Solid secondary battery
By introducing a high void ratio intermediate layer into the solid battery, including amorphous carbon and metal nanoparticles, the problem of unevenness of lithium metal precipitation is solved, and the circulation characteristics and interface adhesion of the solid battery are improved.
Patent Information
- Application Number
- CN202380030297.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-22
- Publication Date
- 2024-11-12
AI Technical Summary
In solid batteries, lithium metal precipitation caused by repeated charging and discharging leads to a decrease in interface bonding, affecting the cycling characteristics of the battery.
An intermediate layer with a higher void ratio than the solid electrolyte layer is introduced into the solid battery. The intermediate layer contains amorphous carbon and metal nanoparticles, and the particle adhesion is improved through the bonding material to suppress the uneven precipitation of lithium metal.
It effectively improves the circulation characteristics of solid batteries, reduces the unevenness and volume expansion of metal precipitation, and enhances electron conductivity and interface adhesion.
Smart Images

Figure CN118946998A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a solid secondary battery. Background Art
[0002] In recent years, in order to ensure that more people have access to affordable, reliable, sustainable and advanced energy, research and development related to secondary batteries that contribute to energy efficiency are being carried out. Among secondary batteries, solid batteries are particularly attractive because they are excellent in terms of improved safety due to the non-flammable solid electrolyte and higher energy density.
[0003] In a solid battery, metals such as lithium used as a charge transfer medium may be precipitated between the solid electrolyte layer and the negative electrode layer due to repeated charge and discharge. The decrease in interfacial bonding caused by the precipitation of the above-mentioned metals may reduce the electrical characteristics of the solid battery. For this problem, a technology is known that by providing a layer of lithium metal that can precipitate the negative electrode current collector, the lithium metal is precipitated roughly uniformly on the surface of the coating layer, thereby making it difficult to produce dead lithium (dead lithium) (for example, refer to patent document 1).
[0004] [Prior Technical Literature]
[0005] (Patent Document)
[0006] Patent Document 1: Japanese Patent Application Publication No. 2018-129159 Summary of the invention
[0007] [Problems to be solved by the invention]
[0008] Patent Document 1 discloses that the coating layer is made of a metal that can form an alloy with lithium. On the other hand, solid batteries undergo volume changes as they are charged and discharged, so if the intermediate layer is made of a material that does not easily follow the volume change, the cycle characteristics may be reduced due to reduced interface adhesion.
[0009] The present invention has been made in view of the above, and an object of the present invention is to provide a solid secondary battery capable of suppressing uneven precipitation of metal on the negative electrode interface of the solid secondary battery, thereby improving cycle characteristics.
[0010] [Technical means to solve the problem]
[0011] (1) The present invention relates to a solid secondary battery comprising: a positive electrode layer; a negative electrode layer comprising at least a negative electrode collector; a solid electrolyte layer comprising a solid electrolyte material; and an intermediate layer disposed between the negative electrode layer and the solid electrolyte layer; and the porosity of the intermediate layer is greater than the porosity of the solid electrolyte layer.
[0012] According to the invention of (1), it is possible to provide a solid secondary battery capable of suppressing uneven precipitation of metal on the negative electrode interface of the solid secondary battery, thereby improving cycle characteristics.
[0013] (2) The solid secondary battery according to (1), wherein the particle size of the particles constituting the intermediate layer is smaller than the particle size of the particles of the solid electrolyte material.
[0014] According to the invention of (2), the adhesion between the solid electrolyte layer and the intermediate layer can be improved, and the contact area between the solid electrolyte layer and the intermediate layer can be increased.
[0015] (3) The solid secondary battery according to (1) or (2), wherein the porosity of the intermediate layer is 40 to 70%.
[0016] According to the invention of (3), the charge transfer medium can easily pass through the intermediate layer and the structure of the intermediate layer can be easily maintained, so that the metal is less likely to precipitate at the interface between the intermediate layer and the solid electrolyte layer.
[0017] (4) The solid secondary battery according to any one of (1) to (3), wherein the intermediate layer contains amorphous carbon.
[0018] According to the invention of (4), the electron conductivity of the intermediate layer can be ensured, and the particles constituting the intermediate layer can be prevented from reacting with the charge transfer medium and forming an alloy.
[0019] (5) The solid secondary battery according to any one of (1) to (4), wherein the intermediate layer contains a binder.
[0020] According to the invention of (5), the adhesion between particles constituting the intermediate layer and between the intermediate layer and the solid electrolyte layer can be improved, so the structure of the intermediate layer can be easily maintained.
[0021] (6) The solid secondary battery according to any one of (1) to (5), wherein the intermediate layer contains metal nanoparticles, and a content of the metal nanoparticles in the intermediate layer exceeds 0 mass % and is 30 mass % or less.
[0022] According to the invention of (6), the volume expansion of the intermediate layer can be reduced, the structural destruction of the intermediate layer and the uneven precipitation of the charge transfer medium can be suppressed, and the electronic conductivity of the intermediate layer can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a cross-sectional schematic diagram showing the structure of the solid secondary battery of this embodiment.
[0024] Figure 2 yes Figure 1, which is an enlarged view of a main part, is a diagram showing the structure of a solid secondary battery before charge and discharge.
[0025] Figure 3 yes Figure 1 , which is an enlarged view of the main part, is a diagram showing the structure of the solid secondary battery after charge and discharge.
[0026] Figure 4A This is a microscope photograph of a main part of a solid secondary battery of a comparative example.
[0027] Figure 4B This is a microscope photograph of a main part of a solid secondary battery of a comparative example.
[0028] Figure 5A This is a microscope photograph of the main part of the solid secondary battery of the example.
[0029] Figure 5B This is a microscope photograph of the main part of the solid secondary battery of the example.
[0030] Figure 6 It is a graph showing the relationship between the cycle number and the capacity retention rate of the solid secondary batteries of the examples and comparative examples.
[0031] Figure 7 It is a graph showing the relationship between the cycle number and the capacity retention rate of the solid secondary batteries of the examples and comparative examples. DETAILED DESCRIPTION
[0032] <Solid State Secondary Batteries>
[0033] like Figure 1 As schematically shown in FIG. 1 , the solid secondary battery 1 of the present embodiment is composed of a positive electrode layer 20, a solid electrolyte layer 40, an intermediate layer 50, and a negative electrode layer 30 stacked in this order. Figure 1 2 is a diagram schematically showing the structure of the solid secondary battery 1 after charge and discharge. Therefore, a metal precipitation layer 60 is formed between the intermediate layer 50 and the negative electrode layer 30 .
[0034] (Positive electrode layer)
[0035] The positive electrode layer 20 is a layer composed of a positive electrode current collector 21 and a positive electrode active material layer 22 containing at least a positive electrode active material.
[0036] Positive electrode current collector 21 is not particularly limited as long as it has the function of collecting electricity in the positive electrode layer, and for example, aluminum, aluminum alloy, stainless steel, nickel, iron and titanium etc. can be listed, wherein aluminum, aluminum alloy and stainless steel are preferred. In addition, as the shape of the positive electrode current collector, for example, foil, plate etc. can be listed.
[0037] The positive electrode active material contained in the positive electrode active material layer 22 can be the same as the positive electrode active material used in the positive electrode layer of a general solid battery, and is not particularly limited. For example, in the case of a lithium ion battery, a layered active material containing lithium, a spinel type active material, an olivine type active material, etc. can be listed. Specific examples of positive electrode active materials include lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), LiNi p Mn q Co r O2(p+q+r=1), LiNi p Al q Co r O2 (p+q+r=1), lithium manganese oxide (LiMn2O4), heterogeneous element substituted Li-Mn spinel represented by Li1+xMn2-x-yMyO4 (x+y=2, M is selected from at least one of Al, Mg, Co, Fe, Ni and Zn), lithium titanate (oxide containing Li and Ti), lithium metal phosphate (LiMPO4, M is selected from at least one of Fe, Mn, Co and Ni), etc.
[0038] From the perspective of improving the conductivity of the charge transfer medium, the positive electrode active material layer 22 may also contain a solid electrolyte. In addition, a conductive aid may be contained arbitrarily to improve conductivity. Furthermore, from the perspective of showing flexibility, a binder may be contained arbitrarily. Regarding the solid electrolyte, conductive aid, and binder, solid electrolytes, conductive aids, and binders commonly used in solid batteries can be used.
[0039] (Negative electrode layer)
[0040] The negative electrode layer 30 is a layer composed of a negative electrode current collector 31 and a negative electrode active material layer 32 containing at least a negative electrode active material.
[0041] The negative electrode current collector 31 is not particularly limited as long as it has the function of collecting current in the negative electrode layer, and examples of the material of the negative electrode current collector include nickel, copper, and stainless steel, etc. In addition, examples of the shape of the negative electrode current collector include foil and plate.
[0042] As the negative electrode active material contained in the negative electrode active material layer 32, a known material that can absorb and release charge transfer media such as lithium ions can be appropriately selected. For example, lithium transition metal oxides such as lithium titanate, transition metal oxides such as TiO2, Nb2O3 and WO3, Si, SiO, metal sulfides, metal nitrides, and carbon materials such as artificial graphite, natural graphite, graphite, soft carbon and hard carbon, as well as metallic lithium, metallic indium and lithium alloys can be listed. As the negative electrode active material, metallic lithium is preferred. This is because, when the solid secondary battery 1 of this embodiment uses metallic lithium as the negative electrode active material, the precipitation of dendrites can be better suppressed. The negative electrode active material can be either powdery or thin-film.
[0043] From the perspective of improving the conductivity of the charge transfer medium, the negative electrode active material layer 32 may also contain a solid electrolyte. In addition, a conductive aid may be contained arbitrarily to improve conductivity. Furthermore, from the perspective of showing flexibility, a binder may be contained arbitrarily. Regarding the solid electrolyte, conductive aid, and binder, solid electrolytes, conductive aids, and binders commonly used in solid batteries can be used.
[0044] (Solid electrolyte layer)
[0045] The solid electrolyte layer 40 is a layer stacked between the positive electrode layer 20 and the negative electrode layer 30, and is a layer containing at least a solid electrolyte material. The solid electrolyte material contained in the solid electrolyte layer enables charge transfer between the positive electrode active material and the negative electrode active material.
[0046] The solid electrolyte material is not particularly limited as long as it has charge transfer medium conductivity, and examples thereof include sulfide solid electrolyte materials, oxide solid electrolyte materials, nitride solid electrolyte materials, and halide solid electrolyte materials.
[0047] As sulfide solid electrolyte materials, for example, in the case of lithium ion batteries, Li2S-P2S5, Li2S-P2S5-LiI, etc. can be cited. In addition, the above description of "Li2S-P2S5" refers to a sulfide solid electrolyte material formed using a raw material composition containing Li2S and P2S5, and the same applies to other similar descriptions.
[0048] As oxide solid electrolyte materials, for example, in the case of lithium ion batteries, sodium superionic conductor (Na superionic conductor, NASICON) type oxides, garnet type oxides, perovskite type oxides, etc. can be listed. As NASICON type oxides, for example, oxides containing Li, Al, Ti, P and O (such as Li 1.5 Al0.5 Ti 1.5 (PO4)3). Examples of garnet-type oxides include oxides containing Li, La, Zr, and O (e.g., Li7La3Zr2O 12 ). Examples of perovskite-type oxides include oxides containing Li, La, Ti, and O (eg, LiLaTiO 3 ).
[0049] The porosity of the solid electrolyte layer 40 is lower than that of the intermediate layer 50 described later, for example, less than 10%. In addition, the particle size of the solid electrolyte material 41 constituting the solid electrolyte layer 40 is, for example, 0.5 μm to 10 μm in terms of median particle size (D50), and is preferably larger than that of the particles constituting the intermediate layer described later.
[0050] The porosity of the solid electrolyte 40 can be obtained, for example, by the following formula (1). In the formula (1), the "filling rate" refers to the percentage of the density of the solid electrolyte layer after molding relative to the true density.
[0051] Void ratio (%) = (100 - filling ratio (%))…(1)
[0052] The method for calculating the porosity is not limited to the above method, and the porosity may be calculated by machine analysis using BET, a porosimeter, gas diffusion or the like, or by image analysis using a scanning electron microscope or the like.
[0053] (Middle layer)
[0054] The intermediate layer 50 is a layer stacked between the negative electrode layer 30 and the solid electrolyte layer 40. The intermediate layer 50 can suppress uneven precipitation of metal on the interface of the negative electrode layer 30 and improve the interface adhesion. Figure 2 and Figure 3 As shown, the intermediate layer 50 preferably includes amorphous carbon 51 and metal nanoparticles 52 .
[0055] use Figure 2 and Figure 3 The function of the intermediate layer 50 will be described. Figure 2 yes Figure 1 1 is an enlarged view of a portion where the solid electrolyte layer 40, the intermediate layer 50, and the negative electrode layer 30 are stacked, and is a schematic diagram showing a state in which the solid secondary battery 1 is immediately produced and before charge and discharge are performed. Figure 3 is with Figure 2The corresponding figure is a schematic diagram showing the state after repeated charging and discharging of the solid secondary battery 1. In the following, it is assumed that the charge transfer medium of the solid secondary battery 1 is Li ions for explanation. If it is an existing solid secondary battery without an intermediate layer 50, metallic lithium will be precipitated at the interface between the solid electrolyte layer and the negative electrode layer as the solid secondary battery is repeatedly charged and discharged. Once metallic lithium is precipitated, the electronic conductivity of the part will become higher, so metallic lithium will be precipitated unevenly, for example, dendrites will be generated. As a result, it is possible that the negative electrode active material layer 32 becomes porous when repeatedly charged and discharged, and the interface adhesion decreases, thereby reducing the battery performance.
[0056] On the other hand, the intermediate layer 50 of the solid secondary battery 1 of this embodiment has electron conductivity and has gaps through which Li ions can pass. Figure 3 As shown, as the solid secondary battery 1 is repeatedly charged and discharged, the Li ions moving from the solid electrolyte layer 40 toward the negative electrode active material layer 32 pass through the intermediate layer 50, and a metal precipitation layer 60 (metal lithium layer) is formed between the intermediate layer 50 and the negative electrode active material layer 32. Thus, the metal precipitation layer 60 can be uniformly formed. In addition, since the intermediate layer 50 has the flexibility to follow the volume changes of each layer accompanying the charge and discharge, the interface adhesion can be maintained even when the solid secondary battery 1 is repeatedly charged and discharged, thereby improving the durability of the solid secondary battery 1.
[0057] The porosity of the intermediate layer 50 is higher than the porosity of the solid electrolyte layer 40. Thus, a gap through which Li ions can pass can be formed inside the intermediate layer 50, and the intermediate layer 50 can flexibly follow the volume change of the solid secondary battery 1. The porosity of the intermediate layer 50 can be set to 40 to 70%, for example. As a method for calculating the porosity of the intermediate layer 50, the same method as the method for calculating the porosity of the solid electrolyte 40 can be applied.
[0058] The intermediate layer 50 preferably includes amorphous carbon 51. Amorphous carbon 51 is different from graphite, etc., and does not react with lithium metal and the like to form an alloy, so the formation of dendrites can be suppressed, thereby improving the cycle characteristics of the solid secondary battery 1. As amorphous carbon 51, for example, carbon black such as acetylene black, furnace black, Ketjen black, coke, activated carbon, etc. can be listed. Amorphous carbon 51 can be easily graphitized carbon (soft carbon), or difficult to graphitize carbon (hard carbon), carbon nanotubes (carbon nano tubes, CNT), fullerene, and graphene.
[0059] The amorphous carbon mentioned here is a substance that does not show a clear crystalline state among carbon allotropes. Strictly speaking, it is not amorphous, but an aggregate of fine crystals of graphite. In other words, amorphous carbon refers to carbon allotropes other than diamond and graphite.
[0060] The intermediate layer 50 preferably includes metal nanoparticles 52. By making the intermediate layer 50 include metal nanoparticles 52, the electronic conductivity of the intermediate layer 50 can be improved, and the metal precipitation layer 60 can be formed more uniformly. In addition, since the metal nanoparticles 52 have a Young's modulus higher than that of the amorphous carbon 51, the structure of the intermediate layer 50 can be maintained even when high pressure pressing is performed when the solid secondary battery 1 is manufactured. As the metal nanoparticles 52, for example, metal nanoparticles such as tin (Sn), silicon (Si), zinc (Zn), magnesium (Mg), gold (Au), platinum (Pt), palladium (Pd), silver (Ag), aluminum (Al), bismuth (Bi), and antimony (Sb) can be listed. The content of the metal nanoparticles 52 is preferably in the intermediate layer 50, exceeding 0% by mass and being less than 30% by mass.
[0061] The particle size of particles such as amorphous carbon 51 and metal nanoparticles 52 constituting the intermediate layer 50 is preferably smaller than the particle size of the solid electrolyte material 41. As a result, the intermediate layer 50 can enter the gap between the solid electrolyte materials 41 constituting the interface of the solid electrolyte layer 40, so the contact area between the solid electrolyte layer 40 and the intermediate layer 50 can be increased, and the adhesion can be improved. The particle size of the amorphous carbon 51 can be, for example, a material with a median particle size (D50) of about 0.04 μm to 0.05 μm, and the particle size of the metal nanoparticles 52 can be, for example, a material with a median particle size (D50) of about 0.07 μm.
[0062] In order to maintain the structure of the intermediate layer 50, the intermediate layer 50 preferably includes an adhesive as a bonding material. Thus, the adhesion between the particles constituting the intermediate layer 50 and between the intermediate layer 50 and the solid electrolyte layer 40 can be improved. As an adhesive, there is no particular limitation, and an adhesive commonly used in solid batteries can be used. For example, acrylic polymers, cellulose polymers, styrene polymers, vinyl acetate polymers, carbamate polymers, fluoroethylene polymers, etc., polyvinylidene fluoride (PVDF) polymers can be cited.
[0063] <Solid State Secondary Batteries>
[0064] The solid secondary battery 1 of this embodiment is formed by combining a positive electrode layer 20, a solid electrolyte layer 40, an intermediate layer 50 and a negative electrode layer 30. Figure 1 In addition, after the above stacking, it is also possible to press and integrate them. Figure 1 A plurality of the structural units shown are stacked as unit cells.
[0065] As mentioned above, although the preferred embodiment of the present invention has been described, the present invention is not limited to the above-mentioned embodiment, and modifications and improvements within the scope that can achieve the object of the present invention are included in the present invention.
[0066] Example
[0067] Hereinafter, the present invention will be described in detail using examples, but the present invention is not limited to these examples.
[0068] <Example 1>
[0069] [Fabrication of Solid Electrolyte Layer]
[0070] As the solid electrolyte material, an argyrodite-type sulfide solid electrolyte was used.
[0071] [Production of positive electrode layer]
[0072] A slurry is made using lithium nickel cobalt manganese composite oxide (NCM622) as a positive electrode active material, an argyrodite-type sulfide solid electrolyte as a solid electrolyte, butyl butyrate as a solvent, carbon black as a conductive aid, and a styrene butadiene rubber (SBR)-based binder as a binder, which is applied to an aluminum foil as a positive electrode collector and dried to produce a positive electrode layer.
[0073] [Production of negative electrode layer]
[0074] Metal lithium was used as the negative electrode active material and joined to a stainless steel (Steel Use Stainless, SUS) foil as an electrode current collector to produce a negative electrode layer.
[0075] [Creation of the middle layer]
[0076] The intermediate layer was produced by using Sn as metal nanoparticles, acetylene black (particle size 0.05 μm) as amorphous carbon, N-methyl-2-pyrrolidinone (NMP) as a solvent, and PVDF-based adhesive as a binder to make a slurry, which was then applied and dried.
[0077] [Fabrication of solid secondary batteries]
[0078] The positive electrode layer, solid electrolyte layer, intermediate layer and negative electrode layer obtained by the above are stacked in sequence and pressed to produce the solid secondary battery of Example 1. The porosity of the intermediate layer after production is 41%. The porosity of the intermediate layer is calculated by the following formula (2). In formula (2), the so-called "filling rate" refers to the percentage of the density of the intermediate layer after molding relative to the true density.
[0079] Void ratio (%) = (100 - filling ratio (%))…(2)
[0080] <Examples 2 to 10, Comparative Examples 1 to 3>
[0081] Solid secondary batteries of other examples and comparative examples were prepared in the same manner as in Example 1, except that the structures of the intermediate layer and the solid electrolyte layer were as shown in Tables 1 and 2. In Comparative Example 1, no intermediate layer was prepared.
[0082]
[0083] [Cross-section observation]
[0084] Using a field emission scanning electron microscope (FE-SEM): S-4300SE (manufactured by Hitachi High-Tech) ( Figure 4A and Figure 5A ) and optical microscope ( Figure 4B and Figure 5B ), the charge and discharge of the solid secondary battery of Example 1 and Comparative Example 1 was observed near the interface of the negative electrode layer or solid electrolyte layer after 20 cycles of charge and discharge at a C rate of 1 / 3C at 25°C. The results of Comparative Example 1 are shown in Figure 4A and Figure 4B The results of Example 1 are shown in Figure 5A and Figure 5B .
[0085] like Figure 4A and Figure 4B As shown in FIG. 1 , the solid secondary battery 1a of Comparative Example 1 was observed to have a metal precipitation layer 60 formed at the interface between the solid electrolyte layer 40 and the negative electrode layer, and the metal precipitation layer 60 was in a porous state. Figure 5A and Figure 5B As shown, in the solid secondary battery 1 of Example 1, it was confirmed that a metal precipitation layer 60 was formed at the interface between the intermediate layer 50 and the negative electrode layer, and the metal precipitation layer 60 was not porous.
[0086] [Capacity maintenance rate measurement]
[0087] Using the solid secondary batteries of Example 1 and Comparative Example 1, a cycle test was performed in which charge and discharge were repeated at a charge upper limit voltage of 4.3 V, a discharge lower limit voltage of 2.65 V, and a C rate of 1 / 3C, and the capacity retention rate was measured. Figure 6 This is the test result at 25℃. Figure 7 This is the test result at 45°C. Figure 6 and Figure 7 The vertical axis of the graph in represents the capacity retention rate (%), and the horizontal axis represents the number of cycles (times).
[0088] like Figure 6 and Figure 7 As shown, the solid secondary battery of Example 1 has a slower decrease in capacity retention rate with an increase in the number of cycles than the solid secondary battery of Comparative Example 1, and thus obtains better cycle characteristics.
[0089] [Battery characteristics evaluation]
[0090] The solid secondary batteries of each embodiment and each comparative example were used to perform 50 cycles of charge and discharge at a C rate of 1 / 3C and 45°C, and the discharge capacity retention rate (%) at a C rate of 1 / 10C and 25°C after the cycle test, the average charge and discharge efficiency (%) of 1 to 50 cycles, and the Li passing condition of the intermediate layer were evaluated. The Li passing condition of the intermediate layer was evaluated by the following criteria. The results are shown in Tables 1 and 2.
[0091] (Li passing condition evaluation criteria of the intermediate layer)
[0092] 2 A metal deposition layer is formed between the intermediate layer and the negative electrode layer.
[0093] 1 A metal precipitation layer is not formed between the intermediate layer and the negative electrode layer, or a metal precipitation layer is formed in the solid electrolyte layer or between the intermediate layer and the solid electrolyte layer.
[0094] According to the results of Table 1 and Table 2, it is clear that in the solid secondary batteries of each embodiment, a metal precipitation layer is formed between the intermediate layer and the negative electrode layer. In addition, the following results are clear: the solid secondary batteries of each embodiment have higher values of discharge capacity retention rate (%) after cycle test and average charge and discharge efficiency (%) of 1 to 50 cycles than the solid secondary batteries of each comparative example, and obtain better cycle characteristics.
[0095] Reference numerals
[0096] 1 Solid state secondary battery
[0097] 20 Positive electrode layer
[0098] 30 Negative electrode layer
[0099] 31. Negative electrode collector
[0100] 40 Solid electrolyte layer
[0101] 41 Solid Electrolyte Materials
[0102] 50 Middle Layer
[0103] 51 Amorphous Carbon
[0104] 52 Metal Nanoparticles
Claims
1. A solid secondary battery having: positive electrode layer; A negative electrode layer, comprising at least a negative electrode current collector; a solid electrolyte layer comprising a solid electrolyte material; and, an intermediate layer disposed between the negative electrode layer and the solid electrolyte layer; and The porosity of the intermediate layer is greater than the porosity of the solid electrolyte layer.
2. The solid secondary battery according to claim 1, in, The particle size of the particles constituting the intermediate layer is smaller than the particle size of the particles of the solid electrolyte material.
3. The solid secondary battery according to claim 1 or 2, in, The void ratio of the intermediate layer is 40 to 70%.
4. The solid secondary battery according to any one of claims 1 to 3, in, The aforementioned intermediate layer contains amorphous carbon.
5. The solid secondary battery according to any one of claims 1 to 4, in, The intermediate layer includes a bonding material.
6. The solid secondary battery according to any one of claims 1 to 5, in, The intermediate layer contains metal nanoparticles, and a content of the metal nanoparticles in the intermediate layer exceeds 0 mass % and is 30 mass % or less.