Ultraviolet absorber
By using the modified fluorene compound to prepare ultraviolet absorbers, the problem of insufficient absorption performance of ultraviolet absorbers on long-wavelength ultraviolet rays in the prior art is solved, and efficient UV-A or UV-B absorption and low coloring properties are achieved, which improves the Stability and mechanical properties of the resin.
Patent Information
- Application Number
- CN202380030928.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-08
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing ultraviolet absorbers lack the absorption performance of long-wavelength ultraviolet rays, and when added in large quantities, it is easy to cause problems of mechanical strength, heat resistance and transparency of the resin, and it is difficult to take into account the absorption performance and low coloring properties of the UV-A region.
Using fluorene compounds as ultraviolet absorbers, a resin with excellent ultraviolet absorption properties is prepared by modifying them with appropriate substituents, specifically absorbing ultraviolet rays of specific wavelengths, and improving its stability in the resin by imparting polymerizable functional groups. sex.
Excellent absorption of UV-A or UV-B is achieved, taking into account the ultraviolet absorption performance and low coloring properties, and improving the exudation resistance and mechanical properties of the resin.
Smart Images

Figure CN118946648A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an ultraviolet absorber having excellent ultraviolet absorbency in the UV-A and UV-B regions, an ultraviolet absorbing resin, an ultraviolet absorbing coating liquid, an ultraviolet absorbing coating resin sheet, an ultraviolet absorbing coated glass, an ultraviolet absorbing molded body, an ultraviolet absorbing film, a polarizer protective film, a polarizing plate, an image display device, a transportation device and a building material component. Background Art
[0002] Ultraviolet rays are roughly divided into long-wavelength ultraviolet rays (UV-A; 320-400nm), medium-wavelength ultraviolet rays (UV-B; 280-320nm) and short-wavelength ultraviolet rays (UV-C; 200-280nm) according to their wavelength range. Among them, UV-C is almost completely absorbed by the ozone layer before reaching the earth's surface, so most of the ultraviolet rays transmitted to the earth are UV-A and UV-B.
[0003] The wavelengths of ultraviolet rays that easily cause degradation of polymer materials vary depending on their type. For example, it is known that many polymer materials such as polyethylene and polyvinyl chloride are significantly degraded by UV-B, causing discoloration or reduction in mechanical strength, etc. Therefore, ultraviolet absorbers that absorb UV-B are widely added.
[0004] In recent years, there is a demand for longer-term stability against ultraviolet rays, so the demand for ultraviolet absorbers that can absorb not only UV-B but also UV-A is increasing, especially in the fields of displays, solar cells, and automobiles. However, existing organic ultraviolet absorbers have little absorption of long-wavelength ultraviolet rays, so it is necessary to increase the amount of addition, but if a large amount is added, there are problems such as bleeding or reduction of the mechanical strength, heat resistance, and transparency of the resin. In addition, ultraviolet absorbers characterized by absorbing long-wavelength ultraviolet rays tend to be colored yellow because they also absorb in the visible light region above 400nm, and it is considered difficult to take into account both ultraviolet absorption performance in the UV-A region and low colorability.
[0005] Among them, optical films used to improve visibility in display devices such as liquid crystal displays (LCDs) or organic EL displays (OLEDs) have the following problems: in addition to being exposed to ultraviolet rays contained in sunlight, they are also exposed to ultraviolet rays contained in the light source of the display device for a long time, so that deterioration such as yellowing progresses over time, reducing visibility. In addition, an excellent ultraviolet absorber is being sought that can still exhibit sufficient ultraviolet absorption performance even if the optical film is made thinner as the demand for miniaturization of display devices increases.
[0006] For example, Patent Document 1 discloses a (meth)acrylic film to which a benzotriazole-based ultraviolet absorber is added. However, generally, the molar absorption coefficient of the benzotriazole-based ultraviolet absorber in the UV-A region is insufficient and needs to be added at a high concentration. Therefore, a composition containing the benzotriazole-based ultraviolet absorber has the problem of being easily whitened or embrittled due to bleeding.
[0007] In addition, Patent Document 2 discloses a triazine-based ultraviolet absorber having strong absorption in a wide range of the UV-A region. However, triazine-based ultraviolet absorbers that generally absorb ultraviolet rays in a wide wavelength band also absorb visible light above 400 nm, and thus have the problem of being easily colored.
[0008] Patent Document 3 discloses a method of combining an ultraviolet absorber having maximum absorption at a wavelength of 200 to 300 nm and an ultraviolet absorber having maximum absorption at a wavelength of 320 to 400 nm. This method can achieve both ultraviolet absorption performance at a wavelength of 380 nm and low coloration, but in order to further improve ultraviolet absorption performance and low coloration, it is estimated that a new ultraviolet absorber that absorbs only ultraviolet rays of a specific wavelength is needed.
[0009] Patent Document 4 discloses an ultraviolet absorber composition characterized in that the maximum absorption wavelength is 350 nm to 400 nm, the half-value width is 55 nm or less, and the molar absorption coefficient at the maximum absorption wavelength is 20000 or more. This can provide a material that absorbs only ultraviolet rays of a specific wavelength and has little coloration, but the compositions disclosed in the present invention have a complex synthesis method and high cost, so there is a problem that it is difficult to use widely.
[0010] In order to prevent the ultraviolet absorber from bleeding out in actual use environments or from sublimating due to heat during drying or molding, it has been proposed to impart a polymerizable functional group to the ultraviolet absorber and cure the ultraviolet absorber itself to form a coating component.
[0011] Patent Document 5 discloses a resin composition obtained by homopolymerizing a benzotriazole derivative compound, and Patent Document 6 discloses a compound obtained by adding a reactive functional group to the terminal of a compound having a triazine skeleton. However, in either invention, the functional group contributing to ultraviolet absorption is a conventionally known functional group such as benzotriazole or triazine, and therefore, there is a problem that the molar absorption coefficient in the UV-A region is insufficient and coloration is easily caused as described above.
[0012] Prior art literature
[0013] Patent Literature
[0014] Patent Document 1: Japanese Patent Application Publication No. 2019-167411
[0015] Patent Document 2: Japanese Patent Application Publication No. 2016-102199
[0016] Patent Document 3: Japanese Patent Application Publication No. 2015-165301
[0017] Patent Document 4: Japanese Patent Application Publication No. 2010-059235
[0018] Patent Document 5: Japanese Patent Application Publication No. 2019-034998
[0019] Patent Document 6: Japanese Patent Application Publication No. 2021-178918 Summary of the invention
[0020] Technical issues to be solved by the invention
[0021] The present invention aims to provide a novel ultraviolet absorber which has excellent absorptivity to UV-A or UV-B and specifically absorbs only ultraviolet rays of a specific wavelength and can be widely used; and an ultraviolet absorbing resin, an ultraviolet absorbing coating liquid, an ultraviolet absorbing coating resin sheet, an ultraviolet absorbing coated glass, an ultraviolet absorbing molded body, an ultraviolet absorbing film, a polarizer protective film, a polarizing plate, an image display device, a transportation device and a building material component which have excellent anti-bleeding properties in addition to the above-mentioned properties.
[0022] Means for solving problems
[0023] In order to achieve the above-mentioned problem, the present inventors conducted intensive research and found that fluorene compounds have excellent ultraviolet absorption properties for UV-A or UV-B and specifically absorb only ultraviolet rays of a specific wavelength, and that ultraviolet rays of various wavelengths can be absorbed by giving appropriate substituents to these fluorene compounds. In addition, it was found that by giving polymerizable functional groups to the above-mentioned fluorene compounds, a resin composition with excellent ultraviolet absorption performance can be prepared, thereby completing the present invention.
[0024] That is, the present invention is as follows.
[0025] [1] An ultraviolet absorber, which is a fluorene compound represented by the general formula (1), or a resin containing the fluorene compound as a constituent unit.
[0026] [Chemical formula 1]
[0027]
[0028] (Where Z 1a and Z 1b Each independently represents an aromatic hydrocarbon ring,
[0029] Y 1aand Y 1b Each independently represents a carboxyl group, a carboxyl ester group, an acyl halide group, an acid anhydride group, a hydroxyl group, or a group having a polymerizable double bond,
[0030] R 1a and R 1b Each independently represents a halogen atom, an acyl group, a nitro group, a cyano group, a mono- or di-substituted amino group, -R A 、-OR A , or -SR A (Among them, R A represents a hydrocarbon group),
[0031] k1 and k2 each independently represent an integer greater than 0,
[0032] m1 and m2 each independently represent an integer of 0 to 4,
[0033] R 2a and R 2b Each independently represents a halogen atom, a cyano group, or a hydrocarbon group other than an aryl group,
[0034] n1 and n2 each independently represent an integer from 0 to 4,
[0035] m1+n1 and m2+n2 are each independently an integer of 4 or less.)
[0036] [2] The ultraviolet absorber according to [1], wherein in the general formula (1), at least one of m1 and m2 is 1 or more.
[0037] [3] The ultraviolet absorber according to [1] or [2], wherein in the general formula (1), Z 1a and Z 1b It is a condensed polycyclic aromatic hydrocarbon ring, and both m1 and m2 are integers of 1 or more.
[0038] [4] The ultraviolet absorber according to any one of [1] to [3], wherein in the general formula (1), Y 1a and Y 1b are each independently a group represented by the following formula (Y1),
[0039] The fluorene compound is a dicarboxylic acid or a derivative thereof,
[0040] The resin is a polyester resin or a polyamide resin having the fluorene compound as a dicarboxylic acid as a constituent unit.
[0041] [Chemical formula 2]
[0042]
[0043] (In the formula, A 1Indicates straight chain or branched chain C 1-6 Alkylene.)
[0044] [5] The ultraviolet absorber according to any one of [1] to [3], wherein in the general formula (1), Y 1a and Y 1b are each independently a group represented by the following formula (Y2),
[0045] The fluorene compound is a diol,
[0046] The resin is a polyester resin or a polycarbonate resin having the fluorene compound as a diol as a constituent unit.
[0047] [Chemical formula 3]
[0048]
[0049] (In the formula, A 2 and A 3 Each independently represents a linear or branched C 1-6 Alkylene,
[0050] p represents an integer greater than or equal to 0).
[0051] [6] The ultraviolet absorber according to any one of [1] to [3], wherein in the general formula (1), Y 1a and Y 1b are each independently a group represented by the following formula (Y3),
[0052] The fluorene compound is a diol,
[0053] The resin is a polyester resin or a polycarbonate resin having the fluorene compound as a diol as a constituent unit.
[0054] [Chemical formula 4]
[0055]
[0056] (Where Z 2 represents an aromatic hydrocarbon ring,
[0057] A 4 Each independently represents a linear or branched C 1-4 Alkylene,
[0058] R 3 Each independently represents a substituent,
[0059] q represents an integer greater than 0,
[0060] r represents an integer greater than 1,
[0061] s represents an integer greater than or equal to 0. )
[0062] [7] The ultraviolet absorber according to [6], wherein in the general formula (Y3), Z 2 It is a condensed polycyclic aromatic hydrocarbon ring.
[0063] [8] The ultraviolet absorber according to any one of [1] to [3], wherein in the general formula (1), Y 1a and Y 1b are each independently a group represented by the following formula (Y4),
[0064] The fluorene compound is di(meth)acrylate,
[0065] The resin is a (meth)acrylic resin having the fluorene compound as a di(meth)acrylate as a constituent unit.
[0066] [Chemical formula 5]
[0067]
[0068] (In the formula, A 5 and A 6 Each independently represents a linear or branched C 1-6 Alkylene,
[0069] R 4 represents a hydrogen atom or a methyl group,
[0070] t represents an integer greater than or equal to 0. )
[0071] [9] The ultraviolet absorber according to any one of [1] to [8], wherein the half-value width in a wavelength band showing 1 / 2 or more of the absorbance at the maximum absorption wavelength is 55 nm or less.
[0072]
[10] The ultraviolet absorber according to any one of [1] to [9], which has a maximum absorption wavelength in the range of 320 to 400 nm.
[0073]
[11] The ultraviolet absorber according to any one of [1] to
[10] , which has a molar absorption coefficient (A) at 380 nm. 380 ) and the molar absorption coefficient (A 400 ) ratio (A 380 / A 400 ) is 50 or more.
[0074]
[12] The ultraviolet absorber according to any one of [1] to
[11] , wherein the content of the structural unit derived from the fluorene compound is 1 to 100 mol % based on all the structural units of the resin.
[0075]
[13] A UV absorbing composition comprising:
[0076] [1] The ultraviolet absorber described in; and
[0077] At least one compound selected from the group consisting of a triazine ring-containing compound, a benzotriazole ring-containing compound, and a benzophenone ring-containing compound as the second ultraviolet absorber.
[0078]
[14] An ultraviolet absorbing resin composition comprising:
[0079] The ultraviolet absorber according to any one of [1] to
[12] ; and
[0080] Any resin,
[0081] The ultraviolet absorber is contained in an amount of 0.1 to 10% by mass based on the total amount.
[0082]
[15] A UV-absorbing coating liquid comprising: the UV absorber described in any one of [1] to
[12] , the UV-absorbing composition described in
[13] , or the UV-absorbing resin composition described in
[14] .
[0083]
[16] A UV-absorbing coated resin sheet comprising a resin sheet and a UV-shielding layer,
[0084] The ultraviolet shielding layer comprises the ultraviolet absorber described in any one of [1] to
[12] , the ultraviolet absorbing composition described in
[13] , or the ultraviolet absorbing resin composition described in
[14] .
[0085]
[17] An ultraviolet absorbing coated glass comprising glass and an ultraviolet shielding layer,
[0086] The ultraviolet shielding layer comprises the ultraviolet absorber described in any one of [1] to
[12] , the ultraviolet absorbing composition described in
[13] , or the ultraviolet absorbing resin composition described in
[14] .
[0087]
[18] An ultraviolet absorbing molded article comprising the ultraviolet absorber described in any one of [1] to
[12] , the ultraviolet absorbing composition described in
[13] , or the ultraviolet absorbing resin composition described in
[14] .
[0088]
[19] An ultraviolet absorbing film comprising the ultraviolet absorber described in any one of [1] to
[12] , the ultraviolet absorbing composition described in
[13] , or the ultraviolet absorbing resin composition described in
[14] .
[0089]
[20] A polarizer protective film comprising the ultraviolet absorbing film described in
[19] .
[0090]
[21] The polarizer protective film according to
[20] , which has a spectral transmittance of 5% or less at 350 nm and a b* value of 0.5 or less in the L*a*b* color space (CIELAB).
[0091]
[22] The polarizer protective film according to
[20] or
[21] , which has a spectral transmittance of 8% or less at 380 nm.
[0092]
[23] A polarizing plate comprising the polarizer protective film according to any one of
[20] to
[22] .
[0093]
[24] An image display device comprising the polarizing plate described in
[23] .
[0094]
[25] A transport device comprising a member comprising the ultraviolet absorber described in any one of [1] to
[12] , the ultraviolet absorbing composition described in
[13] , or the ultraviolet absorbing resin composition described in
[14] .
[0095]
[26] A building component comprising a component comprising the ultraviolet absorber described in any one of [1] to
[12] , the ultraviolet absorbing composition described in
[13] , or the ultraviolet absorbing resin composition described in
[14] .
[0096] Effects of the Invention
[0097] According to the present invention, there can be provided an ultraviolet absorber which has excellent ultraviolet absorbency for UV-A or UV-B, specifically absorbs only ultraviolet rays of a specific wavelength, and can be widely used; and an ultraviolet absorbing resin, an ultraviolet absorbing coating liquid, an ultraviolet absorbing coating resin sheet, an ultraviolet absorbing coated glass, an ultraviolet absorbing molded body, an ultraviolet absorbing film, a polarizer protective film, a polarizing plate, an image display device, a transportation equipment, and a building material component which have excellent oozing resistance in addition to the above-mentioned characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0098] Figure 1A This is a cross-sectional view schematically showing a polarizing plate according to one embodiment of the present invention.
[0099] Figure 1B This is a cross-sectional view schematically showing a polarizing plate according to another embodiment of the present invention.
[0100] Figure 2A This is a cross-sectional view schematically showing an image display device (OLED) according to one embodiment of the present invention.
[0101] Figure 2BThis is a cross-sectional view schematically showing an image display device (LCD) according to an embodiment of the present invention.
[0102] Figure 3 This is a cross-sectional view schematically illustrating a scroll display according to an embodiment of the present invention.
[0103] Figure 4 This is a graph showing the absorbance of the ultraviolet absorbing polyester resins obtained in Examples 8 to 13. DETAILED DESCRIPTION
[0104] Hereinafter, an embodiment of the present invention (hereinafter referred to as "this embodiment") is described in detail, but the present invention is not limited thereto and various modifications can be made without departing from the scope of the present invention. In addition, the same reference numerals are used for the same elements in the drawings, and repeated descriptions are omitted. In addition, unless otherwise specified, the positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings. Moreover, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.
[0105] In addition, in this embodiment, "C 2-8 ” means that the carbon number of a certain group is 2 or more and 8 or less.
[0106] 1. UV absorber
[0107] The ultraviolet absorber of the present embodiment is a fluorene compound represented by the following general formula (1), or a resin containing a fluorene compound represented by the following general formula (1) as a constituent unit.
[0108] [Chemical formula 6]
[0109]
[0110] (Where Z 1a and Z 1b Each independently represents an aromatic hydrocarbon ring,
[0111] Y 1a and Y 1b Each independently represents a carboxyl group, a hydroxyl group or a group having a polymerizable double bond,
[0112] R 1a and R 1b Each independently represents a halogen atom, an acyl group, a nitro group, a cyano group, an amino group, -R A 、-OR A or -SR A (Among them, R A represents a hydrocarbon) group,
[0113] k1 and k2 each independently represent an integer greater than 0,
[0114] m1 and m2 each independently represent an integer of 0 to 4,
[0115] R 2a and R 2b Each independently represents a substituent,
[0116] n1 and n2 each independently represent an integer from 0 to 4,
[0117] m1+n1 and m2+n2 are each independently an integer of 4 or less.)
[0118] By having the structure of the general formula (1), the ultraviolet absorber of the present embodiment shows excellent ultraviolet absorption to UV-A or UV-B, and specifically absorbs only ultraviolet rays of a specific wavelength. Moreover, by changing each group represented by the general formula (1) to an arbitrary structure, the absorption wavelength can be adjusted.
[0119] The ultraviolet absorber of the present embodiment may be a fluorene compound having a structure represented by the general formula (1), or may be a resin having a structure represented by the general formula (1) as a constituent unit.
[0120] Hereinafter, the fluorene compound having the structure represented by the general formula (1) will be described first, and then the resin will be described.
[0121] 1.1. Fluorene compounds
[0122] The fluorene compound has a structure represented by the general formula (1) and may have an aromatic hydrocarbon ring (Z) bonded to the fluorene ring as described in detail below. 1a , Z 1b ) and the substituent (Y 1a , Y 1b , R 1a , R 1b , R 2a , R 2b ).
[0123] 1.1.1. Base [-Z 1a -(R 1a ) k1 ] and base [-Z 1b -(R 1b ) k2 ]
[0124] Z 1a and Z 1b Each independently represents an aromatic hydrocarbon ring bonded to a fluorene ring. Such an aromatic hydrocarbon ring is not particularly limited, and examples thereof include: a monocyclic aromatic hydrocarbon ring such as a benzene ring, a condensed polycyclic aromatic hydrocarbon ring (condensed polycyclic aromatic hydrocarbon ring), a ring-aggregated aromatic hydrocarbon ring (ring-aggregated polycyclic aromatic hydrocarbon ring), etc. Among them, from the viewpoint of the molar absorption coefficient in the UV-A region, a condensed polycyclic aromatic hydrocarbon ring is preferred.
[0125] The condensed polycyclic aromatic hydrocarbon ring is not particularly limited, and examples thereof include naphthalene ring, indene ring, azulene ring, anthracene ring, phenanthrene ring, tetracene ring, pentacene ring, benzopyrene ring, chrysene ring, dibenzochrysene ring, pyrene ring, triphenylene ring, corannulene ring, coronene ring, and ovalbenzene ring, etc. Among them, the naphthalene ring is preferred.
[0126] The ring-aggregated aromatic hydrocarbon ring is not particularly limited, and examples thereof include biphenyl rings, phenylnaphthalene rings, binaphthyl rings and other biaryl hydrocarbon rings; teraryl hydrocarbon rings such as terphenyl rings and other terphenyl rings, etc. Among them, a biphenyl ring is preferred.
[0127] Z 1a and Z 1b The substitution position on the fluorene ring is not particularly limited, but is preferably the 2-position and / or the 7-position from the viewpoint of the industrial synthesis method of the fluorene compound.
[0128] In Z 1a and Z 1b When the aromatic hydrocarbon rings represented independently are naphthalene rings, ring Z 1a , Z 1b The position of bonding to the fluorene skeleton may be either the 1st position or the 2nd position of the naphthalene ring. Of these, the 1st position of the naphthalene ring is preferred from the viewpoint of the 5% mass loss temperature, and the 2nd position of the naphthalene ring is particularly preferred from the viewpoint of the molar absorption coefficient.
[0129] Z 1a and Z 1b The carbon number of is preferably 6-24, more preferably 6-18, and even more preferably 6-12.
[0130] Aromatic ring Z 1a and Z 1b Each of the substituents R may independently have a non-reactive or non-polymerizable 1a and R 1b As a substituent R 1a and R 1b , is not particularly limited, and examples thereof include: a halogen atom, an acyl group, a nitro group, a cyano group, a mono- or di-substituted amino group, -R A 、-OR A or -SR A etc. Here, R A It represents a hydrocarbon group.
[0131] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.
[0132] Examples of the acyl group include C 1-6 Alkyl-carbonyl, etc.
[0133] Examples of the mono- or di-substituted amino group include dialkylamino and bis(alkylcarbonyl)amino groups. Examples of the dialkylamino group include di-C substituted amino groups such as dimethylamino and the like. 1-4 Examples of the bis(alkylcarbonyl)amino group include bis(C)-(diacetylamino) and the like. 1-4 alkyl-carbonyl)amino.
[0134] As R A Examples of the hydrocarbon group represented by include an alkyl group, a cycloalkyl group, an aryl group, and an aralkyl group.
[0135] Examples of the alkyl group include linear or branched C alkyl groups such as methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, and tert-butyl. 1-10 Among them, a linear or branched C 1-6 Alkyl, more preferably a linear or branched C 1-4 alkyl.
[0136] Examples of the cycloalkyl group include C 5-10 Cycloalkyl.
[0137] Examples of the aryl group include C phenyl, alkylphenyl, biphenyl, naphthyl and the like. 6-12 Examples of the alkylphenyl group include mono- or tri-C phenyl groups such as methylphenyl (or tolyl) and dimethylphenyl (or xylyl). 1-4 Alkyl-phenyl.
[0138] Examples of the aralkyl group include C 6-10 Aryl-C 1-4 alkyl.
[0139] As the base [-OR A ], for example, alkoxy, cycloalkoxy, aryloxy, aralkyloxy, etc., specifically, hydrocarbon group R A The examples correspond to the groups.
[0140] Examples of the alkoxy group include linear or branched C alkyl groups such as methoxy, ethoxy, propoxy, n-butoxy, isobutoxy, and tert-butoxy. 1-10 Alkoxy.
[0141] Examples of the cycloalkoxy group include C 5-10 Cycloalkoxy.
[0142] Examples of the aryloxy group include C 6-10 Aryloxy.
[0143] Examples of the aralkyloxy group include C 6-10 Aryl-C1-4 Alkoxy.
[0144] As the base [-SR A ], for example, alkylthio, cycloalkylthio, arylthio, aralkylthio, etc., specifically, the hydrocarbon group R A The examples correspond to the groups.
[0145] Examples of the alkylthio group include C 1-6 groups such as methylthio, ethylthio, propylthio, n-butylthio and tert-butylthio. 1-10 Alkylthio.
[0146] Examples of the cycloalkylthio group include C 5-10 Cycloalkylthio.
[0147] Examples of the arylthio group include C 6-10 Arylthio.
[0148] Examples of the aralkylthio group include C 6-10 Aryl-C 1-4 Alkylthio.
[0149] These substituents R 1a and R 1b In the above formula, -R A 、-OR A , acyl, nitro, cyano, substituted amino, more preferably alkyl, alkoxy, further preferably linear or branched C 1-6 Alkyl, methoxy and other linear or branched C 1-4 Alkoxy, particularly preferably a straight-chain or branched C 1-4 In addition, when the group R 1a or R 1b When it is an aromatic group, the group R 1a or R 1b Can be respectively with ring Z 1a or Z 1b Together they form a ring assembly of aromatic hydrocarbon rings.
[0150] Substitution numbers k1 and k2 represent the substituent R 1a and R 1b Relative to the aromatic ring Z 1a and Z 1b The number of substitutions k1 and k2 can be determined based on the number of bonds in the aromatic hydrocarbon ring Z. 1a and Z 1b The preferred ranges of the substitution numbers k1 and k2 are integers of 0 to 7, integers of 0 to 6, integers of 0 to 5, integers of 0 to 4, integers of 0 to 3, integers of 0 to 2, 0 or 1, 0 in stages.
[0151] The substitution numbers k1 and k2 may be the same or different. In addition, when the substitution number k1 or k2 is 2 or more, in the same ring Z 1a or Z 1b substituted with two or more radicals R 1a or R 1b The types of Z may be the same or different. 1a and Z 1b Substituted radical R 1a and R 1b The types of R may be the same or different. 1a and R 1b The substitution position of ring Z is not particularly limited and may be 1a and Z 1b Type to choose from.
[0152] The substitution numbers m1 and m2 represent the group [-Z 1a -(R 1a ) k1 ] and base [-Z 1b -(R 1b ) k2 ](Hereinafter, they are also referred to as "Z-containing 1 The number of substitutions m1 and m2 each independently represents an integer of 0 to 4, preferably an integer of 1 to 3, more preferably 1 or 2, and further preferably 1.
[0153] Furthermore, from the viewpoint of the molar absorption coefficient and the absorption wavelength, at least one of m1 and m2 is preferably an integer greater than or equal to 1, more preferably both are integers greater than or equal to 1, and even more preferably both are 1.
[0154] When m1 or m2 is 2 or more, in the two benzene rings forming the fluorene skeleton, the two or more Z-containing 1 The types of the groups may be the same or different. In addition, among the two benzene rings forming the fluorene skeleton, the Z-containing groups substituted on different benzene rings may be 1 The type of group, i.e., the group [-Z 1a -(R 1a ) k1 ] and base [-Z 1b -(R 1b ) k2 ] may be the same or different.
[0155] 1.1.2. Base R 2a and base R 2b
[0156] R 2a and R 2bEach independently represents a non-reactive substituent or a non-polymerizable substituent bonded to the fluorene ring. Z1 Any substituent other than the group may be used.
[0157] As such a base R 2a and R 2b Examples of the group include hydrocarbon groups such as alkyl groups and cycloalkyl groups (except aryl groups), halogen atoms such as fluorine atoms, chlorine atoms, bromine atoms and iodine atoms, and cyano groups.
[0158] Examples of the alkyl group include linear or branched C alkyl groups such as methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, and tert-butyl. 1-10 Among them, linear or branched C 1-6 Alkyl, more preferably a straight-chain or branched C 1-4 alkyl.
[0159] The substitution numbers n1 and n2 represent the substituent R 2a and R 2b The number of bonds to the fluorene ring. The substituent numbers n1 and n2 each independently represent an integer of 0 to 4, preferably an integer of 0 to 3, more preferably an integer of 0 to 2, further preferably 0 or 1, particularly preferably 0. n1 and n2 may be the same or different.
[0160] When n1 or n2 is 2 or more, in the two benzene rings forming the fluorene skeleton, the plurality of R substituted on the same benzene ring 2a or R 2b The types of R may be the same or different. In addition, in the two benzene rings forming the fluorene skeleton, R substituted on different benzene rings 2a and R 2b The types of R 2a and R 2b The substitution position is not particularly limited as long as it contains Z 1 Substitution may be carried out at a position other than the substitution position of the group.
[0161] Each of m1+n1 and m2+n2 is, for example, an integer of 0 to 4, preferably an integer of 1 to 3, more preferably 1 or 2, and further preferably 1. m1+n1 and m2+n2 may be the same as or different from each other.
[0162] 1.1.3. Base Y 1a He JiY 1b
[0163] Y 1a and Y 1b Each of Y is independently a group bonded to the five-membered ring in the fluorene ring, more specifically, to the carbon at the 9-position.1a and Y 1b It may be a carboxyl group, a hydroxyl group, or a reactive substituent or a polymerizable substituent having a polymerizable double bond. 1a and Y 1b , are not particularly limited, and examples thereof include the following formula (Y1), the following formula (Y2), the following formula (Y3), and the following formula (Y4).
[0164] 1.1.3.1. Formula (Y1): dicarboxylic acid and its derivatives
[0165] The formula (Y1) is shown below. 1a and Y 1b When represented by the formula (Y1), the fluorene compound of the present embodiment may be dicarboxylic acid and its derivatives.
[0166] [Chemical formula 7]
[0167]
[0168] (In the formula, A 1 represents a straight-chain or branched alkylene group. )
[0169] Examples of the dicarboxylic acid derivatives include ester-forming derivatives such as alkyl esters of the formula (Y1) (for example, lower alkyl esters such as methyl ester and ethyl ester), acid halides (for example, acid chlorides), and acid anhydrides.
[0170] As A 1 Examples of the linear or branched alkylene group include a methylene group, an ethylene group, a propylene group, a trimethylene group, a 1,2-butanediyl group, a 1,3-butanediyl group, a tetramethylene group, and the like. 1-6 Alkylene.
[0171] A 1 The carbon number of is preferably 1-10, more preferably 1-6, and further preferably 1-4.
[0172] By using such A 1 It has excellent ultraviolet absorption of UV-A or UV-B and can specifically absorb only ultraviolet rays of a specific wavelength. In addition, the compatibility with other resins to be mixed tends to be further improved.
[0173] As Y 1a and Y 1bRepresentative compounds of the above dicarboxylic acids and their derivatives represented by formula (Y1) are not particularly limited, and examples thereof include 9,9-bis(2-carboxyethyl)fluorene, 9,9-bis(2-carboxypropyl)fluorene, 9,9-bis(carboxy C4-6alkyl)fluorene, 9,9-bis(2-carboxyethyl)2,7-diphenylfluorene, 9,9-bis(2-carboxypropyl)2,7-diphenylfluorene, 9,9-bis(carboxy C4-6alkyl)2,7-diphenylfluorene, 9,9-bis(2-carboxyethyl)2,7-di(2-naphthyl)fluorene, 9,9-bis(2-carboxypropyl)2,7-di(2-naphthyl)fluorene, 9,9-bis(carboxy C4-6 alkyl)2,7-di(2-naphthyl)fluorene, 9,9-bis(2-carboxyethyl)2,7-di(1-naphthyl)fluorene, 9,9-bis(2-carboxypropyl)2,7-di(1-naphthyl)fluorene, 9,9-bis(carboxy C4-6 alkyl)2,7-di(1-naphthyl)fluorene. The fluorene dicarboxylic acid component may be used alone or in combination of two or more.
[0174] 1.1.3.2. Formula (Y2): diol
[0175] The following formula (Y2) is shown below. 1a and Y 1b When represented by the formula (Y2), the fluorene compound of this embodiment may be a diol.
[0176] [Chemical formula 8]
[0177]
[0178] (In the formula, A 2 and A 3 Each independently represents a linear or branched alkylene group, and p represents an integer greater than 0.)
[0179] As a 2 and A 3 Examples of the linear or branched alkylene group represented by include linear or branched C1-6 alkylene groups such as methylene, ethylene, propylene, trimethylene, 1,2-butanediyl, 1,3-butanediyl, and tetramethylene. Among them, ethylene and propylene are preferred, and ethylene is particularly preferred.
[0180] A 2 and A 3 The carbon number of is preferably 1-6, more preferably 2-6, and further preferably 2-3.
[0181] By using such A 2 and A 3 It has excellent ultraviolet absorption of UV-A or UV-B and can specifically absorb only ultraviolet rays of a specific wavelength. In addition, the compatibility with other resins to be mixed tends to be further improved.
[0182] Oxyalkylene-(A 3 The repetition number p of (poly)oxyalkylene-(A)- is an integer greater than or equal to 0, and can be selected, for example, from a range of about 0 to 20, and preferably ranges are 0 to 15, 0 to 10, 0 to 8, 0 to 5, 0 to 3, 0 to 2, 0 to 1, and particularly 0. The repetition number p may be an average value (or arithmetic mean, arithmetic mean), that is, an average number of added moles, and its range including preferred embodiments is the same as the range of the integer. When p is 2 or greater, (poly)oxyalkylene-(A)- 3 O) p -2 or more A's 3 The types may be the same or different, but are preferably the same.
[0183] In addition, Y 1a and Y 1b The total number of the repetition number p in the formula (1), that is, the total number of oxyalkylene groups in one molecule of the diol compound represented by the formula (1) (or the average value of the total number of added moles) [hereinafter, also referred to as the total number of p] can be selected, for example, from a range of about 0 to 30, and the preferred range is 0 to 20, 0 to 10, 0 to 6, 0 to 4, 0 to 2 in stages, more preferably 0 to 1, and particularly preferably 0. The total number of p may be an integer or the average value of the total number of moles.
[0184] As Y 1a and Y 1b Representative compounds of the above diols represented by formula (Y2) are not particularly limited, and examples thereof include: m1 and m2 are 1, Z 1a , Z 1b They are benzene ring, naphthalene ring, biphenyl ring, etc. 6-12 Aromatic ring, A 2 Straight or branched chain C 1-6 Alkylene, A 3 Straight or branched chain C 2-4 Alkylene, diol compounds wherein p is 0 or 1 to 10, etc.; preferably, m1 and m2 are 1, Z 1a , Z 1b benzene ring or naphthalene ring, A 2 Straight or branched chain C 1-4 Alkylene, A 3 It is a straight-chain or branched C 2-3 Alkylene, diol compounds wherein p is 0 or 1 to 6, and the like.
[0185] In addition, it is more preferred that m1 and m2 are 1, Z 1a , Z 1b are naphthalene ring, A 2 Straight or branched chain C2-4 Alkylene, A 3 It is a diol compound wherein ethylene is present and p is 0 or 1.
[0186] Among them, 9,9-bis(3-hydroxypropyl)-di(1-naphthyl)fluorene, 9,9-bis(3-hydroxypropyl)-di(2-naphthyl)fluorene and the like 9,9-bis(3-hydroxypropyl)-dinaphthylfluorene are preferred; and 9,9-bis(3-hydroxypropyl)-2,7-di(2-naphthyl)fluorene and the like 9,9-bis(3-hydroxypropyl)-2,7-dinaphthylfluorene are particularly preferred.
[0187] 1.1.3.3. Formula (Y3): diol
[0188] The following shows Y 1a and Y 1b In Y 1a and Y 1b When represented by the formula (Y3), the fluorene compound of this embodiment may be a diol.
[0189] [Chemical formula 9]
[0190]
[0191] (Where Z 2 Represents an aromatic hydrocarbon ring, A 4 Each independently represents a linear or branched alkylene group, R 3 Each independently represents a substituent, q represents an integer greater than 0, r represents an integer greater than 1, and s represents an integer greater than 0.)
[0192] In formula (Y3), Z 2 The aromatic hydrocarbon ring represented by may include monocyclic aromatic hydrocarbon rings such as benzene ring, condensed polycyclic aromatic hydrocarbon rings (condensed polycyclic aromatic hydrocarbon rings), ring-aggregated aromatic hydrocarbon rings (ring-aggregated polycyclic aromatic hydrocarbon rings), etc. Among them, condensed polycyclic aromatic hydrocarbon rings are preferred from the viewpoint of the molar absorption coefficient in the UV-A region.
[0193] The condensed polycyclic aromatic hydrocarbon ring is not particularly limited, and examples thereof include naphthalene ring, indene ring, azulene ring, anthracene ring, phenanthrene ring, tetracene ring, pentacene ring, benzopyrene ring, chrysene ring, dibenzochrysene ring, pyrene ring, triphenylene ring, corannulene ring, coronene ring, and ovalbenzene ring, etc. Among them, the naphthalene ring is preferred.
[0194] The ring-aggregated aromatic hydrocarbon ring is not particularly limited, and examples thereof include biphenyl rings, phenylnaphthalene rings, binaphthyl rings and other biaryl hydrocarbon rings; teraryl hydrocarbon rings such as terphenyl rings and other terphenyl rings, etc. Among them, a biphenyl ring is preferred.
[0195] Aromatic ring Z 2 The substituent R may be non-reactive or non-polymerizable 3 As a substituent R 3, examples thereof include hydrocarbon groups such as an alkyl group, halogen atoms such as a fluorine atom, a chlorine atom, and a bromine atom, and a cyano group.
[0196] Examples of the alkyl group include linear or branched C alkyl groups such as methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, and tert-butyl. 1-10 Among them, linear or branched C 1-6 Alkyl, more preferably a straight-chain or branched C 1-4 alkyl.
[0197] The number of substitutions s represents the substituent R 3 Relative to the aromatic ring Z 2 The substitution number s is, for example, an integer of 0 to 4, preferably an integer of 0 to 2, more preferably 0 or 1, particularly 0. 3 The substitution position is not particularly limited as long as the group [-(OA 4 ) q The substitution position of the amine group may be other than the substitution position of the amine group.
[0198] As a 4 Examples of the linear or branched alkylene group include a methylene group, an ethylene group, a propylene group, a trimethylene group, a 1,2-butanediyl group, a 1,3-butanediyl group, a tetramethylene group, and the like. 1-6 Among them, the preferred alkylene group A 4 Straight or branched chain C 2-6 Alkylene, more preferably linear or branched C 2-3 Among the alkylene groups, ethylene and propylene are preferred, and ethylene is particularly preferred.
[0199] As oxyalkylene-(OA 4 The preferred range of the number of repetitions q of (poly)oxyalkylene-(OA)- is 0 to 20, 0 to 15, 0 to 10, 0 to 8, 0 to 5, 0 to 3, 0 to 2, 0 to 1, and 0 in stages. In addition, the number of repetitions q may be an average value (or an arithmetic mean value), that is, an average number of added moles, and its range is the same as the range of the integers including the preferred embodiment. When q is 2 or more, (poly)oxyalkylene-(OA 4 ) q -2 or more A's 4 The types may be different from each other, but are preferably the same.
[0200] In addition, Y 1a and Y 1bThe total number of the repetition number q in the formula (1), that is, the total number of oxyalkylene groups in one molecule of the diol compound represented by the formula (1) (or the average value of the total number of added moles) [hereinafter, also referred to as the total number of q] can be selected, for example, from the range of about 0 to 30. The preferred range is 0 to 20, 0 to 10, 0 to 6, 0 to 4, 0 to 2, more preferably 0 to 1, and particularly preferably 0. The total number of q may be an integer or the average value of the total number of moles.
[0201] The number of substitutions r represents the group [-(OA 4 ) q -OH] relative to the aromatic ring Z 2 The number of substitutions r is, for example, an integer of 1 to 4, preferably an integer of 1 to 2, and more preferably 1. 4 ) q The substitution position of -OH is not particularly limited as long as 3 It can be replaced at any position other than the replacement position.
[0202] As Y 1a and Y 1b Representative compounds of the above diols represented by formula (Y3) are not particularly limited, and examples thereof include: m1 and m2 are 0 or 1, Z 1a , Z 1b , Z 2 They are benzene ring, naphthalene ring, biphenyl ring, etc. 6-12 Aromatic ring, A 4 Straight or branched chain C 2-4 Alkylene, diol compounds wherein q is 0 or 1 to 10, etc.; preferably, m1 and m2 are 0 or 1, Z 1a , Z 1b , Z 2 benzene ring or naphthalene ring, A 4 It is a straight-chain or branched C 2-3 Alkylene, diol compounds wherein q is 0 or 1 to 6, and the like.
[0203] Among them, 9,9-bis[hydroxy(poly)alkoxyphenyl]fluorene represented by 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene, 9,9-bis[4-(2-(2-hydroxyethoxy)ethoxy)phenyl]fluorene, 9,9-bis[4-(2-hydroxypropoxy)phenyl]fluorene, or 9,9-bis[6-(2-hydroxyethoxy)-2-naphthyl]fluorene, 9,9-bis[5-(2-hydroxyethoxy)-1-naphthyl]fluorene, 9,9-bis[6-(2-(2-hydroxyethoxy)ethoxy)-2-naphthyl]fluorene, 9,9-bis[6-(2-hydroxypropoxy)-2-naphthyl]fluorene, etc. are preferred.
[0204] 1.1.3.4. Formula (Y4): di(meth)acrylate
[0205] The following formula (Y4) is shown below. 1a and Y 1b When represented by the formula (Y4), the fluorene compound of the present embodiment may be a di(meth)acrylate.
[0206] [Chemical formula 10]
[0207]
[0208] (In the formula, A 5 and A 6 Each independently represents a linear or branched alkylene group, R 4 represents a hydrogen atom or a methyl group, and t represents an integer greater than 0. )
[0209] As a 5 and A 6 Examples of the linear or branched alkylene group include a methylene group, an ethylene group, a propylene group, a trimethylene group, a 1,2-butanediyl group, a 1,3-butanediyl group, a tetramethylene group, and the like. 1-6 Among them, the preferred alkylene group A 5 and A 6 Straight or branched chain C 2-6 Alkylene, more preferably linear or branched C 2-3 Among the alkylene groups, ethylene and propylene are preferred, and ethylene is particularly preferred.
[0210] The repetition number t of the oxyalkylene group -(A6O)- can be selected, for example, from a range of about 0 to 20, and as a preferred range, it is stepwise selected from 0 to 15, 0 to 10, 0 to 8, 0 to 5, 0 to 3, 0 to 2, 0 to 1, and particularly 0. In addition, the repetition number t may be an average value (or an arithmetic mean value, an arithmetic mean value), that is, an average number of added moles, and its range including the preferred embodiment is the same as the range of the integer. When t is 2 or more, the (poly)oxyalkylene group -(A6O)- 6 O) t -2 or more A's 6 The types may be different from each other, but are preferably the same.
[0211] R 4 The substituent represented by is a hydrogen atom or a methyl group. When the ultraviolet absorber of the present embodiment is used after radical polymerization, a hydrogen atom is preferred from the viewpoint of excellent reactivity with radicals.
[0212] As Y 1a and Y1b Representative compounds of the above di(meth)acrylates represented by formula (Y4) are not particularly limited, and examples thereof include 9,9-bis((meth)acryloyl)fluorene, 9,9-bis((meth)acryloyloxyethyl)fluorene, 9,9-bis((meth)acryloyloxymethyl)fluorene, 9,9-bis((meth)acryloyloxypropyl)2,7-diphenylfluorene, and 9,9-bis((meth)acryloyloxypropyl)2,7-di(2-naphthyl)fluorene. The di(meth)acrylate components may be used alone or in combination of two or more.
[0213] 1.2. Resin
[0214] Next, a resin containing a fluorene compound represented by the general formula (1) as a constituent unit (hereinafter, also referred to as "constituent unit F") is described in detail. The resin of this embodiment has excellent absorptivity to UV-A or UV-B and can specifically absorb only ultraviolet rays of a specific wavelength by containing a fluorene compound represented by the general formula (1) as a constituent unit.
[0215] The resin of the present embodiment is not particularly limited, and examples thereof include polyester resins, polycarbonate resins, polyamide resins, and acrylic resins. Each resin will be described in detail below, but the resin of the present embodiment is not limited to the following as long as it contains structural unit F.
[0216] 1.2.1. Polyester resin
[0217] The polyester resin is formed by stepwise polymerization of a diol and a dicarboxylic acid to form an ester bond, and contains at least one or both of a diol and a dicarboxylic acid as a structural unit F derived from a fluorene compound represented by the general formula (1). Thus, in order to distinguish it from other polyester resins, the polyester resin containing the structural unit F is also called a "ultraviolet absorbing polyester resin".
[0218] The content of the structural unit F contained in the ultraviolet absorbing polyester resin is preferably 1 to 100 mol%, more preferably 5 to 80 mol%, and further preferably 10 to 60 mol% relative to all structural units in terms of molar ratio. When the content ratio of the structural unit F is within the above range, the ultraviolet absorbing property and the absorption specificity of ultraviolet rays of a specific wavelength tend to be further improved.
[0219] 1.2.1.1. Diol component
[0220] The diol components of the ultraviolet absorbing polyester resin may all be constituent units F, or may be a combination of constituent units F of the diol component and other diol components. The constituent units F of the diol component are not particularly limited, and examples thereof include: 1a and Y 1bIn the case of the diol represented by the formula (Y2), the constituent unit derived from 1a and Y 1b Structural unit of diol in the case of being represented by formula (Y3) These diols may be used alone or in combination of two or more.
[0221] The other diol components are not particularly limited, and examples thereof include at least one diol component selected from the group consisting of aliphatic diols, alicyclic diols, and aromatic diols.
[0222] Examples of the aliphatic diol include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, neopentyl glycol, and 1,6-hexanediol. 2-8 Alkane diols, polyalkane diols (e.g., diethylene glycol, dipropylene glycol, triethylene glycol, etc., di- or tri-C 2-4 Among them, ethylene glycol is particularly preferred from the viewpoint of improving mechanical properties such as elongation at break and flexibility.
[0223] Examples of the alicyclic diol include cycloalkane diols such as cyclohexanediol; bis(hydroxyalkyl)cycloalkanes such as cyclohexanedimethanol; hydrogenated products of aromatic diols such as bisphenol A and the like, which are exemplified below.
[0224] Examples of the aromatic diol include dihydroxy aromatic hydrocarbons such as hydroquinone and resorcinol; aromatic aliphatic diols such as benzyl alcohol; bisphenols such as bisphenol A, bisphenol F, bisphenol AD, bisphenol C, bisphenol G, and bisphenol S; and biphenols such as p,p′-biphenol.
[0225] Other diol components may be used alone or in combination of two or more.
[0226] 1.2.1.2. Dicarboxylic acids
[0227] The dicarboxylic acid components of the ultraviolet absorbing polyester resin may all be constituent units F, or may be a combination of constituent units F of dicarboxylic acid components and other dicarboxylic acid components. The constituent units F of dicarboxylic acid components are not particularly limited, and examples thereof include: 1a and Y 1b Structural unit of dicarboxylic acid when represented by formula (Y1) These dicarboxylic acids may be used alone or in combination of two or more.
[0228] The other dicarboxylic acid components are not particularly limited, and examples thereof include at least one dicarboxylic acid component selected from the group consisting of aliphatic dicarboxylic acids, alicyclic dicarboxylic acids, and aromatic dicarboxylic acids.
[0229] The aliphatic dicarboxylic acid is not particularly limited, and examples thereof include alkane dicarboxylic acids (for example, succinic acid, adipic acid, sebacic acid, decanedicarboxylic acid, etc.) 4-14 Alkanedicarboxylic acids, preferably C 6-12 Alkanedicarboxylic acids, etc.), unsaturated aliphatic dicarboxylic acids (e.g., maleic acid, fumaric acid, itaconic acid, etc.) 2-10 Alkene-dicarboxylic acids, etc.) etc. Preferred aliphatic dicarboxylic acids are alkane dicarboxylic acids.
[0230] The alicyclic dicarboxylic acid component is not particularly limited, and examples thereof include cycloalkane dicarboxylic acids (for example, C cyclohexane dicarboxylic acid such as 1,3-cyclohexane dicarboxylic acid and 1,4-cyclohexane dicarboxylic acid). 5-10 cycloalkane dicarboxylic acids, etc.), di- or tri-cycloalkane dicarboxylic acids (e.g., decahydronaphthalene dicarboxylic acid, norbornane dicarboxylic acid, adamantane dicarboxylic acid, tricyclodecane dicarboxylic acid, etc.), cycloolefin dicarboxylic acids (e.g., cyclohexene dicarboxylic acid, etc.), 5-10 Cycloolefin-dicarboxylic acids), di- or tri-cycloolefin dicarboxylic acids (e.g., norbornene dicarboxylic acid, etc.), and the like.
[0231] The aromatic dicarboxylic acid component is not particularly limited, and examples thereof include monocyclic aromatic dicarboxylic acids [e.g., phthalic acid, terephthalic acid, isophthalic acid, alkylisophthalic acids (e.g., 4-methylisophthalic acid, etc.) 1-4 Alkyl isophthalic acid, etc. 6-10 Aromatic dicarboxylic acids, etc.], condensed polycyclic aromatic dicarboxylic acids [for example, naphthalene dicarboxylic acid (for example, 1,5-naphthalene dicarboxylic acid, 1,6-naphthalene dicarboxylic acid, 1,7-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, etc.), anthracene dicarboxylic acid, phenanthrene dicarboxylic acid, etc.] 10-24 Aromatic hydrocarbon-dicarboxylic acid, preferably condensed polycyclic C 10-16 Aromatic hydrocarbon-dicarboxylic acid, preferably condensed polycyclic C 10-14 arene-dicarboxylic acids, etc.], aryl arene dicarboxylic acids [for example, biphenyl dicarboxylic acid (for example, 2,2'-biphenyl dicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, etc.) 6-10 Aryl-C 6-10 arene dicarboxylic acids, etc.], diarylalkane dicarboxylic acids [for example, diphenylalkane dicarboxylic acids (for example, 4,4'-diphenylmethane dicarboxylic acid, etc.) and diC 6-10 Aryl C 1-6 Alkane-dicarboxylic acids, etc.], diaryl ketone dicarboxylic acids [for example, diphenyl ketone dicarboxylic acid (for example, 4,4'-diphenyl ketone dicarboxylic acid, etc.) and the like diC 6-10 Aryl ketone-dicarboxylic acid) etc.] etc.
[0232] Furthermore, the dicarboxylic acid component contained in the ultraviolet absorbing polyester resin is not limited to free carboxylic acid, but also includes ester-forming derivatives of dicarboxylic acid, such as esters [e.g., alkyl esters [e.g., lower alkyl esters such as methyl ester and ethyl ester (e.g., C 1-4 Alkyl esters, especially C 1-2 Alkyl esters) etc.] etc.], acid halides (for example, acid chlorides etc.), acid anhydrides etc. These dicarboxylic acid components may be used alone or in combination of two or more.
[0233] 1.2.1.3. Preparation method of polyester resin
[0234] The ultraviolet absorbing polyester resin can be prepared by the reaction of a dicarboxylic acid component and a diol component. The method for preparing the polyester resin is not particularly limited, and the polyester resin can be prepared by conventional methods, such as melt polymerization methods such as an ester exchange method and a direct polymerization method, a solution polymerization method, an interfacial polymerization method, etc. In the polymerization reaction, an ester exchange catalyst, a polycondensation catalyst, a heat stabilizer, a light stabilizer, a polymerization regulator, etc. can be used.
[0235] The transesterification catalyst is not particularly limited, and examples thereof include compounds (alkoxides, organic acid salts, inorganic acid salts, metal oxides, etc.) of alkaline earth metals (magnesium, calcium, barium, etc.), transition metals (manganese, zinc, cobalt, titanium, etc.), etc. Among them, manganese acetate, calcium acetate, etc. can be preferably used.
[0236] There is no particular limitation on the type of polycondensation catalyst, and examples thereof include compounds of alkaline earth metals, transition metals, metals of Group 13 of the periodic table (aluminum, etc.), metals of Group 14 of the periodic table (germanium, etc.), and metals of Group 15 of the periodic table (antimony, etc.). More specifically, examples thereof include germanium compounds such as germanium dioxide, germanium hydroxide, germanium oxalate, germanium tetraethanol, and germanium n-butoxide, antimony compounds such as antimony trioxide, antimony acetate, and antimony glycol, tetra-n-propyl titanate, tetra-isopropyl titanate, tetra-n-butyl titanate, titanium oxalate, and titanium compounds such as potassium titanium oxalate. These catalysts may be used alone or in combination of two or more.
[0237] The heat stabilizer is not particularly limited, and examples thereof include phosphorus compounds such as trimethyl phosphate, triethyl phosphate, triphenyl phosphate, phosphorous acid, trimethyl phosphite, and triethyl phosphite.
[0238] In the reaction, the ratio of the dicarboxylic acid component to the diol component can be selected from the same range as above, and a predetermined component can be used in excess as needed. For example, a diol component such as ethylene glycol that can be distilled from the reaction system can be used in excess of the ratio of the unit introduced into the polyester resin. In addition, the reaction can be carried out in the presence or absence of a solvent.
[0239] The reaction can be carried out in an inert gas environment (nitrogen, helium, etc.). Alternatively, the reaction can be carried out under reduced pressure (e.g., 1×102 ~1×10 4 The reaction temperature can be selected according to the polymerization method. For example, the reaction temperature in the melt polymerization method can be 150 to 300°C, preferably 180 to 290°C, and more preferably about 200 to 280°C.
[0240] 1.2.1.3. Physical properties of polyester resin
[0241] The glass transition temperature of the ultraviolet absorbing polyester resin is preferably 90 to 190° C., more preferably 100 to 180° C., and even more preferably 110 to 170° C. When the glass transition temperature is 90° C. or higher, the heat resistance of the ultraviolet absorbing polyester resin tends to be further improved. In addition, when the glass transition temperature is 190° C. or lower, the stretchability of the ultraviolet absorbing polyester resin tends to be further improved. The glass transition temperature can be measured by the method described in the examples described later.
[0242] The weight average molecular weight of the ultraviolet absorbing polyester resin is preferably 30,000 to 200,000, more preferably 35,000 to 150,000, and further preferably 40,000 to 110,000. When the weight average molecular weight is within the above range, the molecular chain length, mechanical properties such as elongation at break and flexibility of the ultraviolet absorbing polyester resin tend to be further improved, and the stretchability tends to be further improved. In addition, the weight average molecular weight in this embodiment can be measured by gel permeation chromatography (GPC) by polystyrene conversion. More specifically, it can be measured by the method described in the embodiments described later.
[0243] 1.2.2. Polycarbonate resin
[0244] The polycarbonate resin is obtained by stepwise polymerization of a diol and phosgene to form a carbonate group, and at least a part of the diol has a structural unit F derived from a fluorene compound represented by the general formula (1). In this way, in order to distinguish it from other polycarbonates, the polycarbonate resin containing the structural unit F is also called "ultraviolet absorbing polycarbonate resin".
[0245] The molar ratio of the structural unit F contained in the ultraviolet absorbing polycarbonate resin to the total diol units is preferably 1 to 100 mol%, more preferably 5 to 80 mol%, and further preferably 10 to 60 mol%. When the content ratio of the ultraviolet absorber is within the above range, the ultraviolet absorbency and the absorption specificity of ultraviolet rays of a specific wavelength tend to be further improved.
[0246] 1.2.2.1. Diols
[0247] The diol components of the ultraviolet absorbing polycarbonate resin may all be structural units F, or may be a combination of structural units F of the diol component and other diol components. The structural units F of the diol component are not particularly limited, and examples thereof include: 1a and Y 1b In the case of the diol represented by the formula (Y2), the constituent unit derived from 1a and Y 1b Structural unit of diol in the case of being represented by formula (Y3) These diols may be used alone or in combination of two or more.
[0248] The other diol components are not particularly limited, and examples thereof include at least one diol component selected from the group consisting of aliphatic diols, alicyclic diols, and aromatic diols.
[0249] Examples of the aliphatic diol include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol and other C2-8 alkane diols, polyalkane diols (for example, diethylene glycol, dipropylene glycol, triethylene glycol and other di- or tri-C2-4 alkane diols, etc.), and the like. Among them, ethylene glycol is particularly preferred from the viewpoint of being able to improve mechanical properties such as elongation at break and flexibility.
[0250] Examples of the alicyclic diol include cycloalkane diols such as cyclohexanediol; bis(hydroxyalkyl)cycloalkanes such as cyclohexanedimethanol; hydrogenated products of aromatic diols such as bisphenol A and the like, which are exemplified below.
[0251] Examples of the aromatic diol include dihydroxy aromatic hydrocarbons such as hydroquinone and resorcinol; aromatic aliphatic diols such as benzyl alcohol; bisphenols such as bisphenol A, bisphenol F, bisphenol AD, bisphenol C, bisphenol G, and bisphenol S; and biphenols such as p,p′-biphenol.
[0252] The other diol components may be used alone or in combination of two or more.
[0253] 1.2.2.2. Preparation method of polycarbonate resin
[0254] The ultraviolet absorbing polycarbonate resin can be produced by reacting (polymerizing or condensing) a diol component with phosgene or a carbonic acid diester (such as diphenyl carbonate) using a conventional method, such as a phosgene method (solvent method) or an ester exchange method (melting method). The diol component may contain other diol components as required, as long as it contains at least the ultraviolet light absorber represented by the general formula (1). Among these methods, the ester exchange method is preferred from the perspective of not requiring a solvent, etc.
[0255] In the transesterification method, the ratio of the carbonic acid diester to 1 mol of the diol component may be, for example, about 0.8 to 1.5 mol, preferably about 0.9 to 1.2 mol.
[0256] The transesterification reaction can be carried out in the presence of a catalyst. Examples of the catalyst include various catalysts used in transesterification reactions, such as nitrogen-containing compounds and metal compounds.
[0257] Examples of the nitrogen-containing compound include quaternary ammonium hydroxides (e.g., tetraalkylammonium hydroxides such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, and tetrabutylammonium hydroxide; trialkyl-aralkylammonium hydroxides such as trimethylbenzylammonium hydroxide; and the like); tertiary amines (trialkylamines such as trimethylamine and triethylamine; dimethyl-aralkylamines such as dimethylbenzylamine; triarylamines such as triphenylamine; and the like).
[0258] As the metal compound, for example, a metal compound containing a metal such as an alkali metal (sodium, etc.), an alkaline earth metal (magnesium, calcium, barium, etc.), a transition metal (manganese, zinc, cadmium, lead, cobalt, titanium, etc.), a metal of Group 13 of the Periodic Table (aluminum, etc.), a metal of Group 14 of the Periodic Table (germanium, etc.), a metal of Group 15 of the Periodic Table (antimony, etc.) is used. More specifically, for example, alkoxides, organic acid salts (acetates, propionates, etc.), inorganic acid salts (borates, carbonates, etc.), oxides, hydroxides, etc. of the above metals are listed.
[0259] These catalysts can be used alone or in combination of two or more. Among these catalysts, nitrogen-containing compounds such as quaternary ammonium hydroxides are preferred, and tetraalkylammonium hydroxides such as tetramethylammonium hydroxide are preferred. For example, the amount of the catalyst used can be 0.01×10 -4 ~100×10 -4 mole, preferably 0.1×10 -4 ~40×10 -4 Moore or so.
[0260] Furthermore, the reaction may be carried out in the presence of additives such as stabilizers (antioxidants, heat stabilizers, etc.), as necessary.
[0261] The reaction can usually be carried out in an inert gas (nitrogen; rare gases such as helium and argon). Alternatively, the reaction can also be carried out under reduced pressure (e.g., 1×10 2 ~1×10 4 The reaction temperature can be selected according to the polymerization method. For example, the reaction temperature in the transesterification method can be, for example, 150 to 320° C., preferably 200 to 310° C., and more preferably about 250 to 300° C. In particular, when diphenyl carbonate is used as the carbonic acid diester, it is effective to carry out the polycondensation while distilling off phenol at a high temperature and under reduced pressure.
[0262] 1.2.2.3. Physical properties of polycarbonate resin
[0263] The glass transition temperature of the ultraviolet absorbing polycarbonate resin is preferably 90 to 190° C., more preferably 100 to 180° C., and further preferably 110 to 170° C. When the glass transition temperature is 90° C. or higher, the heat resistance of the ultraviolet absorbing polycarbonate resin tends to be further improved. In addition, when the glass transition temperature is 190° C. or lower, the stretchability of the ultraviolet absorbing polycarbonate resin tends to be further improved. The glass transition temperature can be measured by the method described in the examples described later.
[0264] The weight average molecular weight of the ultraviolet absorbing polycarbonate resin is preferably 30000 to 200000, more preferably 35000 to 150000, and further preferably 40000 to 110000. When the weight average molecular weight is within the above range, the molecular chain length, mechanical properties such as elongation at break and flexibility of the ultraviolet absorbing polycarbonate resin tend to be further improved, and the stretchability tends to be further improved. In addition, in the present embodiment, the weight average molecular weight can be measured by gel permeation chromatography (GPC) by polystyrene conversion. More specifically, it can be measured by the method described in the embodiments described later.
[0265] 1.2.3. Polyamide resin
[0266] The polyamide resin is obtained by stepwise polymerization of a diamine and a dicarboxylic acid to form an amide bond, and at least a part of the dicarboxylic acid has a structural unit F derived from a fluorene compound represented by the general formula (1). In this way, in order to distinguish it from other polyamides, the polyamide resin containing the structural unit F is also called a "ultraviolet absorbing polyamide resin".
[0267] The molar ratio of the structural unit F contained in the ultraviolet absorbing polyamide resin to the total dicarboxylic acid units is preferably 1 to 100 mol%, more preferably 5 to 80 mol%, and still more preferably 10 to 60 mol%. When the content ratio of the ultraviolet absorber is within the above range, the ultraviolet absorbency and the absorption specificity of ultraviolet rays of a specific wavelength tend to be further improved.
[0268] 1.2.3.1. Dicarboxylic acids
[0269] The dicarboxylic acid components of the ultraviolet absorbing polyamide resin may all be structural units F, or structural units F that are dicarboxylic acid components may be a combination of structural units F and other dicarboxylic acid components. The structural units F that are dicarboxylic acid components are not particularly limited, and examples thereof include: 1a and Y 1b Structural unit of dicarboxylic acid when represented by formula (Y1) These dicarboxylic acids may be used alone or in combination of two or more.
[0270] The other dicarboxylic acid components are not particularly limited, and examples thereof include at least one dicarboxylic acid component selected from the group consisting of aliphatic dicarboxylic acids, alicyclic dicarboxylic acids, and aromatic dicarboxylic acids.
[0271] The aliphatic dicarboxylic acid is not particularly limited, and examples thereof include alkane dicarboxylic acids (for example, succinic acid, adipic acid, sebacic acid, decanedicarboxylic acid, etc.) 4-14 Alkanedicarboxylic acids, preferably C 6-12 Alkanedicarboxylic acids, etc.), unsaturated aliphatic dicarboxylic acids (e.g., maleic acid, fumaric acid, itaconic acid, etc.) 2-10 Alkene-dicarboxylic acids, etc.) etc. Preferred aliphatic dicarboxylic acids are alkane dicarboxylic acids.
[0272] The alicyclic dicarboxylic acid component is not particularly limited, and examples thereof include cycloalkane dicarboxylic acids (for example, C cyclohexane dicarboxylic acid such as 1,3-cyclohexane dicarboxylic acid and 1,4-cyclohexane dicarboxylic acid). 5-10 cycloalkane dicarboxylic acids, etc.), di- or tri-cycloalkane dicarboxylic acids (e.g., decahydronaphthalene dicarboxylic acid, norbornane dicarboxylic acid, adamantane dicarboxylic acid, tricyclodecane dicarboxylic acid, etc.), cycloolefin dicarboxylic acids (e.g., cyclohexene dicarboxylic acid, etc.), 5-10 Cycloolefin-dicarboxylic acids), di- or tri-cycloolefin dicarboxylic acids (e.g., norbornene dicarboxylic acid, etc.), and the like.
[0273] The aromatic dicarboxylic acid component is not particularly limited, and examples thereof include monocyclic aromatic dicarboxylic acids [e.g., phthalic acid, terephthalic acid, isophthalic acid, alkylisophthalic acids (e.g., 4-methylisophthalic acid, etc.) 1-4 Alkyl isophthalic acid, etc. 6-10 Aromatic dicarboxylic acids, etc.], condensed polycyclic aromatic dicarboxylic acids [for example, naphthalene dicarboxylic acid (for example, 1,5-naphthalene dicarboxylic acid, 1,6-naphthalene dicarboxylic acid, 1,7-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, etc.), anthracene dicarboxylic acid, phenanthrene dicarboxylic acid, etc.] 10-24 Aromatic hydrocarbon-dicarboxylic acid, preferably condensed polycyclic C 10-16 Aromatic hydrocarbon-dicarboxylic acid, preferably condensed polycyclic C 10-14 arene-dicarboxylic acids, etc.], aryl arene dicarboxylic acids [for example, biphenyl dicarboxylic acid (for example, 2,2'-biphenyl dicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, etc.) 6-10 Aryl-C 6-10 arene dicarboxylic acids, etc.], diarylalkane dicarboxylic acids [for example, diphenylalkane dicarboxylic acids (for example, 4,4'-diphenylmethane dicarboxylic acid, etc.) and diC 6-10 Aryl C 1-6Alkane-dicarboxylic acids, etc.], diaryl ketone dicarboxylic acids [for example, di-6-10 aryl ketone-dicarboxylic acids such as diphenyl ketone dicarboxylic acids (for example, 4,4'-diphenyl ketone dicarboxylic acid, etc.)], etc.
[0274] Furthermore, the dicarboxylic acid component other than the ultraviolet absorber contained in the ultraviolet absorbing polyamide resin is not limited to free carboxylic acid, but also includes ester-forming derivatives of dicarboxylic acid, such as esters [e.g., alkyl esters [e.g., lower alkyl esters such as methyl ester and ethyl ester (e.g., C 1-4 Alkyl esters, especially C 1-2 Alkyl esters) etc.] etc.], acid halides (for example, acid chlorides etc.), acid anhydrides etc. These dicarboxylic acid components may be used alone or in combination of two or more.
[0275] 1.2.3.2. Diamine
[0276] The diamine is not particularly limited, and examples thereof include aliphatic diamines, alicyclic diamines, aromatic diamines, etc. The diamine may be used alone or in combination of two or more.
[0277] Examples of the aliphatic diamine include alkylenediamines (e.g., ethylenediamine, propylenediamine, 1,3-trimethylenediamine, 1,4-tetramethylenediamine, 1,5-pentamethylenediamine, 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 1,10-decamethylenediamine, 1,11-undemethylenediamine, 1,12-dodecamethylenediamine, 2-methyl-1,5-pentamethylenediamine, 2,2,4-trimethyl-1,6-hexamethylenediamine, 2,4,4-trimethyl-1,6-hexamethylenediamine, 2-methyl-1,8-octamethylenediamine, 5-methyl-1,9-nonamethylenediamine, etc.) 2-20 Alkanediamine, preferably C 2-12 Alkanediamine, more preferably C 2-8 The aliphatic diamine may be used alone or in combination of two or more.
[0278] Examples of the alicyclic diamine include monocyclic cycloalkane diamine, crosslinked cycloalkane diamine, isophorone diamine, etc. The alicyclic diamine may be used alone or in combination of two or more.
[0279] Examples of monocyclic cycloalkane diamines include cycloalkane diamines such as diaminocyclohexane (1,4-diaminocyclohexane, etc.) and methylcyclohexane diamine (3-methyl-1,4-diaminocyclohexane, etc.); bis(aminomethyl)cycloalkanes such as bis(aminomethyl)cyclohexane (1,4-aminomethylcyclohexane, etc.) and bis(aminomethyl)methylcyclohexane. Monocyclic cycloalkane diamines are often C 4-10 Cycloalkanediamine, bis(aminomethyl)C 4-10 Cycloalkanes.
[0280] Examples of cross-linked cyclic cycloalkane diamines include bis- or tri-cycloalkane diamines such as bis-cyclooctanediamine, bis-cyclononanediamine, tri-cyclododecanediamine, and norbornanediamine; and bis- or tri-cycloalkanes such as bis-(aminomethyl)bicyclooctane, bis-(aminomethyl)bicyclononane, bis-(aminomethyl)tricyclododecane, and bis-(aminomethyl)norbornane. The cross-linked cyclic cycloalkane diamines are often C 6-14 Bis or triscycloalkanediamine, bis(aminomethyl)C 6-14 Bi- or tricycloalkanes.
[0281] Examples of the aromatic diamine include aromatic diamines (e.g., m-phenylenediamine, p-phenylenediamine, etc.); 6-10 Aromatic diamines), aminoalkyl-aminoaromatics [e.g., amino C1-4 alkyl-amino ... 6-10 aromatic hydrocarbons, etc.], aromatic aliphatic diamines [for example, di(aminoalkyl) aromatic hydrocarbons (for example, di(aminoC1-4alkyl)C1-4alkyl)s such as m-phenylenediamine and p-phenylenediamine 6-10 Aromatic diamines may be used alone or in combination of two or more.
[0282] In addition, the polymerization components of the ultraviolet absorbing polyamide resin may consist only of the above-mentioned dicarboxylic acid components and diamine components, or may contain aminocarboxylic acid components [aminocarboxylic acids (e.g., 6-aminocaproic acid, 12-aminododecanoic acid, etc.), lactams (ε-caprolactam, etc.)] as polymerization components as necessary.
[0283] For example, the ratio of the aminocarboxylic acid component to 1 mol of the dicarboxylic acid component may be 0.5 mol or less, preferably 0.3 mol or less, further preferably 0.2 mol or less, and particularly preferably 0.1 mol or less.
[0284] 1.2.3.3. Preparation method of polyamide resin
[0285] Ultraviolet absorbing polyamide resin can be manufactured by conventional methods. For example, polyamide resin can be manufactured by reacting a dicarboxylic acid component with a diamine component (polymerization or condensation). As a polymerization method (manufacturing method), it can be appropriately selected according to the type of the dicarboxylic acid component used, and conventional methods can be exemplified, such as melt polymerization (or melt polycondensation, a method in which a dicarboxylic acid component and a diamine component are polymerized under melt mixing), solution polymerization (or solution polycondensation), interfacial polymerization (or interfacial polycondensation), etc.
[0286] Specifically, in the melt polycondensation method, raw materials such as salts, dicarboxylic acid components, and diamine components prepared from dicarboxylic acid components and diamine components can be heated to a temperature above their melting point to melt them, and react while removing the disengaged components such as water and alcohol from the reaction system under reduced pressure. In addition, in the solution polycondensation method, the disengaged components can be reacted while being removed in the solvent by azeotropy, acid acceptors such as tertiary amines, and condensing agents such as triphenyl phosphite / pyridine mixed systems. Moreover, in the interfacial polycondensation method, the acyl halide of dicarboxylic acid can be dissolved in a non-polar solvent and reacted with the diamine component at the interface of an aqueous solution of an alkaline compound such as sodium hydroxide.
[0287] In addition, in the melt polycondensation method, the salt of the dicarboxylic acid component and the diamine component can be obtained in the form of a precipitate by dissolving the dicarboxylic acid component and the diamine component in a solvent and mixing them. In this case, as a solvent, as long as it can dissolve the dicarboxylic acid component and the diamine component, it is not particularly limited, for example, ethers (for example, cyclic ethers such as tetrahydrofuran and 1,4-dioxane), ketones (for example, chain ketones such as butanone; cyclic ketones such as cyclohexanone, etc.), halogenated solvents (for example, halogenated hydrocarbons such as dichloromethane and chloroform), amides (for example, N,N'-dimethylacetamide, N,N'-dimethylformamide, etc.), sulfoxides (for example, dimethyl sulfoxide), nitrogen-containing solvents (for example, N-methylpyrrolidone, etc.), etc. The solvent may be a single solvent or a combination of two or more.
[0288] In addition, in the melt polycondensation method, when any component (e.g., diamine component) is easily volatile, an excess amount (e.g., a ratio of 0.01 to 3 mol% or more than the theoretical amount) of the volatile component can be used. In addition, in order to prevent the volatilization of the diamine component, etc., the reaction can be carried out under pressure in the early stage of the reaction. The polymerization reaction can be carried out under normal pressure or under reduced pressure, but in the later stage of the polymerization, it is preferably reduced to about 150 Pa to promote the removal of the dissociated components such as water and alcohol from the reaction system.
[0289] 1.2.3.3. Physical properties of polyamide resin
[0290] The glass transition temperature of the ultraviolet absorbing polyamide resin can be selected from a range of 120°C or more (e.g., 140°C or more), for example, 150°C or more (e.g., 160 to 400°C), preferably 165°C or more (e.g., 165 to 370°C), more preferably 170°C or more (e.g., 175 to 350°C), particularly 180°C or more (e.g., 190 to 320°C), and can also be set to 200°C or more (e.g., 200 to 350°C, preferably 210 to 300°C, and more preferably 215 to 280°C). The glass transition temperature can be measured by the method described in the examples described below.
[0291] The weight average molecular weight of the ultraviolet absorbing polyamide resin is preferably 30000 to 200000, more preferably 35000 to 150000, and further preferably 40000 to 110000. By the weight average molecular weight being within the above range, the molecular chain length of the ultraviolet absorbing polyamide resin, mechanical properties such as elongation at break and flexibility are in a tendency to be further improved, and the stretchability is in a tendency to be further improved. In addition, in the present embodiment, the weight average molecular weight can be measured by gel permeation chromatography (GPC) via polystyrene conversion. More specifically, it can be measured by the method described in the embodiments described later.
[0292] 1.2.4. (Meth)acrylic resin
[0293] The (meth)acrylic resin is obtained by polymerizing a (meth)acrylic ester and has a structural unit F derived from a fluorene compound represented by the general formula (1) as a (meth)acrylic ester. Thus, in order to distinguish from other (meth)acrylic resins, the (meth)acrylic resin containing the structural unit F is also referred to as a "ultraviolet absorbing (meth)acrylic resin".
[0294] When the ultraviolet absorber represented by the general formula (1) of the present invention is a reactive di(meth)acrylate, it can be radically polymerized to obtain an ultraviolet absorbing (meth)acrylic resin having the ultraviolet absorber component as a constituent unit.
[0295] The structural unit F contained in the ultraviolet absorbing (meth) acrylic resin is preferably contained in a molar ratio of 1 to 100 mol%, more preferably 5 to 80 mol%, and further preferably 10 to 60 mol% relative to the total radical polymerizable compounds. When the content ratio of the ultraviolet absorber is within the above range, the ultraviolet absorbency and the absorption specificity of ultraviolet rays of a specific wavelength tend to be further improved.
[0296] 1.2.4.1. (Meth)acrylate monomers
[0297] The (meth)acrylate units of the ultraviolet absorbing (meth)acrylic resin may all be constituent units F, or may be a combination of constituent units F of (meth)acrylate and other free radical polymerizable components. The constituent units F of (meth)acrylate are not particularly limited, and examples thereof include: 1a and Y 1b Structural unit of (meth)acrylate when represented by formula (Y4) These (meth)acrylates may be used alone or in combination of two or more.
[0298] Although it does not specifically limit as another radical polymerizable component, vinyl compound, monofunctional (meth)acrylate, polyfunctional (meth)acrylate, etc. are mentioned.
[0299] Examples of the vinyl compound include aromatic vinyl compounds such as styrene, α-methylstyrene and vinyltoluene, fatty acid vinyl esters such as vinyl acetate, vinyl propionate and vinyl pivalate, and N-vinyl compounds such as N-vinylpyrrolidone and N-vinylacetamide.
[0300] Examples of the monofunctional (meth)acrylate include alkyl (meth)acrylates [e.g., C1-20 alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate], hydroxyalkyl (meth)acrylates, alkoxyalkyl (meth)acrylates, cyclohexyl (meth)acrylates, aryl (meth)acrylates (e.g., phenyl (meth)acrylate), aryloxyalkyl (meth)acrylates (e.g., phenoxyethyl (meth)acrylate), aralkyl (meth)acrylates (e.g., benzyl (meth)acrylate), aryloxy ((poly)alkoxy)alkyl (meth)acrylates (e.g., phenoxyethoxyethyl (meth)acrylate), alkylaryloxy ((poly)alkoxy)alkyl (meth)acrylates (e.g., nonylphenoxy (poly)ethoxyethyl (meth)acrylate), arylaryl (oxy ((poly)alkoxy)alkyl (meth)acrylates (e.g., 2-(o-phenylphenoxy)ethyl ester, phenylphenoxy(poly)ethoxyethyl(meth)acrylate, etc.); (meth)acrylates having a sulfur atom [e.g., alkylthio(meth)acrylates (e.g., methylthio(meth)acrylate, etc.), arylthio(meth)acrylates (e.g., phenylthio(meth)acrylate, etc.), arylalkylthio(meth)acrylates (e.g., benzylthio(meth)acrylate, etc.), arylthioalkyl(meth)acrylates (e.g., phenylthioethyl(meth)acrylate, etc.)] ; N,N-dialkyl(meth)acrylamide (for example, N,N-dimethyl(meth)acrylamide, etc.), N,N-dialkylaminoalkyl(meth)acrylate (for example, N,N-dimethylaminoethyl(meth)acrylate, etc.), mono(meth)acrylate of bisphenol or its alkylene oxide adduct (for example, mono(meth)acrylate of ethylene oxide adduct of bisphenol A, etc.), (meth)acrylate having a fluorene skeleton (for example, 9-(meth)acryloyloxymethylfluorene, etc.), etc.
[0301] Examples of the polyfunctional (meth)acrylate include difunctional (meth)acrylates [e.g., C2-10 alkylene glycol di(meth)acrylates such as ethylene glycol di(meth)acrylate and butanediol di(meth)acrylate, polyalkylene glycol di(meth)acrylates such as diethylene glycol di(meth)acrylate, and di(meth)acrylates of bisphenol A (or its alkylene oxide adduct)], trifunctional or higher (meth)acrylates [e.g., trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, tri- or tetra(meth)acrylates of triols or tetraols], oligo(meth)acrylates [urethane (meth)acrylate, epoxy (meth)acrylate, polyester (meth)acrylate, etc.], etc. These monofunctional and polyfunctional (meth)acrylates may be used alone or in combination of two or more.
[0302] 1.2.4.2. Preparation method of (meth)acrylic resin
[0303] The ultraviolet absorbing (meth)acrylic resin can be prepared by the reaction of (meth)acrylic esters. The method for preparing the (meth)acrylic resin is not particularly limited, and the (meth)acrylic resin can be prepared by a conventional method such as free radical polymerization. In the polymerization reaction, a polymerization initiator, a photosensitizer, etc. can be used.
[0304] 1.2.4.1. Polymerization initiator
[0305] The curable composition may contain a polymerization initiator. The polymerization initiator may be a thermal polymerization initiator (thermal radical generator) or a photopolymerization initiator (photoradical generator).
[0306] Examples of the thermal polymerization initiator include organic peroxides [dialkyl peroxides (e.g., di-tert-butyl peroxide, etc.), diacyl peroxides (e.g., lauroyl peroxide, benzoyl peroxide, etc.), peracids (or peresters) (e.g., tert-butyl hydroperoxide, cumene hydroperoxide, tert-butyl peracetate, etc.), ketone peroxides, peroxycarbonates, peroxyketals], azo compounds [e.g., azonitrile compounds such as 2,2'-azobis(isobutyronitrile), azoamide compounds, azoamidine compounds, etc.], etc. These thermal polymerization initiators can be used alone or in combination of two or more.
[0307] Examples of the photopolymerization initiator include benzoins (benzoin, benzoin ethyl ether and other benzoin alkyl ethers), acetophenones (acetophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, etc.), aminoacetophenones {2-methyl-1-[4-(methylthio)phenyl]-2-morpholinylaminopropanone-1, etc.}, anthraquinones (anthraquinone, 2-methylanthraquinone, etc.), thioxanthones (2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, etc.), ketals (acetophenone dimethyl ketal, benzyl dimethyl ketal, etc.), benzophenones (benzophenone, etc.), xanthones, etc. These photopolymerization initiators may be used alone or in combination of two or more.
[0308] The amount of the polymerization initiator (thermal or photopolymerization initiator) used may be 0.1 to 15 parts by mass, preferably 0.5 to 10 parts by mass (eg, 1 to 8 parts by mass), and more preferably about 2 to 5 parts by mass, based on 100 parts by mass of the total amount of the radical polymerizable components.
[0309] The photopolymerization initiator may be combined with a photosensitizer. Examples of the photosensitizer include tertiary amines {e.g., trialkylamines, trialkanolamines (e.g., triethanolamine), dialkylaminobenzoic acid alkyl esters such as N,N-dimethylaminobenzoic acid ethyl ester [p-(dimethylamino)benzoic acid ethyl ester, etc.], N,N-dimethylaminobenzoic acid pentyl ester [p-(dimethylamino)benzoic acid pentyl ester, etc.], bis(dialkylamino)benzophenones such as 4,4-bis(diethylamino)benzophenone, dialkylaminobenzophenones such as 4-(dimethylamino)benzophenone, etc.}, etc. These photosensitizers may be used alone or in combination of two or more.
[0310] The amount of the photosensitizer used may be 1 to 200 parts by mass, preferably 5 to 150 parts by mass, and more preferably about 10 to 100 parts by mass, relative to 100 parts by mass of the polymerization initiator.
[0311] The ultraviolet absorber having a di(meth)acrylate structure is easily cured by applying active energy (active energy rays) to form an ultraviolet absorbing (meth)acrylic resin. Among the active energy, thermal energy and / or light energy (ultraviolet rays, X-rays, electron beams, etc.) are useful.
[0312] When utilizing thermal energy, the heating temperature may be, for example, about 50 to 200°C, preferably about 60 to 150°C, and more preferably about 70 to 120°C.
[0313] In addition, when light irradiation (for example, ultraviolet irradiation) is performed, the light irradiation energy can be appropriately selected according to the application, and can be, for example, 50 to 10000 mJ / cm 2 , preferably 70 to 8000 mJ / cm 2, more preferably 100 to 5000 mJ / cm 2 (For example, 500 to 3000 mJ / cm 2 )about.
[0314] Curing can be performed in air or in an inert gas environment (eg, nitrogen, noble gas, etc.).
[0315] 1.2.4.1. Physical properties of acrylic resin
[0316] The glass transition temperature of the ultraviolet absorbing (meth)acrylic resin can be selected from the range of -60°C to 300°C, preferably -40 to 250°C, and more preferably about -20 to 200°C. The glass transition temperature can be measured by the method described in the examples below.
[0317] The weight average molecular weight of the ultraviolet absorbing (meth) acrylic resin can be selected from the range of 400 to 15000 (e.g., 600 to 12000), and can be 800 to 10000 (e.g., 1000 to 7500), and more preferably about 1200 to 6000 (e.g., 1500 to 5000). In addition, in the present embodiment, the weight average molecular weight can be measured by gel permeation chromatography (GPC) in terms of polystyrene. More specifically, it can be measured by the method described in the examples described later.
[0318] 1.3.Physical properties
[0319] The fluorene compound of the present embodiment and the resin having the constituent unit F (hereinafter, also collectively referred to as "ultraviolet absorber") may be in a crystalline form or an amorphous form according to its chemical structure and manufacturing method. Furthermore, when the ultraviolet absorber forms a crystalline form, there may be a plurality of crystal polymorphs, and when used for the purpose of the present invention, it may be in any form or a mixture thereof.
[0320] The half-value width of the ultraviolet absorber of the present embodiment is preferably 55nm or less, more preferably 50nm or less, further preferably 40nm or less, and further preferably 30nm or less. The smaller the lower limit of the half-value width, the more preferred, for example, 3nm or more. By having a half-value width of 55nm or less, it is possible to selectively absorb only ultraviolet rays in a specific range, and it is possible to take into account both excellent UV absorptivity and low colorability. Here, the half-value width refers to a wavelength band with a wavelength width of more than 1 / 2 of the absorbance, based on the absorption wavelength at which the absorbance reaches the maximum.
[0321] The ultraviolet absorber of the present embodiment preferably has a maximum absorption wavelength in the range of 320 to 400 nm. When the maximum absorption wavelength is in the above range, ultraviolet rays in the long wavelength region which are generally considered difficult to absorb can be suitably absorbed.
[0322] Molar absorption coefficient at 380 nm (A 380 ) is preferably 200 to 2000 L / (mol)·cm, more preferably 400 to 1500 L / (mol)·cm, and further preferably 600 to 1000 L / (mol)·cm.
[0323] Molar absorption coefficient at 400 nm (A 400 ) is preferably 0.5 to 50 L / (mol)·cm, more preferably 1.0 to 25 L / (mol)·cm, and further preferably 2.0 to 10 L / (mol)·cm.
[0324] The molar absorptivity at the maximum absorption wavelength (A max ) is preferably 20,000 to 100,000 L / (mol)·cm, more preferably 30,000 to 90,000 L / (mol)·cm, and further preferably 40,000 to 80,000 L / (mol)·cm.
[0325] The molar absorption coefficient (A 380 ) or molar absorption coefficient (A400) is within the above range, and there is a tendency that the excellent UV absorbency in the long wavelength region is further improved and the colorability is further reduced.
[0326] Molar absorptivity (A 380 ) and molar absorption coefficient (A 400 ) ratio (A 380 / A 400 ) is preferably 50 or more, more preferably 100 or more, and further preferably 200 or more. 380 / A 400 The larger the upper limit of ), the more preferably it is, for example, 1000 or less. 380 / A 400 ) is 50 or more, which can achieve both excellent UV absorbency in the long wavelength region and low coloring.
[0327] The melting point of the ultraviolet absorber of the present embodiment may be, for example, about 100 to 250°C, and preferred ranges are 150 to 240°C, 175 to 230°C, and 180 to 225°C in stages.
[0328] The 5% mass reduction temperature of the ultraviolet absorber of the present embodiment may be, for example, about 250 to 500°C, and preferably ranges thereof are 350 to 480°C, 370 to 450°C, and 400 to 430°C in stages.
[0329] 2. Ultraviolet absorbing composition
[0330] The ultraviolet absorbing composition of the present embodiment comprises the ultraviolet absorber of the present embodiment, and at least one of a triazine ring-containing compound, a benzotriazole ring-containing compound, or a benzophenone ring-containing compound as a second ultraviolet absorber. The ultraviolet absorber of the present embodiment may be the above-mentioned fluorene compound, or may be a resin such as an ultraviolet absorbing polyester resin, an ultraviolet absorbing polycarbonate resin, an ultraviolet absorbing polyamide resin, or an ultraviolet absorbing (meth) acrylic resin. In this way, by mixing the ultraviolet absorber of the present embodiment and the second ultraviolet absorber in any proportion, ultraviolet rays of a wider range of wavelengths can be absorbed.
[0331] The second ultraviolet absorber can be freely selected according to the target absorption wavelength, compatibility with the resin described later, etc. As an example, when the purpose is to absorb ultraviolet rays of a wide wavelength in the UV-A region, it is preferred to select a compound containing a triazine ring, when the purpose is to be compatible with a general resin, it is preferred to select a compound containing a benzotriazole ring, and when the purpose is to be compatible with a resin with low polarity, it is preferred to select a compound containing a benzophenone ring. The proportion of the second ultraviolet absorber contained in the ultraviolet absorbing composition of this embodiment can be freely selected according to the purpose, and specifically, it is preferably 0.01 to 50% by mass.
[0332] 3. Ultraviolet absorbing resin composition
[0333] The ultraviolet absorbing resin composition of this embodiment includes the ultraviolet absorber of this embodiment and any resin. The ultraviolet absorber of this embodiment can be the above-mentioned fluorene compound, or can be a resin such as an ultraviolet absorbing polyester resin, an ultraviolet absorbing polycarbonate resin, an ultraviolet absorbing polyamide resin, or an ultraviolet absorbing (meth) acrylic resin.
[0334] The content of the ultraviolet absorber of the present embodiment is preferably 0.1 to 10% by mass, more preferably 0.5 to 8.0% by mass, and further preferably 1.0 to 5.0% by mass relative to the total amount of the ultraviolet absorbing resin composition. If the amount of the ultraviolet absorber is 0.1% by mass or more, the ultraviolet absorption performance tends to be further improved. On the other hand, when the amount of the ultraviolet absorber is 10% by mass or less, physical properties such as rigidity and toughness tend to be further improved.
[0335] In addition, as an arbitrary resin, a thermoplastic resin, a thermosetting resin, etc. are mentioned.
[0336] The ultraviolet absorbing resin composition can be processed into any form such as a plate, a sheet, or a film as required. The resin composition used in the ultraviolet absorbing resin composition is preferably a thermoplastic resin from the viewpoint of excellent moldability and processability.
[0337] 3.1. Thermoplastic resin
[0338] Thermoplastic resins are not particularly limited as long as they are compatible with the ultraviolet absorber of the present embodiment, and examples thereof include: polyolefin resins such as chain olefin resins and cyclic olefin resins (or cycloolefin resins); (meth) acrylic resins; styrene resins such as polystyrene, AS resin, and ABS resin; polyester resins such as polyalkylene arylate resins, polyarylate resins, polyethylene terephthalate, and polycarbonate resins; polyamide resins; cellulose resins such as cellulose triacetate; vinyl resins such as polyvinyl chloride, polyvinyl acetate, and polyvinyl alcohol; thermoplastic polyurethane resins, and the like.
[0339] 3.2. Thermosetting resin
[0340] The thermosetting resin is not particularly limited as long as it is compatible with the ultraviolet absorber of the present embodiment, and examples thereof include phenolic resins, epoxy resins, melamine resins, urea resins, unsaturated polyester resins, alkyd resins, thermosetting polyurethane resins, and thermosetting polyimide resins.
[0341] 3.3. Preparation method of composition
[0342] As the means of melt kneading of the ultraviolet absorbing resin composition, known means can be adopted, for example, single screw extruder, twin screw extruder, Henschel mixer, Banbury mixer, tandem mixer, co-kneader, etc. Usually, the melt kneading performed by using a twin screw extruder is preferably performed because it can be mixed uniformly and completely.
[0343] 3.4. Other ingredients
[0344] In addition, the ultraviolet absorbing resin composition may contain various additives as needed [for example, fillers or reinforcing agents, colorants (dyes and pigments), conductive agents, flame retardants, plasticizers, lubricants, stabilizers (antioxidants, ultraviolet absorbers, heat stabilizers, etc.), mold release agents, antistatic agents, dispersants, flow regulators, leveling agents, defoamers, surface modifiers, stress reducing agents (silicone oil, silica gel, various plastic powders, various process plastic powders, etc.), heat resistance improvers (sulfur compounds, polysilanes, etc.), carbon materials, etc.]. These additives may be used alone or in combination of two or more.
[0345] 4. Ultraviolet absorbing coating liquid
[0346] The ultraviolet absorbing coating liquid of the present embodiment includes the ultraviolet absorber of the present embodiment, the ultraviolet absorbing composition of the present embodiment, or the ultraviolet absorbing resin composition of the present embodiment; and a solvent. Thus, the ultraviolet absorber, ultraviolet absorbing composition, or ultraviolet absorbing resin composition of the present embodiment can be dissolved in any solvent to form an ultraviolet absorbing coating liquid.
[0347] As the solvent that can be used for the ultraviolet absorbing coating liquid, for example, there can be listed: aromatic solvents such as benzene, toluene, and xylene; ketone solvents such as diacetone alcohol, acetone, cyclohexanone, cyclopentanone, butanone, and methyl isopropyl ketone; cycloalkane solvents such as cyclohexane, ethylcyclohexane, and 1,2-dimethylcyclohexane; halogen-containing solvents such as dichloromethane and chloroform; ether solvents such as tetrahydrofuran and dioxane. From the viewpoint of obtaining a viscosity suitable for coating, the concentration of the resin in the coating liquid can be 1% to 50% by mass. The solvent can be used alone or in combination of two or more in any proportion.
[0348] The ultraviolet absorbing coating liquid may contain additives such as a defoaming agent, a leveling agent, an antioxidant, a light stabilizer, a lubricant, a flame retardant, and an antistatic agent as needed. These additives may be used alone or in combination of two or more.
[0349] 5. Ultraviolet absorbing coated resin sheet and ultraviolet absorbing coated glass
[0350] The ultraviolet absorbing coated resin sheet of the present embodiment comprises a resin sheet and an ultraviolet shielding layer, and the ultraviolet shielding layer comprises the ultraviolet absorber, ultraviolet absorbing composition, or ultraviolet absorbing resin composition of the present embodiment. In addition, the ultraviolet absorbing coated glass of the present embodiment comprises glass and an ultraviolet shielding layer, and the ultraviolet shielding layer comprises the ultraviolet absorber, ultraviolet absorbing composition, or ultraviolet absorbing resin composition of the present embodiment.
[0351] The resin sheet is not particularly limited as long as it can be coated with the ultraviolet absorber, ultraviolet absorbing composition, or ultraviolet absorbing resin composition of the present embodiment. For example, sheets composed of the following resins can be listed: polycarbonate resins, polyamide resins, polyvinyl alcohol resins, cellulose ester resins such as cellulose triacetate film and cellulose acetate propionate film, polyester resins such as polyethylene terephthalate and polyethylene naphthalate, polyarylate resins, polyimide resins, cycloolefin resins, polysulfone resins, polyethersulfone resins, polyethylene, polypropylene and other polyolefin resins.
[0352] The glass is not particularly limited as long as it can be coated with the ultraviolet absorbing coating liquid, and examples thereof include float glass, tempered glass, semi-tempered glass, chemically tempered glass, green glass, and quartz glass.
[0353] The coating method of the ultraviolet shielding layer is not limited. The coating of the ultraviolet absorber, ultraviolet absorbing composition, or ultraviolet absorbing resin composition can be performed by coating the ultraviolet absorbing coating liquid on the resin sheet or glass.
[0354] Examples of the coating method include curtain coating, extrusion coating, roll coating, spin coating, dip coating, bar coating, spray coating, oblique plate coating, print coating, gravure coating, die coating, slit coating, and dipping.
[0355] The method for drying the ultraviolet absorbing coating liquid is not limited, and for example, a drying method such as heating drying or reduced pressure drying can be adopted.
[0356] 6. Ultraviolet absorbing film and ultraviolet absorbing molded body
[0357] The ultraviolet absorbing film of the present embodiment includes the ultraviolet absorber, ultraviolet absorbing composition, or ultraviolet absorbing resin composition of the present embodiment. In addition, the ultraviolet absorbing molded body of the present embodiment includes the ultraviolet absorber, ultraviolet absorbing composition, or ultraviolet absorbing resin composition of the present embodiment.
[0358] The ultraviolet absorbing molded body can be formed into an ultraviolet absorbing molded body by any method. The shape of the molded body is not particularly limited, and examples thereof include: a two-dimensional structure such as a film, a sheet, or a plate; a three-dimensional structure such as a rod, a tube, a test tube, or a hollow shape. In addition, the ultraviolet absorbing molded body of the present invention is particularly suitable for optical components such as optical films, optical lenses, and optical sheets because of its excellent optical properties, mechanical properties, and high heat resistance.
[0359] In addition, the ultraviolet absorbing thermoformed body may contain various additives as needed [for example, fillers or reinforcing agents, colorants (dyes and pigments), conductive agents, flame retardants, plasticizers, lubricants, stabilizers (antioxidants, ultraviolet absorbers, heat stabilizers, etc.), mold release agents, antistatic agents, dispersants, flow regulators, leveling agents, defoamers, surface modifiers, stress reducing agents (silicone oil, silica gel, various plastic powders, various process plastic powders, etc.), heat resistance improvers (sulfur compounds, polysilanes, etc.), carbon materials, etc.]. These additives may be used alone or in combination of two or more.
[0360] The ultraviolet absorbing molded article can be produced by, for example, injection molding, injection compression molding, extrusion molding, transfer molding, blow molding, press molding, casting molding, or the like.
[0361] The resin or the ultraviolet absorbing resin composition as the ultraviolet absorber of the present embodiment can be formed into a film to form an ultraviolet absorbing film. In this case, a single-layer film containing only the resin or the ultraviolet absorbing resin composition as the ultraviolet absorber can be formed.
[0362] The method for forming a single-layer film is not particularly limited, and examples thereof include melt extrusion such as a solution casting method, an expansion method, and a T-die method, a calendering method, etc. Among them, a melt extrusion method such as a T-die method is preferred from the viewpoint of excellent productivity and prevention of reduction in optical properties due to residual solvents, and a solution casting method is preferred from the viewpoint of being able to control the film thickness with high precision and forming a thin single-layer film.
[0363] In the solution casting method, a UV-absorbing polyester resin, a UV-absorbing polycarbonate resin, a UV-absorbing polyamide resin, a UV-absorbing (meth)acrylic resin or a UV-absorbing resin composition is dissolved in a solvent, the obtained coating solution is applied to a substrate, and the substrate is peeled off after drying to remove the solvent, thereby obtaining a single-layer film. The substrate may be a resin film, a resin sheet or glass, and from the viewpoint of productivity, a resin film is preferred, and among them, a resin film that has been subjected to a release treatment and can be easily peeled off is more preferred.
[0364] There is no limitation on the coating method of the coating liquid. Examples of the coating method include curtain coating, extrusion coating, roll coating, spin coating, dip coating, bar coating, spray coating, oblique plate coating, printing coating, gravure coating, die coating, slit coating, and dipping.
[0365] The method for drying the coating liquid is not limited, and for example, a drying method such as heating drying or reduced pressure drying can be adopted.
[0366] In a melt extrusion method such as the T-die method, the molding conditions can be adjusted according to the glass transition temperature and melting point of the ultraviolet-absorbing polyester resin, ultraviolet-absorbing polycarbonate resin, ultraviolet-absorbing polyamide resin, ultraviolet-absorbing (meth) acrylic resin or ultraviolet-absorbing resin composition, and the molding is carried out according to the usual method. As a specific molding condition, the melting temperature of the resin to be extruded is preferably above Tg+80°C, more preferably above Tg+100°C, preferably below Tg+180°C, and more preferably below Tg+150°C. For example, in the T-die method, the melting temperature represents the melting temperature of the resin in the extruder having the T-die. When the melting temperature of the resin to be extruded is above the lower limit of the range, the fluidity of the resin can be fully improved to make the moldability good. In addition, when it is below the upper limit, the degradation of the resin can be suppressed.
[0367] The ultraviolet absorbing film of the present invention may be not only a single-layer film but also a laminated film laminated with other films.
[0368] The forming method of the laminated film is not particularly limited, and examples thereof include coextrusion forming, solution casting, extrusion lamination forming, etc. Among them, coextrusion forming is preferred from the viewpoint of not only excellent productivity but also being able to prevent reduction in optical and mechanical properties caused by residual solvents.
[0369] The coextrusion T-die method, which is one of the coextrusion molding methods, includes a feed block method and a multi-manifold method. The multi-manifold method is particularly preferred because it can reduce thickness variations of each layer.
[0370] The ultraviolet absorbing film of the present invention may be an unstretched film, but from the viewpoint of mechanical properties, it may also be a stretched film. In addition, stretching is effective as a means of thin filmization. If the unstretched film reaches a thickness of about 50 μm or more, the film thickness can be controlled by sandwiching the lamination roller after the T-die casting, and the film thickness accuracy is improved. By selecting the stretching conditions that obtain uniform tensile stress and performing the stretching, a film can be made and the film thickness accuracy is good.
[0371] The ultraviolet absorbing film obtained by any of the above-mentioned methods can be stretched and formed while being heated to an appropriate temperature between the melting point and the glass transition temperature. The stretching can be either biaxial stretching or uniaxial stretching, which can be selected in combination with the following embodiments. For example, in order to be used as a polarizer protective film described later, biaxial stretching with less delay caused by stretching is suitable. Biaxial stretching can be performed by stretching the film in both directions in the longitudinal and transverse directions, and the in-plane delay Ro can be offset in the longitudinal and transverse directions to become a value close to zero. On the other hand, in order to be used as a film that appropriately reflects the required phase difference, such as a 1 / 4λ phase difference film, uniaxial stretching is suitable.
[0372] 7. Polarizer protective film
[0373] The ultraviolet absorbing film of the present embodiment can be used as a polarizer protective film.
[0374] The total thickness of the polarizer protective film is preferably 5 to 90 μm, more preferably 10 to 80 μm, and further preferably 20 to 50 μm. When the total thickness is within the above range, the film can be more suitably used as a polarizer protective film.
[0375] The polarizer protective film of this embodiment preferably has a spectral transmittance of 5% or less at 350nm, more preferably 3% or less, and further preferably 1% or less. When the spectral transmittance at a wavelength of 350nm is within the above range, the polarizer can be prevented from being deteriorated by ultraviolet rays contained in external light, etc., and can be more suitably used as a polarizer protective film.
[0376] The b* value in the L*a*b* color space (CIELAB) of the polarizer protective film of the present embodiment is preferably 0.8 or less, more preferably 0.6 or less, and further preferably 0.5 or less. In addition, the b* value is preferably -0.8 or more, more preferably -0.6 or more, and further preferably -0.5 or more. By having the b* value within the above range, a polarizer protective film with excellent visibility can be obtained. In addition, the above b* value refers to the value calculated in accordance with JIS Z8781-4:2013.
[0377] The a* value is preferably 0.3 or less, more preferably 0.2 or less, and further preferably 0.1 or less. The a* value is preferably -0.4 or more, more preferably -0.3 or more, and further preferably -0.2 or more.
[0378] The L* value may preferably be 100 or less, 99 or less, or 98 or less. The L* value may preferably be 90 or more, 92 or more, or 94 or more.
[0379] The polarizer protective film of this embodiment preferably has a spectral light transmittance of 8% or less at 380nm, more preferably 5% or less, and further preferably 1% or less. By having a spectral light transmittance of 380nm wavelength within the above range, the polarizer can be prevented from being degraded by ultraviolet rays contained in external light, etc., and can be more suitably used as a polarizer protective film.
[0380] 8. Polarizer
[0381] The polarizing plate of this embodiment includes the above-mentioned polarizer protective film and may further include other layers as required. Figure 1A and Figure 1B The polarizing plate of this embodiment is described below. The polarizing plate includes the polarizer protective film of this embodiment. Figure 1A and 1B This is a cross-sectional view schematically illustrating one embodiment of a polarizing plate.
[0382] Figure 1A The polarizing plate 20 shown is formed by sequentially stacking a phase difference film 21, a polarizer 23, and a polarizer protective film 10. As shown in the figure, an adhesive layer 22 may be provided between the phase difference film 21 and the polarizer 23, and an adhesive layer 24 may be provided between the polarizer 23 and the polarizer protective film 10.
[0383] Figure 1B The polarizing plate 30 shown is formed by sequentially stacking a phase difference film 31, a polarizer protective film 10, a polarizer 34, and a polarizer protective film 10. An adhesive layer or adhesive layer 32 may be provided between the phase difference film 31 and the polarizer protective film 10, and adhesive layers 33 and 35 may be provided between the polarizer 34 and the polarizer protective film 10.
[0384] The polarizer protective film 10 may be subjected to corona treatment, plasma treatment, or surface modification treatment with a strong alkali aqueous solution such as sodium hydroxide or potassium hydroxide to improve adhesion with the polarizers 23 and 34. These surface modification treatments may be performed after the film forming step or after the stretching step.
[0385] The polarizers 23 and 34 are not particularly limited as long as they are conventionally known polarizers, and examples thereof include: polarizers obtained by dyeing and stretching hydrophilic polymer films such as polyvinyl alcohol films, partially formalized polyvinyl alcohol films, and partially saponified films of ethylene / vinyl acetate copolymers with dichroic substances such as iodine or dichroic dyes; polyolefin-based oriented films such as dehydrated polyvinyl alcohol films and dehydrochlorinated polyvinyl chloride films, etc. In addition, polarizers obtained by dyeing a polyvinyl alcohol film with iodine and uniaxially stretching the film can be cited.
[0386] The above-mentioned polarizer protective film can be used as the polarizer protective film 10. The polarizer protective film 10 and the polarizers 23 and 34 formed of a polyvinyl alcohol resin or the like can be bonded together using an ultraviolet curing adhesive (adhesive layers 24, 33, 35).
[0387] 9. Image display device
[0388] The image display device of this embodiment includes the above-mentioned polarizing plate. Figure 2A and 2B , the image display device of this embodiment is described. The image display device of this embodiment is not particularly limited as long as it has the above-mentioned polarizer, and examples thereof include organic electroluminescent (EL) display devices and liquid crystal display devices. In addition, the image display device is not limited to a device that is circulated in the market as a monomer in the form of a final product, and may also be a part of an information processing device described later, such as a smart phone. Figure 2A is a cross-sectional view schematically illustrating an organic EL display device according to one embodiment of the present invention. Figure 2B This is a cross-sectional view schematically illustrating a liquid crystal display device according to one form of the present embodiment.
[0389] like Figure 2AAs shown, the organic EL display device 40 sequentially comprises: an organic EL display panel 41, a polarizing plate 20 having a polarizer protective film 10 of the present embodiment, and a front panel 43. In the organic EL display device 40, by using the polarizing plate 20 having the polarizer protective film 10, it is possible to suppress the degradation of the polarizing plate 20 due to ultraviolet rays or moisture permeation, and in addition, the mechanical strength against bending etc. is excellent, and a thinner device can be achieved.
[0390] In addition, the organic EL display device 40 may include other components such as a touch sensor 42 as needed. By equipping the touch sensor 42, the organic EL display device 40 functions as an information input interface in addition to functioning as a display device. The layers constituting the organic EL display device 40 may be bonded using an adhesive or an adhesive.
[0391] like Figure 2B As shown in FIG. 1 , the liquid crystal display device 50 includes a light source 51, a polarizing plate 30, a liquid crystal panel 52, a polarizing plate 30, and a front panel 53 in this order. The light source 51 may be a direct-under type in which light sources are evenly arranged directly below the liquid crystal panel, or may be an edge-under type in which a reflector and a light guide are provided. Figure 2B In FIG. 5 , the front panel 53 is shown, but the liquid crystal display device 50 does not need to include the front panel 53. Furthermore, the liquid crystal display device 50 may further include a touch sensor (not shown).
[0392] In addition, the screen of the image display device is not limited to a quadrilateral, but may also have a circular, elliptical, or triangular, pentagonal or other polygonal shape. Furthermore, the image display device may be flexible and may change its shape by warping, bending, curling, or folding. For example, Figure 3 As shown, the image display device includes a roll-up display that can be used by pulling out the image display device 61 stored in a cylindrical shape in the image display device storage section 62.
[0393] 10. Transport equipment
[0394] The ultraviolet absorber, ultraviolet absorbing composition, or ultraviolet absorbing resin composition, ultraviolet absorbing coating liquid, ultraviolet absorbing coating resin sheet, ultraviolet absorbing coated glass, ultraviolet absorbing molded body, ultraviolet absorbing film, polarizer protective film, polarizing plate or image display device of this embodiment can be suitably used as a component of transportation equipment such as automobiles, ships, and airplanes.
[0395] 11. Building components
[0396] The ultraviolet absorber, ultraviolet absorbing composition, or ultraviolet absorbing resin composition, ultraviolet absorbing coating liquid, ultraviolet absorbing coating resin sheet, ultraviolet absorbing coated glass, ultraviolet absorbing molded body, ultraviolet absorbing film, polarizer protective film, polarizing plate or image display device of this embodiment can be used as structural materials such as columns or beams, roof materials, wall materials, floor materials, door or window fittings such as doors and windows, and can be suitably used as window components for the purpose of absorbing ultraviolet rays that invade during lighting.
[0397] Example 1
[0398] Hereinafter, the present invention will be described in more detail based on examples, but the present invention is not limited to these examples. Evaluation methods and raw materials are shown below.
[0399] 1. Evaluation Method
[0400] 1.1. Glass transition temperature (Tg)
[0401] A sample was placed in an aluminum pan using a differential scanning calorimeter ("DSC 6220" manufactured by Seiko Instruments Co., Ltd.), and Tg was measured in the range of 30°C to 200°C in accordance with JIS K 7121.
[0402] 1.2. Weight average molecular weight
[0403] Using a gel permeation chromatograph ("HLC-8120GPC" manufactured by Tosoh Corporation), a sample was dissolved in chloroform, and the weight average molecular weight Mw of each resin was measured in terms of polystyrene.
[0404] 1.3.5% mass reduction temperature
[0405] The temperature at which the mass of the sample decreased by 5% by mass was measured using a thermogravimetric measuring apparatus ("TGA 4000" manufactured by PerkinElmer) under a nitrogen atmosphere at a temperature increase rate of 10°C / min.
[0406] 1.4. Film thickness
[0407] Using a thickness gauge ("Micrometer" manufactured by Mitutoyo Corporation), three points were measured at equal intervals between the jigs in the longitudinal direction of the film, and the average value was calculated.
[0408] 1.5. Molar absorptivity, maximum absorption wavelength and half-value width
[0409] For each sample, a tetrahydrofuran solution of a concentration suitable for the measurement described below was prepared, and the UV-visible spectrum was measured using a UV-visible spectrophotometer ("V-650" manufactured by JASCO Corporation) with a 1 cm quartz cuvette. The concentration suitable for measurement here refers to the range of absorbance indicating 0.1 to 2.0. The molar absorption coefficient was calculated from the slope obtained by plotting the measured concentration and absorbance at more than 3 points within this range. In addition, the maximum absorption wavelength and half-value width were calculated based on the obtained spectrum.
[0410] 1.4. Transmittance
[0411] The transmittance of each film at 350 nm and 380 nm was measured using an ultraviolet-visible spectrophotometer ("V-650" manufactured by JASCO Corporation) in accordance with JIS K7361:1997.
[0412] 1.5.L*a*b* color space
[0413] Each film was measured using an ultraviolet-visible spectrophotometer ("V-650" manufactured by JASCO Corporation) in accordance with JIS Z8729. The L* value represents brightness, and the a* value and b* value represent hue.
[0414] 2. Fluorene compounds
[0415] 2.1. Example 1: Modulation of DNFDP-m
[0416] 200 ml of 1,4-dioxane and 54.7 g (0.17 mol) of 2,7-dibromo-9H-fluorene were placed in the reactor, and the fluorene was dissolved by stirring. Then, 3.0 ml of a 40% by mass methanol solution of trimethylbenzylammonium hydroxide (Triton B40 manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise while cooling to 10°C, and stirred for 30 minutes. Next, 37.9 g (0.44 mol) of methyl acrylate was added and stirred for about 3 hours. After the reaction was completed, 200 ml of toluene and 50 ml of 0.5N hydrochloric acid were added for washing. After removing the water layer, the organic layer was washed 3 times with 30 ml of distilled water. By distilling off the solvent, 9,9-bis (2-methoxycarbonylethyl) -2,7-dibromofluorene (DBrFDP-m) was obtained.
[0417] Next, 192.3 g (0.39 mol) of the obtained DBrFDP-m, 200 g (1.2 mol) of 2-naphthylboronic acid, 4.3 L of dimethoxyethane and 1 L of 2M sodium carbonate aqueous solution were placed in the reactor, and 22.4 g (19.4 mmol) of tetrakis(triphenylphosphine)palladium (0) [or Pd(PPh3)4] was added under nitrogen flow, and the mixture was heated to reflux for 5 hours at an internal temperature of 71 to 78°C to react. After cooling to room temperature, 2.0 L of toluene and 500 mL of ion exchange water were added, and the mixture was separated and extracted 5 times, and washed. The organic layer changed from dark orange to brown. The insoluble matter was filtered and concentrated to obtain brown crude crystals. The obtained crude crystals were heated and dissolved in a mixed solution of 1.5 kg of ethyl acetate and 300 g of isopropyl alcohol (IPA), cooled to below 10°C with ice water, and stirred for 1 hour to precipitate crystals. After filtering the precipitated crystals, they were dried under reduced pressure to obtain 130 g of gray-brown crystals. The obtained gray-brown crystals were purified by column chromatography (silica gel carrier, developing solvent chloroform:ethyl acetate (volume ratio) = 4:1), recrystallized from methanol and dried under reduced pressure to obtain 9,9-bis(2-methoxycarbonylethyl)-2,7-di(2-naphthyl)fluorene (DNFDP-m). 1 The results of H-NMR and FD-MS are shown below.
[0418] 1 H-NMR (CDCl3, 300MHz): δ (ppm) 1.7 (t, 4H), 2.6 (t, 4H), 3.4 (s, 6H), 7.5 (m, 4H), 7.7-8.0 (m, 14H), 8.1 (s, 2H).
[0419] FD-MS: m / z 590 (M+)
[0420] 2.2. Example 2: Modulation of DNFPO
[0421] Under nitrogen atmosphere, 1.2 kg (2.03 mol) of DNFDP-m obtained as above and 9.78 kg of tetrahydrofuran (THF) were added to a 20 L separable flask, and the mixture was cooled to 10°C or less in an ice-water bath. 230 g (6.08 mol) of sodium borohydride was added little by little to the obtained solution over 13 minutes, and then 856 g (6.09 mol) of boron trifluoride ether complex was added dropwise over 45 minutes, and then the mixture was heated to room temperature and stirred for 4 hours. After cooling in an ice-water bath, 1.0 kg (17.2 mol) of acetone was added dropwise over 1 hour, and the solvent was removed by reduced pressure concentration. Thereafter, 12 kg of chloroform, 1.0 kg of ion exchange water, and 3.0 kg of ice were added, and the water layer was removed. The water layer was removed by adding 4.0 kg of ion exchange water twice (washing with ion exchange water twice), and only the organic layer was taken out. The obtained organic layer was concentrated under reduced pressure to obtain 9,9-bis(3-hydroxypropyl)-2,7-di(2-naphthyl)fluorene (DNFPO). 1 The results of H-NMR and FD-MS are shown below.
[0422] 1 H-NMR (DMSO-d6, 300MHz): δ (ppm) 0.9 (m, 4H), 2.2 (m, 4H), 3.2 (t, 4H), 4.2 (t, 2H), 7.5-8.4 (m, 20H).
[0423] FD-MS: m / z 535 (M+).
[0424] 2.3. Example 3: Modulation of DNFPA
[0425] 30.0 g (0.06 mol) of DNFPO, 10.5 g (0.15 mol) of acrylic acid, 55 g of toluene and 0.12 g (1.0 mmol) of 2-methoxyphenol obtained by the above operation were placed in a 500 mL three-necked flask equipped with a Dean-Stark. The system was purged with nitrogen, heated to 95°C, and after the components were homogenized, 1.33 g (7.0 mmol) of p-toluenesulfonic acid monohydrate was added, and nitrogen was purged again, and refluxed for dehydration for 4 hours. The reaction temperature was 110-115°C.
[0426] The obtained solution was washed with 195 g of toluene and 20 g of 20% by mass saline (internal temperature 60 to 70° C.), and then neutralized with 20 g of 10% sodium hydroxide water (10% by mass sodium hydroxide aqueous solution) and 20 g of 20% by mass saline (internal temperature 60 to 70° C.), and it was confirmed that the pH of the water layer was 10 or more. 500 mass ppm of 2-methoxyphenol was added to the entire organic layer to make the solution uniform, and then washed twice with 20 g of 20% by mass saline and twice with 20 g of ion exchange water (internal temperature 60 to 70° C.), and it was confirmed that the pH of the water layer was 7. Then, 6 g of activated carbon (FP-6 manufactured by Mizusawa Chemical) was added to the organic layer, stirred at room temperature for 1 hour, filtered through cerium silica, concentrated, and dried under reduced pressure at 100° C. overnight to obtain 9,9-bis(3-acryloyloxypropyl)-2,7-di(2-naphthyl)fluorene.
[0427] 2.4. Example 4: Modulation of DPFDP-m
[0428] 192.3 g (0.39 mol) of DBrFDP-m, 150 g (1.2 mol) of phenylboronic acid, 4.3 L of dimethoxyethane and 1 L of 2M sodium carbonate aqueous solution obtained by the above operation were loaded into the reactor, and 22.4 g (19.4 mmol) of tetrakis (triphenylphosphine) palladium (0) [or Pd (PPh3) 4] was added under nitrogen flow, and heated to reflux for 5 hours at an internal temperature of 71-78 ° C to react. After cooling to room temperature, 2.0 L of toluene and 500 mL of ion exchange water were added, and the liquid was separated and extracted 5 times, and washed. The organic layer changed from dark orange to brown. The insoluble matter was filtered and concentrated to obtain brown crude crystals. The obtained crude crystals were heated and dissolved in a mixed solution of 1.5 kg of ethyl acetate and 300 g of isopropyl alcohol (IPA), cooled to below 10 ° C with ice water, and stirred for 1 hour to precipitate crystals. The precipitated crystals were filtered and dried under reduced pressure to obtain 110 g of gray-brown crystals. The obtained gray-brown crystals were purified by column chromatography (silica gel carrier, developing solvent: chloroform:ethyl acetate (volume ratio) = 4:1), recrystallized from methanol and dried under reduced pressure to obtain 9,9-bis(2-methoxycarbonylethyl)-2,7-diphenylfluorene (DPFDP-m).
[0429] 2.5. Example 5: Modulation of BNEF
[0430] 45 g (0.25 mol) of 9-fluorenone (manufactured by Osaka Gas Chemical Co., Ltd.), 188 g (1 mol) of ethylene glycol mono(2-naphthyl) ether, and 1 g of 3-mercaptopropionic acid were added to a 1L separable flask, and then heated to 60°C to completely dissolve. Then, 54 g of sulfuric acid was slowly added, and stirred for 5 hours while maintaining 60°C. HPLC (high performance liquid chromatography) confirmed that the conversion rate of 9-fluorenone was 99% or more. 48% sodium hydroxide water was added to the obtained reaction solution for neutralization, and then 400 g of xylene was added, washed with distilled water several times, and cooled to precipitate crystals. After filtering and drying, 9,9-bis[6-(2-hydroxyethoxy)-2-naphthyl]fluorene (BNEF) was obtained.
[0431] 2.6. Example 6: BPEF
[0432] In Example 6, BPEF: 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene, manufactured by Osaka Gas Chemical Co., Ltd., was used as a fluorene compound.
[0433] 2.7. Example 7: Modulation of FDP-m
[0434] 200 ml of 1,4-dioxane and 33.2 g (0.2 mol) of fluorene were placed in the reactor. After the fluorene was dissolved by stirring, 3.0 ml of a 40% methanol solution of trimethylbenzylammonium hydroxide (Triton B40 manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise while cooling to 10°C, and stirred for 30 minutes. Next, 37.9 g (0.44 mol) of methyl acrylate was added and stirred for about 3 hours. After the reaction was completed, 200 ml of toluene and 50 ml of 0.5 N hydrochloric acid were added for washing. After removing the water layer, the organic layer was washed three times with 30 ml of distilled water. By distilling off the solvent, 9,9-bis(methyl propionate)fluorene was obtained. It was then dissolved in 300 ml of isopropanol at 70°C, and then recrystallized by cooling to 10°C to obtain 9,9-bis(methyl propionate)fluorene (FDP-m).
[0435] Table 1 shows the evaluation results of the light absorption characteristics of the various fluorene compounds obtained as described above.
[0436] [Table 1]
[0437]
[0438] Tinuvin 928: manufactured by BASF, UV absorber
[0439] LA-F70: Made by ADEKA, UV absorber
[0440] The fluorene compounds of Examples 1 to 7 are all ultraviolet absorbers that have a small half-value width and can selectively absorb only ultraviolet rays in a specific range, and can have both excellent UV absorbency and low coloring. In particular, the fluorene compounds of Examples 1 to 3 have a larger value of the molar absorption coefficient at 380nm relative to the molar absorption coefficient at 400nm, so they can have both excellent UV absorbency and low coloring in the long wavelength region. In addition, all the fluorene compounds have a 5% mass reduction temperature higher than the existing benzotriazole ultraviolet absorber shown in Comparative Example 1, showing excellent heat resistance.
[0441] 3. Resin
[0442] 3.1. Example 8
[0443] 0.90 mol BPEF, 2.10 mol ethylene glycol (EG), 0.90 mol FDP-m, 0.10 mol DNFDP-m, and 2×10 -4 molar manganese acetate·4 hydrate and 8×10 -4 1 mol of calcium acetate monohydrate was slowly heated to melt while stirring. After the temperature reached 230°C, 14×10 -4 molar trimethyl phosphate, 20×10 -4 The germanium oxide was molten, and EG was removed while gradually increasing the temperature and reducing the pressure until it reached 270° C. and 0.13 kPa or less. After reaching a predetermined stirring torque, the contents were taken out from the reactor to prepare pellets of an ultraviolet absorbing polyester resin.
[0444] In passing 1 H-NMR analysis of the obtained particles revealed that 90 mol% of the diol component introduced into the ultraviolet absorbing polyester resin was derived from BPEFm and 10 mol% was derived from EG, and 90 mol% of the dicarboxylic acid component introduced was derived from FDP-m and 10 mol% was derived from DNFDP-m.
[0445] 3.2. Examples 9 to 13
[0446] As shown in Table 2 below, an ultraviolet absorbing polyester resin was obtained by carrying out the same operation as in Example 8 except that the monomer compositions of the diol component and the dicarboxylic acid component were changed.
[0447] Table 2 shows the ratio of each component in the ultraviolet absorbing polyester resin described in Examples 8 to 13.
[0448] [Table 2]
[0449]
[0450] The ultraviolet absorbing polyester resins of Examples 8 to 13 all showed a molar absorption coefficient (A380 ) and molar absorption coefficient (A 400 ) ratio (A 380 / A 400 ) and has both excellent UV absorbency in the long wavelength region and low coloring.
[0451] In addition, any of the ultraviolet absorbing polyester resins show a Tg of 130 to 160°C and a weight average molecular weight within the range of 50,000 to 110,000, and are excellent in processability such as stretching, elongation at break, and mechanical properties such as flexibility, and have a 5% mass reduction temperature that is higher than that of previously known benzotriazole and triazine ultraviolet absorbers, and are also excellent in heat resistance.
[0452] The ultraviolet absorbing polyester resins obtained in Examples 8 to 13 were dissolved in tetrahydrofuran to prepare 50 mg / L solutions of each, and the absorbance was measured. Figure 4 As shown. Figure 4 As shown, the ultraviolet absorbing polyester resins of Examples 8 to 13 show high absorbance to ultraviolet rays in a wide wavelength band and low absorbance to visible light.
[0453] 4. Resin composition and film
[0454] 4.1. Examples 14 to 19, Comparative Examples 3 to 6
[0455] (Preparation of Ultraviolet Absorbing Resin Composition)
[0456] A raw material obtained by dry-blending 95 parts by mass of dry pellets of a base polymer shown in Table 3 below (PC: polycarbonate, Iupilon S-3000, manufactured by Mitsubishi Engineering-Plastics Co., Ltd., PMMA: polymethyl methacrylate, Parapet HR-S, manufactured by Kuraray Co., Ltd.) and 5 parts by mass of an ultraviolet absorber was supplied to a twin-screw extruder (manufactured by Technovel Co., Ltd., model "KZW 15 / 45", screw diameter D = 15 mm, L / D = 32), and kneading was performed at a screw temperature of 280° C. and a rotation speed of 200 rpm to prepare a ultraviolet absorbing resin composition.
[0457] (Production of UV-absorbing film)
[0458] The ultraviolet absorbing resin composition obtained by the above operation was supplied to a twin-screw extruder equipped with a T die, and a film having a film thickness shown in Table 3 below was extruded and wound into a roll, thereby producing an ultraviolet absorbing film. The evaluation results of each ultraviolet absorbing film are shown in Table 3 below. As shown in Table 3, the ultraviolet absorbing films of Examples 14 to 19 showed high ultraviolet absorbing performance and low coloring. These ultraviolet absorbing films can be particularly suitable for polarizer protective film applications.
[0459] [Table 3]
[0460]
[0461] 4.2. Examples 20 to 25
[0462] (Production of UV-absorbing film)
[0463] The ultraviolet-absorbing polyester resin obtained in the above Examples 8 to 13 was supplied to a twin-screw extruder equipped with a T-die, and a film with a thickness of 50 μm was extruded and wound into a roll. Subsequently, a tenter stretching device was used to perform simultaneous biaxial stretching treatment under the condition of stretching temperature = Tg + 10°C, thereby producing an ultraviolet-absorbing film with a film thickness shown in the following Table 4.
[0464] The evaluation results of each ultraviolet absorbing film are shown in Table 4 below.
[0465] [Table 4]
[0466]
[0467] The ultraviolet absorbing films of Examples 17 to 22 showed high ultraviolet absorbing performance even when the film thickness was 14 μm or less.
[0468] Industrial Applicability
[0469] The ultraviolet absorber of the present invention has industrial applicability as a raw material for an ultraviolet absorbing coating liquid or composition, or a film obtained using these.
[0470] Description of Reference Numerals
[0471] 10…polarizer protective film; 20, 30…polarizing plate; 22, 24, 32, 33, 35…adhesive layer; 23, 34…polarizer; 21, 31…phase difference film; 40…organic EL display device; 41…organic EL display panel; 42…touch sensor; 43…front panel; 50…liquid crystal display device; 51…light source; 52…liquid crystal panel; 53…front panel.
Claims
1. An ultraviolet absorber, which is a fluorene compound represented by the general formula (1), or a resin containing the fluorene compound as a constituent unit, [Chemical formula 1] In the formula, Z 1a and Z 1b Each independently represents an aromatic hydrocarbon ring, Y 1a and Y 1b Each independently represents a carboxyl group, a carboxyl ester group, an acyl halide group, an acid anhydride group, a hydroxyl group, or a group having a polymerizable double bond, R 1a and R 1b Each independently represents a halogen atom, an acyl group, a nitro group, a cyano group, a mono- or di-substituted amino group, -R A 、-OR A , or -SR A , where R A represents a hydrocarbon group, k1 and k2 each independently represent an integer greater than 0, m1 and m2 each independently represent an integer of 0 to 4, R 2a and R 2b Each independently represents a halogen atom, a cyano group, or a hydrocarbon group other than an aryl group, n1 and n2 each independently represent an integer from 0 to 4, m1+n1 and m2+n2 are each independently an integer of 4 or less.
2. The ultraviolet absorber according to claim 1, wherein In the general formula (1), at least one of m1 and m2 is 1 or more.
3. The ultraviolet absorber according to claim 1, wherein In the general formula (1), Z 1a and Z 1b It is a condensed polycyclic aromatic hydrocarbon ring, and both m1 and m2 are integers of 1 or more.
4. The ultraviolet absorber according to claim 1, wherein In the general formula (1), Y 1a and Y 1b are each independently a group represented by the following formula (Y1), The fluorene compound is a dicarboxylic acid or a derivative thereof, The resin is a polyester resin or a polyamide resin having the fluorene compound as a dicarboxylic acid as a constituent unit, [Chemical formula 2] In the formula, A 1 Indicates straight chain or branched chain C 1-6 Alkylene.
5. The ultraviolet absorber according to claim 1, wherein In the general formula (1), Y 1a and Y 1b are each independently a group represented by the following formula (Y2), The fluorene compound is a diol, The resin is a polyester resin or a polycarbonate resin having the fluorene compound as a diol as a constituent unit, [Chemical formula 3] In the formula, A 2 and A 3 Each independently represents a linear or branched C 1-6 Alkylene, p represents an integer greater than or equal to 0.
6. The ultraviolet absorber according to claim 1, wherein In the general formula (1), Y 1a and Y 1b are each independently a group represented by the following formula (Y3), The fluorene compound is a diol, The resin is a polyester resin or a polycarbonate resin having the fluorene compound as a diol as a constituent unit, [Chemical formula 4] In the formula, Z 2 represents an aromatic hydrocarbon ring, A 4 Each independently represents a linear or branched C 1-4 Alkylene, R 3 Each independently represents a substituent, q represents an integer greater than 0, r represents an integer greater than 1, s represents an integer greater than or equal to 0.
7. The ultraviolet absorber according to claim 6, wherein In the general formula (Y3), Z 2 It is a condensed polycyclic aromatic hydrocarbon ring.
8. The ultraviolet absorber according to claim 1, wherein In the general formula (1), Y 1a and Y 1b are each independently a group represented by the following formula (Y4), The fluorene compound is di(meth)acrylate, The resin is a (meth)acrylic resin having the fluorene compound as a di(meth)acrylate as a constituent unit, [Chemical formula 5] In the formula, A 5 and A 6 Each independently represents a linear or branched C 1-6 Alkylene, R 4 represents a hydrogen atom or a methyl group, t represents an integer greater than or equal to 0. 9 . The ultraviolet absorber according to claim 1 , wherein the half-value width, which is a wavelength band of 1 / 2 or more of the absorbance at the maximum absorption wavelength, is 55 nm or less. 10 . The ultraviolet absorber according to claim 1 , which has a maximum absorption wavelength in the range of 320 to 400 nm.
11. The ultraviolet absorber according to claim 1, wherein the molar absorption coefficient (A) at 380 nm is 380 ) and the molar absorption coefficient (A 400 ) ratio (A 380 / A 400 ) is 50 or more.
12. The ultraviolet absorber according to claim 1, wherein The content of the structural unit derived from the fluorene compound is 1 to 100 mol % based on all the structural units of the resin.
13. A UV-absorbing composition comprising: The ultraviolet absorber according to claim 1; and At least one compound selected from the group consisting of a triazine ring-containing compound, a benzotriazole ring-containing compound, and a benzophenone ring-containing compound as the second ultraviolet absorber.
14. An ultraviolet absorbing resin composition comprising: The ultraviolet absorber according to claim 1; and Any resin, The content of the ultraviolet absorber is 0.1 to 10% by mass based on the total amount. 15 . An ultraviolet absorbing coating liquid comprising: the ultraviolet absorber according to claim 1 , the ultraviolet absorbing composition according to claim 13 , or the ultraviolet absorbing resin composition according to claim 14 .
16. An ultraviolet absorbing coated resin sheet comprising a resin sheet and an ultraviolet shielding layer, The ultraviolet shielding layer comprises the ultraviolet absorber according to any one of claims 1 to 12, the ultraviolet absorbing composition according to claim 13, or the ultraviolet absorbing resin composition according to claim 14.
17. An ultraviolet absorbing coated glass comprising glass and an ultraviolet shielding layer, The ultraviolet shielding layer comprises the ultraviolet absorber according to any one of claims 1 to 12, the ultraviolet absorbing composition according to claim 13, or the ultraviolet absorbing resin composition according to claim 14. 18 . An ultraviolet absorbing molded article comprising the ultraviolet absorber according to claim 1 , the ultraviolet absorbing composition according to claim 13 , or the ultraviolet absorbing resin composition according to claim 14 . 19 . An ultraviolet absorbing film comprising the ultraviolet absorber according to claim 1 , the ultraviolet absorbing composition according to claim 13 , or the ultraviolet absorbing resin composition according to claim 14 . 20 . A polarizer protective film comprising the ultraviolet absorbing film according to claim 19 . 21 . The polarizer protective film according to claim 20 , which has a spectral light transmittance of 5% or less at 350 nm and a b* value of 0.5 or less in the L*a*b* color space (CIELAB). 22 . The polarizer protective film according to claim 20 , which has a spectral light transmittance of 8% or less at 380 nm. 23 . A polarizing plate comprising the polarizer protective film according to claim 20 . 24 . An image display device comprising the polarizing plate according to claim 23 . 25 . A transport equipment comprising a member comprising the ultraviolet absorber according to claim 1 , the ultraviolet absorbing composition according to claim 13 , or the ultraviolet absorbing resin composition according to claim 14 . 26 . A building component comprising a component comprising the ultraviolet absorber according to claim 1 , the ultraviolet absorbing composition according to claim 13 , or the ultraviolet absorbing resin composition according to claim 14 .