, polyacrylonitrile (PAN), aromatic polyamide, or phenolic resin; carbon fibers useful in the present invention can also be obtained from pitch materials.

[0138] The carbon fiber usable in the present invention is preferably selected from the group consisting of PAN-based carbon fiber (PAN-CF), pitch-based carbon fiber, graphitized pitch-based carbon fiber, and a mixture thereof.

[0139] The PAN-based carbon fibers (PAN-CF) advantageously have a diameter between 3 and 20 μm, preferably 4 to 15 μm, more preferably 5 to 10 μm, most preferably 6 to 8 μm. Good results were obtained using PAN-based carbon fibers (PAN-CF) having a diameter of 7 μm.

[0140] PAN-CF can be of any length. Generally, the length of PAN-CF is at least 50 μm.

[0141] Graphitized pitch-based carbon fibers are readily available from commercial sources, containing at least about 50 wt% graphitic carbon, greater than about 75 wt% graphitic carbon, and up to substantially 100 wt% graphitic carbon. Highly graphitized carbon fibers particularly suitable for use in the practice of the present invention may further be characterized as being highly conductive, and such fibers having a modulus of about 550 to about 830 GPa are typically used. In certain embodiments, the highly graphitized carbon fibers have a modulus of about 590 to about 830 GPa, and in certain other embodiments have a modulus of about 690 to about 793 GPa.

[0142] The bitumen-based CF advantageously has a diameter between 5 and 20 μm, preferably from 7 to 15 μm, more preferably from 8 to 12 μm.

[0143] The bitumen-based-CF may be of any length. The bitumen-based-CF advantageously has a length of at least 50 μm.

[0144] additive

[0145] The composition may further comprise optional additives including, but not limited to, antioxidants (eg, UV stabilizers and heat stabilizers), processing aids, nucleating agents, lubricants, flame retardants, smoke suppressants, antistatic agents, anti-caking agents, colorants, pigments.

[0146] In some embodiments, antioxidants can be particularly desirable additives. Antioxidants can improve the thermal stability and light stability of the composition. For example, antioxidants as heat stabilizers can improve the thermal stability of the composition during manufacture (or in high heat application environments), for example, by making the polymer processable at higher temperatures while helping to prevent polymer degradation.

[0147] When present, the additive is typically included in the composition in an amount of no more than 10.0 wt%, even no more than 8.0 wt%, relative to the total weight of the composition. The additive is usually present in an amount of at least 0.5 wt%, such as at least 1.0 wt%, relative to the total weight of the composition.

[0148] Composition (C) can be prepared by melt compounding a powder mixture of polymer and filler. Conventional melt compounding equipment can be used, such as co-rotating and counter-rotating extruders, single screw extruders, co-kneaders, disk stack processors and various other types of extrusion equipment. Preferably, an extruder, more preferably a twin screw extruder, can be used.

[0149] Advantageously, strand extrudates of the composition (C) of the invention can be obtained. Such strand extrudates can be chopped in the form of pellets or beads, which can then be further used to produce the mould of the invention.

[0150] Another object of the invention is a method for making a mould, which is the first object of the invention.Any method suitable for making a three-dimensional object having a length of at least 1.0 m in at least one direction from a polymer composition can be used to make the mould of the invention.

[0151] Suitable techniques may be, for example, rotational moulding or injection moulding.

[0152] In a preferred aspect of the present invention, the mold of the present invention is prepared by an additive manufacturing technique, preferably a fused deposition additive manufacturing technique. The fused deposition additive manufacturing techniques that can be employed include both filament-based methods (fused filament fabrication, FFF) and large-format fused deposition by direct extrusion.

[0153] Therefore, another object of the present invention is a method for manufacturing the mold of the present invention, the method comprising:

[0154] - providing a part material comprising the composition (C) as described in detail above; and

[0155] - Depositing layers of a three-dimensional object from the part material.

[0156] The expression "part material" refers here to a material, notably a blend of polymer compounds, intended to form at least a part of a three-dimensional object. According to the present disclosure, the part material serves as a raw material to be used for manufacturing a three-dimensional object.

[0157] Part materials can be in the form of filaments or particles.

[0158] The expression "filament" refers to a thread-like object or fiber formed from a material or a blend of materials, in particular composition (C). The expression "microparticle" refers to a particle having a size comprised between 1 μm and 200 μm, for example between 10 μm and 100 μm or between 20 μm and 80 μm. Microparticles can be prepared, for example, by feeding composition (C) through a blade, roller or screw pump printhead.

[0159] According to an embodiment, a method for manufacturing a three-dimensional mold using an additive manufacturing system includes the following steps, which include extruding a part material. This step can be performed, for example, when printing or depositing a strip or layer of the part material. The method of manufacturing a 3D object using an extrusion-based additive manufacturing system is also called fused filament fabrication technology (FFF).

[0160] According to another fused deposition additive manufacturing technique, direct extrusion is used without the use of prefabricated filaments to produce the strand-by-strand and layer-by-layer build-up of the part being produced. This technique, which often uses a vertically positioned extruder, is known in the art as "large area additive manufacturing" (BAAM). It is a more practical technique for additive manufacturing of parts (such as the mold that is the subject of the present invention) that exceed 1.0 m in at least one direction.

[0161] Another object of the present invention is a method of manufacturing an article, the method comprising shaping a material on the molding surface of a mold of the present invention. Any known technique can be used to shape the material on the molding surface of the mold, the technique comprising coating, extrusion coating or depositing a separate material layer.

[0162] The above embodiments are intended to be illustrative rather than restrictive. Other embodiments are within the inventive concept. In addition, although the present invention has been described with reference to specific embodiments, those skilled in the art will recognize that changes may be made in form and detail without departing from the spirit and scope of the present invention.

[0163] Examples

[0164] The formulations and test data presented in this example document illustrate the practice of the invention and demonstrate the unexpected benefits and utility of the invention. These examples are intended to illustrate the invention by selected embodiments and do not imply any limitation to the broad scope and generality of the invention.

[0165] Starting materials used

[0166] Poly(biphenyl sulfone): (PPSU) Grade R-5600NT, available from Solvay Specialty Polymers, Inc. This grade has a melt flow rate of 31-40 g / 10 min as measured according to ASTM D1238 at 365C and 5.0 kg weight.

[0167] Poly(ethersulfone) (PES) - Brand 3300 is also available from Solvay Specialty Polymers, Inc. This grade has a melt flow rate of 25-35 g / 10 min as measured according to ASTM D1238 using a temperature of 380°C and a 2.16 kg weight.

[0168] Poly(etherimide) (PEI), which is a high melt flow rate grade, is available from Saudi Basic Innovative Plastics as 1010 available.

[0169] The carbon fiber reinforcement used is made by Teijin Co., Ltd. A P742 Chopped Carbon Fiber for sale.

[0170] Other additives include zinc oxide – brand R-609, which was purchased from Lanxess Corporation.

[0171] Preparation of formulations

[0172] The formulation of the example was prepared by first tumbling the pellets or powders of the polymers constituting the composition at the desired composition ratio with zinc oxide for about 20 minutes, followed by melt compounding using a 26 mm diameter Coperion ZSK-26 co-rotating partially intermeshing twin screw extruder with an L / D ratio of 48: 1. The extruder had 12 barrel sections, of which barrel sections 2 to 11 were heated with a set point temperature of 350° C. The die section was also set to a temperature of 350° C.

[0173] The polymer plus zinc oxide pre-blend is fed at a nominal rate ranging from 7.9-12.7 kg / hr using a gravity feeder at barrel section 1, while the carbon fiber reinforcement is fed to the extruder at barrel section 7 with a corresponding rate to allow the carbon fiber loading level in all final compounds to be 30% by weight. The extruder is operated at a screw speed of about 200 rpm, and vacuum ventilation is applied at barrel section 10 during compounding to remove moisture and any possible residual volatiles from the compound. A single-hole die is used for all compounds, and the molten polymer strands leaving the die are cooled in a water trough and then cut in a granulator to form pellets of about 3.0 mm long and 2.7 mm in diameter. A comparative example consisting of only one polymer in the formulation is also similarly prepared by feeding a polymer or a polymer / zinc oxide mixture at barrel section 1 and feeding carbon fibers at barrel section 7 under the same conditions as described above.

[0174] Injection molding was used to produce test specimens for measuring mechanical properties and heat distortion temperature. 25 tensile specimens and 25 flexural specimens were prepared from each composition. According to ASTM specification D638, the tensile test specimens were Type I ASTM tensile test bars 3.2 mm (0.125 inches) thick, and the flexural specimens were 127 mm × 12.7 mm × 3.2 mm in size. The mechanical test specimens were injection molded using the following approximate set point conditions, which are consistent with the supplier's recommended injection molding guidelines for different polymers: rear barrel section: 680°F (360°C); middle barrel section: 690°F (365°C); front barrel section: 700°F (371°C); nozzle: 700°F (371°C); mold: 330°F (165°C);

[0175] test

[0176] All compositions were evaluated using the following ASTM test methods:

[0177] D638: Tensile properties

[0178] D790: Flexural Characteristics

[0179] D256: Notched Izod Impact Resistance

[0180] D4812: Unnotched Izod Impact Resistance

[0181] D648: Heat deformation temperature at 1.82MPa

[0182] All tests except heat deflection temperature were performed on as-molded test parts. Heat deflection temperature testing was performed on annealed specimens using annealing conditions of 200°C for 1 hour in a forced air oven.

[0183] The formulations of all Examples 1 to 5 and Comparative Examples 1 to 3 are shown in Table 1 together with the corresponding mechanical evaluation results.

[0184] Table 1

[0185]

[0186]

[0187] The data show that the compositions of Examples 1-5 exhibit a good balance of strength, modulus, impact resistance, and heat distortion temperature. It is expected that these property enhancements will extend to the long-term properties of the molds of the present invention, such as fatigue resistance and creep rupture resistance. The high heat distortion temperatures of the compositions of Examples 1 to 5, together with their good mechanical properties, make them particularly suitable for use in molds for forming thermoplastic composites where processing temperatures can be as high as 200°C.

Claims

1. A mold for molding an article, the mold comprising at least one molding surface for receiving a material to be molded, the molding surface having a length of at least 1.0 m in at least one direction, wherein the mold comprises a composition (C) comprising: - 0.5 wt % to 40.0 wt % of at least one poly(etherimide) polymer; - 0.0 wt % to 70.0 wt % of at least one poly(biphenyl sulfone) polymer; - 0.0 wt% to 70.0 wt% of at least one poly(ethersulfone) polymer; and - 5.0 wt% to 50.0 wt% of at least one reinforcing carbon filler, preferably a carbon fiber filler, The composition is characterized in that 10.0≤(X PPSU +X PES )≤94.5 and X PPSU and X PES are not zero at the same time, where X PPSU is the weight percentage of the at least one poly(biphenyl sulfone) polymer in composition (C), and X PES is the weight percent of the at least one poly(ethersulfone) polymer in composition (C).

2. The mold according to claim 1, in, The moulding surface has a length of at least 1.0 m and / or up to 50.0 m in at least two directions.

3. The mold according to claim 1 or 2, in, The composition (C) comprises: - 0.5 wt % to 40.0 wt % of at least one poly(etherimide) polymer; - 0.0 wt % to 70.0 wt % of at least one poly(biphenyl sulfone) polymer; - 30.0 wt% to 70.0 wt% of at least one poly(ethersulfone) polymer; and - 5.0 to 50.0 wt% of at least one reinforcing carbon filler, preferably a carbon fiber filler.

4. The mold according to claim 1 or 2, in, The composition (C) comprises: - 0.5 wt % to 40.0 wt % of at least one poly(etherimide) polymer; - 10.0 wt % to 70.0 wt % of at least one poly(biphenyl sulfone) polymer; - 0.0 wt% to 70.0 wt% of at least one poly(ethersulfone) polymer; and - 5.0 to 50.0 wt% of at least one reinforcing carbon filler, preferably a carbon fiber filler.

5. A mould according to any one of the preceding claims, in, Composition (C) comprises 5.0 wt% to 35.0 wt% of at least one poly(etherimide) polymer and / or 15.0 wt% to 45.0 wt% of at least one reinforcing carbon fiber filler.

6. A mould according to any one of the preceding claims, in, The at least one poly(etherimide) polymer comprises greater than 50 mol%, preferably greater than 90 mol%, based on the total moles of repeating units in the polymer, of repeating units selected from the group consisting of those in imide form having formula (XXV), their corresponding amic acid forms having formula (XXVI) and (XXVII), and mixtures thereof: Wherein in formulae (XXVI) and (XXVII), the → represents isomerism, such that in any repeating unit two groups pointed by an arrow from the same aromatic ring may be present as shown or in interchanged positions.

7. A mould according to any one of the preceding claims, in, The at least one poly(biphenyl sulfone) polymer comprises at least 50 mol %, preferably at least 90 mol %, of repeating units having formula (B), the mol % being based on the total moles of repeating units in the polymer:

8. A mould according to any one of the preceding claims, in, The at least one poly(ethersulfone) polymer comprises at least 50 mol %, preferably at least 90 mol %, of repeating units having formula (D), the mol % being based on the total moles of repeating units in the polymer:

9. A mould according to any one of the preceding claims, in, The carbon fiber filler is selected from the group consisting of PAN-based carbon fibers (PAN-CF), pitch-based carbon fibers, graphitized pitch-based carbon fibers, and mixtures thereof.

10. A method for manufacturing a mold according to any one of claims 1 to 9, the method include: - providing a component material comprising a composition (C) as defined in any one of claims 1 to 9, - Depositing layers of a three-dimensional object from the part material.

11. The method according to claim 10, in, The part material is in the form of filaments or particles.

12. The method according to claim 10, in, The step of depositing a layer includes extruding the part material.

13. A method for manufacturing an article, the method comprising shaping a material on at least one moulding surface of a mould as claimed in any one of claims 1 to 9.

14. A composition (C) comprising: - 0.5 wt % to 40.0 wt % of at least one poly(etherimide) polymer; - 0.0 wt % to 70.0 wt % of at least one poly(biphenyl sulfone) polymer; - 30.0 wt% to 70.0 wt% of at least one poly(ethersulfone) polymer; and - 5.0 to 50.0 wt% of at least one reinforcing carbon filler, preferably a carbon fiber filler.

15. The composition (C) according to claim 14, in, The at least one poly(etherimide) polymer comprises greater than 50 mol%, preferably greater than 90 mol%, based on the total moles of repeating units in the polymer, of repeating units selected from the group consisting of those in imide form having formula (XXV), their corresponding amic acid forms having formula (XXVI) and (XXVII), and mixtures thereof: Wherein in formulae (XXVI) and (XXVII), the → represents isomerism, such that in any repeating unit two groups pointed by an arrow from the same aromatic ring may be present as shown or in interchanged positions.

16. The composition (C) according to claim 14 or 15, in, The at least one poly(biphenyl sulfone) polymer comprises at least 50 mol %, preferably at least 90 mol %, of repeating units having formula (B), the mol % being based on the total moles of repeating units in the polymer:

17. The composition (C) according to any one of claims 14 to 16, in, The at least one poly(ethersulfone) polymer comprises at least 50 mol %, preferably at least 90 mol %, of repeating units having formula (D), the mol % being based on the total moles of repeating units in the polymer:

18. The composition (C) according to any one of claims 14 to 17, in, The carbon fiber filler is selected from the group consisting of PAN-based carbon fibers (PAN-CF), pitch-based carbon fibers, graphitized pitch-based carbon fibers, and mixtures thereof.