Branched organopolysiloxane and method for producing same

By using branched organopolysiloxanes with specific structures in cosmetics, the compatibility of low molecular weight organopolysiloxanes in cosmetics and through the hydrosilylation reaction of organohydrogen polysiloxanes with olefins is solved and Stability issues achieve good compatibility with polar oil agents and durability of cosmetic films.

CN118946571APending Publication Date: 2024-11-12SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030691.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing low-molecular-weight organopolysiloxanes have problems in cosmetics with strong skin irritability, poor compatibility, difficulty in transparent mixing and affecting the stability of cosmetics. Moreover, the synthesis of high-molecular-weight organopolysiloxanes is difficult to produce The rate is low, especially when using acid catalysts, there is a problem of siloxane bond cracking.

Method used

It provides a branched organopolysiloxane composed of siloxane units of a specific structure, and is produced by a hydrosilylation reaction process of organohydrogen polysiloxane with an olefin having 2 or 3 carbon atoms, and has excellent Compatibility with polar oil agents and hydrosilylation reactions with platinum or rhodium catalysts simplify the synthesis process.

Benefits of technology

It achieves good compatibility with polar oils, etc., is suitable for various solvents and cosmetics, provides a gentle feeling of use and a long-lasting makeup film, improves the stability and hardness of cosmetics, and is simple and high-purity. Branched organopolysiloxane was obtained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946571A_ABST
    Figure CN118946571A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a branched organopolysiloxane which can be a substitute for conventional low-molecular-weight siloxanes and has good compatibility with polar oil agents and the like. The purpose of the present invention is also to provide a method for producing the branched organopolysiloxane in a simple manner and with high purity. The branched organopolysiloxane is represented by formula (1) (in the formula, R1 independently represents an alkyl group having 1-3 carbon atoms, R2 independently represents an alkyl group having 2 or 3 carbon atoms, and R3 independently represents an alkyl group having 1-3 carbon atoms. N is 1 or 2, m is an integer of 0-3 when n = 1, and m is 0 or 1 when n = 2. In addition, the bonding sequence of the siloxane units is not limited to the sequence, and the bonding state of the siloxane units can be block or random. ). # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a branched organopolysiloxane and a method for producing the same. Background Art

[0002] Organopolysiloxanes with 6 or less silicon atoms are often highly volatile and highly compatible with organic compounds. Therefore, they have been used as substitutes for organic solvents and oils for cosmetics (Patent Document 1). Among them, cyclic polysiloxanes with 4 to 6 silicon atoms have been used in many applications because they are easy to synthesize. However, in recent years, there are concerns about the impact of cyclic polysiloxanes on the environment and safety.

[0003] In addition, straight-chain organopolysiloxanes with less than 6 silicon atoms and branched tris(trimethylsiloxy)methylsilane have also been used for various purposes. However, low-molecular-weight organopolysiloxanes with less than 3 silicon atoms have the problem of strong skin irritation, and are not preferred in cosmetic applications in particular. In addition, these straight-chain and branched organopolysiloxanes are mostly manufactured by hydrolysis. Therefore, the generation of the low-molecular-weight siloxanes and the time required to separate the various products have become problems.

[0004] In addition, the organopolysiloxane has poor compatibility with polar oils added to cosmetics and cannot be transparently mixed, which sometimes impairs the feel and stability of the cosmetics. This tendency is particularly evident when an organic ultraviolet absorber is used. In addition, when the organopolysiloxane has low affinity with oily components such as wax that are added for the purpose of solidifying the cosmetics, the crystallization of the oily components is hindered, and the expected hardness of the preparation can no longer be obtained.

[0005] As a method for producing branched tetrasiloxane with high purity, Patent Document 2 discloses a method in which a trialkoxysilane compound is added to a mixed solution of a disiloxane compound, an alcohol and an acid catalyst, and the mixture is reacted, and then water is added to perform co-hydrolysis. However, when the disiloxane is substituted with an alkyl group having 2 or more carbon atoms, it is difficult for the acid catalyst to cause the cleavage of the siloxane bond, and there is a tendency for the yield to decrease. Therefore, there are problems such as the necessity to use a large amount of an acid catalyst.

[0006] An example of synthesizing a compound in which the alkyl group bonded to the silicon atom as a branch point in a branched tetrasiloxane has two or more carbon atoms is reported (Patent Document 2). However, there is no example of synthesizing a compound in which the alkyl group of the trialkylsiloxy group as a terminal group has two or more carbon atoms.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: International Publication No. 2001 / 015658

[0010] Patent Document 2: Japanese Patent Application Publication No. 2004-352677 Summary of the invention

[0011] Problems to be solved by the invention

[0012] The present invention has been made in view of the above-mentioned actual situation, and its object is to provide a branched organopolysiloxane which can be a substitute for conventional low-molecular siloxane and has good compatibility with polar oils, etc. Another object is to provide a method for producing the branched organopolysiloxane simply and at high purity.

[0013] Means for solving problems

[0014] The present inventors have conducted intensive studies to achieve the above-mentioned object and have found that the branched organopolysiloxane of the present invention has excellent compatibility with various organic compounds and is suitable for use as various solvents and oils for cosmetics, thereby completing the present invention.

[0015] Therefore, the present invention provides a branched organopolysiloxane and a method for producing the same.

[0016] 1. A branched organopolysiloxane represented by the following formula (1).

[0017] [Chemistry 1]

[0018]

[0019] (Where R 1 are independently an alkyl group having 1 to 3 carbon atoms, R 2 are independently an alkyl group having 2 or 3 carbon atoms, R 3 Each of the siloxane units is independently an alkyl group having 1 to 3 carbon atoms. n is 1 or 2, and when n=1, m is an integer of 0 to 3, and when n=2, m is 0 or 1. In addition, the bonding sequence of each siloxane unit is not limited to the above sequence, and the bonding state of the siloxane unit can be block or random.

[0020] 2. The branched organopolysiloxane according to 1, wherein the boiling point at 10 hPa is in the range of 87 to 119°C.

[0021] 3. The branched organopolysiloxane according to 1 or 2, wherein in the formula (1), R 1 is methyl or ethyl, R 2 Ethyl, R 3 is methyl, n is 1, and m is 0.

[0022] 4. A method for producing a branched organopolysiloxane according to 1, comprising a step of hydrosilylation reaction of an organohydrogenpolysiloxane represented by the following formula (2) with an olefin having 2 or 3 carbon atoms.

[0023] [Chemistry 2]

[0024]

[0025] (Where R 4 are independently a hydrogen atom, or R 1 The group represented by R 5 are independently a hydrogen atom, or R 3 In addition, m and n are the same as those in the formula (1), and the bonding sequence of each siloxane unit is not limited to the above sequence, and the bonding state of the siloxane unit can be block or random.

[0026] Effects of the Invention

[0027] According to the present invention, a branched organopolysiloxane which can be a substitute for conventional low molecular weight siloxane and has good compatibility with polar oils and the like can be provided, and the branched organopolysiloxane is suitable for use as an oil for various solvents and cosmetics. In addition, a method for producing the branched organopolysiloxane in a simple and high purity can also be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a chart of the 1H-NMR spectrum of the branched organopolysiloxane synthesized in Synthesis Example 1.

[0029] Figure 2 The branched organopolysiloxane synthesized in Synthesis Example 1 29 Figure 1 shows Si-NMR spectrum. DETAILED DESCRIPTION

[0030] The present invention is described in detail below.

[0031] I. Branched organopolysiloxane

[0032] The branched organopolysiloxane of the present invention is represented by the following formula (1).

[0033] [Chemistry 3]

[0034]

[0035] (Where R 1 are independently an alkyl group having 1 to 3 carbon atoms, R 2 are independently an alkyl group having 2 or 3 carbon atoms, R 3Each of the siloxane units is independently an alkyl group having 1 to 3 carbon atoms. n is 1 or 2, and when n=1, m is an integer of 0 to 3, and when n=2, m is 0 or 1. The bonding sequence of each siloxane unit is not limited to the above sequence, and the bonding state of the siloxane unit may be block or random.

[0036] R 1 R is independently an alkyl group having 1 to 3 carbon atoms, and specific examples thereof include methyl, ethyl, and n-propyl. Among them, methyl or ethyl is preferred. 2 R is independently an alkyl group having 2 or 3 carbon atoms, and specifically includes ethyl and n-propyl. Among them, ethyl is preferred. 3 It is independently an alkyl group having 1 to 3 carbon atoms, specifically, methyl, ethyl, and n-propyl. Among them, methyl or ethyl is preferred. n is 1 or 2, preferably 1. m is an integer of 0 to 3 when n=1, preferably an integer of 0 to 2. When n=2, m is 0 or 1, preferably 0. In addition, the bonding order of each siloxane unit is not limited to the above order, and the bonding state of the siloxane unit can be block or random.

[0037] In the formula (1), preferably R 1 is methyl or ethyl, R 2 Ethyl, R 3 A branched organopolysiloxane in which n is 1 and m is 0 is a methyl group. When such a branched organopolysiloxane is blended in a cosmetic, a cosmetic having a soft feel and good spreading is given. In addition, the cosmetic has excellent water repellency and a uniform cosmetic film. Furthermore, there is no strong oily feeling, and a good feeling of use can be achieved. In addition, even if various oils such as silicone, hydrocarbon oil and ester, oily components that are solid at 25°C, or organic ultraviolet absorbers are blended, a cosmetic having excellent stability over time and makeup durability can be obtained.

[0038] Examples of the branched organopolysiloxane represented by the formula (1) include the following organopolysiloxanes.

[0039] [Chemistry 4]

[0040]

[0041] In addition, the branched organopolysiloxane of the present invention preferably has a boiling point at 10 hPa in the range of 87 to 119°C. If it is within this range, the handling property is particularly excellent, and when mixed in a cosmetic, even if it is applied to the skin, it will not give a dry feeling, and after application, it will not feel strongly oily. In addition, if the boiling point is less than 87°C, the volatilization rate is fast, which may give a dry feeling. In addition, by making it below 119°C, it is more difficult to feel oily. In the present invention, the so-called boiling point is a balanced reflux boiling point measured by a method of heating a sample at 10 hPa and recording the internal temperature of a state in which it is repeatedly refluxed at a rate of several drops per second.

[0042] The branched organopolysiloxane of the present invention preferably has a kinematic viscosity at 25°C of 2.0 to 6.0 mm 2 / s, more preferably 2.2 to 3.5 mm 2 The viscosity is a value measured at 25° C. using a Canon Fenske viscometer according to JIS Z8803:2011.

[0043] The branched organopolysiloxane of the present invention has good compatibility with polar oils, etc. Examples of polar oils include organic ultraviolet absorbers such as ethylhexyl methoxycinnamate and octocrylene, and the polar oil has excellent compatibility with ethylhexyl methoxycinnamate.

[0044] II. Method for producing branched organopolysiloxane

[0045] The branched organopolysiloxane of the present invention may be produced by a method having the following steps. According to this production method, the branched organopolysiloxane of formula (1) can be obtained simply and at a high purity.

[0046] [Chemistry 5]

[0047]

[0048] (Where R 4 are independently a hydrogen atom, or R 1 The group represented by R 5 are independently a hydrogen atom, or R 3 In addition, m and n are the same as those in the formula (1), and the bonding sequence of each siloxane unit is not limited to the above sequence, and the bonding state of the siloxane unit can be block or random.

[0049] The step of hydrosilylation reaction of the organohydrogenpolysiloxane represented by the present invention and an olefin having 2 or 3 carbon atoms.

[0050] R 4 are independently a hydrogen atom, or R 1Specific examples of the group represented by include a hydrogen atom, a methyl group, an ethyl group, and an n-propyl group. 5 are independently a hydrogen atom, or R 3 The group represented by , specifically, includes a hydrogen atom, a methyl group, an ethyl group, and an n-propyl group. In addition, m and n are the same as those in the above formula (1). As the olefin having 2 or 3 carbon atoms, ethylene and propylene can be mentioned.

[0051] The blending ratio of the olefin having 2 or 3 carbon atoms to the organohydrogenpolysiloxane represented by the formula (2) is represented by the molar ratio of the olefin having 2 or 3 carbon atoms per 1 mol of the hydrosilyl group in the formula (2), and is preferably 1.0 to 2.0, more preferably 1.0 to 1.2.

[0052] The hydrosilylation reaction is preferably carried out in the presence of a platinum catalyst or a rhodium catalyst, and specifically, chloroplatinic acid, alcohol-modified chloroplatinic acid, chloroplatinic acid-vinylsiloxane complex, etc. are preferably used. The amount of the catalyst used may be a catalytic amount, and in particular, the amount of platinum or rhodium is preferably 50 ppm or less, and more preferably 20 ppm or less, relative to the compounding amount of the organohydrogenpolysiloxane represented by the formula (2).

[0053] When the hydrosilylation reaction is carried out, it can be carried out in the absence of a solvent, and an organic solvent can be used as needed. As the organic solvent, for example, aromatic hydrocarbons such as toluene and xylene, aliphatic or alicyclic hydrocarbons such as n-pentane, n-hexane, and cyclohexane, cyclic ether compounds such as tetrahydrofuran and dioxane, ketones such as acetone and methyl ethyl ketone, etc. can be listed. Among them, it is preferred to carry out the hydrosilylation reaction in the absence of a solvent, or to use hydrocarbons or ether compounds as organic solvents to carry out the hydrosilylation reaction.

[0054] The hydrosilylation reaction conditions are not particularly limited, but the reaction is preferably carried out at 40 to 100° C. for 1 to 10 hours while introducing gaseous ethylene or propylene into or out of the liquid in the reaction vessel.

[0055] III. Cosmetics

[0056] Branched organopolysiloxanes are suitable for various solvents and oil applications in cosmetics due to their good compatibility with polar oils and the like. When the branched organopolysiloxane of the present invention is blended in cosmetics and the like, the blending amount thereof is not particularly limited, and it is appropriately blended in a range of 0.01% to less than 100% by mass. There are no particular limitations on its dosage form, use, optional component blending, and blending amount, and known contents can be appropriately selected. In particular, due to its excellent compatibility with ethylhexyl methoxycinnamate, it is suitable for sunscreen preparations such as sunscreens. It is also clear that cosmetics blended with the branched organopolysiloxane of the present invention are soft in feel, spread well, and obtain a uniform film with high water repellency, so that a uniform film with good durability of the cosmetic film is obtained, and a sunscreen with excellent storage stability at low and high temperatures is obtained.

[0057] When a UV shielding effect is required in a cosmetic, it is preferred to mix a UV absorber. Since the branched organopolysiloxane in the present invention has excellent compatibility with the UV absorber, a cosmetic containing such a UV absorber becomes a cosmetic with good feel during use, excellent stability over time, and long-lasting makeup. In addition, the compound name may be described as a cosmetic name, INCI (International Nomenclature of Cosmetic Ingredients). When the cosmetic name corresponds to INCI, the English description may be omitted.

[0058] The ultraviolet absorber is not particularly limited as long as it is a raw material that can be blended in general cosmetics. Specific examples thereof include oxybenzone-1 (indicative name (INCI: Benzophenone-1)), oxybenzone-2 (indicative name (INCI: Benzophenone-2)), oxybenzone-3 (indicative name (INCI: Benzophenone-3)), oxybenzone-4 (indicative name (INCI: Benzophenone-4)), oxybenzone-5 (indicative name (INCI: Benzophenone-5)), oxybenzone-6 (indicative name (INCI: Benzophenone-6)), oxybenzone-9 (indicative name (INCI: Benzophenone-9)), homosalate (INCI), octocrylene, t-butyl methoxydibenzoylmethane, ethylhexyl salicylate, diethylaminohydroxybenzoyl hexyl benzoate, polysilicone-15, octyl dimethoxybenzylidene dioxoimidazolinium propionate (indicative name (INCI: Ethylhexyl Dimethoxybenzylidene DioxoimidazolidinePropionate), Terephthalylidene DicamphorSulfonic Acid (Indicative Name (INCI: Terephthalylidene DicamphorSulfonic Acid)), Ethylhexyl Triazone (INCI), Isopentyl Trimethoxycinnamate (Indicative Name (INCI: Isopentyl Trimethoxycinnamate Trisiloxane)), Drometrizole Trisiloxane (INCI), Ethylhexyl Dimethyl PABA (Indicative Name (INCI: Ethylhexyl Dimethyl PABA)), Isopropyl Methoxycinnamate (Indicative Name (INCI: Isopropyl Methoxycinnamate)), Ethylhexyl Methoxycinnamate, Bis-Ethylhexyloxyphenol Methoxyphenyl Triazine, Phenylbenzimidazole Sulfonic Acid (Indicative Name (INCI: Phenylbenzimidazole Sulfonic Acid), Methylene Bisbenzotriazolyl Tetramethylbutylphenol, Glyceryl Ethylhexanoate Dimethoxycinnamate (Indicative Name (INCI: Glyceryl Ethylhexanoate Dimethoxycinnamate)), Glyceryl PABA (INCI), Methyl Diisopropyl Cinnamate (Indicative Name (INCI: Diisopropyl Methyl Cinnamate)), Cinoxate (INCI), Ethylhexyl Dimethoxybenzylidene Dioxoimidazolinium Propionate (Indicative Name (INCI: EthylhexylDimethoxybenzylidene DioxoimidazolidinePropionate)) etc.

[0059] In addition, a UVA absorber (for example, diethylaminohydroxybenzoyl hexyl benzoate) and a UVB absorber (for example, ethylhexyl methoxycinnamate) may be used together, or they may be arbitrarily combined.

[0060] In this case, the ultraviolet absorber is preferably one or more organic ultraviolet absorbers selected from ethylhexyl methoxycinnamate (INCI: Ethylhexyl Methoxycinnamate), diethylamino hydroxybenzoyl hexyl benzoate (INCI: Diethylamino Hydroxybenzoyl Hexyl Benzoate), ethylhexyl salicylate (INCI: Ethylhexyl Salicylate), polysilicone-15 (INCI), t-butyl methoxydibenzoylmethane (INCI: Butyl Methoxydibenzoylmethane), oxybenzophenone (INCI: Benzophenone), methylene bisbenzotriazolyl tetramethylbutylphenol (INCI), bis-ethylhexyloxyphenol methoxyphenyl triazine (INCI), and octocrylene (INCI). Such an organic ultraviolet absorber is particularly preferred because the ultraviolet absorbing effect is improved and the compatibility with the branched organopolysiloxane of the present invention is excellent.

[0061] The amount of the ultraviolet absorber is preferably 1 to 50% by mass in the cosmetic, more preferably 3 to 20% by mass in the cosmetic.

[0062] Example

[0063] The following are synthesis examples and examples to specifically illustrate the present invention, but the present invention is not limited to the following examples. It should be noted that the method for synthesizing the branched organopolysiloxane of the present invention is used as a synthesis example, and the example of compounding the branched organopolysiloxane of the present invention is used as an example. 1 H-NMR was measured using ECX-500 manufactured by JEOL 29Si-NMR. Purity is the area % of the chromatogram measured by gas chromatography. In addition, the kinematic viscosity is the value measured at 25°C using a Canon Fenske viscometer according to JIS Z8803:2011. It should be noted that the synthesis examples are examples of branched organopolysiloxanes, and the embodiments and comparative examples are examples of cosmetics. The blending amount described by the product name is the blending amount of the blended product.

[0064] [Synthesis example 1]

[0065] 1,5-Diethyl-3-ethyldimethylsiloxy-1,1,3,5,5-pentamethyltrisiloxane

[0066] In a 1L four-necked flask, add the following formula (3):

[0067] [Chemistry 6]

[0068]

[0069] 580 g of the organohydrogenpolysiloxane (purity 100%) and 0.6 g of a 0.5 mass % toluene solution of a chloroplatinic acid-vinylsiloxane complex were prepared. The liquid was stirred at 40-50°C and ethylene gas was blown into the liquid. The temperature was maintained at 60-70°C to carry out the hydrosilylation reaction. The reaction was followed by gas chromatography to confirm that the ratio of the product was 95% or more, and the reaction was terminated. Vacuum distillation was carried out (oil bath temperature 90-130°C, 1-30 hPa) to obtain 630 g of a colorless transparent liquid fraction. The obtained fraction was 1 H-NMR and 29 Si-NMR spectral analysis confirmed that the target product represented by the following formula (4) was obtained with a purity of 100% and a yield of 83%.

[0070] [Chemistry 7]

[0071]

[0072] The kinematic viscosity is 2.5 mm 2 / s, boiling point is 113℃ / 10hPa. 1 The H-NMR spectrum is shown in Figure 1 ,Will 29 Si-NMR spectrum is shown in Figure 2 .

[0073] [Synthesis example 2]

[0074] 1,5-Diethyl-3-trimethylsiloxy-1,1,3,5,5-pentamethyltrisiloxane

[0075] In a 1L four-necked flask, add the following formula (5):

[0076] [Chemistry 8]

[0077]

[0078] 490 g of the organohydrogenpolysiloxane (purity 72%) and 0.5 g of a 0.5 mass % toluene solution of a chloroplatinic acid-vinylsiloxane complex were prepared. The liquid was stirred at 40-50°C and ethylene gas was blown into the liquid. The temperature was maintained at 60-70°C to carry out a hydrosilylation reaction. The reaction was followed by gas chromatography to confirm that the ratio of the product was 95% or more, and the reaction was terminated. Vacuum distillation was carried out (oil bath temperature 90-130°C, 1-30 hPa) to obtain 153 g of a colorless transparent liquid fraction. The obtained fraction was 1 H-NMR and 29 Si-NMR spectral analysis confirmed that the target product represented by the following formula (6) was obtained with a purity of 100% and a yield of 36%.

[0079] [Chemistry 9]

[0080]

[0081] The organopolysiloxane having the structure represented by (1,5-diethyl-3-trimethylsiloxy-1,1,3,5,5-pentamethyltrisiloxane) has a kinematic viscosity of 2.2 mm 2 / s, boiling point is 97℃ / 10hPa.

[0082] [Compatibility test with ethylhexyl methoxycinnamate]

[0083] The compatibility of the branched organopolysiloxane obtained in Synthesis Examples 1 and 2 and other silicon compounds with ethylhexyl methoxycinnamate (organic ultraviolet absorber) was evaluated by the method shown below. The evaluation results are shown in Table 1.

[0084] (Evaluation method)

[0085] The branched organopolysiloxane obtained in Synthesis Examples 1 and 2 and other silicon compounds and ethylhexyl methoxycinnamate (sometimes referred to as OMC) were collected at the mass ratio shown in Table 1. The mixture was shaken and mixed at room temperature, and the dissolution state on the next day was observed. The dissolution state was represented by dissolution: ○, separation: ×.

[0086] [Table 1]

[0087]

[0088] KF-96L-1.5cs: Decamethyltetrasiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0089] KF-96L-2cs: Dodecamethylpentasiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0090] TMF-1.5: Tris(trimethylsiloxy)methylsilane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0091] KF-995: Decamethylcyclopentasiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0092] D6: Dodecamethylhexasiloxane

[0093] As shown in Table 1, it can be seen that the branched organopolysiloxanes obtained in Synthesis Examples 1 and 2 of the present invention have higher compatibility with ethylhexyl methoxycinnamate than other silicon compounds.

[0094] [Compatibility and crystallization test with oily components that are solid at 25°C]

[0095] The branched organopolysiloxane obtained in Synthesis Example 2 and other organopolysiloxanes were evaluated for compatibility with oily components that are solid at 25° C. and their influence on crystallization by the following method.

[0096] (Evaluation method)

[0097] Each oil component that is solid at 25°C, the branched organopolysiloxane obtained in Synthesis Example 2, and other organopolysiloxanes were obtained at a mass ratio of 1:9, heated at 90°C / 20 minutes, and their dissolution states were visually observed. Evaluation was based on the following criteria.

[0098] Evenly dissolve: ◎

[0099] Uniform dispersion: 0

[0100] Separation: ×

[0101] Then, each heated mixed solution was placed in a tank container and left to stand at 25°C for 2 days to solidify, and the rheometer hardness of the solid was measured. The measurement was performed using a rheometer RT2002D·D (manufactured by Reotech), and the range was 200g, the adapter was φ3mm (rod type), the sample stage speed was 5cm / min, and the immersion width was 1cm. The average of the three measured values ​​was calculated. The higher the value, the harder it is (unit: g).

[0102] [Table 2]

[0103]

[0104] KF-96L-1.5cs: Decamethyltetrasiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0105] KF-96L-2cs: Dodecamethylpentasiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0106] TMF-1.5: Tris(trimethylsiloxy)methylsilane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0107] KF-995: Decamethylpentasiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0108] KF-4422: Diethyloctamethyltetrasiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0109] As shown in Table 2, the branched organopolysiloxane in the present invention is well dissolved or uniformly dispersed in all solid oily components. It can be seen that, in particular, when candelilla wax is used, other silicon compounds are separated, while the branched organopolysiloxane in the present invention is uniformly dispersed. In addition, it can be seen that when polyethylene is used, the compatibility is better than that of linear dimethylpolysiloxane. It can also be seen that the mixed composition can be solidified by cooling the heated composition.

[0110] Generally, it is known that when a mixed composition is prepared using an oil agent having high compatibility with solid oily components such as wax, the hardness of the composition after being cooled and solidified after being heated and dissolved decreases, and even if it is uniformly dissolved or dispersed during heating, it is sometimes difficult to obtain sufficient hardness for obtaining a cosmetic material with excellent stability over time after cooling. When the branched organopolysiloxane in the present invention is used, it is known that it is well dissolved or uniformly dispersed in all solid oily components and has a higher hardness after cooling than other silicon compounds.

[0111] The following are examples of formulations of cosmetics containing the branched organopolysiloxane obtained in Synthesis Examples 1 and 2 of the present invention and comparative examples to specifically illustrate the present invention, but the present invention is not limited to these examples. The amount of the compounding is expressed in % (mass %) unless otherwise specified.

[0112] [Examples 1, 2, Comparative Examples 1 to 3] W / O type sunscreen

[0113] In Examples 1 and 2, the branched organopolysiloxane obtained in Synthesis Examples 1 and 2 was used, and in Comparative Examples 1 to 3, no branched organopolysiloxane was used, and W / O type sunscreens were prepared according to the following production method.

[0114] [Table 3]

[0115]

[0116] (Note 1) Decamethylcyclopentasiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0117] (Note 2) Tris(trimethylsiloxy)methylsilane (INCI: Methyl trimethyl polysiloxane) (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0118] (Note 3) Diphenylsiloxyphenyl trimethyl polysiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0119] (Note 4) A mixture of 70-80% dimethyl polysiloxane and 20-30% (dimethyl polysiloxane / (PEG-10 / 15)) cross-linked polymer (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0120] (Note 5) A mixture of 80-85% diphenylsiloxyphenyl trimethyl polysiloxane and 15-20% cross-linked phenyl-modified dimethyl polysiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0122] (Note 6) Cetyl PEG / PPG-10 / 1 dimethyl polysiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0123] [Manufacturing method]

[0124] Components 1 to 12 were stirred and mixed to be uniform. Components 13 to 16 were uniformly dissolved in component 17, and the mixture of components 1 to 12 was added steadily and stirred to form an emulsion. The mixture was filled into a predetermined container to obtain a sunscreen.

[0125] The W / O type sunscreen obtained was subjected to a usage test based on the following scoring by a panel of 10 women for (1) good feeling (soft feeling), (2) good spreading, (3) good film uniformity, and (4) durability of the makeup film. The results are shown based on the obtained average score according to the following evaluation criteria. In addition, (5) the state of the cosmetic material when it was left at 40°C for 1 month and (6) the state of the cosmetic material when it was left at 5°C for 1 month were also observed. The evaluation results are shown in Table 4.

[0126] (score)

[0127] 5 points: Very good

[0128] 4 points: Good

[0129] 3 points: Average

[0130] 2 points: Slightly poor

[0131] 1 point: Poor

[0132] (Evaluation Criteria)

[0133] ◎: Average score is 4.5 or above

[0134] ○: Average score is 3.5 or more and less than 4.5

[0135] △: Average score is 2.5 or more and less than 3.5

[0136] ×: The average score is 1.5 or more and less than 2.5

[0137] ××: The average score is less than 1.5 points

[0138] [Table 4]

[0139] serial number Evaluation Project <![CDATA[Example 1]]> Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 (1) Good feeling (soft feeling) ○ ○ ○ ○ × (2) Good spreading ◎ ◎ ◎ ○ ◎ (3) Good film uniformity ◎ ◎ ◎ Δ ○ (4) Durability of cosmetic mask ○ ○ ○ Δ Δ (5) The state of cosmetics (40℃) Stablize Stablize Increased viscosity Separation Stablize (6) The state of cosmetics (5℃) Stablize Stablize Separation Separation Stablize

[0140] As shown in Table 4, the sunscreens of Examples 1 and 2 were found to be softer and spread better than Comparative Examples 1 to 3, and to form a uniform film with high water repellency, and thus were sunscreens with good cosmetic film durability and a uniform film. In addition, it was also found that they were sunscreens with excellent storage stability.

[0141] Industrial Applicability

[0142] The branched organopolysiloxane of the present invention has high volatility and high compatibility with organic compounds, and is therefore suitable as a substitute for organic solvents and an oil for cosmetics, etc. In addition, the production method of the present invention can easily and highly pure obtain the branched organopolysiloxane, and thus can be suitably used even for applications where impurities are a problem.

Claims

1. A branched organopolysiloxane represented by the following formula (1): [Chemistry 1] In the formula, R 1 are independently an alkyl group having 1 to 3 carbon atoms, R 2 are independently an alkyl group having 2 or 3 carbon atoms, R 3 They are independently alkyl groups having 1 to 3 carbon atoms, n is 1 or 2, and when n=1, m is an integer of 0 to 3, and when n=2, m is 0 or 1. Furthermore, the bonding sequence of each siloxane unit is not limited to the above, and the bonding state of the siloxane units can be block or random. 2 . The branched organopolysiloxane according to claim 1 , which has a boiling point at 10 hPa in the range of 87 to 119° C.

3. The branched organopolysiloxane according to claim 1 or 2, in, In the formula (1), R 1 is methyl or ethyl, R 2 Ethyl, R 3 is methyl, n is 1, and m is 0.

4. A method for producing a branched organopolysiloxane according to claim 1, comprising a step of hydrosilylation of an organohydrogenpolysiloxane represented by the following formula (2) with an olefin having 2 or 3 carbon atoms, [Chemistry 2] In the formula, R 4 are independently a hydrogen atom, or R 1 The group represented by R 5 are independently a hydrogen atom, or R 3 wherein m and n are the same as those in the formula (1); the bonding sequence of each siloxane unit is not limited to the above sequence, and the bonding state of the siloxane unit may be block or random.