Hybrid bonding insulating film forming material, method for manufacturing semiconductor device, and semiconductor device

By using a mixed-bonded insulating film material formed by polymerizable unsaturated polyimide precursors and oxime photopolymerization initiators, the problems of foreign matter caused by inorganic materials and insufficient heat resistance of organic insulating films are solved, thus achieving high exposure sensitivity and low cost in semiconductor device manufacturing.

CN118946610APending Publication Date: 2024-11-12HD MICROSYSTEMS LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029889.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-01-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the hybrid bonding method using inorganic materials is prone to generating foreign matter during the three-dimensional mounting process of semiconductor chips, resulting in reduced yield and increased manufacturing costs. Meanwhile, the heat resistance of organic insulating films is insufficient, and they cannot effectively prevent the formation of pores during bonding.

Method used

A mixed bonding insulating film forming material is used, consisting of a polyimide precursor containing polymerizable unsaturated bond sites, a solvent, and an oxime-based photopolymerization initiator. This material forms a highly sensitive organic insulating film through photopolymerization, suppressing the formation of porosity during bonding.

Benefits of technology

This invention achieves high exposure sensitivity organic insulating film, avoids porosity formation during bonding, improves semiconductor device yield, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005056890160000021
    Figure BDA0005056890160000021
  • Figure BDA0005056890160000031
    Figure BDA0005056890160000031
  • Figure BDA0005056890160000032
    Figure BDA0005056890160000032
Patent Text Reader

Abstract

Provided is a material for forming a hybrid-bonded insulating film, which contains (A) a polyimide precursor having a polymerizable unsaturated bond site, (B) a solvent, and (C) an oxime-based photopolymerization initiator.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a hybrid bonding insulating film forming material, a method for manufacturing a semiconductor device, and a semiconductor device. Background Art

[0002] In recent years, in order to improve the integration degree of LSI (Large Scale Integrated Circuit), three-dimensional mounting of semiconductor chips has been studied. Non-patent document 1 discloses an example of three-dimensional mounting of semiconductor chips.

[0003] In the case of three-dimensional mounting of semiconductor chips by C2W (Chip-to-Wafer) bonding, the use of a hybrid bonding technology used in W2W (Wafer-to-Wafer) bonding is being studied in order to perform fine bonding of wirings between devices.

[0004] In C2W hybrid bonding, heating during bonding may cause positional deviation mainly due to thermal expansion of substrates, chips, etc. To address such a problem, Patent Document 1 discloses an example of a technology for lowering the bonding temperature by using a cyclic olefin resin.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2019-204818

[0008] Non-patent literature

[0009] Non-patent document 1: F.C. Chen et al., “System on Integrated Chips (SoIC TM) for 3D Heterogeneous Integration”, 2019 IEEE 69th Electronic Components and Technology Conference (ECTC), p. 594-599 (2019) Summary of the invention

[0010] Problems to be solved by the invention

[0011] In the method of C2W bonding by hybrid bonding technology, the practical application of the method of using inorganic materials such as silicon dioxide (SiO2) in the insulating film is explored. However, since inorganic materials are hard materials, foreign matter from inorganic materials generated when cutting semiconductor chips for singulation, for example, will adhere to the surface of the insulating film, and it is possible to produce large gaps at the bonding interface. As a result, the yield of semiconductor device manufacturing is reduced, or equipment such as clean rooms with high cleanliness are required to remove foreign matter, so the manufacturing cost becomes higher.

[0012] On the other hand, the method of performing C2W bonding using an organic insulating film through a hybrid bonding technique is still in the research stage and has not yet been put into practical use. When the cyclic olefin resin described in Patent Document 1 is used, the heat resistance of the resulting organic insulating film is insufficient. If the heat resistance of the organic insulating film is low, for example, during C2W bonding, it will be exposed to high temperatures during subsequent annealing, which may cause voids to form at the bonding interface, causing poor bonding.

[0013] In addition, when a method of forming a plurality of pillars made of metal such as copper (Cu) after bonding is adopted, a photolithography process is performed to remove the insulating film in a predetermined region where the pillars are formed. From the viewpoint of manufacturing cost, etc., it is desirable that the organic insulating film has high exposure sensitivity.

[0014] The present disclosure has been made in view of the above circumstances, and an object of the present disclosure is to provide a hybrid bonding insulating film forming material, a method for manufacturing a semiconductor device, and a semiconductor device that are excellent in exposure sensitivity and can suppress the generation of voids during bonding.

[0015] Means for solving problems

[0016] The specific means for achieving the above-mentioned objects are as follows.

[0017] <1> A hybrid bonding insulating film forming material comprises (A) a polyimide precursor having a polymerizable unsaturated bond site, (B) a solvent, and (C) an oxime-based photopolymerization initiator.

[0018] <2> according to <1> In the hybrid bonding insulating film forming material, the (C) oxime-based photopolymerization initiator comprises a compound represented by the following formula (I):

[0019] [Chemistry 1]

[0020]

[0021] In formula (I), R 1 represents an alkyl group, an alkoxy group, a phenyl group or a phenoxy group, R 2 represents an alkyl group, R 3 It represents a carbonyl group or a monovalent organic group connected via a single bond.

[0022] <3> according to <2> The hybrid bonding insulating film forming material, the (C) oxime-based photopolymerization initiator comprises R in the formula (I) 1 A compound represented by an alkoxy group.

[0023] <4> according to <2> or <3> The hybrid bonding insulating film forming material, the (C) oxime-based photopolymerization initiator comprises R in the formula (I) 1 The compound A represented by an alkoxy group and R in the formula (I) 1 The compound B is represented by an alkyl group or a phenyl group.

[0024] <5> according to <1> ~ <4> The hybrid bonding insulating film forming material described in any one of the preceding claims, wherein the polyimide precursor (A) comprises a compound having a structural unit represented by the following general formula (1),

[0025] [Chemistry 2]

[0026]

[0027] In the general formula (1), X represents a tetravalent organic group, Y represents a divalent organic group, and R 6 and R 7 Each independently represents a hydrogen atom or a monovalent organic group, R 6 and R 7 At least one of them has a polymerizable unsaturated bond.

[0028] <6> according to <5> In the hybrid bonding insulating film forming material, in the general formula (1), the tetravalent organic group represented by X is a group represented by the following formula (E):

[0029] [Chemistry 3]

[0030]

[0031] In formula (E), C represents a single bond, an alkylene group, a halogenated alkylene group, a carbonyl group, a sulfonyl group, an ether bond (-O-), a thioether bond (-S-), a phenylene group, an ester bond (-OC(=O)-), a silene bond (-Si(R A )2-, 2 R A each independently represents a hydrogen atom, an alkyl group or a phenyl group), a siloxane bond (-O-(Si(R B )2-O-) n , 2 R B Each independently represents a hydrogen atom, an alkyl group or a phenyl group, and n represents an integer of 1 or 2 or more), or a divalent group formed by combining at least two of them.

[0032] <7> according to <5> or <6> In the hybrid bonding insulating film forming material, in the general formula (1), the divalent organic group represented by Y is a group represented by the following formula (H):

[0033] [Chemistry 4]

[0034]

[0035] In formula (H), R each independently represents an alkyl group, an alkoxy group, a haloalkyl group, a phenyl group or a halogen atom, and n each independently represents an integer of 0 to 4. D represents a single bond, an alkylene group, a haloalkylene group, a carbonyl group, a sulfonyl group, an ether bond (-O-), a thioether bond (-S-), a phenylene group, an ester bond (-OC(=O)-), a silene bond (-Si(R A )2-, 2 R A each independently represents a hydrogen atom, an alkyl group or a phenyl group), a siloxane bond (-O-(Si(R B )2-O-) n , 2 R B Each independently represents a hydrogen atom, an alkyl group or a phenyl group, and n represents an integer of 1 or 2 or more), or a divalent group formed by combining at least two of them.

[0036] <8> according to <7> In the hybrid bonding insulating film forming material, D in the formula (H) contains an ether bond (—O—).

[0037] <9> according to <5> ~ <8> The hybrid bonding insulating film forming material according to any one of the preceding claims, wherein in the general formula (1), R 6 And the R 7 The monovalent organic group in the formula (2) is any one of an ethyl group, an isobutyl group, and a tert-butyl group, wherein R 6 And the R 7 At least one of the groups is a group represented by the general formula (2),

[0038] [Chemistry 5]

[0039]

[0040] In the general formula (2), R 8 ~R 10 Each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 3 carbon atoms, and R x represents a divalent linking group.

[0041] <10> according to <1> The hybrid bond insulating film forming material according to any one of <9>, further comprising (D) a sensitizer.

[0042] <11> according to <1> The hybrid bond insulating film forming material according to any one of to <10>, further comprising (E) a polymerizable monomer.

[0043] <12> according to <1> The hybrid bond insulating film forming material according to any one of <11>, wherein the glass transition temperature of the hybrid bond insulating film forming material when it is cured is 50° C. to 300° C.

[0044] <13> A method for manufacturing a semiconductor device,

[0045] Preparing a first semiconductor substrate, wherein the first semiconductor substrate has a first substrate body, and a first electrode and a first organic insulating film provided on one surface of the first substrate body;

[0046] preparing a semiconductor chip having a semiconductor chip substrate body, and a second organic insulating film and a second electrode provided on one surface of the semiconductor chip substrate body;

[0047] The first electrode and the second electrode are bonded together, and the first organic insulating film and the second organic insulating film are bonded together.

[0048] 5 In the production of at least one of the first organic insulating film and the second organic insulating film,

[0049] use <1> ~ <12> The hybrid bonding insulating film forming material described in any one of the above.

[0050] <14> according to <13> In the method for manufacturing a semiconductor device, the first electrode and the second electrode are bonded together after the first organic insulating film and the second organic insulating film are bonded together.

[0051] <15> according to <13> ~ <14> In any one of the methods for manufacturing a semiconductor device, before performing any of the bonding of the first electrode and the second electrode, and the bonding of the first organic insulating film and the first organic insulating film, at least one of the one surface of the first semiconductor substrate and the one surface side of the semiconductor chip is ground.

[0052] <16> according to <15> In the method for manufacturing a semiconductor device, the polishing includes chemical mechanical polishing.

[0053] 5 <17> according to <16> In the method for manufacturing a semiconductor device, the grinding further comprises mechanical grinding.

[0054] <18> according to <13> ~ <17> In any one of the methods for manufacturing a semiconductor device, in the bonding between the first electrode and the second electrode, at least one of the following conditions is satisfied: the thickness of the first organic insulating film is thicker than the thickness of the first electrode, and the thickness of the second organic insulating film is thicker than the thickness of the second electrode.

[0055] <19> A semiconductor device comprising:

[0056] A first semiconductor substrate including a first substrate body, and a first organic insulating film and a first electrode provided on one surface of the first substrate body; and

[0057] A semiconductor chip having a semiconductor chip substrate body, and a second organic insulating film and a second electrode provided on one surface of the semiconductor chip substrate body.

[0058] The first organic insulating film is bonded to the second organic insulating film, the first electrode is bonded to the second electrode,

[0059] At least one of the first organic insulating film and the second organic insulating film is <1> ~ <12> A cured product of any one of the above-mentioned hybrid bond insulating film forming materials.

[0060] Effects of the Invention

[0061] According to the present disclosure, it is possible to provide a hybrid bonding insulating film forming material, a method for manufacturing a semiconductor device, and a semiconductor device that are excellent in exposure sensitivity and can suppress the generation of voids during bonding. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] [ Figure 1 ] Figure 1 FIG. 1 is a cross-sectional view schematically showing an example of a semiconductor device manufactured by a method for manufacturing a semiconductor device according to an embodiment.

[0063] [ Figure 2 ] Figure 2 is shown in sequence for manufacturing Figure 1 A method of manufacturing a semiconductor device is shown in FIG.

[0064] [ Figure 3 ] Figure 3 is shown in more detail Figure 2 A diagram showing a bonding method in a method for manufacturing a semiconductor device.

[0065] [ Figure 4 ] Figure 4 It is used to manufacture Figure 1 The semiconductor device method shown is sequentially shown Figure 2 A diagram of the process following the process shown.

[0066] [ Figure 5 ] Figure 5 A diagram showing an example in which a method for manufacturing a semiconductor device according to an embodiment is applied to Chip-to-Wafer (C2W). DETAILED DESCRIPTION

[0067] Hereinafter, the mode for implementing the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiment.

[0068] In the present disclosure, unless otherwise specified, the constituent elements (including element steps, etc.) are not essential. The same applies to numerical values ​​and their ranges, and they do not limit the present disclosure.

[0069] In the present disclosure, the term "step" includes not only steps that are independent of other steps, but also steps that cannot be clearly distinguished from other steps as long as the purpose of the step can be achieved.

[0070] In the present disclosure, in a numerical range expressed using “to”, the numerical values ​​described before and after “to” are included as the minimum value and the maximum value, respectively.

[0071] In the numerical range recorded in stages in the present disclosure, the upper limit or lower limit recorded by a numerical range can also be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In addition, in the numerical range recorded in the present disclosure, the upper limit or lower limit of the numerical range can also be replaced by the value shown in the embodiment.

[0072] In the present disclosure, each component may contain a plurality of corresponding substances. When a plurality of substances corresponding to each component are present in the composition, unless otherwise specified, the content or content of each component refers to the total content or content of the plurality of substances present in the composition.

[0073] In the present disclosure, the term "layer" or "film" includes not only a case where a layer or film is formed on the entire region when a region where the layer or film exists is observed, but also a case where the layer or film is formed on only a part of the region.

[0074] In the present disclosure, the thickness of a layer or a film is a value obtained by measuring the thickness of five points of the target layer or film and providing the measured thickness as the arithmetic mean value.

[0075] The thickness of a layer or film can be measured using a micrometer or the like. In the present disclosure, when the thickness of a layer or film can be directly measured, a micrometer is used for measurement. On the other hand, when measuring the thickness of one layer or the total thickness of a plurality of layers, the measurement can be performed by observing a cross section of the measurement object using an electron microscope.

[0076] In the present disclosure, “(meth)acrylic” means “acrylic” and “methacrylic”, “(meth)acrylate” means “acrylate” and “methacrylate”, and “(meth)acryloyl” means “acryloyl” and “methacryloyl”.

[0077] In the present disclosure, when a functional group has a substituent, the number of carbon atoms in the functional group refers to the total number of carbon atoms including the number of carbon atoms of the substituent.

[0078] When the embodiments are described with reference to the drawings in the present disclosure, the configuration of the embodiments is not limited to the configuration shown in the drawings. In addition, the sizes of components in each figure are conceptual, and the relative relationship between the sizes of the components is not limited to this.

[0079] <Hybrid Bonding Insulating Film Forming Material>

[0080] The hybrid bonded insulating film forming material disclosed herein comprises (A) a polyimide precursor having a polymerizable unsaturated bond site, (B) a solvent, and (C) an oxime-based photopolymerization initiator. Hereinafter, the hybrid bonded insulating film forming material disclosed herein is also referred to as an "insulating film forming material", and (A) a polyimide precursor having a polymerizable unsaturated bond site is also referred to as a "(A) polyimide precursor". In addition, the "oxime system" in the present disclosure includes an oxime structure: a structure in which the H of OH in C=N-OH is substituted.

[0081] By adopting the configuration of the hybrid bonding insulating film forming material of the present disclosure, the exposure sensitivity is excellent and the generation of voids during bonding can be suppressed. The reason for this is not clear, but it is considered as follows.

[0082] Compared with the (A) polyimide precursor of the present disclosure, the (C) oxime-based photopolymerization initiator has absorption at a longer wavelength than other photopolymerization initiators, and thus has a higher exposure sensitivity. In addition, since the 5% thermal weight loss temperature is high, volatilization can be suppressed during heating for bonding, etc., and the generation of voids can be suppressed.

[0083] Hereinafter, components contained in the insulating film forming material of the present disclosure and components that may be contained are described.

[0084] ((A) Polyimide precursor)

[0085] The insulating film forming material of the present disclosure includes (A) a polyimide precursor having a polymerizable unsaturated bond site.

[0086] (A) The polyimide precursor is preferably at least one resin selected from the group consisting of polyamic acid, polyamic acid ester, polyamic acid salt and polyamic acid amide. Polyamic acid ester and polyamic acid amide are compounds in which at least a part of the hydrogen atoms of the carboxyl groups in the polyamic acid are substituted by a monovalent organic group, and polyamic acid salt is a compound in which at least a part of the carboxyl groups in the polyamic acid form a salt structure with a basic compound having a pH exceeding 7.

[0087] (A) The polyimide precursor preferably contains a compound having a structural unit represented by the following general formula (1): This tends to provide a semiconductor device having an insulating film exhibiting high reliability.

[0088] [Chemistry 6]

[0089]

[0090] In the general formula (1), X represents a tetravalent organic group, and Y represents a divalent organic group. 6 and R 7 Each independently represents a hydrogen atom or a monovalent organic group, R 6 and R 7 At least one of them has a polymerizable unsaturated bond.

[0091] The polyimide precursor may have a plurality of structural units represented by the general formula (1), wherein X, Y, R 6 and R 7 They may be the same or different.

[0092] It should be noted that R 6 and R 7 As long as each is independently a hydrogen atom or a monovalent organic group, the combination thereof is not particularly limited. 6 and R 7 At least one of them may be a hydrogen atom and the rest may be monovalent organic groups described below, or they may be the same or different monovalent organic groups. As described above, when the polyimide precursor has a plurality of structural units represented by the general formula (1), R of each structural unit is 6 and R 7 The combinations can be the same or different.

[0093] In the general formula (1), the tetravalent organic group represented by X preferably has 4 to 30 carbon atoms, more preferably 4 to 25 carbon atoms, further preferably 5 to 13 carbon atoms, and particularly preferably 6 to 12 carbon atoms.

[0094] The tetravalent organic group represented by X may contain an aromatic ring. Examples of the aromatic ring include aromatic hydrocarbon groups (e.g., carbon atoms constituting the aromatic ring are 6 to 20), aromatic heterocyclic groups (e.g., atoms constituting the heterocyclic ring are 5 to 20), and the like. The tetravalent organic group represented by X is preferably an aromatic hydrocarbon group. Examples of the aromatic hydrocarbon group include a benzene ring, a naphthalene ring, a phenanthrene ring, and the like.

[0095] When the tetravalent organic group represented by X includes an aromatic ring, each aromatic ring may have a substituent or may be unsubstituted. Examples of the substituent of the aromatic ring include an alkyl group, a fluorine atom, a halogenated alkyl group, a hydroxyl group, and an amino group.

[0096] When the tetravalent organic group represented by X includes a benzene ring, the tetravalent organic group represented by X preferably includes 1 to 4 benzene rings, more preferably includes 1 to 3 benzene rings, and further preferably includes 1 or 2 benzene rings.

[0097] When the tetravalent organic group represented by X contains two or more benzene rings, the benzene rings may be connected by a single bond, or by an alkylene group, a halogenated alkylene group, a carbonyl group, a sulfonyl group, an ether bond (-O-), a thioether bond (-S-), a silene bond (-Si(R-)), or a silene bond (-Si(R-)). A )2-, 2 R A each independently represents a hydrogen atom, an alkyl group or a phenyl group), a siloxane bond (-O-(Si(R B )2-O-) n , 2 R B Each independently represents a hydrogen atom, an alkyl group or a phenyl group, and n represents an integer greater than 1 or 2) and the like, a composite connecting group formed by combining at least two of these connecting groups, etc. In addition, two benzene rings may be bonded at two locations by a single bond and at least one of the connecting groups, and a 5-membered ring or a 6-membered ring containing the connecting group is formed between the two benzene rings.

[0098] In the general formula (1), -COOR 6 The -COOR group and the -CONH- group are preferably located in ortho positions relative to each other. 7 The -CO- group and the -CO- group are preferably located in ortho positions with respect to each other.

[0099] As specific examples of the tetravalent organic group represented by X, groups represented by the following formulae (A) to (F) can be cited. Among them, from the viewpoint of obtaining an insulating film having excellent flexibility and further suppressing the generation of voids at the bonding interface, a group represented by the following formula (E) is preferred, and a group represented by the following formula (E) in which C contains an ether bond is more preferred, and an ether bond is further preferred. The following formula (F) is a structure in which C in the following formula (E) is a single bond.

[0100] It should be noted that the present disclosure is not limited to the following specific examples.

[0101] [Chemistry 7]

[0102]

[0103] In formula (D), A and B are each independently a single bond or a divalent group not conjugated with the benzene ring. However, A and B are not both single bonds. Examples of divalent groups not conjugated with the benzene ring include methylene, halogenated methylene, halogenated methyl methylene, carbonyl, sulfonyl, ether bond (-O-), thioether bond (-S-), silene bond (-Si(R-)), and silylated bond (-Si(R-). A )2-, 2 R A Each independently represents a hydrogen atom, an alkyl group or a phenyl group) etc. Among them, A and B each independently represent preferably a methylene group, a bis(trifluoromethyl)methylene group, a difluoromethylene group, an ether bond, a thioether bond etc., and more preferably an ether bond.

[0104] In formula (E), C represents a single bond, an alkylene group, a halogenated alkylene group, a carbonyl group, a sulfonyl group, an ether bond (-O-), a thioether bond (-S-), a phenylene group, an ester bond (-OC(=O)-), a silene bond (-Si(R A )2-, 2 R A each independently represents a hydrogen atom, an alkyl group or a phenyl group), a siloxane bond (-O-(Si(R B )2-O-) n , 2 R B Each independently represents a hydrogen atom, an alkyl group or a phenyl group, and n represents an integer of 1 or 2 or more) or a divalent group formed by combining at least two of them. C preferably contains an ether bond, and is preferably an ether bond.

[0105] Furthermore, C may include a structure represented by the following formula (C1).

[0106] [Chemistry 8]

[0107]

[0108] The alkylene group represented by C in the formula (E) is preferably an alkylene group having 1 to 10 carbon atoms, more preferably an alkylene group having 1 to 5 carbon atoms, and still more preferably an alkylene group having 1 or 2 carbon atoms.

[0109] Specific examples of the alkylene group represented by C in formula (E) include straight-chain alkylene groups such as methylene, ethylene, trimethylene, tetramethylene, pentamethylene, and hexamethylene; methylmethylene, methylethylene, ethylmethylene, dimethylmethylene, 1,1-dimethylethylene, 1-methyltrimethylene, 2-methyltrimethylene, ethylethylene, 1-methyltetramethylene, 2-methyltetramethylene, 1-ethyltrimethylene, 2-ethyltrimethylene, 1,1 - Branched chain alkylene groups such as dimethyltrimethylene, 1,2-dimethyltrimethylene, 2,2-dimethyltrimethylene, 1-methylpentamethylene, 2-methylpentamethylene, 3-methylpentamethylene, 1-ethyltetramethylene, 2-ethyltetramethylene, 1,1-dimethyltetramethylene, 1,2-dimethyltetramethylene, 2,2-dimethyltetramethylene, 1,3-dimethyltetramethylene, 2,3-dimethyltetramethylene, and 1,4-dimethyltetramethylene. Among them, methylene is preferred.

[0110] The haloalkylene group represented by C in formula (E) is preferably a haloalkylene group having 1 to 10 carbon atoms, more preferably a haloalkylene group having 1 to 5 carbon atoms, and still more preferably a haloalkylene group having 1 to 3 carbon atoms.

[0111] Specific examples of the halogenated alkylene group represented by C in formula (E) include alkylene groups in which at least one hydrogen atom contained in the alkylene group represented by C in formula (E) is substituted with a halogen atom such as a fluorine atom or a chlorine atom. Among them, fluoromethylene, difluoromethylene, hexafluorodimethylmethylene, etc. are preferred.

[0112] As R contained in the above-mentioned silene bond or siloxane bond A or R B The alkyl group represented by is preferably an alkyl group having 1 to 5 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and still more preferably an alkyl group having 1 or 2 carbon atoms. A or R B Specific examples of the alkyl group represented by include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl and the like.

[0113] Specific examples of the tetravalent organic group represented by X may be groups represented by the following formula (J) to formula (O).

[0114] [Chemistry 9]

[0115]

[0116] In the general formula (1), the divalent organic group represented by Y preferably has 4 to 25 carbon atoms, more preferably 6 to 20 carbon atoms, and even more preferably 12 to 18 carbon atoms.

[0117] The skeleton of the divalent organic group represented by Y may be the same as the skeleton of the tetravalent organic group represented by X, and the preferred skeleton of the divalent organic group represented by Y may be the same as the preferred skeleton of the tetravalent organic group represented by X. The skeleton of the divalent organic group represented by Y may be a structure in which two bonding positions in the tetravalent organic group represented by X are substituted with atoms (e.g., hydrogen atoms) or functional groups (e.g., alkyl groups).

[0118] The divalent organic group represented by Y may be a divalent aliphatic group or a divalent aromatic group. From the viewpoint of heat resistance, the divalent organic group represented by Y is preferably a divalent aromatic group. As the divalent aromatic group, there may be mentioned a divalent aromatic hydrocarbon group (for example, the number of carbon atoms constituting the aromatic ring is 6 to 20), a divalent aromatic heterocyclic group (for example, the number of atoms constituting the heterocyclic ring is 5 to 20), etc., preferably a divalent aromatic hydrocarbon group.

[0119] Specific examples of the divalent aromatic group represented by Y include groups represented by the following formula (G) and formula (H). Among them, from the viewpoint of obtaining an insulating film having excellent flexibility and further suppressing the generation of voids at the bonding interface, a group represented by the following formula (H) is preferred, wherein in the following formula (H), D is more preferably a single bond or a group containing an ether bond, further preferably a single bond or a group containing an ether bond, particularly preferably a group containing an ether bond, and extremely preferably an ether bond.

[0120] [Chemistry 10]

[0121]

[0122] In formula (G) to formula (H), R each independently represents an alkyl group, an alkoxy group, a halogenated alkyl group, a phenyl group or a halogen atom, and n each independently represents an integer of 0 to 4.

[0123] In formula (H), D represents a single bond, an alkylene group, a halogenated alkylene group, a carbonyl group, a sulfonyl group, an ether bond (-O-), a thioether bond (-S-), a phenylene group, an ester bond (-OC(=O)-), a silene bond (-Si(R A )2-, 2 R A each independently represents a hydrogen atom, an alkyl group or a phenyl group), a siloxane bond (-O-(Si(R B )2-O-) n , 2 R B Each independently represents a hydrogen atom, an alkyl group or a phenyl group, and n represents an integer greater than 1 or 2) or a divalent group formed by combining at least two of them. In addition, D can be a structure represented by the above formula (C1). The specific examples of D in formula (H) are the same as the specific examples of C in formula (E).

[0124] D in the formula (H) is preferably each independently a single bond, an ether bond, a group including an ether bond and a phenylene group, a group including an ether bond, a phenylene group, and an alkylene group, or the like.

[0125] The alkyl group represented by R in formula (G) to formula (H) is preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 5 carbon atoms, and still more preferably an alkyl group having 1 or 2 carbon atoms.

[0126] Specific examples of the alkyl group represented by R in formula (G) to formula (H) include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl and the like.

[0127] The alkoxy group represented by R in formula (G) to formula (H) is preferably an alkoxy group having 1 to 10 carbon atoms, more preferably an alkoxy group having 1 to 5 carbon atoms, and still more preferably an alkoxy group having 1 or 2 carbon atoms.

[0128] Specific examples of the alkoxy group represented by R in formula (G) to formula (H) include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, sec-butoxy, tert-butoxy and the like.

[0129] The haloalkyl group represented by R in formula (G) to formula (H) is preferably a haloalkyl group having 1 to 5 carbon atoms, more preferably a haloalkyl group having 1 to 3 carbon atoms, and still more preferably a haloalkyl group having 1 or 2 carbon atoms.

[0130] Specific examples of the halogenated alkyl group represented by R in formula (G) to (H) include alkyl groups in which at least one hydrogen atom contained in the alkyl group represented by R in formula (G) to (H) is substituted with a halogen atom such as a fluorine atom or a chlorine atom. Among them, fluoromethyl, difluoromethyl, trifluoromethyl, etc. are preferred.

[0131] In formula (G) to formula (H), n is each independently preferably 0 to 2, more preferably 0 or 1, and even more preferably 0.

[0132] Specific examples of the divalent aliphatic group represented by Y include a linear or branched alkylene group, a cycloalkylene group, and a divalent group having a polyalkylene oxide structure.

[0133] The linear or branched alkylene group represented by Y is preferably an alkylene group having 1 to 20 carbon atoms, more preferably an alkylene group having 1 to 15 carbon atoms, and still more preferably an alkylene group having 1 to 10 carbon atoms.

[0134] Specific examples of the alkylene group represented by Y include tetramethylene, hexamethylene, heptamethylene, octamethylene, nonamethylene, decamethylene, undecamethylene, dodecamethylene, 2-methylpentamethylene, 2-methylhexamethylene, 2-methylheptamethylene, 2-methyloctamethylene, 2-methylnonamethylene, and 2-methyldecamethylene.

[0135] The cycloalkylene group represented by Y is preferably a cycloalkylene group having 3 to 10 carbon atoms, and more preferably a cycloalkylene group having 3 to 6 carbon atoms.

[0136] Specific examples of the cycloalkylene group represented by Y include cyclopropylene group, cyclohexylene group, and the like.

[0137] As the unit structure contained in the divalent group having a polyalkylene oxide structure represented by Y, an alkylene oxide structure having 1 to 10 carbon atoms is preferred, an alkylene oxide structure having 1 to 8 carbon atoms is more preferred, and an alkylene oxide structure having 1 to 4 carbon atoms is further preferred. Among them, as the polyalkylene oxide structure, a polyethylene oxide structure or a polypropylene oxide structure is preferred. The alkylene group in the alkylene oxide structure may be linear or branched. The unit structure in the polyalkylene oxide structure may be one or more.

[0138] The divalent organic group represented by Y may be a divalent group having a polysiloxane structure. Examples of the divalent group having a polysiloxane structure represented by Y include a divalent group having a polysiloxane structure in which a silicon atom in the polysiloxane structure is bonded to a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 18 carbon atoms.

[0139] Specific examples of the alkyl group having 1 to 20 carbon atoms bonded to the silicon atom in the polysiloxane structure include methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-octyl, 2-ethylhexyl, n-dodecyl, etc. Among them, methyl is preferred.

[0140] The aryl group having 6 to 18 carbon atoms bonded to the silicon atom in the polysiloxane structure may be unsubstituted or substituted. Specific examples of the substituent when the aryl group has a substituent include a halogen atom, an alkoxy group, a hydroxyl group, etc. Specific examples of the aryl group having 6 to 18 carbon atoms include a phenyl group, a naphthyl group, a benzyl group, etc. Among them, a phenyl group is preferred.

[0141] The number of the alkyl group having 1 to 20 carbon atoms or the aryl group having 6 to 18 carbon atoms in the polysiloxane structure may be one or two or more.

[0142] The silicon atom constituting the divalent group having a polysiloxane structure represented by Y may be bonded to the NH group in the general formula (1) via an alkylene group such as a methylene group or an ethylene group, an arylene group such as a phenylene group, or the like.

[0143] The group represented by formula (G) is preferably a group represented by the following formula (G'), and the group represented by formula (H) is preferably a group represented by the following formula (H'), formula (H") or formula (H'"), and from the viewpoint of having a flexible skeleton and excellent bonding properties, a group represented by the following formula (H') or formula (H") is more preferable.

[0144] [Chemistry 11]

[0145]

[0146] In the formula (H'"), R each independently represents an alkyl group, an alkoxy group, a haloalkyl group, a phenyl group or a halogen atom. R is preferably an alkyl group, and more preferably a methyl group.

[0147] The combination of the tetravalent organic group represented by X and the divalent organic group represented by Y in the general formula (1) is not particularly limited. Examples of the combination of the tetravalent organic group represented by X and the divalent organic group represented by Y include a combination in which X is a group represented by the formula (E) and Y is a group represented by the formula (H).

[0148] R 6 and R 7 Each independently represents a hydrogen atom or a monovalent organic group, at least one of which has a polymerizable unsaturated bond. As the monovalent organic group, it is preferably an aliphatic hydrocarbon group having 1 to 4 carbon atoms or an organic group having an unsaturated double bond, more preferably a group represented by the following general formula (2), an ethyl group, an isobutyl group or a tert-butyl group, and further preferably an aliphatic hydrocarbon group having 1 or 2 carbon atoms or a group represented by the following general formula (2). In this case, R 6 and R 7 At least one of them is a group represented by the general formula (2).

[0149] When the monovalent organic group contains an organic group having an unsaturated double bond, preferably a group represented by the following general formula (2), the i-ray transmittance is high, and there is a tendency to form a good cured product even at a low temperature of 400° C. or less. In addition, when the monovalent organic group contains an organic group having an unsaturated double bond, preferably a group represented by the following general formula (2), at least a part of the unsaturated double bond portion is released by the (C) compound.

[0150] Specific examples of the aliphatic hydrocarbon group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, and a tert-butyl group. Among them, an ethyl group, an isobutyl group, and a tert-butyl group are preferred.

[0151] [Chemistry 12]

[0152]

[0153] In the general formula (2), R 8 ~R 10 Each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 3 carbon atoms, and R x represents a divalent linking group.

[0154] R in the general formula (2) 8 ~R 10 The aliphatic hydrocarbon group represented by is 1 to 3 carbon atoms, preferably 1 or 2. 8 ~R 10 Specific examples of the aliphatic hydrocarbon group represented by include methyl group, ethyl group, n-propyl group, isopropyl group and the like, and methyl group is preferred.

[0155] As R in the general formula (2) 8 ~R 10 Combination of R 8 and R 9 is a hydrogen atom, R 10 A combination of hydrogen atoms or methyl groups.

[0156] R in the general formula (2) x It is a divalent linking group, and is preferably a hydrocarbon group having 1 to 10 carbon atoms. Examples of the hydrocarbon group having 1 to 10 carbon atoms include a linear or branched alkylene group.

[0157] R x The number of carbon atoms in is preferably 1 to 10, more preferably 2 to 5, further preferably 2 or 3.

[0158] In the general formula (1), preferably R 6 and R 7 At least one of them is a group represented by the general formula (2), and more preferably R 6 and R 7 Both are groups represented by the general formula (2).

[0159] When the (A) polyimide precursor contains a compound having a structural unit represented by the above general formula (1), R relative to all structural units contained in the compound is 6 and R 7 The total of R 6 and R 7 The ratio of the group represented by the general formula (2) is preferably 60 mol% or more, more preferably 70 mol% or more, and further preferably 80 mol% or more. The upper limit is not particularly limited and may be 100 mol%.

[0160] It should be noted that the above ratio may be greater than or equal to 0 mol % and less than 60 mol %.

[0161] The group represented by the general formula (2) is preferably a group represented by the following general formula (2').

[0162] [Chemistry 13]

[0163]

[0164] In the general formula (2'), R 8 ~R 10 Each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 3 carbon atoms, and q represents an integer of 1 to 10.

[0165] In the general formula (2′), q is an integer of 1 to 10, preferably an integer of 2 to 5, and more preferably 2 or 3.

[0166] The content of the structural unit represented by the general formula (1) contained in the compound having the structural unit represented by the general formula (1) is preferably 60 mol% or more, more preferably 70 mol% or more, and further preferably 80 mol% or more relative to all structural units. The upper limit of the above content is not particularly limited and can be 100 mol%.

[0167] The (A) polyimide precursor may be a material synthesized using tetracarboxylic dianhydride and a diamine compound. In this case, in the general formula (1), X corresponds to a residue derived from tetracarboxylic dianhydride, and Y corresponds to a residue derived from a diamine compound. It should be noted that the (A) polyimide precursor may also be synthesized using tetracarboxylic acid instead of tetracarboxylic dianhydride.

[0168] Specific examples of tetracarboxylic dianhydrides include pyromellitic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-biphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 2,3,5,6-pyridinetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 3,4, 9,10-perylenetetracarboxylic dianhydride, m-terphenyl-3,3',4,4'-tetracarboxylic dianhydride, p-terphenyl-3,3',4,4'-tetracarboxylic dianhydride, 1,1,4,4'-(4,4'-isopropylidene diphenyloxy) diphthalic anhydride, 1,3,3,3-hexafluoro-2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 1,1,1,3,3,3-hexafluoro-2,2-bis(3,4-dicarboxyphenyl)propane dianhydride phenyl)propane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis{4'-(2,3-dicarboxyphenoxy)phenyl}propane dianhydride, 2,2-bis{4'-(3,4-dicarboxyphenoxy)phenyl}propane dianhydride, 1,1,1,3,3,3-hexafluoro-2,2-bis{4'-(2,3-dicarboxyphenoxy)phenyl}propane dianhydride 1,1,1,3,3,3-hexafluoro-2,2-bis{4'-(3,4-dicarboxyphenoxy)phenyl}propane dianhydride, 4,4'-oxydiphthalic dianhydride, 4,4'-sulfonyldiphthalic dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, cyclopentanone dispiro norbornane tetracarboxylic dianhydride, 2,2-bis{4-(4'-phenoxy)phenyl}propane tetracarboxylic dianhydride, etc. Among these, 3,3',4,4'-biphenyl ether tetracarboxylic dianhydride and 3,3',4,4'-biphenyl tetracarboxylic dianhydride are preferred, and 3,3',4,4'-biphenyl ether tetracarboxylic dianhydride is more preferred from the viewpoint of bonding at a lower temperature.

[0169] Tetracarboxylic dianhydride may be used alone or in combination of two or more.

[0170] Specific examples of the diamine compound include 2,2'-dimethylbiphenyl-4,4'-diamine, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2'-difluoro-4,4'-diaminobiphenyl, p-phenylenediamine, m-phenylenediamine, p-phenylenediamine, m-phenylenediamine, 1,5-diaminonaphthalene, benzidine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 2,4'-diaminodiphenyl ether, 2,2'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 2,4'-diaminodiphenyl ether, 2,2'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 2,4'-diaminodiphenyl ether, 2,2'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 3 ,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 2,4'-diaminodiphenyl sulfone, 2,2'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 2,4'-diaminodiphenyl sulfide, 2,2'-diaminodiphenyl sulfide, o-tolidine, o-tolidine sulfone, 4,4'-methylenebis(2,6-diethylaniline), 4,4'-methylenebis(2,6-diisopropylaniline), 2,4-diaminotrimethylbenzene, 1,5 -diaminonaphthalene, 4,4'-benzophenone diamine, bis{4-(4'-aminophenoxy)phenyl}sulfone, 2,2-bis{4-(4'-aminophenoxy)phenyl}propane, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, bis{4-(3'-aminophenoxy)phenyl}sulfone, 2,2-bis(4-aminophenyl)propane, 9,9-bis(4-aminophenyl)fluorene, 1,3-bis(3-aminophenoxy)benzene, 1,4-diaminobutane, 1,6 1,2-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diaminododecane, 2-methyl-1,5-diaminopentane, 2-methyl-1,6-diaminohexane, 2-methyl-1,7-diaminoheptane, 2-methyl-1,8-diaminooctane, 2-methyl-1,9-diaminononane, 2-methyl-1,10-diaminodecane, 1,4-cyclohexanediamine, 1,3-cyclohexanediamine, diaminopolysiloxane, etc. As the diamine compound, 2,2'-dimethylbiphenyl-4,4'-diamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether and 1,3-bis(3-aminophenoxy)benzene are preferred. Among them, 4,4′-diaminodiphenyl ether, 1,3-bis(3-aminophenoxy)benzene, and 2,2-bis{4-(4′-aminophenoxy)phenyl}propane are more preferred because they have a flexible skeleton and are excellent in adhesiveness.

[0171] The diamine compounds may be used alone or in combination of two or more.

[0172] It has a structural unit represented by the general formula (1) and R in the general formula (1) 6 and R 7 The compound in which at least one of the components is a monovalent organic group can be obtained, for example, by the following method (a) or (b).

[0173] (a) After reacting tetracarboxylic dianhydride (preferably tetracarboxylic dianhydride represented by the following general formula (8)) with a compound represented by R-OH in an organic solvent to prepare a diester derivative, the diester derivative is subjected to a condensation reaction with a diamine compound represented by H2N-Y-NH2.

[0174] (b) Tetracarboxylic dianhydride and a diamine compound represented by H2N-Y-NH2 are reacted in an organic solvent to obtain a polyamic acid solution, and a compound represented by R-OH is added to the polyamic acid solution to react in an organic solvent to introduce an ester group.

[0175] Here, Y in the diamine compound represented by H2N-Y-NH2 is the same as Y in the general formula (1), and the specific examples and preferred examples are also the same. In addition, R in the compound represented by R-OH represents a monovalent organic group, and the specific examples and preferred examples are the same as R in the general formula (1). 6 and R 7 The same situation.

[0176] The tetracarboxylic dianhydride represented by the general formula (8), the diamine compound represented by H2N-Y-NH2, and the compound represented by R-OH may be used alone or in combination of two or more.

[0177] Examples of the organic solvent include N-methyl-2-pyrrolidone, γ-butyrolactone, dimethoxyimidazolidinone, and 3-methoxy-N,N-dimethylpropionamide. Among them, 3-methoxy-N,N-dimethylpropionamide is preferred.

[0178] The polyimide precursor may be synthesized by allowing a dehydration condensation agent to act on the polyamic acid solution together with the compound represented by R—OH. The dehydration condensation agent preferably includes at least one selected from the group consisting of trifluoroacetic anhydride, N,N′-dicyclohexylcarbodiimide (DCC), and 1,3-diisopropylcarbodiimide (DIC).

[0179] (A) The compound contained in the polyimide precursor can be obtained as follows: a compound represented by R-OH is allowed to act on a tetracarboxylic dianhydride represented by the following general formula (8) to prepare a diester derivative, a chlorinating agent such as thionyl chloride is allowed to act to convert it into an acid chloride, and then a diamine compound represented by H2N-Y-NH2 is allowed to react with the acid chloride.

[0180] (A) The compound contained in the polyimide precursor can be obtained by allowing the compound represented by R-OH to act on the tetracarboxylic dianhydride represented by the following general formula (8) to prepare a diester derivative, and then allowing the diamine compound represented by H2N-Y-NH2 to react with the diester derivative in the presence of a carbodiimide compound.

[0181] The compound contained in the (A) polyimide precursor can be obtained by reacting the tetracarboxylic dianhydride represented by the following general formula (8) with the diamine compound represented by H2N-Y-NH2 to prepare polyamic acid, isimidizing the polyamic acid in the presence of a dehydration condensation agent such as trifluoroacetic anhydride, and then allowing the compound represented by R-OH to act. Alternatively, the compound represented by R-OH can also be allowed to act on a part of the tetracarboxylic dianhydride in advance, so that the partially esterified tetracarboxylic dianhydride reacts with the diamine compound represented by H2N-Y-NH2.

[0182] [Chemistry 14]

[0183]

[0184] In the general formula (8), X is the same as X in the general formula (1), and the specific examples and preferred examples are also the same.

[0185] The compound represented by R—OH used in the synthesis of the compound contained in the polyimide precursor (A) may be R of the group represented by the general formula (2). x A compound having a hydroxyl group bonded thereto, a compound having a hydroxyl group bonded to the terminal methylene group of the group represented by the general formula (2'), etc. Specific examples of the compound represented by R-OH include methanol, ethanol, n-propanol, isopropanol, n-butanol, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 2-hydroxybutyl acrylate, 2-hydroxybutyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, etc. Among them, 2-hydroxyethyl methacrylate and 2-hydroxyethyl acrylate are preferred.

[0186] (A) The molecular weight of the polyimide precursor is not particularly limited, but is, for example, preferably 10,000 to 200,000, more preferably 10,000 to 100,000 in terms of weight average molecular weight.

[0187] The weight average molecular weight can be measured by, for example, gel permeation chromatography, and can be calculated by conversion using a standard polystyrene calibration curve.

[0188] The insulating film forming material of the present disclosure may further include a dicarboxylic acid, and the (A) polyimide precursor contained in the insulating film forming material may have a structure in which a part of the amino group in the (A) polyimide precursor reacts with the carboxyl group in the dicarboxylic acid. For example, when synthesizing the polyimide precursor, a part of the amino group of the diamine compound may react with the carboxyl group of the dicarboxylic acid.

[0189] The dicarboxylic acid may be a dicarboxylic acid having a (meth)acrylic acid group, for example, a dicarboxylic acid represented by the following formula: In this case, when synthesizing the polyimide precursor (A), a methacrylic acid group derived from the dicarboxylic acid can be introduced into the polyimide precursor (A) by reacting a part of the amino group of the diamine compound with the carboxyl group of the dicarboxylic acid.

[0190] [Chemistry 15]

[0191]

[0192] The insulating film forming material disclosed herein may further include a polyimide resin in addition to (A) a polyimide precursor. By combining a polyimide precursor and a polyimide resin, it is possible to suppress the generation of volatiles due to dehydration cyclization during the formation of an imide ring, thereby tending to suppress the generation of pores. The polyimide resin referred to herein refers to a resin having an imide skeleton in all or part of the resin skeleton. The polyimide resin is preferably soluble in a solvent in the insulating film forming material using a polyimide precursor.

[0193] The polyimide resin is not particularly limited as long as it is a polymer compound having a plurality of structural units including imide bonds, and preferably contains a structural unit represented by the following general formula (X). This tends to provide a semiconductor device having an insulating film with high reliability.

[0194] [Chemistry 16]

[0195]

[0196] In the general formula (X), X represents a tetravalent organic group, and Y represents a divalent organic group. Preferred examples of the substituents X and Y in the general formula (X) are the same as the preferred examples of the substituents X and Y in the general formula (1).

[0197] When the insulating film forming material of the present disclosure includes a polyimide resin, the ratio of the polyimide resin to the total of the polyimide precursor and the polyimide resin may be 15% by mass to 50% by mass, or 10% by mass to 20% by mass.

[0198] The insulating film forming material disclosed herein may also include other resins other than (A) the polyimide precursor and the polyimide resin. As other resins, for example, from the viewpoint of heat resistance, novolac resins, acrylic resins, polyether nitrile resins, polyether sulfone resins, epoxy resins, polyethylene terephthalate resins, polyethylene naphthalate resins, polyvinyl chloride resins, etc. may be cited. Other resins may be used alone or in combination of two or more.

[0199] In the insulating film forming material of the present disclosure, the content of the (A) polyimide precursor relative to the total amount of the resin component is preferably 50 to 100% by mass, more preferably 70 to 100% by mass, and further preferably 90 to 100% by mass.

[0200] ((B)Solvent)

[0201] The insulating film forming material disclosed herein contains a (B) solvent (hereinafter also referred to as "component (B)"). The (B) component may be used alone or in combination of two or more. For example, from the perspective of reducing reproductive toxicity and environmental load of the insulating film forming material, the (B) component preferably contains at least one selected from the group consisting of compounds represented by the following formulae (3) to (8).

[0202] [Chemistry 17]

[0203]

[0204] In formulas (3) to (8), R 1 , R 2 , R 8 , R 10 and R 11 are each independently an alkyl group having 1 to 4 carbon atoms, R 3 ~R 7 and R 9 Each is independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. s is an integer of 0 to 8, t is an integer of 0 to 4, r is an integer of 0 to 4, and u and v are integers of 0 to 3.

[0205] In formula (3), s is preferably 0.

[0206] In formula (4), as R 2 The alkyl group is preferably a methyl group or an ethyl group. t is preferably 0, 1 or 2, and more preferably 1.

[0207] In formula (5), as R 3 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group, an ethyl group, a propyl group or a butyl group. 4 and R 5 The alkyl group has 1 to 4 carbon atoms, preferably a methyl group or an ethyl group.

[0208] In formula (6), as R 6 ~R 8 The alkyl group is an alkyl group having 1 to 4 carbon atoms, preferably a methyl group or an ethyl group. r is preferably 0 or 1, and more preferably 0.

[0209] In formula (7), as R 9 and R 10 The alkyl group is preferably a methyl group or an ethyl group. u is preferably 0 or 1, and more preferably 0.

[0210] In formula (8), as R 11 The alkyl group is preferably a methyl group or an ethyl group. v is preferably 0 or 1, and more preferably 0.

[0211] The component (B) may be, for example, at least one of the compounds represented by formulae (4), (5), (6), (7) and (8), or at least one of the compounds represented by formulae (5), (7) and (8).

[0212] Specific examples of the component (B) include the following compounds.

[0213] [Chemistry 18]

[0214]

[0215] The component (B) contained in the insulating film forming material of the present disclosure is not limited to the above compounds, and may be other solvents. The component (B) may be an ester solvent, an ether solvent, a ketone solvent, a hydrocarbon solvent, an aromatic hydrocarbon solvent, a sulfoxide solvent, etc.

[0216] Examples of the ester solvent include ethyl acetate, n-butyl acetate, isobutyl acetate, amyl formate, isoamyl acetate, isobutyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate, ethyl lactate, γ-butyrolactone, ε-caprolactone, δ-valerolactone, alkyl alkoxyacetates such as methyl alkoxyacetate, ethyl alkoxyacetate, and butyl alkoxyacetate (e.g., methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, and ethyl ethoxyacetate), alkyl 3-alkoxypropionates such as methyl 3-methoxypropionate, ethyl 3-methoxypropionate, and ethyl 3-alkoxypropionate. 2-alkoxypropionic acid alkyl esters (for example, methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, methyl 2-ethoxypropionate and ethyl 2-ethoxypropionate), methyl 2-alkoxypropionate, ethyl 2-alkoxypropionate, propyl 2-alkoxypropionate and the like, methyl 2-methoxypropionate, methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-ethoxypropionate and the like, ethyl 2-alkoxy-2-methylpropionate such as methyl 2-methoxy-2-methylpropionate, ethyl 2-alkoxy-2-methylpropionate such as ethyl 2-ethoxy-2-methylpropionate, methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, methyl 2-oxobutanoate and ethyl 2-oxobutanoate, and the like.

[0217] Examples of the ether solvent include diethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and propylene glycol monopropyl ether acetate.

[0218] Examples of the ketone solvent include methyl ethyl ketone, cyclohexanone, cyclopentanone, 2-heptanone, 3-heptanone, and N-methyl-2-pyrrolidone (NMP).

[0219] Examples of hydrocarbon solvents include limonene and the like.

[0220] Examples of the aromatic hydrocarbon solvent include toluene, xylene, and anisole.

[0221] Examples of the sulfoxide-based solvent include dimethyl sulfoxide and the like.

[0222] Preferred examples of the solvent of the component (B) include γ-butyrolactone, cyclopentanone, ethyl lactate, and 3-methoxy-N,N-dimethylpropionamide.

[0223] In the insulating film forming material of the present disclosure, the content of NMP may be 1% by mass or less relative to the total amount of the insulating film forming material, or 3% by mass or less relative to the total amount of the (A) polyimide precursor, from the viewpoint of reducing toxicity such as reproductive toxicity.

[0224] In the insulating film forming material of the present disclosure, the content of the component (B) is preferably 1 to 10,000 parts by mass, more preferably 50 to 10,000 parts by mass, based on 100 parts by mass of the polyimide precursor (A).

[0225] The component (B) preferably comprises at least one of a solvent (1) and a solvent (2), wherein the solvent (1) is at least one selected from the group consisting of compounds represented by formula (3) to formula (6), and the solvent (2) is at least one selected from the group consisting of ester solvents, ether solvents, ketone solvents, hydrocarbon solvents, aromatic hydrocarbon solvents and sulfoxide solvents.

[0226] The content of the solvent (1) may be 5% by mass to 100% by mass, or 5% by mass to 50% by mass, relative to the total of the solvent (1) and the solvent (2).

[0227] The content of the solvent (1) may be 10 to 1000 parts by mass, 10 to 100 parts by mass, or even 10 to 50 parts by mass, based on 100 parts by mass of the (A) polyimide precursor.

[0228] ((C) Oxime-based photopolymerization initiator)

[0229] The insulating film forming material disclosed herein contains (C) an oxime-based photopolymerization initiator. This provides excellent exposure sensitivity and can suppress the generation of voids during bonding. The (C) oxime-based photopolymerization initiator may be used alone or in combination of two or more.

[0230] The (C) oxime-based photopolymerization initiator preferably contains a compound represented by the following formula (I) from the viewpoint of excellent exposure sensitivity and suppression of voids generated during bonding.

[0231] [Chemistry 19]

[0232]

[0233] In formula (I), R 1 represents an alkyl group, an alkoxy group, a phenyl group or a phenoxy group, R 2 represents an alkyl group, R 3 It represents a carbonyl group or a monovalent organic group connected via a single bond.

[0234] In formula (I), R 1 It is preferably an alkyl group, an alkoxy group or a phenyl group, and is more preferably an alkoxy group from the viewpoint of excellent resolution and pattern profile. 1 More preferred is an alkyl group or a phenyl group.

[0235] From the viewpoint of maintaining high exposure sensitivity and excellent resolution and pattern profile, it is preferred to use R in formula (I) in combination. 1 The compound A represented by an alkoxy group and R in formula (I) 1 The compound B is represented by an alkyl group or a phenyl group.

[0236] The mixing ratio of compound A to compound B (compound A:compound B) is preferably 1:1 to 1:0.01, more preferably 1:0.5 to 1:0.01, and even more preferably 1:0.2 to 1:0.01 on a mass basis.

[0237] R 1 The number of carbon atoms in the alkoxy group represented by is preferably 1 to 10, more preferably 1 to 5, and even more preferably 1 to 3. 1 The alkoxy group represented may be any of linear, branched, and cyclic, and is preferably linear.

[0238] R 1 The number of carbon atoms in the alkyl group represented by is preferably 1 to 10, more preferably 1 to 5, and even more preferably 1 to 3. 1 The alkyl group represented may be any of linear, branched, and cyclic, and is preferably linear.

[0239] R 1 The alkyl group, alkoxy group, phenyl group, and phenoxy group represented by the above-mentioned may have a substituent or may be unsubstituted, but are preferably unsubstituted.

[0240] In formula (I), R 2 It is preferably an alkyl group, more preferably an alkyl group having 1 to 10 carbon atoms, and still more preferably an alkyl group having 1 to 6 carbon atoms. 2 The alkyl group represented may be any of linear, branched, and cyclic, and is preferably linear.

[0241] In formula (I), R 3 Represents a carbonyl group or a monovalent organic group connected by a single bond. As a monovalent organic group, a phenyl group which may have a substituent can be cited. As a substituent possessed by the phenyl group, a phenoxy group, a phenylthio group, a phenyl group, an amino group, an alkyl group, etc. can be cited, and these groups can further have a substituent. The substituents possessed by the phenyl group can be bonded to each other to form a ring. As the ring formed, a carbazole ring can be cited. The ring formed can further have a substituent. As a substituent possessed by the ring formed, an alkyl group, a phenyl group, an acyl group, etc. can be cited, and these groups can further have a substituent.

[0242] Specific examples of the (C) oxime-based photopolymerization initiator include 1-phenyl-1,2-butanedione-2-(O-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(O-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(O-benzoyl)oxime, 1,3-diphenylpropanetrione-2-(O-ethoxycarbonyl)oxime, ) oxime, 1-phenyl-3-ethoxypropanetrione-2-(O-benzoyl) oxime, 1-[4-(phenylthio)phenyl]octane-1,2-dione=2-(O-benzoyl oxime), O-acetyl-1-[6-(2-methylbenzoyl)-9-ethyl-9H-carbazole-3-yl]ethanone oxime, 1-[4-(4-hydroxyethoxy-phenylthio)phenyl]-1,2-propanedione-2-(O-acetyl oxime), etc.

[0243] The insulating film forming material disclosed in the present invention may contain other photopolymerization initiators while containing (C) an oxime-based photopolymerization initiator. As other photopolymerization initiators, acetophenone derivatives such as acetophenone, 2,2-diethoxyacetophenone, 3'-methylacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2-hydroxy-2-methylpropiophenone, 4'-(methylthio)-α-morpholino-α-methylpropiophenone, and 1-hydroxycyclohexyl phenyl ketone; thioxanthone derivatives such as thioxanthone, 2-methylthioxanthone, 2-isopropylthioxanthone, 2-chlorothioxanthone, and diethylthioxanthone; benzyl derivatives such as benzyl, benzyl dimethyl ketal, and benzyl-β-methoxyethyl acetal; benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin phenyl ether, methylbenzene, and the like. Benzoin derivatives such as benzoin, ethylbenzoin, and propylbenzoin; N-arylglycines such as N-phenylglycine; peroxides such as benzoyl peroxide; aromatic bisimidazoles such as 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, and 2-(o- or p-methoxyphenyl)-4,5-diphenylimidazole dimer; acylphosphine oxide derivatives such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide; Irgacure OXE03 (manufactured by BASF), Irgacure OXE04 (manufactured by BASF), etc. Other photopolymerization initiators may be used alone or in combination of two or more.

[0244] The content of the (C) oxime photopolymerization initiator relative to the total amount of the photopolymerization initiator is preferably 60% by mass or more, more preferably 80% by mass or more, further preferably 90% by mass or more, particularly preferably 95% by mass or more.

[0245] The total amount of the photopolymerization initiator is preferably 0.1 to 20 parts by mass, more preferably 1 to 20 parts by mass, and further preferably 5 to 20 parts by mass, based on 100 parts by mass of the (A) polyimide precursor.

[0246] The insulating film forming material disclosed herein comprises (A) a polyimide precursor, (B) a solvent and (C) an oxime-based photopolymerization initiator, and may comprise (D) a sensitizer, (E) a polymerizable monomer, (F) a thermal polymerization initiator, (G) a polymerization inhibitor, an antioxidant, a coupling agent, a surfactant, a leveling agent, a rust inhibitor, a nitrogen-containing compound, etc. as required, and may also comprise other components and unavoidable impurities within a range that does not impair the effects of the present disclosure. The insulating film forming material disclosed herein preferably further comprises the components (D) and (E).

[0247] Hereinafter, (D) sensitizer is also referred to as (D) component, (E) polymerizable monomer is also referred to as (E) component, (F) thermal polymerization initiator is also referred to as (F) component, and (G) polymerization inhibitor is also referred to as (G) component.

[0248] The insulating film forming material disclosed in the present invention may contain the following components, for example, at more than 80 mass%, more than 90 mass%, more than 95 mass%, more than 98 mass% or 100 mass%, including: (A) polyimide precursor to (C) component, (A) polyimide precursor to (D) component, (A) polyimide precursor to (E) component, (A) polyimide precursor to (F) component, (A) polyimide precursor to (G) component, (A) polyimide precursor to (G) component, and at least one selected from the group consisting of an antioxidant, a coupling agent, a surfactant, a leveling agent, a rust inhibitor and a nitrogen-containing compound.

[0249] Hereinafter, preferred aspects of each component will be described.

[0250] ((D) Sensitizer)

[0251] The insulating film forming material disclosed herein preferably contains a (D) sensitizer. Examples of the (D) sensitizer include benzophenone, N,N'-tetramethyl-4,4'-diaminobenzophenone (Michler's ketone), N,N'-tetraethyl-4,4'-diaminobenzophenone, 4-methoxy-4'-dimethylaminobenzophenone, 4-chlorobenzophenone, 4,4'-dimethoxybenzophenone, 4,4'-diaminobenzophenone, 4,4'-bis(diethylamino)benzophenone, methyl o-benzoylbenzoate, 4-benzoyl-4'-methyldiphenyl ketone, dibenzyl ketone, fluorenone and other benzophenone derivatives. The (D) sensitizer may be used alone or in combination of two or more.

[0252] When the insulating film forming material of the present disclosure contains the (D) sensitizer, the content of the (D) sensitizer is not particularly limited, but is preferably 0.01 to 3 parts by mass, more preferably 0.1 to 1 part by mass, based on 100 parts by mass of the (A) polyimide precursor.

[0253] ((E) polymerizable monomer)

[0254] The insulating film forming material disclosed herein preferably contains (E) a polymerizable monomer. The (E) component preferably has at least one group containing a polymerizable unsaturated double bond, and more preferably has at least one (meth)acrylic group from the viewpoint of being able to be suitably polymerized by use with a photopolymerization initiator. From the viewpoint of increasing the crosslinking density and increasing the exposure sensitivity, it is preferred to have 2 to 6 groups containing a polymerizable unsaturated double bond, and more preferably 2 to 4 groups.

[0255] The polymerizable monomer may be used alone or in combination of two or more.

[0256] The polymerizable monomer having a (meth)acrylic group is not particularly limited, and examples thereof include diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, trimethylolpropane diacrylate, trimethylolpropane triacrylate, trimethylolpropane dimethacrylate, trimethylolpropane trimethacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, and pentaerythritol trimethacrylate. Tetraol tetraacrylate, pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, dipentaerythritol hexaacrylate, dipentaerythritol hexamethacrylate, ethoxylated pentaerythritol tetraacrylate, ethoxylated isocyanuric acid triacrylate, ethoxylated isocyanuric acid trimethacrylate, acryloxyethyl isocyanurate, methacryloyloxyethyl isocyanurate, tricyclodecane dimethanol diacrylate, 2-hydroxyethyl (meth)acrylate, 1,3-bis((meth)acryloyloxy)-2-hydroxypropane, ethylene oxide (EO)-modified bisphenol A diacrylate, and ethylene oxide (EO)-modified bisphenol A dimethacrylate.

[0257] The polymerizable monomer other than the polymerizable monomer having a (meth)acrylic group is not particularly limited, and examples thereof include styrene, divinylbenzene, 4-vinyltoluene, 4-vinylpyridine, N-vinylpyrrolidone, methylenebisacrylamide, N,N-dimethylacrylamide, and N-methylolacrylamide.

[0258] (E) Component is not limited to a compound having a group containing a polymerizable unsaturated double bond, and may be a compound having a polymerizable group (for example, an ethylene oxide ring) other than an unsaturated double bond group.

[0259] When the insulating film forming material of the present disclosure contains the component (E), the content of the component (E) is not particularly limited, but is preferably 1 to 100 parts by mass, more preferably 1 to 75 parts by mass, and even more preferably 1 to 50 parts by mass, relative to 100 parts by mass of the polyimide precursor (A).

[0260] ((F) Thermal polymerization initiator)

[0261] From the viewpoint of improving the physical properties of the cured product, the insulating film forming material of the present disclosure may contain (F) a thermal polymerization initiator.

[0262] Specific examples of the component (F) include ketone peroxides such as methyl ethyl ketone peroxide, peroxyketals such as 1,1-di(tert-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(tert-hexylperoxy)cyclohexane, and 1,1-di(tert-butylperoxy)cyclohexane, hydroperoxides such as 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroperoxide, p-menthane hydroperoxide, diisopropylbenzene hydroperoxide, and diisopropylbenzene hydroperoxide. Alkyl peroxide, dilauroyl peroxide, dibenzoyl peroxide and other diacyl peroxides, di(4-tert-butylcyclohexyl)peroxydicarbonate, di(2-ethylhexyl)peroxydicarbonate and other peroxydicarbonates, tert-butyl peroxy-2-ethylhexanoate, tert-hexyl peroxyisopropyl monocarbonate, tert-butyl peroxybenzoate, peroxyesters such as 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, bis(1-phenyl-1-methylethyl)peroxide, etc. The thermal polymerization initiator may be used alone or in combination of two or more.

[0263] When the insulating film forming material of the present disclosure contains the component (F), the content of the component (F) may be 0.1 to 20 parts by mass, 1 to 15 parts by mass, or 1 to 10 parts by mass based on 100 parts by mass of the polyimide precursor.

[0264] ((G) Inhibitor)

[0265] From the viewpoint of ensuring good storage stability, the insulating film forming material of the present disclosure may contain the component (G). Examples of the polymerization inhibitor include radical polymerization inhibitors and radical polymerization inhibitors.

[0266] Specific examples of the component (G) include p-methoxyphenol, diphenyl-p-benzoquinone, benzoquinone, hydroquinone, pyrogallol, phenothiazine, resorcinol, o-dinitrobenzene, p-dinitrobenzene, m-dinitrobenzene, phenanthrenequinone, N-phenyl-2-naphthylamine, cupferroquinone, 2,5-toluoquinone, tannic acid, p-benzylaminophenol, nitrosamines, hindered phenol compounds, and the like. The inhibitor may be used alone or in combination of two or more. By combining two or more inhibitors, it is easy to adjust the photosensitivity due to different reactivity. The hindered phenol compound may have both the function of an inhibitor and the function of an antioxidant described later, or may have either function.

[0267] The hindered phenol compound is not particularly limited, and examples thereof include 2,6-di-tert-butyl-4-methylphenol, 2,5-di-tert-butyl-hydroquinone, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, isooctyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 4,4'-methylenebis(2,6-di-tert-butylphenol), 4,4'-thio-bis(3-methyl-6-tert-butylphenol), 4,4'-butylene-bis(3-methyl-6-tert-butylphenol), triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2,2-thio 2,2'-Methylene-bis(4-methyl-6-tert-butylphenol), 2,2'-Methylene-bis(4-ethyl-6-tert-butylphenol), pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris-(3,5-di-tert-butyl-4-hydroxybenzyl)-isocyanurate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-isopropylbenzyl)-1,3,5-triazine-2, 4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-sec-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-(1-ethylpropyl)-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-triethylmethyl-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1 H,3H,5H)-trione, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-phenylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,5,6-trimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-5-ethyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-6-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione5H)-trione, 1,3,5-tris(4-tert-butyl-6-ethyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-5,6-diethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5 -Tris(4-tert-butyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-5-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], and 1,4,4-trimethyl-2,3-diazabicyclo[3.2.2]non-2-ene-2,3-dioxide. ,

[0268] When the insulating film forming material disclosed in the present invention contains component (G), from the viewpoint of the storage stability of the insulating film forming material and the heat resistance of the obtained cured product, the content of component (G) is preferably 0.01 to 30 parts by mass, more preferably 0.01 to 10 parts by mass, and further preferably 0.05 to 5 parts by mass relative to 100 parts by mass of the polyimide precursor (A).

[0269] (Antioxidant)

[0270] The insulating film forming material of the present disclosure may contain an antioxidant from the viewpoint of suppressing the decrease in adhesion by capturing oxygen radicals and peroxide radicals generated during high temperature storage, reflow treatment, etc. The insulating film forming material of the present disclosure may contain an antioxidant to suppress electrode oxidation during insulation reliability testing.

[0271] Specific examples of the antioxidant include the compounds exemplified as the hindered phenol compounds, N,N'-bis[2-[2-(3,5-di-tert-butyl-4-hydroxyphenyl)ethylcarbonyloxy]ethyl]oxalamide, N,N'-bis-3-(3,5-di-tert-butyl-4'-hydroxyphenyl)propionylhexamethylenediamine, 1,3,5-tris(3-hydroxy-4-tert-butyl-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, and 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanuric acid.

[0272] The antioxidants may be used alone or in combination of two or more.

[0273] When the insulating film forming material of the present disclosure contains an antioxidant, the content of the antioxidant is preferably 0.1 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the (A) polyimide precursor.

[0274] (Coupling agent)

[0275] The insulating film forming material disclosed herein may contain a coupling agent. The coupling agent reacts with the (A) polyimide precursor during the heat treatment to form crosslinks, or the coupling agent itself polymerizes. This tends to further improve the adhesion between the obtained cured product and the substrate.

[0276] Specific examples of coupling agents are not particularly limited. Examples of coupling agents include 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-methacryloxypropyldimethoxymethylsilane, 3-methacryloxypropyltrimethoxysilane, dimethoxymethyl-3-piperidinylpropylsilane, diethoxy-3-glycidoxypropylmethylsilane, N-(3-diethoxymethylsilylpropyl)succinimide, N-〔3-(triethoxysilyl)propyl〕phthalic acid, Silane coupling agents such as amic acid, benzophenone-3,3'-bis(N-〔3-triethoxysilyl〕propylamide)-4,4'-dicarboxylic acid, benzene-1,4-bis(N-〔3-triethoxysilyl〕propylamide)-2,5-dicarboxylic acid, 3-(triethoxysilyl)propylsuccinic anhydride, N-phenylaminopropyltrimethoxysilane, N,N'-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, 3-ureidopropyltriethoxysilane; aluminum-based adhesive agents such as tri(ethylacetoacetate)aluminum, tri(acetylacetonate)aluminum, ethylacetoacetate aluminum diisopropionate, etc.

[0277] The coupling agent may be used alone or in combination of two or more.

[0278] When the insulating film forming material of the present disclosure contains a coupling agent, the content of the coupling agent is preferably 0.1 to 20 parts by mass, more preferably 0.3 to 10 parts by mass, and further preferably 1 to 10 parts by mass, based on 100 parts by mass of the (A) polyimide precursor.

[0279] (Surfactants and leveling agents)

[0280] The insulating film forming material disclosed herein may include at least one of a surfactant and a leveling agent. By including at least one of a surfactant and a leveling agent in the insulating film forming material, it is possible to improve coating properties (e.g., suppressing streaks (uneven film thickness)), improve adhesion, and improve compatibility of compounds in the insulating film forming material.

[0281] Examples of the surfactant or leveling agent include polyoxyethylene urea ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, and polyoxyethylene octylphenol ether.

[0282] The surfactant and the leveling agent may be used alone or in combination of two or more.

[0283] In the case where the insulating film forming material disclosed herein contains at least one of a surfactant and a leveling agent, the total content of the surfactant and the leveling agent is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and further preferably 0.05 to 3 parts by mass, relative to 100 parts by mass of the (A) polyimide precursor.

[0284] (Rust Inhibitor)

[0285] The insulating film forming material of the present disclosure may contain a rust inhibitor from the viewpoint of suppressing corrosion of metals such as copper and copper alloys and suppressing discoloration of the metals. Examples of the rust inhibitor include azole compounds and purine derivatives.

[0286] Specific examples of the azole compound include 1H-triazole, 5-methyl-1H-triazole, 5-ethyl-1H-triazole, 4,5-dimethyl-1H-triazole, 5-phenyl-1H-triazole, 4-tert-butyl-5-phenyl-1H-triazole, 5-hydroxyphenyl-1H-triazole, phenyltriazole, p-ethoxyphenyltriazole, 5-phenyl-1-(2-dimethylaminoethyl)triazole, 5-benzyl-1H-triazole, hydroxyphenyltriazole, 1,5-dimethyltriazole, 4,5-diethyl-1H-triazole, 1H-benzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl) )phenyl]-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-tert-butyl-5-methyl-2-hydroxyphenyl)-benzotriazole, 2-(3,5-di-tert-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, hydroxyphenylbenzotriazole, tolyltriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, 4-carboxy-1H-benzotriazole, 5-carboxy-1H-benzotriazole, 1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, 5-amino-1H-tetrazole, 1-methyl-1H-tetrazole, and the like.

[0287] Specific examples of purine derivatives include purine, adenine, guanine, hypoxanthine, xanthine, theobromine, caffeine, uric acid, isoguanine, 2,6-diaminopurine, 9-methyladenine, 2-hydroxyadenine, 2-methyladenine, 1-methyladenine, N-methyladenine, N,N-dimethyladenine, 2-fluoroadenine, 9-(2-hydroxyethyl)adenine, guanine oxime, N-(2-hydroxyethyl)adenine, 8-aminoadenine, The invention also includes purine, 6-amino-8-phenyl-9H-purine, 1-ethyladenine, 6-ethylaminopurine, 1-benzyladenine, N-methylguanine, 7-(2-hydroxyethyl)guanine, N-(3-chlorophenyl)guanine, N-(3-ethylphenyl)guanine, 2-azaadenine, 5-azaadenine, 8-azaadenine, 8-azaguanine, 8-azapurine, 8-azaxanthine and 8-azahypoxanthine, and derivatives thereof.

[0288] The rust preventive agent may be used alone or in combination of two or more.

[0289] When the insulating film forming material of the present disclosure contains a rust inhibitor, the content of the rust inhibitor is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and further preferably 0.5 to 3 parts by mass, relative to 100 parts by mass of the (A) polyimide precursor. In particular, when the insulating film forming material of the present disclosure is applied to the surface of copper or a copper alloy, surface discoloration of the copper or a copper alloy is suppressed by making the content of the rust inhibitor 0.1 parts by mass or more.

[0290] The resin composition of the present disclosure may contain a nitrogen-containing compound from the viewpoint of promoting the imidization reaction of the component (A) to obtain a cured product having high reliability.

[0291] Specific examples of the nitrogen-containing compound include 2-(methylphenylamino)ethanol, 2-(ethylanilino)ethanol, N-phenyldiethanolamine, N-methylaniline, N-ethylaniline, N,N'-dimethylaniline, N-phenylethanolamine, 4-phenylmorpholine, 2,2'-(4-methylphenylimino)diethanol, 4-aminobenzamide, 2-aminobenzamide, nicotinamide, 4-amino-N-methylbenzamide, 4-aminoacetanilide, 4-aminoacetophenone, etc. Among them, N-phenyldiethanolamine, N-methylaniline, N-ethylaniline, N,N'-dimethylaniline, N-phenylethanolamine, 4-phenylmorpholine, 2,2'-(4-methylphenylimino)diethanol, etc. are preferred. The nitrogen-containing compound may be used alone or in combination of two or more.

[0292] The nitrogen-containing compound preferably includes a compound represented by the following formula (17).

[0293] [Chemistry 20]

[0294]

[0295] In formula (17), R 31A ~R 33A are each independently a hydrogen atom, a monovalent aliphatic hydrocarbon group, a monovalent aliphatic hydrocarbon group having a hydroxyl group, or a monovalent aromatic group, and R 31A ~R 33A At least one (preferably one) of R is a monovalent aromatic group. 31A ~R 33A A ring structure may also be formed by adjacent groups. Examples of the ring structure formed include a 5-membered ring or a 6-membered ring which may have a substituent such as a methyl group or a phenyl group. The hydrogen atom of the monovalent aliphatic hydrocarbon group may be substituted by a functional group other than a hydroxyl group.

[0296] In formula (17), preferably R 31A ~R 33A At least one (preferably one) of the groups is a monovalent aliphatic hydrocarbon group, a monovalent aliphatic hydrocarbon group having a hydroxyl group, or a monovalent aromatic group.

[0297] In formula (17), regarding R 31A ~R 33A The monovalent aliphatic hydrocarbon group preferably has 1 to 10 carbon atoms, and more preferably has 1 to 6 carbon atoms. The monovalent aliphatic hydrocarbon group is preferably a methyl group, an ethyl group, or the like.

[0298] In formula (17), R 31A ~R 33A The monovalent aliphatic hydrocarbon group having a hydroxyl group is preferably 31A ~R 33A A group in which one or more hydroxyl groups are bonded to a monovalent aliphatic hydrocarbon group, and more preferably a group in which 1 to 3 hydroxyl groups are bonded. Specific examples of the monovalent aliphatic hydrocarbon group having a hydroxyl group include a hydroxymethyl group and a hydroxyethyl group, and among these, a hydroxyethyl group is preferred.

[0299] As R in formula (17) 31A ~R 33A The monovalent aromatic group includes a monovalent aromatic hydrocarbon group, a monovalent aromatic heterocyclic group, etc., and a monovalent aromatic hydrocarbon group is preferred. The monovalent aromatic hydrocarbon group preferably has 6 to 12 carbon atoms, and more preferably has 6 to 10 carbon atoms.

[0300] Examples of the monovalent aromatic hydrocarbon group include a phenyl group and a naphthyl group.

[0301] R in formula (17) 31A ~R 33A The monovalent aromatic group of formula (17) may have a substituent. Examples of the substituent include31A ~R 33A The monovalent aliphatic hydrocarbon group and R 31A ~R 33A The same group as the monovalent aliphatic hydrocarbon group having a hydroxyl group.

[0302] When the resin composition of the present disclosure contains a nitrogen-containing compound, the content of the nitrogen-containing compound is preferably 0.1 to 20 parts by mass, more preferably 0.3 to 15 parts by mass, and even more preferably 0.5 to 10 parts by mass, relative to 100 parts by mass of the component (A).

[0303] (Characteristics of Insulating Film Forming Material)

[0304] From the viewpoint of bonding at low temperature, the insulating film forming material of the present disclosure preferably has a glass transition temperature of 50° C. to 300° C., more preferably 50° C. to 250° C. when formed into a cured product. The glass transition temperature when formed into a cured product may be 200° C. or less.

[0305] The glass transition temperature of the cured product is measured as follows. First, the insulating film forming material is heated for 2 hours at a predetermined curing temperature (e.g., 150°C to 375°C) at which a curing reaction can proceed under a nitrogen atmosphere to obtain a cured product. The obtained cured product is cut into a 5 mm × 50 mm × 3 mm rectangular parallelepiped, and the dynamic viscoelasticity is measured using a dynamic viscoelasticity measuring device (e.g., RSA-G2 manufactured by TA Instruments) and a tensile fixture at a frequency of 1 Hz and a heating rate of 5°C / min in a temperature range of 50°C to 350°C. The glass transition temperature (Tg) is set to the temperature of the peak portion of tanδ obtained by the ratio of the storage modulus to the loss modulus obtained by the above method.

[0306] The insulating film forming material disclosed in the present invention may be a negative photosensitive insulating film forming material or a positive photosensitive insulating film forming material. In addition, the negative photosensitive insulating film forming material or the positive photosensitive insulating film forming material may also be used for at least one of the following operations: providing a plurality of through holes for configuring a plurality of terminal electrodes in a first organic insulating film provided on one surface of a first substrate body described later; and providing a plurality of through holes for configuring a plurality of terminal electrodes in a second organic insulating film provided on one surface of a second substrate body.

[0307] The thermal expansion coefficient of the insulating film forming material disclosed in the present invention when made into a cured product is preferably 150 ppm / K or less, more preferably 100 ppm / K or less, and further preferably 70 ppm / K or less. As a result, the thermal expansion coefficient of the insulating film as a cured product becomes equal to or close to the thermal expansion coefficient of the electrode, so even if heat is generated when the semiconductor device is used, it is possible to suppress the damage of the semiconductor device caused by the difference in thermal expansion coefficients between the insulating layer and the electrode. The thermal expansion coefficient is a value that represents the ratio of the expansion of the length of the cured product caused by the temperature rise per unit temperature. The thermal expansion coefficient can be calculated by measuring the change in the length of the cured product at 100°C to 150°C using a thermomechanical analysis device or the like.

[0308] From the viewpoint of suppressing the generation of voids during bonding or the like, the 5% thermal weight loss temperature of the insulating film forming material of the present disclosure when formed into a cured product is preferably 200° C. or higher, more preferably 250° C. or higher.

[0309] The 5% thermal weight loss temperature is calculated by measuring the temperature at which the weight of the sample decreases by 5% when the temperature is increased from 25°C to 800°C at a rate of 10°C per minute using a differential thermal thermogravimetric simultaneous measuring apparatus using 10 mg of a polyimide resin film as a measurement sample.

[0310] <Semiconductor Device>

[0311] The semiconductor device disclosed in the present invention comprises a first semiconductor substrate and a semiconductor chip, wherein the first semiconductor substrate has a first substrate body and the first organic insulating film and a first electrode arranged on one surface of the first substrate body, and the semiconductor chip has a semiconductor chip substrate body and the second organic insulating film and a second electrode arranged on one surface of the semiconductor chip substrate body, the first organic insulating film is bonded to the second organic insulating film, the first electrode is bonded to the second electrode, and at least one of the first organic insulating film and the second organic insulating film is a solidified product of the insulating film forming material disclosed in the present invention.

[0312] In the semiconductor device of the present disclosure, at least one of the first organic insulating film and the organic insulating film portion is a cured product of the insulating film forming material of the present disclosure, and therefore, there are few voids at the bonding interface of the insulating film.

[0313] <Method for manufacturing semiconductor device>

[0314] In the manufacturing method of the semiconductor device of the present disclosure, the insulating film forming material of the present disclosure is used to manufacture the semiconductor device. Specifically, in the manufacturing method of the semiconductor device of the present disclosure, a first semiconductor substrate having a first substrate body and a first electrode and a first organic insulating film provided on one surface of the first substrate body is prepared, a semiconductor chip having a semiconductor chip substrate body and a second organic insulating film and a second electrode provided on one surface of the semiconductor chip substrate body is prepared, the first electrode and the second electrode are bonded and the first organic insulating film and the second organic insulating film are bonded, and the insulating film forming material of the present disclosure is used in the production of the organic insulating film of at least one of the first organic insulating film and the second organic insulating film.

[0315] Hereinafter, an embodiment of a semiconductor device disclosed in the present invention and an embodiment of a method for manufacturing a semiconductor device disclosed in the present invention will be described in detail with reference to the accompanying drawings. In the following description, the same reference numerals are used for the same or equivalent parts, and repeated descriptions are omitted. In addition, unless otherwise specified, the positional relationships such as up, down, left, and right are based on the positional relationships shown in the accompanying drawings. Moreover, the dimensional ratios of the accompanying drawings are not limited to the ratios shown in the drawings.

[0316] (An example of a semiconductor device)

[0317] Figure 1 Schematically shows a cross-sectional view of an example of a semiconductor device disclosed in the present invention. Figure 1 As shown, the semiconductor device 1 is an example of a semiconductor package, and includes a first semiconductor chip 10 (first semiconductor substrate), a second semiconductor chip 20 (semiconductor chip), a pillar 30 , a redistribution layer 40 , a substrate 50 , and a circuit substrate 60 .

[0318] The first semiconductor chip 10 is a semiconductor chip such as an LSI (large-scale integrated circuit) chip or a CMOS (Complementary Metal Oxide Semiconductor) sensor, and is a three-dimensional mounting structure in which the second semiconductor chip 20 is mounted below. The second semiconductor chip 20 is a semiconductor chip such as an LSI or a memory, and is a chip component having a smaller area than the first semiconductor chip 10 when viewed from above. The second semiconductor chip 20 is bonded to the back of the first semiconductor chip 10 in a chip-to-chip (C2C) manner. The first semiconductor chip 10 and the second semiconductor chip 20 are firmly and finely bonded to each other by hybrid bonding, which will be described in detail later, to bond their respective terminal electrodes to the insulating film surrounding them.

[0319] The column portion 30 is a connection portion in which a plurality of columns 31 formed of a metal such as copper (Cu) are sealed by a resin 32. The plurality of columns 31 are conductive members extending from the upper surface of the column portion 30 toward the lower surface. The plurality of columns 31 may, for example, have a cylindrical shape with a diameter of 3 μm or more and 20 μm or less (in one example, a diameter of 5 μm), or may be arranged in such a manner that the center distance between each column 31 is 15 μm or less. The plurality of columns 31 connect the terminal electrode on the lower side of the first semiconductor chip 10 to the terminal electrode on the upper side of the rewiring layer 40 by flip-chip connection. By using the column portion 30, in the semiconductor device 1, a connection electrode can be formed without using a technique called TMV (Throughmold via) for opening a mold and soldering. The column portion 30, for example, has the same thickness as the second semiconductor chip 20 and is arranged on the side of the second semiconductor chip 20 in the horizontal direction. It should be noted that a plurality of solder balls may be disposed instead of the pillars 30 , and the lower terminal electrodes of the first semiconductor chip 10 and the upper terminal electrodes of the rewiring layer 40 may be electrically connected via the solder balls.

[0320] The rewiring layer 40 is a wiring layer having a terminal pitch conversion function as a package substrate, and is a layer having a rewiring pattern formed by polyimide and copper wiring on the insulating film on the lower side of the second semiconductor chip 20 and the lower surface of the pillar 30. The rewiring layer 40 is formed in a state where the first semiconductor chip 10, the second semiconductor chip 20, etc. are turned upside down (see Figure 4 (d)).

[0321] The rewiring layer 40 electrically connects the terminal electrodes on the lower surface of the second semiconductor chip 20 and the terminal electrodes of the first semiconductor chip 10 separated by the pillar portion 30 to the terminal electrodes of the substrate 50. The terminal pitch of the substrate 50 is wider than the terminal pitch of the pillar 31 and the terminal pitch of the second semiconductor chip 20. It should be noted that various electronic components 51 can also be mounted on the substrate 50. In addition, in the case where there is a large difference in the terminal pitch between the rewiring layer 40 and the substrate 50, an inorganic interposer or the like can be used between the rewiring layer 40 and the substrate 50 to realize the electrical connection between the rewiring layer 40 and the substrate 50.

[0322] The circuit substrate 60 is a substrate on which the first semiconductor chip 10 and the second semiconductor chip 20 are mounted, and has a plurality of through electrodes electrically connected to the substrate 50 connected to the first semiconductor chip 10, the second semiconductor chip 20, and the electronic component 51. In the circuit substrate 60, each terminal electrode of the first semiconductor chip 10 and the second semiconductor chip 20 is electrically connected to the terminal electrode 61 provided on the back side of the circuit substrate 60 through the plurality of through electrodes.

[0323] (An Example of a Method for Manufacturing a Semiconductor Device)

[0324] Next, refer to Figure 2 to Figure 4 An example of a method for manufacturing the semiconductor device 1 will be described. Figure 2 is shown in sequence for manufacturing Figure 1 A diagram of a method for a semiconductor device is shown. Figure 3 is shown in more detail Figure 2 A diagram showing a bonding method (hybrid bonding) in a method for manufacturing a semiconductor device. Figure 4 It is used to manufacture Figure 1 The semiconductor device method is shown in sequence Figure 2 A diagram of the process following the process shown.

[0325] The semiconductor device 1 can be manufactured through, for example, the following steps (a) to (n).

[0326] (a) A step of preparing a first semiconductor substrate 100 corresponding to the first semiconductor chip 10 .

[0327] (b) A step of preparing a second semiconductor substrate 200 corresponding to the second semiconductor chip 20 .

[0328] (c) A step of polishing the first semiconductor substrate 100 .

[0329] (d) A step of polishing the second semiconductor substrate 200 .

[0330] (e) A step of singulating the second semiconductor wafer 200 to obtain a plurality of semiconductor chips 205 .

[0331] (f) A step of aligning the terminal electrodes 203 of each of the plurality of semiconductor chips 205 with respect to the terminal electrodes 103 of the first semiconductor substrate 100 is performed.

[0332] (g) A step of bonding the insulating film 102 of the first semiconductor substrate 100 and the insulating film portions 202b of the plurality of semiconductor chips 205 to each other (see Figure 3 (b)).

[0333] (h) A step of bonding the terminal electrodes 103 of the first semiconductor substrate 100 to the terminal electrodes 203 of the plurality of semiconductor chips 205 (see Figure 3 (c)).

[0334] (i) A step of forming pillars 300 (corresponding to the pillars 31 ) on the connection surface of the first semiconductor substrate 100 and between the plurality of semiconductor chips 205 .

[0335] (j) A step of molding resin 301 on the connection surface of the first semiconductor substrate 100 so as to cover the semiconductor chip 205 and the pillar 300 to obtain a semi-finished product M1.

[0336] (k) A step of grinding and thinning the resin 301 side of the semi-finished product M1 molded in the step (j) to obtain a semi-finished product M2.

[0337] (l) A step of forming a wiring layer 400 corresponding to the rewiring layer 40 on the semi-finished product M2 thinned in step (k).

[0338] (m) A step of cutting the semi-finished product M3 on which the wiring layer 400 is formed in the step (l) along the cutting line A so as to form individual semiconductor devices 1 .

[0339] (n) A step of turning over the semiconductor device 1a singulated in step (m) and placing the semiconductor device 1a on the substrate 50 and the circuit board 60 (see Figure 1 ).

[0340] The insulating film forming material disclosed herein may be an insulating film forming material for producing an insulating film of at least one of a first organic insulating film and a second organic insulating film by a semiconductor device manufacturing method including at least one step corresponding to step (f) and steps (i) to (n).

[0341] [Step (a) and Step (b)]

[0342] Step (a) is a step of preparing a first semiconductor substrate 100, which is a silicon substrate on which an integrated circuit composed of semiconductor elements and wiring connecting them is formed corresponding to a plurality of first semiconductor chips 10. In step (a), Figure 2 As shown in (a), on one surface 101a of a first substrate main body 101 composed of silicon or the like, a plurality of terminal electrodes 103 (first electrodes) composed of copper, aluminum or the like are arranged at predetermined intervals, and an insulating film 102 (first insulating film) which is a solidified product of the insulating film forming material disclosed in the present invention is arranged in the interval portion. The plurality of terminal electrodes 103 may be arranged after the insulating film 102 is arranged on one surface 101a of the first substrate main body 101, or the insulating film 102 may be arranged after the plurality of terminal electrodes 103 are arranged on one surface 101a of the first substrate main body 101. It should be noted that, in order to form a column 300 in the process described later, a predetermined interval is provided between the plurality of terminal electrodes 103, and other terminal electrodes (not shown) connected to the column 300 are formed between them.

[0343] Step (b) is a step of preparing a second semiconductor substrate 200, which is a silicon substrate on which an integrated circuit having semiconductor elements and wiring connecting them is formed corresponding to the plurality of second semiconductor chips 20. In step (b), Figure 2As shown in (a), a plurality of terminal electrodes 203 (a plurality of second electrodes) made of copper, aluminum, etc. are continuously provided on one surface 201a of a second substrate body 201 made of silicon, etc., and an insulating film 202 (a second insulating film, an organic insulating region) which is a cured product of the insulating film forming material disclosed herein is provided. The plurality of terminal electrodes 203 may be provided after the insulating film 202 is provided on one surface 201a of the second substrate body 201, or the insulating film 202 may be provided after the plurality of terminal electrodes 203 are provided on one surface 201a of the second substrate body 201.

[0344] The insulating films 102 and 202 used in the steps (a) and (b) may both be cured products of the insulating film forming material disclosed herein, or one of the insulating films 102 and 202 may be a cured product of the insulating film forming material disclosed herein and the other may be another cured product. As the insulating film forming material for forming the other cured product, there may be mentioned a material that does not contain (A) a polyimide precursor but contains other resins other than (A) a polyimide precursor, and a material that does not contain (C) an oxime-based photopolymerization initiator. As other resins, there may be mentioned insulating film forming materials containing a polyimide precursor having no polymerizable unsaturated bond site, polyimide, polyamide-imide, benzocyclobutene (BCB), polybenzoxazole (PBO), a PBO precursor, and the like. The tensile elastic modulus of the insulating films 102 and 202 at 25° C. is preferably 7.0 GPa or less, more preferably 5.0 GPa or less, further preferably 3.0 GPa or less, particularly preferably 2.0 GPa or less, and further preferably 1.5 GPa or less.

[0345] The thermal expansion coefficient of the insulating films 102 and 202 is preferably 150 ppm / K or less, more preferably 100 ppm / K or less, and further preferably 90 ppm / K or less.

[0346] The thickness of the insulating films 102 and 202 is preferably 0.1 μm to 50 μm, and more preferably 1 μm to 15 μm. This ensures uniformity in the thickness of the insulating films and reduces processing time in the subsequent polishing step.

[0347] From the viewpoint of facilitating the work in step (c) and step (d) and simplifying these steps, it is preferred that at least one of the polishing rate of the insulating film 102 is 0.1 to 5 times the polishing rate of the terminal electrode 103 and the polishing rate of the insulating film 202 is 0.1 to 5 times the polishing rate of the terminal electrode 203 (preferably both are satisfied). As an example, when the terminal electrode 103 or 203 is made of copper and the polishing rate of copper is 50 nm / min, the polishing rate of the insulating film 102 or 202 is preferably 200 nm / min or less (4 times or less of the polishing rate of copper), more preferably 100 nm / min or less (2 times or less of the polishing rate of copper), and further preferably 50 nm / min or less (same or less of the polishing rate of copper).

[0348] Next, the method for producing the insulating film is described. The insulating film is obtained by curing the insulating film forming material. Examples of the method for producing the above insulating film include: (α) a method comprising the steps of applying the insulating film forming material on a substrate and drying it to form a resin film and the step of heat-treating the resin film; (β) a method comprising the steps of forming a film with a certain film thickness using the insulating film forming material on a film subjected to a demolding treatment, transferring the resin film to a substrate by laminating, and the step of heat-treating the resin film formed on the substrate after the transfer. From the viewpoint of flatness, the above method (α) is preferred.

[0349] Examples of a method for applying the insulating film forming material include a spin coating method, an ink jet method, and a slit coating method.

[0350] In the spin coating method, the insulating film forming material can be spin-coated at a rotation speed of 300 rpm to 3,500 rpm, preferably 500 rpm to 1,500 rpm, an acceleration of 500 rpm / sec to 15,000 rpm / sec, and a spin time of 30 seconds to 300 seconds.

[0351] A drying step may be included after the insulating film forming material is applied to a support, a film, or the like. Drying may be performed using a hot plate, an oven, or the like. The drying temperature is preferably 75° C. to 130° C., and more preferably 90° C. to 120° C. from the viewpoint of improving the flatness of the insulating film. The drying time is preferably 30 seconds to 5 minutes.

[0352] Drying may be performed two or more times. In this way, the insulating film forming material can be formed into a film shape to obtain a resin film.

[0353] In the slit coating method, for example, the insulating film forming material can be slit coated under the conditions of a liquid discharge speed of 10 μL / s to 400 μL / s, a liquid discharge portion height of 0.1 μm to 1.0 μm, a worktable speed (or liquid discharge portion speed) of 1.0 mm / s to 50.0 mm / s, a worktable acceleration of 10 mm / s to 1000 mm / s, a vacuum degree of 10 Pa to 100 Pa during reduced pressure drying, a reduced pressure drying time of 30 seconds to 600 seconds, a drying temperature of 60°C to 150°C, and a drying time of 30 to 300 seconds.

[0354] The formed resin film may be subjected to a heat treatment. The heating temperature is preferably 150° C. to 450° C., more preferably 150° C. to 350° C. By setting the heating temperature within the above range, damage to the substrate, devices, etc. can be suppressed to achieve energy saving of the process, and an insulating film can be appropriately produced.

[0355] The heating time is preferably 5 hours or less, more preferably 30 minutes to 3 hours. When the heating time is within the above range, the crosslinking reaction or the dehydration ring-closure reaction can be sufficiently carried out.

[0356] The atmosphere for the heat treatment may be air or an inert atmosphere such as nitrogen. However, from the viewpoint of preventing oxidation of the resin film, a nitrogen atmosphere is preferred.

[0357] Examples of the apparatus used for the heat treatment include a quartz tube furnace, a hot plate, a rapid thermal annealing furnace, a vertical diffusion furnace, an infrared curing furnace, an electron beam curing furnace, and a microwave curing furnace.

[0358] When using the insulating film forming material of the present disclosure as a negative photosensitive insulating film forming material or a positive photosensitive insulating film forming material, after the insulating film 202 is provided on one surface 201a of the second substrate body 201, a method including the following steps can be used, for example: a step of applying the insulating film forming material on the substrate; a step of drying to form a resin film; a step of pattern-exposing the resin film and developing it with a developer to obtain a patterned resin film; and a step of heating the patterned resin film. Thus, a cured patterned insulating film can be obtained.

[0359] Alternatively, when the plurality of terminal electrodes 203 are provided after the insulating film 202 is provided on one surface 201a of the second substrate body 201, a method including the following steps may be used, for example: a step of applying an insulating film forming material other than the insulating film forming material disclosed herein on the substrate; a step of drying to form a resin film; a step of applying the insulating film forming material disclosed herein as a negative photosensitive insulating film forming material or a positive photosensitive insulating film forming material on the resin film, drying, performing pattern exposure, and developing with a developer to obtain a patterned resin film; and a step of heating the patterned resin film. Thus, a cured patterned insulating film can be obtained.

[0360] The pattern exposure is performed by, for example, exposing to a predetermined pattern through a photomask.

[0361] Examples of the active light to be irradiated include i-rays, broadband ultraviolet rays, visible rays, radiation, etc., and i-rays are preferred. As the exposure apparatus, a parallel exposure machine, a projection exposure machine, a stepper exposure machine, a scanner exposure machine, etc. can be used.

[0362] By developing after exposure, a patterned resin film can be obtained as a resin film having a pattern formed thereon. When the insulating film forming material of the present disclosure is a negative-type photosensitive insulating film forming material, the unexposed portion is removed with a developer.

[0363] Regarding the organic solvent used as a negative-type developer, a good solvent for the photosensitive resin film may be used alone as the developer, or a good solvent and a poor solvent may be appropriately mixed and used.

[0364] Examples of the good solvent include N-methyl-2-pyrrolidone, N-acetyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, α-acetyl-γ-butyrolactone, 3-methoxy-N,N-dimethylpropionamide, cyclopentanone, cyclohexanone, and cycloheptanone.

[0365] Examples of the poor solvent include toluene, xylene, methanol, ethanol, isopropyl alcohol, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, and water.

[0366] When the insulating film forming material of the present disclosure is a positive photosensitive insulating film forming material, the exposed portion is removed with a developing solution.

[0367] Examples of the solution used as the positive developer include a tetramethylammonium hydroxide (TMAH) solution and a sodium carbonate solution.

[0368] At least one of the negative-type developer and the positive-type developer may contain a surfactant. The content of the surfactant is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the developer.

[0369] The development time can be set to, for example, twice the time required for immersing the photosensitive resin film in the developer until the resin film is completely dissolved.

[0370] The development time can be adjusted according to the (A) polyimide precursor contained in the insulating film forming material of the present disclosure, and is, for example, preferably 10 seconds to 15 minutes, more preferably 10 seconds to 5 minutes, and further preferably 20 seconds to 5 minutes from the viewpoint of productivity.

[0371] The developed pattern resin film may be cleaned with a rinse solution.

[0372] As the rinse liquid, distilled water, methanol, ethanol, isopropyl alcohol, toluene, xylene, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, etc. may be used alone or in appropriate mixtures, and these may be used in combination in stages.

[0373] It should be noted that, as an organic material constituting the insulating films 102 and 202 other than the cured product of the insulating film forming material disclosed in the present invention, a photosensitive resin, a thermosetting non-conductive film (NCF: Non Conductive Film) or a thermosetting resin may also be used. The organic material may also be an underfill material. In addition, the organic material constituting the insulating films 102 and 202 may also be a heat-resistant resin.

[0374] [Step (c) and Step (d)]

[0375] Step (c) is a step of grinding the first semiconductor substrate 100. In step (c), if Figure 3 As shown in (a), the surface of the first semiconductor substrate 100, i.e., one surface 101a side, is polished using a chemical mechanical polishing method (CMP method) in such a manner that each surface 103a of the terminal electrode 103 is at the same position or slightly higher (protruding) relative to the surface 102a of the insulating film 102. In step (c), for example, the first semiconductor substrate 100 may be polished by the CMP method under the condition of selectively cutting deeper the terminal electrode 103 made of copper or the like. In step (c), the CMP method may be used to polish the surface 103a of the terminal electrode 103 in such a manner that it is consistent with the surface 102a of the insulating film 102. The polishing method is not limited to the CMP method, and back grinding or the like may also be used. Before polishing based on the CMP method, mechanical polishing may also be performed using a polishing device such as a surface planer.

[0376] When each surface 103 a of the terminal electrode 103 is slightly higher than the surface 102 a of the insulating film 102 , the height difference between each surface 103 a and the surface 102 a may be 1 nm to 150 nm, or 1 nm to 15 nm.

[0377] Step (d) is a step of grinding the second semiconductor substrate 200. In step (d), if Figure 3 As shown in (a), the surface of the second semiconductor substrate 200, i.e., one surface 201a side, is ground using the CMP method in such a manner that each surface 203a of the terminal electrode 203 is at the same position or slightly higher (protruding) relative to the surface 202a of the insulating film 202. In step (d), for example, the second semiconductor substrate 200 is ground by the CMP method under the condition of selectively cutting deeper the terminal electrode 203 made of copper or the like. In step (d), the second semiconductor substrate 200 may also be ground by the CMP method in such a manner that each surface 203a of the terminal electrode 203 is consistent with the surface 202a of the insulating film 202. The grinding method is not limited to the CMP method, and back grinding or the like may also be used.

[0378] When each surface 203 a of the terminal electrode 203 is slightly higher than the surface 202 a of the insulating film 202 , the height difference between each surface 203 a and the surface 202 a may be 1 nm to 50 nm, or 1 nm to 15 nm.

[0379] In step (c) and step (d), grinding can be performed in a manner that the thickness of the insulating film 102 is the same as the thickness of the insulating film 202, for example, grinding can be performed in a manner that the thickness of the insulating film 202 is greater than the thickness of the insulating film 102. On the other hand, grinding can be performed in a manner that the thickness of the insulating film 202 is less than the thickness of the insulating film 102. In the case where the thickness of the insulating film 202 is greater than the thickness of the insulating film 102, the insulating film 202 can be used to cover most of the foreign matter attached to the bonding interface when the second semiconductor substrate 200 is singulated or when the chip is mounted, and poor bonding can be further reduced. On the other hand, in the case where the thickness of the insulating film 202 is less than the thickness of the insulating film 102, a low-profile semiconductor chip 205, that is, the semiconductor device 1, can be achieved.

[0380] At least one of step (c) and step (d) may be performed, but preferably both step (c) and step (d) are performed.

[0381] [Step (e)]

[0382] Step (e) is a step of singulating the second semiconductor substrate 200 to obtain a plurality of semiconductor chips 205. In step (e), Figure 2As shown in (b), the second semiconductor substrate 200 is singulated into a plurality of semiconductor chips 205 by cutting means such as cutting. When cutting the second semiconductor substrate 200, a protective material or the like may be coated on the insulating film 202, and then singulated. Through step (e), the insulating film 202 of the second semiconductor substrate 200 is divided into insulating film portions 202b corresponding to each semiconductor chip 205. As a cutting method for singulating the second semiconductor substrate 200, plasma cutting, stealth cutting, laser cutting, etc. may be cited. As a surface protective material of the second semiconductor substrate 200 during cutting, for example, an organic film that can be removed by water, TMAH, etc., or a thin film such as a carbon film that can be removed by plasma, etc. may be provided.

[0383] It should be noted that, in this embodiment, after preparing the second semiconductor substrate 200 with a large area, it is singulated to obtain a plurality of semiconductor chips 205 , but the method of preparing the semiconductor chips 205 is not limited to this.

[0384] [Step (f)]

[0385] Step (f) is a step of aligning the terminal electrodes 203 of each of the plurality of semiconductor chips 205 with respect to the terminal electrodes 103 of the first semiconductor substrate 100. In step (f), Figure 2 As shown in (c), each semiconductor chip 205 is aligned so that the terminal electrode 203 of each semiconductor chip 205 faces the corresponding plurality of terminal electrodes 103 of the first semiconductor substrate 100. For this alignment, alignment marks or the like may be provided on the first semiconductor substrate 100.

[0386] [Step (g)]

[0387] Step (g) is a step of bonding the insulating film 102 of the first semiconductor substrate 100 and the insulating film portions 202b of the plurality of semiconductor chips 205. In step (g), after removing organic matter, metal oxides, etc. attached to the surfaces of the semiconductor chips 205, Figure 2 As shown in (c), the semiconductor chip 205 is aligned with respect to the first semiconductor substrate 100, and then the insulating film portion 202b of each of the plurality of semiconductor chips 205 is bonded to the insulating film 102 of the first semiconductor substrate 100 as a hybrid bonding (see Figure 3(b)). At this time, the insulating film portions of the plurality of semiconductor chips 205 and the insulating film 102 of the first semiconductor substrate 100 can be uniformly heated before bonding. By bonding while heating, the insulating film 102 and the insulating film portion 202b expand compared to the terminal electrodes 103, 203 due to the difference in thermal expansion coefficient between the insulating film 102 and the insulating film portion 202b and the terminal electrodes 103, 203. Due to the thermal expansion caused by heating, the first semiconductor substrate 100 can be ground in step (c) so that the height of the insulating film 102 becomes equal to or greater than the height of the terminal electrode 103, and the second semiconductor substrate 200 can be ground in step (d) so that the height of the insulating film portion 202b becomes equal to or greater than the height of the terminal electrode 203. The temperature difference between the semiconductor chip 205 and the first semiconductor substrate 100 during bonding is preferably within 10°C, for example. By such a heat bonding at a highly uniform temperature, the insulating film 102 and the insulating film portion 202b are bonded to form an insulating bonding portion S1, and a plurality of semiconductor chips 205 are mechanically and firmly mounted on the first semiconductor substrate 100. In addition, since it is a heat bonding at a highly uniform temperature, it is not easy to cause positional deviation of the bonding portion, and high-precision bonding can be performed. In this mounting stage, the terminal electrode 103 of the first semiconductor substrate 100 and the terminal electrode 203 of the semiconductor chip 205 are separated from each other and are not connected (but aligned). The bonding of the semiconductor chip 205 to the first semiconductor substrate 100 can also be performed by other bonding methods, for example, bonding can also be performed by room temperature bonding.

[0388] The thickness of the insulating joint portion formed by the insulating film 102 and the insulating film portion 202b, i.e., the organic insulating film, is not particularly limited, and can be, for example, greater than 0.1 μm. From the perspective of suppressing the influence of foreign matter and device design, it can be 1 μm to 20 μm, and preferably 1 μm to 5 μm.

[0389] [Process (h)]

[0390] Step (h) is a step of bonding the terminal electrodes 103 of the first semiconductor substrate 100 to the terminal electrodes 203 of each of the plurality of semiconductor chips 205. In step (h), Figure 2 As shown in (d), when the bonding of step (g) is completed, heat H, pressure, or both are applied to bond the terminal electrode 103 of the first semiconductor substrate 100 to each terminal electrode 203 of the plurality of semiconductor chips 205 as a hybrid bond (see Figure 3(c)). When the terminal electrodes 103 and 203 are made of copper, the annealing temperature in step (g) is preferably above 150°C and below 400°C, and more preferably above 200°C and below 300°C. Through such a joining process, the terminal electrode 103 and the corresponding terminal electrode 203 are joined to form an electrode joining portion S2, and the terminal electrode 103 and the terminal electrode 203 are mechanically and electrically firmly joined. It should be noted that the electrode joining in step (h) can be performed after the bonding in step (g), or it can be performed at the same time as the bonding in step (g).

[0391] As described above, on the first semiconductor substrate 100, a plurality of semiconductor chips 205 are electrically and mechanically arranged at predetermined positions with high precision. Figure 2 At the semi-finished product stage shown in (d), for example, a reliability test (connection test, etc.) is performed on the product, and only qualified products are used in subsequent processes. Figure 4 A method for manufacturing an example of a semiconductor device using such a semi-finished product will be described.

[0392] [Step (i)]

[0393] Step (i) is a step of forming a plurality of pillars 300 on the connection surface 100a of the first semiconductor substrate 100 and between the plurality of semiconductor chips 205. In step (i), Figure 4 As shown in (a), a plurality of pillars 300, for example, made of copper, are formed between a plurality of semiconductor chips 205. The pillars 300 can be formed by copper plating, conductive paste, copper pins, etc. The pillars 300 are formed so that one end is connected to a terminal electrode of the first semiconductor substrate 100 that is not connected to the terminal electrode 203 of the semiconductor chip 205, and the other end extends upward. The pillar 300 has a diameter of, for example, greater than 10 μm and less than 100 μm, and a height of greater than 10 μm and less than 1000 μm. It should be noted that, for example, more than one and less than 10,000 pillars 300 may be provided between a pair of semiconductor chips 205.

[0394] [Step (j)]

[0395] Step (j) is a step of molding resin 301 on the connection surface 100a of the first semiconductor substrate 100 so as to cover the plurality of semiconductor chips 205 and the plurality of pillars 300. In step (j), as shown in FIG. Figure 4 As shown in (b), epoxy resin or the like is molded to integrally cover the plurality of semiconductor chips 205 and the plurality of pillars 300. As a molding method, for example, compression molding, transfer molding, a method of laminating a film-like epoxy film, etc. By this resin molding, the plurality of pillars 300 and the space between the pillars 300 and the semiconductor chip 205 are filled with resin 301.

[0396] Thus, a semi-finished product M1 filled with resin is formed. It should be noted that the epoxy resin or the like may be cured after molding. In addition, when step (i) and step (j) are performed substantially simultaneously, that is, when the column 300 is formed at the same time as the resin molding, the column may be formed using stamping as a fine transfer and a conductive paste or electroplating.

[0397] [Step (k)]

[0398] Step (k) is a step of grinding and thinning the semi-finished product M1 composed of the resin 301 molded in step (j), the plurality of pillars 300 and the plurality of semiconductor chips 205 from the resin 301 side, thereby obtaining a semi-finished product M2. Figure 4 As shown in (c), the top of the semi-finished product M1 is ground with a grinder or the like, thereby thinning the first semiconductor substrate 100 after resin molding to form a semi-finished product M2. Through the grinding in step (k), the thickness of the semiconductor chip 205, the pillar 300 and the resin 301 is thinned to, for example, several tens of μm, and the semiconductor chip 205 becomes a shape corresponding to the second semiconductor chip 20, and the pillar 300 and the resin 301 become a shape corresponding to the pillar portion 30.

[0399] [Step (1)]

[0400] Step (1) is a step of forming a wiring layer 400 corresponding to the rewiring layer 40 on the semi-finished product M2 thinned in step (k). Figure 4 As shown in (d), a rewiring pattern is formed on the second semiconductor chip 20 and the pillar 30 of the ground semi-finished product M2 using polyimide, copper wiring, etc. Thus, a semi-finished product M3 having a wiring structure with a larger terminal pitch between the second semiconductor chip 20 and the pillar 30 is formed.

[0401] [Step (m) and Step (n)]

[0402] Step (m) is a step of cutting the semi-finished product M3 having the wiring layer 400 formed thereon in step (l) along the cutting line A so as to form individual semiconductor devices 1. In step (m), Figure 4 As shown in (d), the semiconductor device substrate is cut along the cutting line A by dicing or the like so as to form individual semiconductor devices 1. Then, in step (n), the semiconductor device 1a singulated in step (m) is turned over and placed on the substrate 50 and the circuit board 60 to obtain a plurality of semiconductor devices 1. Figure 1 The semiconductor device 1 is shown.

[0403] According to the above embodiment as an example of a method for manufacturing a semiconductor device, the insulating film 102 of the first semiconductor substrate 100 and the insulating film 202 of the second semiconductor substrate 200 are cured products of the insulating film forming material disclosed herein. The insulating film forming material disclosed herein has high exposure sensitivity and can suppress the generation of voids during bonding or the like.

[0404] An embodiment of the method for manufacturing a semiconductor device of the present disclosure has been described in detail above, but the present disclosure is not limited to the above embodiment. Figure 4 In the process shown, after the step (i) of forming the pillar 300, the step (j) of molding the resin 301 and the step (k) of grinding and thinning the resin 301 are sequentially performed, but the step (j) of molding the resin 301 on the connection surface of the first semiconductor substrate 100 may be performed first, followed by the step (k) of grinding and thinning the resin 301 to a predetermined thickness, and then the step (i) of forming the pillar 300 may be performed. In this case, the work of cutting the pillar 300 can be reduced, and since the cutting portion of the pillar 300 is not required, the material cost can be reduced.

[0405] In addition, in the above-mentioned embodiment, an example of C2C bonding is described, but the present invention can also be applied to Figure 5 The bonding using Chip-to-Wafer (C2W) is shown. In C2W, a semiconductor wafer 410 (first semiconductor substrate) having a substrate body 411 (first substrate body), an insulating film 412 (first insulating film) provided on one surface of the substrate body 411, and a plurality of terminal electrodes 413 (first electrodes) is prepared, and a semiconductor substrate (second semiconductor substrate) before singulation of a plurality of semiconductor chips 420 having a substrate body 421 (second substrate body), an insulating film portion 422 (second insulating film) provided on one surface of the substrate body 421, and a plurality of terminal electrodes 423 (second electrodes) is prepared. Then, similarly to the above-mentioned steps (c) and (d), one surface side of the semiconductor wafer 410 and one surface side of the second semiconductor substrate before singulation into semiconductor chips 420 are polished by CMP method or the like. Thereafter, the second semiconductor substrate is subjected to the same singulation process as in step (e) to obtain a plurality of semiconductor chips 420.

[0406] Then, if Figure 5As shown in (a), the terminal electrode 423 of the semiconductor chip 420 is aligned with the terminal electrode 413 of the semiconductor wafer 410 (step (f)). Then, the insulating film 412 of the semiconductor wafer 410 and the insulating film portion 422 of the semiconductor chip 420 are bonded to each other (step (g)), and the terminal electrode 413 of the semiconductor wafer 410 and the terminal electrode 423 of the semiconductor chip 420 are bonded (step (h)), thereby obtaining Figure 5 Thus, the insulating film 412 and the insulating film portion 422 are bonded to form an insulating bonding portion S3, and the semiconductor chip 420 is mechanically firmly and accurately mounted on the semiconductor wafer 410. In addition, the terminal electrode 413 and the corresponding terminal electrode 423 are bonded to form an electrode bonding portion S4, and the terminal electrode 413 and the terminal electrode 423 are mechanically and electrically firmly bonded.

[0407] Afterwards, if Figure 5 As shown in (c) and (d) of FIG. 4 , a plurality of semiconductor chips 420 are bonded to a semiconductor wafer 410 as a semiconductor wafer by the same method, thereby obtaining a semiconductor device 401. It should be noted that the plurality of semiconductor chips 420 can be bonded to the semiconductor wafer 410 one by one by hybrid bonding, or can be bonded to the semiconductor wafer 410 together by hybrid bonding.

[0408] In such a method for manufacturing a semiconductor device 401, similarly to the method for manufacturing the semiconductor device 1 described above, at least one of the insulating film 412 of the semiconductor wafer 410 and the insulating film portion 422 of the semiconductor chip 420 is an insulating film that is a solidified product of the insulating film forming material disclosed herein. Therefore, even if foreign matter generated by cutting when singulating into semiconductor chips 420 adheres to the insulating film, the insulating film around the foreign matter is easily deformed, and the foreign matter can be enclosed in the insulating film without causing large gaps in the insulating film. That is, the influence of foreign matter can be suppressed by the insulating film. Therefore, in the above-mentioned C2W manufacturing method, similarly to C2C, it is possible to perform fine bonding between the semiconductor wafer 410 and the semiconductor chip 420, and reduce poor bonding.

[0409] Furthermore, in the above-described method for manufacturing a semiconductor device, within the scope of achieving the effects of the present invention, inorganic materials may be included in a portion of the insulating film 102 of the semiconductor substrate 110 , the insulating film 202 of the semiconductor chip 205 , and the like.

[0410] The disclosure of Japanese Patent Application No. 2022-050451 is incorporated into this specification by reference in its entirety.

[0411] All documents, patent applications, and technical standards described in this specification are cited and incorporated into this specification to the same extent as if each individual document, patent application, and technical standard was specifically and individually described as being incorporated by reference.

[0412] Example

[0413] Hereinafter, the present disclosure will be described in more detail based on examples and comparative examples. It should be noted that the present disclosure is not limited to the following examples.

[0414] (Synthesis Example 1 (Synthesis of A1))

[0415] 62g of 3,3',4,4'-biphenyl ether tetracarboxylic acid dianhydride (ODPA), 23g of 4,4'-diaminodiphenyl ether (ODA) and 5g of metaphenylenediamine (MPD) were dissolved in 915g of 3-methoxy-N,N-dimethylpropionamide. The obtained solution was stirred at 30°C for 2 hours to obtain polyamic acid. 78g of trifluoroacetic anhydride and 109g of 2-hydroxyethyl methacrylate (HEMA) were added thereto at room temperature (25°C) and stirred at 45°C for 10 hours. The reaction solution was added dropwise to distilled water, the precipitate was collected by filtration, and it was dried under reduced pressure to obtain polyimide precursor A1.

[0416] The weight average molecular weight of A1 was determined by gel permeation chromatography (GPC) and conversion to standard polystyrene. The weight average molecular weight of A1 was 22000. Specifically, the weight average molecular weight was measured under the following conditions using a solution obtained by dissolving 0.5 mg of A1 in 1 mL of a solvent [tetrahydrofuran (THF) / dimethylformamide (DMF) = 1 / 1 (volume ratio)].

[0417] (Measurement conditions)

[0418] Measuring device: Shimadzu Corporation SPD-M20A

[0419] Pump: Shimadzu Corporation LC-20AD

[0420] Column oven: Shimadzu Corporation: CTO-20A

[0421] Measurement conditions: Chromatographic column Gelpack GL-S300MDT-5 × 2

[0422] Eluent: THF / DMF = 1 / 1 (volume ratio)

[0423] LiBr(0.03mol / L), H3PO4(0.06mol / L)

[0424] Flow rate: 1.0 mL / min, detector: UV270 nm, column temperature: 40 °C

[0425] Standard polystyrene: TSKgel standard Polystyrene Type F-1, F-4, F-20, F-80, and A-2500 manufactured by Tosoh were used to prepare a standard curve.

[0426] <Esterification rate>

[0427] The esterification rate of A1 (the ratio of ester groups formed by reaction with HEMA to the total of ester groups formed by reaction with HEMA and carboxyl groups not reacted with HEMA) was calculated by NMR measurement under the following conditions. The esterification rate was 78 mol % and the ratio of unreacted carboxyl groups was 22 mol %.

[0428] (Measurement conditions)

[0429] Measurement equipment: Bruker BioSpin AV400M

[0430] Magnetic field strength: 400MHz

[0431] Reference material: Tetramethylsilane (TMS)

[0432] Solvent: dimethyl sulfoxide (DMSO)

[0433] (Synthesis Example 2 (Synthesis of A2))

[0434] Polyimide precursor A2 was obtained by the same operation as in Synthesis Example 1 except that 23 g of 4,4′-diaminodiphenyl ether (ODA) and 5 g of metaphenylenediamine (MPD) were changed to 51 g of 1,3-bis(3-aminophenoxy)benzene (APB-1,3,3). The weight average molecular weight of A2 was 25,000.

[0435] The esterification rate of A2 was calculated by NMR measurement under the above conditions. The esterification rate was 75 mol % and the ratio of unreacted carboxyl groups was 25 mol %.

[0436] (Synthesis Example 3 (Synthesis of A3))

[0437] A polyimide precursor A3 was obtained by performing the same operation as in Synthesis Example 2 except that ODPA in Synthesis Example 2 was changed to 104 g of 4,4′-(4,4′-isopropylidenediphenoxy)diphthalic anhydride (BPADA). The weight average molecular weight of A3 was 25,000.

[0438] The esterification rate of A4 was calculated by NMR measurement under the above conditions. The esterification rate was 78 mol %, and the ratio of unreacted carboxyl groups was 22 mol %.

[0439] (Synthesis Example 4 (Synthesis of A4))

[0440] Polyimide precursor A4 was obtained by the same operation as in Synthesis Example 1 except that 23 g of 4,4'-diaminodiphenyl ether (ODA) and 5 g of metaphenylenediamine (MPD) in Synthesis Example 1 were changed to 36 g of 2,2'-dimethylbiphenyl-4,4'-diamine (DMAP). The weight average molecular weight of A4 was 25,000.

[0441] The esterification rate of A2 was calculated by NMR measurement under the above conditions. The esterification rate was 74 mol % and the ratio of unreacted carboxyl groups was 26 mol %.

[0442] [Examples 1 to 14, Comparative Examples 1 to 2]

[0443] (Preparation of Insulating Film Forming Material)

[0444] According to the components and amounts shown in Table 1, the insulating film forming materials of Examples 1 to 14 and Comparative Examples 1 to 2 were prepared as follows. The units of the amounts of each component in Table 1 are parts by mass. In addition, a blank column in Table 1 means that the component is not mixed. In each of the Examples and Comparative Examples, the mixture of each component was kneaded overnight at room temperature (25°C) in a general solvent-resistant container and then pressure filtered using a filter with a pore size of 0.2 μm. The obtained insulating film forming materials were used for the following evaluations.

[0445] The components in Table 1 are as follows.

[0446] Component (A): polyimide precursor

[0447] A1 to A4 above

[0448] Component (B): solvent

[0449] B1: 3-methoxy-N,N-dimethylpropionamide

[0450] B2: γ-Butyrolactone

[0451] Component (C): photopolymerization initiator

[0452] C1: 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl)oxime

[0453] C2: 1-[4-(phenylthio)phenyl]octane-1,2-dione = 2-(O-benzoyl oxime)

[0454] C3: O-acetyl-1-[6-(2-methylbenzoyl)-9-ethyl-9H-carbazol-3-yl]ethanone oxime

[0455] C4: 1-[4-(4-Hydroxyethoxy-phenylthio)phenyl]-1,2-propanedione-2-(O-acetyloxime)

[0456] C5: 2-Hydroxy-2-methylpropiophenone (IRGACURE1173)

[0457] C6: 4'-(Methylthio)-α-morpholino-α-methylpropiophenone (Irgacure907)

[0458] Component (D): Sensitizer

[0459] D1: 4,4'-bis(diethylamino)benzophenone (EMK)

[0460] Component (E): polymerizable monomer

[0461] E1: Triethylene glycol dimethacrylate (TEGDMA)

[0462] Component (G): polymerization inhibitor

[0463] G1: 1,4,4-trimethyl-2,3-diazabicyclo[3.2.2]non-2-ene-2,3-dioxide

[0464] Component (H): coupling agent

[0465] H1: 50 mass % methanol solution of 3-ureidopropyltriethoxysilane

[0466] (Evaluation of the presence or absence of pores)

[0467] Using a coating device spin coater, the insulating film forming materials of Examples 1 to 14 and Comparative Examples 1 to 2 were spin-coated on an 8-inch Si wafer, and heated and dried at 100°C for 240 seconds to form a resin film. A mask capable of making a circular resin film with a diameter of 180 mm was placed on the obtained resin film, and light of a wavelength of 365 nm (i-ray) with a predetermined exposure amount was irradiated. Then, it was developed with cyclopentanone or 2.38 volume % TMAH for a predetermined time. Using a vertical diffusion furnace μ-TF, the obtained patterned resin film was cured at 200°C for 2 hours under a nitrogen atmosphere, and 10 mm was removed from the periphery of the resin film on the Si wafer to make a patterned resin film.

[0468] The obtained cured film was polished by the CMP method, and a thickness of 10 μm was obtained in the measurement using an AFM (atomic force microscope). 2 The surface roughness Ra of the polished cured film is 0.5 nm to 3 nm. After the polished cured film is scrubbed with a general cleaning solution, a portion of the cleaned polished cured film is cut into 5 mm squares using a blade dicing machine (DISCO Co., Ltd., DFD-6362), thereby obtaining a chip with resin.

[0469] The obtained chip with resin was pressed onto the polished cured film at a predetermined pressure and 250° C. for 15 seconds using a flip chip bonder to prepare a cured film with chip. For each insulating film forming material, five chips pressed onto the polished cured film were evaluated as described below.

[0470] The obtained cured film with chip was observed using SAT (scanning acoustic tomography) to see if there were pores indicating poor adhesion at the interface of the insulating film. The evaluation criteria for pores are as follows. The results are shown in Table 1. If the evaluation is A, the generation of pores is suppressed and the evaluation is judged to be good.

[0471] - Evaluation criteria for pores -

[0472] A: Among 5 chips, voids were observed in 2 or less chips.

[0473] B: Pores were observed in more than 2 of the 5 chips.

[0474] C: One or more chips peeled off during SAT measurement.

[0475] (Evaluation of sensitivity)

[0476] The insulating film forming material was spin-coated on the Si substrate and dried on a hot plate at 100°C for 240 seconds to form a resin film with a thickness of about 12 μm after coating. The resin film was subjected to a 100-1100 mJ / cm2 radiation using an i-ray stepper NES2WA06 (manufactured by Nikon Corporation) through a photomask. 2 The i-ray is 100mJ / cm 2 The resin film was then developed for 20 seconds using a coating developer ACT8 (manufactured by Tokyo Electron Co., Ltd.) with cyclopentanone. The minimum exposure amount when the film thickness of the resin film in the exposed part became 70% or more of the initial film thickness was taken as the sensitivity.

[0477] The evaluation criteria of sensitivity are as follows. The results are shown in Table 1. If the evaluation is A, the sensitivity is high and the evaluation is judged to be good.

[0478] -Evaluation criteria for sensitivity-

[0479] A: Sensitivity is 300mJ / cm 2 the following

[0480] B: Sensitivity greater than 300mJ / cm 2 And 500mJ / cm 2 the following

[0481] C: Sensitivity greater than 500mJ / cm2

[0482] (Evaluation of Pattern Profile (PP))

[0483] Cut out the sample with a diamond pen at 600 mJ / cm in the above sensitivity evaluation. 2 The exposed area was observed with a scanning electron microscope (SEM) in a cross section of a 100 μm line pattern, and the shape of the pattern cross section was evaluated for pattern profile.

[0484] The evaluation criteria of the pattern profile are as follows. The results are shown in Table 1. If the evaluation is A, the pattern profile is excellent and the evaluation is judged to be good.

[0485] -Evaluation criteria for pattern profile (PP)-

[0486] A: In the cross-sectional shape, the intersection of the upper surface and the side surface is clear, and there are no abnormalities such as protrusions at the intersection.

[0487] B: In the cross-sectional shape, the tapered side surface is deformed and the intersection of the upper surface and the side surface is unclear.

[0488] C: In the cross-sectional shape, there is an abnormality such as a protrusion at the intersection of the upper surface and the side surface.

[0489] (Evaluation of Low-temperature Bonding Properties)

[0490] The patterned resin film and the chip with resin were prepared in the same way as the evaluation of the above-mentioned void generation, and the chip with resin was placed on the patterned resin film, and covered with a carbon sheet for height difference absorption. Using a crimping device (manufactured by EVG), a load of 100N was applied to a 1 cm pressurized area at 180°C for 180 seconds under atmospheric conditions to perform crimping. Three chips were crimped, and the fact that the chip did not fall off even when a small external force was applied to the crimped chip was used as an indicator of low-temperature bonding.

[0491] The evaluation criteria of low temperature bondability are as follows. The results are shown in Table 1. If the evaluation is A, the low temperature bondability is excellent and the evaluation is judged to be good.

[0492] -Evaluation criteria for low temperature bonding-

[0493] A: Adhesion was confirmed for all three chips.

[0494] B: Adhesion was confirmed in one or two chips among three chips.

[0495] C: No adhesion was observed in any of the three chips.

[0496] [Table 1]

[0497]

[0498] As shown in Table 1, compared with Comparative Examples 1 to 2, Examples 1 to 14 have excellent exposure sensitivity and the generation of voids at the interface of the insulating film is suppressed. Among the examples, Examples 1 to 4, 6, 9, 11 to 14 using C1 as a photopolymerization initiator have excellent pattern profiles. In addition, Examples 4, 6, 9, and 12 using C1 and any one of C2 to C4 as photopolymerization initiators maintain the pattern profile and have further excellent exposure sensitivity.

[0499] On the other hand, in Comparative Examples 1 and 2, more voids were generated at the bonding interface, and the sensitivity was also lower than that of the Example. The pattern profiles in Comparative Examples 1 and 2 were also worse than that of the Example.

[0500] (Measurement of Glass Transition Temperature (Tg) of Cured Film)

[0501] The insulating film forming materials of Examples 1, 13, 14 and Comparative Example 1 were used to form cured films as follows, and then the glass transition temperatures were measured. The photosensitive insulating film forming material was spin-coated on a Si substrate and dried on a hot plate at 100° C. for 240 seconds to form a photosensitive resin film having a thickness of about 10 μm after curing.

[0502] A mask aligner MA-8 (manufactured by SUSS MicroTec) was used at 800 mJ / cm 2 The obtained photosensitive resin film was subjected to broadband (BB) exposure at an exposure amount of 1.5 %. The exposed resin film was developed for 20 seconds using a coating developer ACT8 (manufactured by Tokyo Electron Co., Ltd.) with cyclopentanone to obtain a 10 mm wide strip-shaped patterned resin film.

[0503] The obtained patterned resin film was cured at 200°C for 2 hours in a nitrogen atmosphere using a vertical diffusion furnace μ-TF to obtain a patterned cured product with a film thickness of 10 μm. The obtained patterned cured product was immersed in a 4.9 mass % hydrofluoric acid aqueous solution, and the 10 mm wide patterned cured product was peeled off from the Si substrate.

[0504] The storage modulus and loss modulus of the patterned cured product peeled from the Si substrate were measured using RSA-G2 manufactured by TA Instruments under the conditions of test frequency 1 Hz, heating rate 5°C / min, measurement mode: tensile, N2 atmosphere, measurement range -50°C to 400°C, chuck distance 10 mm, and sample width 2.0 mm. The loss tangent was calculated from the obtained storage modulus and loss modulus, and the peak of the loss tangent was taken as Tg (glass transition temperature).

[0505] The Tg of Example 1 was 210°C, the Tg of Example 13 was 160°C, the Tg of Example 14 was 220°C, and the Tg of Comparative Example 1 was 170°C.

[0506] Description of Reference Numerals

[0507] 1, 1a, 401: semiconductor device, 10: first semiconductor chip, 20: second semiconductor chip, 30: pillar, 40: rewiring layer, 50: substrate, 60: circuit substrate, 61: terminal electrode, 100: first semiconductor substrate, 101: first substrate body, 101a: one surface, 102: insulating film (first insulating film), 103: terminal electrode (first electrode), 103a: surface, 200: second semiconductor substrate, 201: second substrate body, 201a: one surface, 202: insulating film (second insulating film), 203: terminal electrode (second electrode), 203a: surface, 20 5: semiconductor chip, 300: pillar, 301: resin, 410: semiconductor wafer (first semiconductor substrate), 411: substrate body (first substrate body), 412: insulating film (first insulating film), 413: terminal electrode (first electrode), 420: semiconductor chip (second semiconductor substrate), 421: substrate body (second substrate body), 422: insulating film part (second insulating film), 423: terminal electrode (second electrode), A: cutting line, H: heat, M1~M3: semi-finished product, S1: insulating bonding part, S2: electrode bonding part, S3: insulating bonding part, S4: electrode bonding part.

Claims

1. A hybrid bonded insulating film forming material comprising (A) a polyimide precursor having a polymerizable unsaturated bond site, (B) a solvent, and (C) an oxime-based photopolymerization initiator.

2. The hybrid bonding insulating film forming material according to claim 1, wherein the (C) oxime-based photopolymerization initiator comprises a compound represented by the following formula (I): [Chemistry 1] In formula (I), R 1 represents an alkyl group, an alkoxy group, a phenyl group or a phenoxy group, R 2 represents an alkyl group, R 3 It represents a carbonyl group or a monovalent organic group connected via a single bond.

3. The hybrid bonding insulating film forming material according to claim 2, wherein the (C) oxime-based photopolymerization initiator comprises R 1 A compound represented by an alkoxy group.

4. The hybrid bonding insulating film forming material according to claim 2 or 3, wherein the (C) oxime-based photopolymerization initiator comprises R 1 The compound A represented by an alkoxy group and R in the formula (I) 1 The compound B is represented by an alkyl group or a phenyl group.

5. The hybrid bonding insulating film forming material according to any one of claims 1 to 4, wherein the (A) polyimide precursor comprises a compound having a structural unit represented by the following general formula (1): [Chemistry 2] In the general formula (1), X represents a tetravalent organic group, Y represents a divalent organic group, and R 6 and R 7 Each independently represents a hydrogen atom or a monovalent organic group, R 6 and R 7 At least one of them has a polymerizable unsaturated bond.

6. The hybrid bonding insulating film forming material according to claim 5, wherein in the general formula (1), the tetravalent organic group represented by X is a group represented by the following formula (E): [Chemistry 3] In formula (E), C represents a single bond; an alkylene group; a halogenated alkylene group; a carbonyl group; a sulfonyl group; an ether bond, i.e. -O-; a thioether bond, i.e. -S-; a phenylene group; an ester bond, i.e. -OC(=O)-; a silene bond, i.e. -Si(R A ) 2 -, 2 of which are R A Each independently represents a hydrogen atom, an alkyl group or a phenyl group; a siloxane bond, i.e., -O-(Si(R B ) 2 -O-) n , of which 2 R B Each independently represents a hydrogen atom, an alkyl group or a phenyl group, and n represents an integer of 1 or 2 or more; or a divalent group formed by combining at least two of them.

7. The hybrid bonding insulating film forming material according to claim 5 or 6, wherein in the general formula (1), the divalent organic group represented by Y is a group represented by the following formula (H): [Chemistry 4] In formula (H), R each independently represents an alkyl group, an alkoxy group, a haloalkyl group, a phenyl group or a halogen atom, n each independently represents an integer of 0 to 4, and D represents a single bond; an alkylene group; a haloalkylene group; a carbonyl group; a sulfonyl group; an ether bond, i.e. -O-; a thioether bond, i.e. -S-; a phenylene group; an ester bond, i.e. -OC(=O)-; a silene bond, i.e. -Si(R A ) 2 -, 2 of which are R A Each independently represents a hydrogen atom, an alkyl group or a phenyl group; a siloxane bond, i.e., -O-(Si(R B ) 2 -O-) n , of which 2 R B Each independently represents a hydrogen atom, an alkyl group or a phenyl group, and n represents an integer of 1 or 2 or more; or a divalent group formed by combining at least two of them. 8 . The hybrid bonding insulating film forming material according to claim 7 , wherein D in the formula (H) includes an ether bond, that is, —O—.

9. The hybrid bonding insulating film forming material according to any one of claims 5 to 8, wherein in the general formula (1), R 6 And the R 7 The monovalent organic group in the formula (2) is any one of an ethyl group, an isobutyl group, and a tert-butyl group, wherein R 6 And the R 7 At least one of the groups is a group represented by the general formula (2), [Chemistry 5] In the general formula (2), R 8 ~R 10 Each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 3 carbon atoms, and R x represents a divalent linking group. 10 . The hybrid bonding insulating film forming material according to claim 1 , further comprising (D) a sensitizer. 11 . The hybrid bonded insulating film forming material according to claim 1 , further comprising (E) a polymerizable monomer. 12 . The hybrid bonded insulating film forming material according to claim 1 , wherein the glass transition temperature of the hybrid bonded insulating film forming material when cured is 50° C. to 300° C.

13. A method for manufacturing a semiconductor device, preparing a first semiconductor substrate having a first substrate body, and a first electrode and a first organic insulating film provided on one surface of the first substrate body; preparing a semiconductor chip having a semiconductor chip substrate body, and a second organic insulating film and a second electrode provided on one surface of the semiconductor chip substrate body; The first electrode and the second electrode are bonded together, and the first organic insulating film and the second organic insulating film are bonded together. In forming at least one of the first organic insulating film and the second organic insulating film, the hybrid bond insulating film forming material according to any one of claims 1 to 12 is used. 14 . The method for manufacturing a semiconductor device according to claim 13 , wherein the first electrode and the second electrode are bonded together after the first organic insulating film and the second organic insulating film are bonded together.

15. A method for manufacturing a semiconductor device according to any one of claims 13 to 14, comprising grinding at least one of the one surface of the first semiconductor substrate and the one surface side of the semiconductor chip before performing any of the bonding of the first electrode and the second electrode and the bonding of the first organic insulating film and the first organic insulating film. 16 . The method for manufacturing a semiconductor device according to claim 15 , wherein the polishing comprises chemical mechanical polishing. 17 . The method for manufacturing a semiconductor device according to claim 16 , wherein the polishing further comprises mechanical polishing.

18. A method for manufacturing a semiconductor device according to any one of claims 13 to 17, wherein in the bonding between the first electrode and the second electrode, at least one of the following conditions is satisfied: the thickness of the first organic insulating film is thicker than the thickness of the first electrode, and the thickness of the second organic insulating film is thicker than the thickness of the second electrode.

19. A semiconductor device comprising: A first semiconductor substrate including a first substrate body, and a first organic insulating film and a first electrode provided on one surface of the first substrate body; and A semiconductor chip having a semiconductor chip substrate body, and a second organic insulating film and a second electrode provided on one surface of the semiconductor chip substrate body. The first organic insulating film is bonded to the second organic insulating film, the first electrode is bonded to the second electrode, At least one of the first organic insulating film and the second organic insulating film is a cured product of the hybrid bond insulating film forming material according to any one of claims 1 to 12.