Method for manufacturing solid-state battery and device for manufacturing solid-state battery
By adopting specific mold design and segmentation processes during the manufacturing process of solid batteries, the problem of short-circuiting of the positive electrode layer and the negative electrode layer during the laminated body segmentation process is solved, the yield and reliability of the solid battery are improved, and the partitioning surface is ensured. Smoothness.
Patent Information
- Application Number
- CN202380029933.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-28
- Filing Date
- 2023-02-24
- Publication Date
- 2024-11-12
AI Technical Summary
In the conventional solid battery manufacturing method, short circuits between the positive electrode layer and the negative electrode layer are easily caused during the partitioning process of the laminated body, resulting in low yield and poor reliability.
By adopting a specific mold design and division process, by dividing the blade portion of the second mold within the position range of the main surface SA1 of the positive electrode layer, combined with the placement process, we ensure that the main surface SA1 of the laminated body is closer to the first than the main surface SA2. The mold is used to make the blade portion and the first mold close to each other to divide the laminated body.
The short circuit between the positive electrode layer and the negative electrode layer is effectively suppressed, the yield and reliability of the solid battery are improved, the division surface is smooth, and the roughness of the division surface is reduced.
Smart Images

Figure CN118947000A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a solid battery, a method for manufacturing a solid battery, and a device for manufacturing a solid battery. Background Art
[0002] At present, solid batteries have attracted attention. Solid batteries include a laminate (power generation element) in which a solid electrolyte layer is arranged between a positive electrode collector and a negative electrode collector. When manufacturing a solid battery, sometimes after manufacturing a large laminate including power generation elements of a plurality of batteries, the laminate is divided into pieces corresponding to each battery. In the past, various methods have been proposed for dividing the laminate.
[0003] Patent document 1 (Japanese Patent Gazette No. 2020-61258) discloses "a method for manufacturing a solid battery, comprising: a stack extrusion process, extruding a stack having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer between the positive electrode layer and the negative electrode layer; and a shearing process, punching the stack into a specified shape by shearing the stack to form a plurality of single cell components."
[0004] Patent document 2 (International Publication No. 2019 / 131503) discloses "a method for manufacturing an all-solid-state battery, characterized in that it includes: a stacking body forming process for forming a stacking body, wherein the stacking body includes a first electrode layer, a second electrode layer having a polarity opposite to that of the first electrode layer, and a solid electrolyte layer between the first electrode layer and the second electrode layer; and a cutting process for cutting off the outer peripheral end of the stacking body, wherein the stacking body includes a powder material." Prior art literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2020-61258 Patent Document 2: International Publication No. 2019 / 131503 Summary of the invention
[0006] However, in the method of punching the laminate in the previous shearing process as in Patent Document 1, there is a problem that the cross section of the laminate is rough and a short circuit between the positive electrode layer and the negative electrode layer is easily generated. Under such circumstances, one of the objects of the present invention is to provide a manufacturing method and a manufacturing device that can manufacture a solid battery with a good yield rate and is not prone to short circuit between the positive electrode layer and the negative electrode layer.
[0007] One embodiment of the present invention relates to a method for manufacturing a solid battery. The manufacturing method is a method for manufacturing a solid battery using a laminate including a power generation element, the power generation element including a positive electrode layer, a negative electrode layer, and a solid electrolyte layer arranged between the positive electrode layer and the negative electrode layer, the laminate having a main surface SA1 and a main surface SA2 on the opposite side of the main surface SA1, the solid electrolyte layer having a main surface SB1 on the main surface SA1 side and a main surface SB2 on the main surface SA2 side, the manufacturing method including: a placement step of placing the laminate on a placement surface of the first mold in a manner that the main surface SA1 is closer to the first mold than the main surface SA2; and a splitting step of splitting the laminate by bringing the blade of the second mold close to the first mold in a manner that the blade approaches the first mold from the main surface SA2 side, and in the splitting step, the laminate is split by bringing the blade close to the first mold within a range where at least a portion of the blade does not pass through the main surface SA1.
[0008] Another embodiment of the present invention relates to a manufacturing device for a solid battery. The manufacturing device is a manufacturing device for a solid battery that performs a process of splitting a stacked body including a power generation element, the manufacturing device for a solid battery including a first mold on which the stacked body is placed, a second mold, and a drive mechanism that reversibly brings the first mold and the second mold close to each other, the power generation element including a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, the stacked body having a main surface SA1 and a main surface SA2, the solid electrolyte layer having a main surface SB1 on the main surface SA1 side and a main surface SB2 on the main surface SA2 side, the stacked body is placed on the placement surface of the first mold in a manner that the main surface SA1 is closer to the first mold than the main surface SA2, the driving mechanism brings the blade and the first mold close to each other in a manner that the blade of the second mold approaches the first mold from the main surface SA2 side, and the stacked body is split by the driving mechanism bringing the blade and the first mold close to each other within a range where at least a portion of the blade does not pass through the main surface SA1.
[0009] As long as they can be combined, the matters described in two or more claims arbitrarily selected from the plurality of claims described in the appended claims can be combined. In addition, various structures described in the following embodiments can be arbitrarily combined as long as they can be combined.
[0010] According to the present invention, a solid battery in which a short circuit between a positive electrode layer and a negative electrode layer is unlikely to occur can be manufactured with a high yield. The novel features of the present invention are described in the appended claims, both in terms of structure and content, and together with other objects and features of the present invention, will be better understood through the following detailed description with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 A cross-sectional view schematically shows an example of a laminate divided by the production method of the first embodiment. Figure 2A This is a cross-sectional view schematically showing one step of the manufacturing method according to the first embodiment. Figure 2B It is schematically indicated Figure 2A A cross-sectional view of an example of a process subsequent to a process of. Figure 3 It is schematically indicated Figure 2A An overhead view of a process. Figure 4 It is schematically indicated Figure 2A A cross-sectional view of another example of a process subsequent to a process of. Figure 5 This is a diagram schematically showing an example of a production apparatus according to the first embodiment. Figure 6 This is a diagram schematically showing a part of another example of the production apparatus according to the first embodiment. DETAILED DESCRIPTION
[0012] Below, the embodiments of the present invention are illustrated, but the present invention is not limited to the examples described below. In the following description, there are cases where specific numerical values and materials are illustrated, but other numerical values and other materials can also be applied as long as the invention of the present invention can be implemented. In this specification, the description of "numerical value A to numerical value B" includes numerical value A and numerical value B, which can be replaced by "above numerical value A and below numerical value B". In the following description, when the lower limit and upper limit of numerical values related to specific physical properties, conditions, etc. are illustrated, as long as the lower limit is not above the upper limit, any one of the exemplified lower limits and any one of the exemplified upper limits can be arbitrarily combined.
[0013] The manufacturing method of this embodiment is described below. Hereinafter, the manufacturing method is sometimes referred to as "manufacturing method (M)". Examples of solid batteries manufactured by manufacturing method (M) include batteries called by names such as all-solid batteries, semi-solid batteries, quasi-solid batteries, and all-resin batteries.
[0014] The manufacturing method (M) is particularly preferably used for the manufacture of all-solid batteries. The following mainly describes the embodiments of all-solid batteries, but in the case of manufacturing solid batteries other than all-solid batteries, as power generation elements, it is sufficient to use power generation elements of corresponding solid batteries. In the following description, in the description other than the description that can only be applied to specific batteries, as long as the record does not cause contradiction, "all-solid battery" can also be replaced by "solid battery". In addition, "all-solid batteries" are sometimes referred to as "solid batteries" in the world. Therefore, as long as the record does not cause contradiction, in the following description, "all-solid batteries" can also be referred to as "solid batteries".
[0015] In addition, the present invention relates to a solid battery (e.g., a fully solid battery) manufactured by a manufacturing method (M). The split surface of the power generation element split by the splitting process described later is less likely to cause a short circuit than the split surface of the power generation element split by a conventional shearing process. Therefore, the solid battery is less likely to cause a short circuit after manufacturing, and has high reliability.
[0016] In this specification, examples of solid batteries include batteries that do not contain liquid components as a constituent element of the electrolyte. For example, examples of solid batteries include batteries that do not contain liquid components as a constituent element required to function as a battery, such as batteries that do not contain liquid components. Here, "liquid component" refers to a component that is liquid at room temperature (25°C). In addition, examples of solid batteries generally include batteries referred to as all-solid batteries or semi-solid batteries. In addition, examples of solid batteries also include batteries generally referred to as quasi-solid batteries. That is, solid batteries may also contain trace amounts of liquid components.
[0017] (Manufacturing method (M)) The manufacturing method (M) of this embodiment is a manufacturing method of a solid battery using a laminate including a power generation element. The power generation element includes a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer. The laminate has a main surface SA1 and a main surface SA2 on the opposite side of the main surface SA1. The solid electrolyte layer has a main surface SB1 on the main surface SA1 side and a main surface SB2 on the main surface SA2 side.
[0018] The manufacturing method (M) includes a placement step and a segmentation step in sequence. The placement step is a step of placing the laminate on the placement surface of the first mold in such a manner that the main surface SA1 is closer to the first mold than the main surface SA2. The segmentation step is a step of segmenting the laminate by bringing the blade of the second mold close to the first mold from the main surface SA2 side. In addition, the blade of the second mold refers to a portion (corner) in the second mold that contacts the laminate in order to segment the laminate in the segmentation step.
[0019] In the dividing step, the following conditions (1) and / or (2) are satisfied. In the dividing step, the following conditions (2) and / or (3) may be satisfied, or the following conditions (2) and / or (4) may be satisfied. (1) In the dividing step, the stacked body is divided by bringing the blade and the first mold closer together within a range where at least a portion of the blade of the second mold (hereinafter sometimes referred to as "a portion (P)") does not pass through the placement surface of the first mold (the surface in contact with the main surface SA1 of the stacked body). (2) In the splitting step, the stacked body is split by bringing the blade and the first mold closer together within a range where at least a portion (P) of the blade of the second mold does not pass through the position of the main surface SA1 of the stacked body. In this case, when the blade and the first mold are closest, the portion (P) is located at the same position as the main surface SA1 or between the main surface SA1 and the main surface SA2. (3) In the splitting step, the blade of the second mold is brought close to the first mold within a range where at least a portion (P) of the blade of the second mold does not reach the main surface SB1 of the solid electrolyte layer to split the laminate. According to this structure, short circuits between the positive electrode layer and the negative electrode layer can be particularly suppressed. In this case, the closest position of the portion (P) can be located at a position farther from the placement surface of the first mold than the main surface SB1 of the solid electrolyte layer. (4) In the splitting step, the blade of the second mold is brought close to the first mold within a range where at least a portion (P) of the blade of the second mold does not reach the position of the main surface SB2 of the solid electrolyte layer to split the laminate. According to this structure, short circuits between the positive electrode layer and the negative electrode layer can be particularly suppressed. In this case, the closest position of the above-mentioned portion (P) can be located at a position farther from the placement surface of the first mold than the main surface SB2 of the solid electrolyte layer.
[0020] The "range of the position that does not pass through the placement surface of the first mold" of condition (1) includes the case where the arrival position of the blade is the position of the placement surface of the first mold. The "range of the position that does not pass through the main surface SA1" of condition (2) includes the case where the arrival position of the blade is the position of the main surface SA1. In the splitting process, the above-mentioned part (P) moves to the main surface SA1 side closer to the main surface SA2. That is, in the splitting process, the above-mentioned part (P) moves within the range that passes through the main surface SA2 and does not pass through the main surface SA1.
[0021] The splitting step may satisfy the following condition (1') instead of condition (1), or the following condition (2') instead of condition (2). That is, in the description of this specification, condition (1) may be replaced by condition (1'), or condition (2) may be replaced by condition (2'). (1') In the splitting step, the blade of the second mold is brought close to the first mold within a range where at least a portion (P) of the blade does not reach the placement surface of the first mold to split the laminate. (2') In the splitting step, the blade of the second mold is brought close to the first mold within a range where at least a portion (P) of the blade does not reach the main surface SA1 of the laminate to split the laminate.
[0022] The above-mentioned position refers to a coordinate position when the direction in which the mold moves in the splitting step is used as a coordinate axis. This also applies to the following description, for example, the description of conditions (5) to (7) described later.
[0023] In Patent Document 1, a plurality of single cell components are formed by punching out a laminate (power generating element) into a predetermined shape by shearing. However, if the laminate including the power generating element is cut by the conventional shearing method, the cut surface is rough and short circuits are likely to occur.
[0024] In the previous shearing method, the workpiece is sheared by moving the upper mold so that the blade of the lower mold crosses the blade of the upper mold. Since the laminate constituting the solid battery is thin, it is common knowledge for those skilled in the art that the workpiece can be divided by methods other than the previous shearing method. However, the inventors of the present application have newly discovered that the laminate can be divided by a method completely different from the previous shearing method, and thereby the short circuit between the positive electrode layer and the negative electrode layer can be suppressed. The present invention is based on this new insight.
[0025] In the segmentation process of the manufacturing method (M), the blade of the second mold does not cross the stack in the thickness direction. In addition, compared with the previous shearing process, in the segmentation process of the manufacturing method (M), the segmentation surface of the stack is less rubbed by the first mold and / or the second mold. Therefore, it is possible to suppress the roughness of the segmentation surface during segmentation, and as a result, it is possible to suppress the short circuit between the positive electrode layer and the negative electrode layer. That is, according to the manufacturing method (M), a solid battery with high characteristics can be manufactured with a good yield. An example of a placement process and an example of a segmentation process are described below.
[0026] (Placement process) As described above, the placing step is a step of placing the stack on the placing surface of the first mold so that the main surface SA1 of the stack is closer to the first mold than the main surface SA2 of the stack. In other words, the stack is placed so that the main surface SA2 of the stack is closer to the second mold than the main surface SA1.
[0027] In the placement step, the laminate may be arranged so that the positive electrode layer is closer to the main surface SA1 than the negative electrode layer. Alternatively, the laminate may be placed so that the negative electrode layer is closer to the main surface SA1 than the positive electrode layer.
[0028] (Separation process) As described above, the dividing step is a step of dividing the stacked body by bringing the blade of the second die closer to the first die from the main surface SA2 side.
[0029] Through the splitting process, the laminate is split at the linear splitting position. At the splitting position, the shoulder of the first mold and the blade of the second mold are close to each other. As a result, the blade of the second mold contacts the laminate, and the laminate located between the shoulder of the first mold and the blade of the second mold is split. From one point of view, the shoulder of the first mold is the blade of the first mold.
[0030] The linear division position is usually when the laminate is viewed from above (see Figure 3 ) is a straight line. However, as long as the stack can be divided, the dividing position may not be a straight line, and may include a straight line portion and a non-straight line portion. When the stack is viewed from above (refer to Figure 3 ), the splitting position may include a curve or a bend. The splitting position may be curved. The splitting position may be bent at an angle greater than 90°. By changing the shape of the shoulder of the first mold and the shape of the blade of the second mold, the shape of the splitting position can be changed. For example, by making the shoulder of the first mold and the blade of the second mold extend in a straight line, the shape of the splitting position can be a straight line.
[0031] In an example of a typical configuration of the first and second molds, the first mold is the lower mold and the second mold is the upper mold. In this case, by moving the second mold downward, the second mold can be brought close to the first mold. However, as long as the splitting process can be implemented, the configuration of the first mold and the second mold is not limited to this typical configuration. For example, the first mold can be used as the upper mold and the second mold can be used as the lower mold. Alternatively, the two molds can be configured in the horizontal direction.
[0032] Typically, when the blade of the second die is brought close to the first die, only the second die is moved. Therefore, the following mainly describes the case where only the blade of the second die is moved. However, as long as the splitting process can be implemented, the blade of the second die may be brought close to the first die by only moving the first die toward the second die. Alternatively, the blade of the second die may be brought close to the first die by moving both the first die and the second die.
[0033] In the splitting step, the approach speed between the first and second molds (eg, the moving speed of the second mold) may be in the range of 10 to 1000 mm / s (preferably 70 to 700 mm / s). By setting it in this range, the splitting step can be easily and appropriately performed.
[0034] In the segmentation process, when the second mold is stopped at the closest position, the speed of the second mold can be gradually reduced or the speed of the second mold can be sharply reduced. By sharply reducing the speed of the second mold, it is easy to appropriately segment the laminate. In order to sharply reduce the moving speed of the second mold at the closest position, a drive mechanism that does not include a crank mechanism can also be used to move the second mold. Examples of such a drive mechanism include a hydraulic (e.g., oil-pressure) drive mechanism and a pneumatic drive mechanism. Alternatively, in order to sharply reduce the moving speed of the second mold at the closest position, a stopper for stopping the second mold at the closest position can also be used.
[0035] As the first and second molds, the first and second molds described in the manufacturing apparatus (D) to be described later can be used.
[0036] In the splitting process, the above-mentioned part (P) of the blade of the second mold moves to a position closer to the main surface SA1 side (the placement surface side of the first mold) than the position of the main surface SA2 of the stack. Specifically, the closest position of the part (P) is located at the position of the main surface SA1 or a position between the position of the main surface SA1 and the main surface SA2. The placement surface of the first mold is the surface on which the stack is placed, and is the surface in contact with the main surface SA1 of the stack.
[0037] The closest position of the portion (P) of the blade of the second die is the position of the portion (P) when the portion (P) is closest to the placement surface of the first die in the splitting process. In an example where the drive mechanism includes a crank mechanism, the position of the portion (P) at the bottom dead center corresponds to the closest position.
[0038] When the splitting process satisfies at least one of the above conditions (1) to (4), the splitting process may also satisfy any one of the following conditions (5), (6), and (7) as long as it does not conflict with the above conditions. In addition, in the following description, the "main surface SA1 of the stacked body" may be replaced with the "placement surface of the first mold". (5) In the splitting step, the closest position of at least a portion (P) of the blade of the second mold is closer to the main surface SA1 of the stack than the main surface SA2 of the stack and farther from the main surface SB2 of the solid electrolyte layer than the first mold. (6) In the splitting step, at least a portion (P) of the blade of the second mold is moved to the position of the main surface SB2 of the solid electrolyte or to a position closer to the placement surface than the position of SB2. For example, in the splitting step, the closest position of at least a portion (P) of the blade of the second mold may be located at the position of the main surface SB2 of the solid electrolyte layer or at a position closer to the placement surface than the position of the main surface SB2. (7) In the splitting step, at least a portion (P) of the blade of the second mold is moved to the position of the main surface SB1 of the solid electrolyte or to a position closer to the placement surface than the position of the main surface SB1. For example, in the splitting step, the closest position of at least a portion (P) of the blade of the second mold may be located at the position of the main surface SB1 of the solid electrolyte layer or at a position closer to the placement surface than the position of the main surface SB1.
[0039] In the description of conditions (1) to (7), the position of the main surface refers to the position of the main surface in the stack placed on the placement surface of the first mold. The stack may include only one power generation element or multiple power generation elements stacked. In the case where the stack includes multiple power generation elements, the main surfaces SB1 and SB2 refer to the main surfaces of the solid electrolyte layer of any one of the power generation elements included in the stack. For example, the main surfaces SB1 and SB2 can be the main surfaces of the solid electrolyte layer closest to the main surface SA1, or the main surfaces of the solid electrolyte layer closest to the main surface SA2.
[0040] As described above, the segmentation process is performed in such a manner that the position of the above-mentioned at least a portion (P) of the blade portion becomes the above-mentioned prescribed position. In a preferred example, the segmentation process is performed in such a manner that most or all of the blade portion becomes the above-mentioned prescribed position. Therefore, as long as there is no contradiction in the description, in this specification, the description such as "at least a portion (or a portion (P)) of the blade portion" may also be replaced with "blade portion".
[0041] The ratio L1 / L0 of the length L1 of at least a portion (P) of the blade to the length (total length) L0 of the blade may be 0.5 or more, 0.6 or more, 0.7 or more, 0.8 or more, 0.9 or more, or 0.95 or more, and 1.0 or less. As an example, the ratio L1 / L0 is 1.0.
[0042] As an example, consider the following case: the main surfaces of the layers of the stack are not curved but parallel to each other, and the blade of the second mold is parallel to the main surfaces of the layers of the stack and extends in a straight line. In this case, if the second mold is moved while maintaining the blade of the second mold parallel to the main surfaces of the layers of the stack to perform the splitting process, the ratio L1 / L0 can be 1.0.
[0043] When the blade of the second mold is not parallel to the main surfaces of the layers of the stack, the ratio L1 / L0 is sometimes less than 1.0. In addition, when the blade of the second mold is not linear, the ratio L1 / L0 is sometimes less than 1.0. For example, when the shape of the projection is curved when the blade of the second mold is projected onto a plane perpendicular to the direction PD described later, the ratio L1 / L0 is sometimes less than 1.0. In the splitting process, the blade other than the portion (P) may be located at a position farther away from the first mold than the portion (P), or may be located in a position in the opposite direction thereof. For example, in the splitting process, at least a portion of the blade other than the portion (P) may also pass through the position of the main surface SA1. In this case, the effect based on the manufacturing method (M) is also obtained in the portion of the portion (P).
[0044] The manufacturing method (M) may further include the following steps before the placing step: measuring the distance (interlayer distance) between a main surface of the stack (e.g., main surface SA1 or main surface SA2) and the main surface of the layer constituting the stack (e.g., main surface SB1 or main surface SB2), and adjusting the moving range of the blade of the second mold based on the obtained measurement value. By performing this step, the blade of the second mold can be accurately moved within the desired range. The method for adjusting the moving range of the blade of the second mold will be described later. For example, the cross-section of the stack can be photographed using an electron microscope, and the above-mentioned interlayer distance can be measured based on the obtained image. Thus, the ratio of the thickness of each layer can be calculated. In addition, the calculated ratio of the thickness of each layer can also be used as a reference ratio. For example, in the mass production process, the thickness of the divided stack can also be measured by a known method, and the moving range of the blade of the second mold can be adjusted based on the ratio of the measured thickness and the above-mentioned reference.
[0045] If the positive electrode layer and the negative electrode layer are short-circuited during the splitting step, the manufacturing yield may be reduced, or the reliability and long-term characteristics of the stacked body after the splitting may be reduced. Therefore, the splitting step is preferably performed in a state where the positive electrode layer and the negative electrode layer are not short-circuited.
[0046] In the segmentation process, at least one of the following conditions (a) to (c) may be satisfied. For example, any one of the conditions (a) to (c) may be satisfied, or two of them may be satisfied. For example, the conditions (a) and (b) may be satisfied, the conditions (a) and (c) may be satisfied, or the conditions (b) and (c) may be satisfied. Alternatively, all of the conditions (a) to (c) may be satisfied. (a) The dividing step is performed in a state where the first mold and the second mold are electrically insulated from each other. (b) The placement surface of the first mold is formed of an insulating material. (c) Among the surfaces of the second mold, the surface that contacts the laminated body in the dividing step is formed of an insulating material.
[0047] In the case where the closest position of the blade of the second mold is located on the main surface SA2 side of the stack body that is closer to the main surface SB1 of the solid electrolyte layer, the second mold does not contact the positive electrode layer and the negative electrode layer at the same time during the splitting process. In the case where the second mold does not contact the positive electrode layer and the negative electrode layer at the same time during the splitting process, by satisfying conditions (a) and / or conditions (b), a short circuit between the positive electrode layer and the negative electrode layer can be prevented. In the case where the closest position of the blade of the second mold is located on the main surface SA1 side of the stack body that is closer to the main surface SB1 of the solid electrolyte layer, in the splitting process, the second mold sometimes contacts the positive electrode layer and the negative electrode layer at the same time. In this case, by satisfying condition (c), a short circuit between the positive electrode layer and the negative electrode layer can also be prevented. In addition, as long as condition (c) is satisfied, a short circuit between the positive electrode layer and the negative electrode layer in the splitting process can be prevented in any case.
[0048] In order to satisfy condition (b) and / or condition (c), the first mold and / or the second mold may be formed of an insulating material. Alternatively, the surface of the first mold and / or the surface of the second mold may be coated with an insulating material. Examples of insulating materials include insulating inorganic compounds (e.g., oxides, nitrides, ceramics). Examples of insulating inorganic compounds include insulating metal compounds (e.g., metal oxides, metal nitrides).
[0049] In the splitting step, the stack is preferably split while the stack is fixed to the placement surface of the first mold. According to this structure, the stack can be split accurately and appropriately at the splitting position. Furthermore, according to this structure, the roughness of the splitting surface can be further reduced, so that the short circuit between the positive electrode layer and the negative electrode layer can be particularly suppressed.
[0050] The method of fixing the stack is not particularly limited, and as long as the stack can be fixed, a method of pressing the stack using a member (e.g., a pressing plate), a vacuum adsorption method, etc. can also be used. In the placement process, the stack can be fixed to the placement surface of the first mold, and the splitting process is performed in this state.
[0051] Typically, the dividing step is performed in a state where the portion of the stacked body protruding from the placement surface of the first mold is not fixed.
[0052] The stack may further include at least one metal layer. The metal layer may be a layer containing metal particles, or a metal layer formed by a gas phase method (evaporation method, sputtering method, etc.) or a liquid phase method. Alternatively, the metal layer may be a metal foil. The stack may include only one metal layer, or may include multiple metal layers. The metal layer may be arranged on the surface of the stack, or may be arranged inside the stack. For example, in the case where the stack includes multiple stacked power generation elements, the metal layer may also be arranged between adjacent power generation elements.
[0053] The at least one metal layer may also include at least one metal foil disposed on the main surface SA1 and / or the main surface SA2. In this case, the surface exposed by the metal foil becomes the main surface of the laminate. The metal layer may also be configured to cover the entire surface (or substantially the entire surface) of at least one main surface (single or both surfaces) of the power generation element.
[0054] When the laminate includes a metal foil, the metal foil may be arranged at a position where the blade of the second die passes. For example, when the laminate includes a metal foil arranged only on one surface, the splitting process may be performed while the laminate is placed so that the surface of the metal foil becomes the main surface SA2.
[0055] In the case where a metal layer (such as a metal foil) is only arranged on one side of the power generation element, the metal layer can be arranged on the positive electrode layer side or on the negative electrode layer side. For example, the laminate can have a laminate structure such as metal layer / positive electrode layer / solid electrolyte layer / negative electrode layer, or a laminate structure such as metal layer / negative electrode layer / solid electrolyte layer / positive electrode layer. In addition, the power generation element itself is also a laminate having a laminate structure such as positive electrode layer / solid electrolyte layer / negative electrode layer. In the case where the metal layer is arranged on both sides of the power generation element, the laminate has a laminate structure such as metal layer / positive electrode layer / solid electrolyte layer / negative electrode layer / metal layer. In addition, these laminates may also include layers other than the above-mentioned layers between the above-mentioned layers.
[0056] The electrical characteristics between the main surface SA1 and the main surface SA2 can also be measured when the laminate is placed on the placement surface of the first mold. The measured electrical characteristics can also be characteristics used to determine whether there is a short circuit between the positive electrode layer and the negative electrode layer. Examples of such electrical characteristics include resistance and voltage. The electrical characteristics can be measured after the splitting process, or before and after the splitting process. Alternatively, the splitting process can be performed while measuring the electrical characteristics. By measuring the electrical characteristics, it can be determined whether a short circuit has occurred during the splitting process.
[0057] In the manufacturing method (M), a stacked body larger than the size of the stacked body used in one solid battery (hereinafter sometimes referred to as the "final size") is divided by a dividing step. The stacked body is finally divided into the final size. The manufacturing method (M) includes a placement step and a division step, but the placement step and the division step may be repeated multiple times.
[0058] In a typical example, a stack having a size when arranged in a matrix in a final size is divided into a plurality of strip-shaped stacks by multiple segmentation steps. Then, by repeatedly performing the segmentation step on each strip-shaped stack, a plurality of stacks of final size are obtained. In another example, a stack slightly larger than the final size is made, and the end of the stack is segmented and removed by a segmentation step, thereby obtaining a stack of final size. The number of stacks of final size formed by the initial stack is one or more or two or more, and may also be in the range of 1 to 1000 (e.g., a range of 1 to 100, a range of 2 to 100).
[0059] The plane shape of the laminate placed in the placement process and the plane shape of the laminate of the final size are not limited. These plane shapes are preferably shapes composed of straight lines, and can also be rectangles (squares or rectangles) or rhombuses. The size of the plane shape of the laminate of the final size is not limited, and each side of the plane shape can be more than 1 cm or less than 50 cm. The plane shape of the laminate of the final size can also be a square size that converges in the range of 1 cm to 50 cm (for example, a range of 1 cm to 30 cm, a range of 1 cm to 20 cm) on one side.
[0060] The material and formation method of the laminate are not particularly limited. For example, the material and formation method of the positive electrode layer, the negative electrode layer, and the solid electrolyte layer may also be applied to known materials and formation methods. The power generation element may also be formed only by the positive electrode layer, the negative electrode layer, and the solid electrolyte layer. Alternatively, as long as the laminate can be divided in the dividing step, the power generation element may also include other layers. Examples of such other layers include a thin conductive layer composed of a material containing a conductive powder, etc.
[0061] The manufacturing method (M) may also include a preparatory step of preparing the laminate before the placing step. The preparatory step may be a step of making the laminate from a material, or a step of obtaining an already manufactured laminate. In the case of making the laminate from a material, the laminate is preferably formed by a manufacturing method including a step of extruding the material constituting the laminate. An example of a method for manufacturing a laminate is described below.
[0062] In the preparation process, after stacking the materials of the positive electrode layer, the solid electrolyte layer and the negative electrode layer, the stacked materials are concentratedly extruded (formal extrusion) to prepare the laminate. At this time, the materials of each layer and the metal foil can also be stacked and extruded together. For example, in one example of the preparation process, after the materials of the positive electrode layer, the materials of the solid electrolyte layer and the negative electrode layer (and the metal foil as required) are stacked on the metal foil in a prescribed order, the stacked materials and one or two metal foils are concentratedly extruded (formal extrusion) to form a laminate. This formation method is preferably used to manufacture a laminate of an all-solid-state battery. Through this formal extrusion, one or two metal foils and each layer are integrated to obtain a laminate. The pressure of the formal extrusion can be appropriately changed according to the material, thickness, etc., and can be more than 50MPa and less than 5000MPa (for example, more than 300MPa and less than 3000MPa). In the case of stacking the positive electrode layer on the metal foil, the metal foil uses a metal foil that becomes a positive electrode collector. When the negative electrode layer is stacked on the metal foil, the metal foil used is a metal foil that serves as a negative electrode current collector. Alternatively, after forming the power generating element, the power generating element and at least one metal foil may be integrated to obtain a stacked body.
[0063] The configured materials may also be pre-extruded at any stage after configuring the material of the positive electrode layer, after configuring the material of the solid electrolyte layer, and after configuring the material of the negative electrode layer. The pre-extrusion is usually performed at a pressure less than the pressure of the above-mentioned formal extrusion. The pressure of the pre-extrusion is not particularly limited and may be in the range of 1 MPa to 10 MPa. In order to reduce the voids in the stack, at least a part of the process of forming the stack may also be performed under reduced pressure.
[0064] In the preparation process, at least one layer selected from the group consisting of a positive electrode layer, a solid electrolyte layer and a negative electrode layer can also be formed using a material that does not contain a liquid component (for example, a material that contains a powder but does not contain a liquid component). For example, all layers constituting the power generation element can be formed by a material that does not contain a liquid component, and all layers constituting the stack can be formed by a material that does not contain a liquid component. As a method for configuring a material that does not contain a liquid component (dispersion medium) into a layered state, an electrostatic spraying method, a scraper film forming method, or an electrostatic coating method can also be used. A stack is formed by a method (dry method) of extruding a material that does not contain a liquid component, thereby obtaining a stack that is easily split in a splitting process.
[0065] At least one layer (e.g., all layers) selected from the group consisting of a positive electrode layer, a solid electrolyte layer, and a negative electrode layer can also be formed using a mixture (e.g., a slurry) containing a material constituting the layer and a liquid component. In this case, for example, each layer and a laminate can be formed by coating, drying, and extruding the mixture. In the case of using a mixture containing a liquid component, a laminate that is easily divided in the division process can also be obtained by drying (removal of the liquid component) and / or extrusion. The liquid component is not particularly limited, and a known liquid component (dispersion medium) used to form a known power generation element can be used. Examples of liquid components include, for example, butyl butyrate, dibutyl ether, heptane, water, ethanol, acetone, tetrahydrofuran, N-methyl-2-pyrrolidone, and the like.
[0066] Furthermore, the method for forming the laminate and each layer constituting the laminate is not particularly limited as long as the laminate can be divided in the dividing step. For example, any of the layers may be formed by spraying or other methods.
[0067] The proportion of the powder material in at least one layer (for example, all layers) constituting the power generation element may be 50% by mass or more, 70% by mass or more, or 100% by mass or less. In the case of a layer in which the proportion of the powder material is 50% by mass or more, the power generation element has high brittleness and is easy to be divided in the division process. The proportion of the powder material in the positive electrode layer, the proportion of the powder material in the negative electrode layer, and the proportion of the powder material in the solid electrolyte layer may also be within the range specified by the lower limit and upper limit of the proportion of the above-mentioned powder material, respectively. The powder material may be a powder of an inorganic material, or a mixture of a powder of an inorganic material and a powder of an organic material.
[0068] The material of at least one layer (e.g., all layers) selected from the group consisting of a positive electrode layer, a solid electrolyte layer, and a negative electrode layer may or may not contain a binder. From the viewpoint of facilitating the segmentation process, the material preferably does not contain a binder or contains a small amount of binder. As long as the segmentation process can be performed, the content of the binder in each layer may be 10% by mass or less (e.g., 5% by mass or less, 3% by mass or less), or more than this. In the case where the material contains a binder, the binder is not particularly limited, and a known binder for forming a known power generation element can be used. Examples of binders include rubbers such as styrene-butadiene rubber and butene rubber, polyvinylidene fluoride polymers, acrylic resins, and the like.
[0069] In addition, the materials of each layer extruded by the formal extrusion may be arranged in a pre-layered state. That is, when forming a power generation element, at least one layer selected from the group consisting of a positive electrode layer, a solid electrolyte layer, and a negative electrode layer may be formed as a separate layer by drying and / or extruding the material in advance. In addition, the separate layer may be arranged on a metal foil or other layer and formally extruded to form a laminate.
[0070] The laminate may be a laminate formed by extrusion without heating at a high temperature (e.g., above 100° C.). For example, the laminate may not be a sintered body. Alternatively, the preparation step may include a step of heating the material and / or the laminate at a high temperature during and / or after the extrusion of the material to sinter the material.
[0071] As described above, the laminate can be produced. However, the laminate can also be produced by methods other than the above.
[0072] The thickness of the metal layer (eg, metal foil) may be in the range of 1 μm to 50 μm (eg, in the range of 5 μm to 20 μm).
[0073] The thickness of the power generation element may also be in the range of 100 μm to 1000 μm (for example, in the range of 200 μm to 800 μm). If a power generation element of such thickness is cut by shearing, a short circuit caused by the roughness of the cut surface is particularly prone to occur. The thickness of the positive electrode layer may also be in the range of 50 μm to 500 μm (for example, in the range of 100 μm to 300 μm). The thickness of the solid electrolyte layer may also be in the range of 10 μm to 300 μm (for example, in the range of 30 μm to 100 μm). The thickness of the negative electrode layer may also be in the range of 50 μm to 500 μm (for example, in the range of 100 μm to 300 μm). The manufacturing method (M) is preferably used to manufacture a solid battery using a thin power generation element.
[0074] The above-mentioned segmentation process can segment the stack. After the stack is segmented into the final size, it is used to manufacture a solid battery. Through the manufacturing method (M), a solid battery including a stack having a power generation element can be manufactured. In at least one side of the stack, the power generation element may have an end face formed by the segmentation process.
[0075] The method for making a solid battery using the laminate obtained in the segmentation process is not particularly limited, and a known method can be used. In the case where the laminate does not include a metal layer (collector), the manufacturing method (M) may also include a step of configuring a metal layer on the surface of the laminate. In an example of a manufacturing method (M) in which a laminate having a metal layer only on one side of a power generation element is prepared, first, other collectors are formed on one side of the metal layer of the above-mentioned laminate, to form a power generation body (laminate) including a laminated structure such as a metal layer / power generation element / collector. Other collectors may be metal foils, or may be vapor-deposited layers, etc. In the preparation process, when a laminate having a metal layer configured on both sides of a power generation element is prepared, the laminate after segmentation can be directly used as a power generation body.
[0076] Next, after the positive electrode side lead and / or the negative electrode side lead are connected to the obtained power generation body as needed, the power generation body is housed in an outer packaging body, thereby obtaining a solid battery. The power generation body may also be pressurized in the stacking direction before or after being housed in the outer packaging body. The solid battery may include only one of the above-mentioned stacked bodies, or may include a power generation body composed of a plurality of stacked stacked bodies. In addition, the formation of the above-mentioned other collectors may also be omitted.
[0077] The outer packaging body is not particularly limited, and a known outer packaging body can be used. The outer packaging body may also include a shell and / or a bag-shaped body formed by a film. For example, the generator may be enclosed in a bag-shaped body formed by a laminated film, or the bag-shaped body enclosed with the generator may be further accommodated in the shell. In this case, the generator may be enclosed in the bag-shaped body while the inside of the bag-shaped body or the shell is decompressed.
[0078] The following describes examples of constituent elements of a solid battery manufactured in this embodiment. However, the following constituent elements are illustrative, and solid batteries using other constituent elements can also be manufactured by the manufacturing method of this embodiment. In addition, the following mainly describes examples of all-solid batteries (particularly all-solid lithium-ion batteries).
[0079] (Positive electrode layer) The positive electrode layer contains a positive electrode active material and may also contain other components as needed. Examples of the other components include known components used in the positive electrode in an all-solid-state battery. From the viewpoint of improving the lithium ion conductivity in the positive electrode layer, the positive electrode layer preferably contains a solid electrolyte that exhibits lithium ion conductivity together with the positive electrode active material. As a solid electrolyte, there is no particular limitation as long as it exhibits lithium ion conductivity, and a solid electrolyte used in a solid electrolyte layer in an all-solid-state battery can be used. Usually, the positive electrode active material is used in the form of particles (powder). As described above, the positive electrode layer can be formed by compression molding a powder of a positive electrode active material, a positive electrode mixture (comprising a powder of a positive electrode active material and additives, etc.).
[0080] The positive electrode active material may be a material that can be used as a positive electrode active material in an all-solid-state battery. In the case of an all-solid-state lithium-ion battery, examples of the positive electrode active material include lithium-containing composite oxides and compounds other than oxides. Examples of lithium-containing composite oxides include lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, and other lithium-containing composite oxides (LiNi 0.8 Co 0.15 Al 0.05 O2, etc.). Examples of compounds other than oxides include olivine compounds (LiMPO4), sulfur-containing compounds (Li2S, etc.). In the above formula, M represents a transition metal. The positive electrode active material may be used alone or in combination of two or more.
[0081] In the case of using a powdered positive electrode active material, the average particle size of the positive electrode active material can be, for example, 3 μm or more or 4 μm or more, or 15 μm or less or 11 μm or less. In this specification, the average particle size is the median particle size (D50) in the volume-based particle size distribution measured using a laser diffraction particle size distribution measuring device.
[0082] (Negative electrode layer) The negative electrode layer contains a negative electrode active material and may contain other components as needed. Examples of the other components include known components used in the negative electrode in an all-solid-state battery. The negative electrode layer may also contain a negative electrode active material and a solid electrolyte that exhibits lithium ion conductivity. Usually, the negative electrode active material is used in the form of particles (powder). As described above, the negative electrode layer can be formed by compression molding a powder of a negative electrode active material or a negative electrode mixture (containing a powder of a negative electrode active material and additives, etc.).
[0083] The negative electrode active material can use materials that can be used as negative electrode active materials in all-solid batteries. In the case of all-solid lithium ion batteries, the negative electrode active material can use a specified material (carbonaceous material, metal, semi-metal monomer or alloy, or compound, etc.) that can reversibly adsorb and release lithium ions. Examples of carbonaceous materials include graphite (natural graphite, artificial graphite, etc.), hard carbon, amorphous carbon, etc. Examples of metal, semi-metal monomers and alloys include lithium metal, alloys, Si monomers, etc. Examples of compounds include oxides (titanium oxide, silicon oxide, etc.), sulfides, nitrides, hydrates, silicides (lithium silicide, etc.), etc. The negative electrode active material can be used alone or in combination of two or more. For example, silicon oxide and carbonaceous material can be used in combination. As the negative electrode active material, particles containing graphite particles and amorphous carbon covering the graphite particles can also be used.
[0084] When a powdered negative electrode active material is used, the average particle size of the negative electrode active material is, for example, 3 μm or more or 4 μm or more, and may be 50 μm or less or 30 μm or less.
[0085] (Solid electrolyte layer) The solid electrolyte layer disposed between the positive electrode and the negative electrode includes a solid electrolyte that conducts charge carriers. Typically, the solid electrolyte is used in the form of particles (powder). As described above, the solid electrolyte layer can be formed by compression molding a material containing a powder of the solid electrolyte.
[0086] The solid electrolyte may be a material that can be used as a solid electrolyte in an all-solid battery. In the case of an all-solid lithium ion battery, the solid electrolyte may be a material having lithium ion conductivity. Examples of such solid electrolytes include inorganic solid electrolytes such as sulfides (sulfide-based solid electrolytes) and hydrides (hydride-based solid electrolytes).
[0087] Examples of sulfides include Li2S-SiS2, Li2S-P2S5, Li2S-GeS2, Li2S-B2S3, Li2S-Ga2S3, Li2S-Al2S3, Li2S-GeS2-P2S5, Li2S-Al2S3-P2S5, Li2S-P2S3, Li2S-P2S3-P2S5, LiX-Li2S-P2S5, LiX-Li2S-SiS2, LiX-Li2S-B2S3 (X: I, Br or Cl), etc. Examples of hydrides include LiBH4-LiI complex hydrides and LiBH4-LiNH2 complex hydrides, etc.
[0088] (Positive electrode collector) A metal layer (positive electrode current collector) is usually disposed outside the positive electrode layer of the power generation element. A metal foil may also be used for the metal layer (positive electrode current collector). Examples of materials of the positive electrode current collector (e.g., metal foil) include aluminum, magnesium, stainless steel, titanium, iron, cobalt, zinc, tin, or alloys thereof.
[0089] (Negative electrode current collector) A metal layer (negative electrode collector) is usually arranged outside the negative electrode layer of the power generation element. The metal layer (negative electrode collector) may also be made of metal foil. Examples of materials of the metal layer (negative electrode collector) include copper, nickel, stainless steel, titanium, and alloys thereof.
[0090] In addition, in the case of manufacturing a solid battery other than an all-solid battery, the power generation element uses a power generation element corresponding to the solid battery. The power generation element of a solid battery other than an all-solid battery may also use a power generation element of a known solid battery other than an all-solid battery. As long as the stack including these power generation elements can be split in the splitting process, the manufacturing method (M) can be used. Examples of stacks that can be split in the splitting process include stacks in which the positive electrode layer, the solid electrolyte layer, and the negative electrode layer are respectively formed of solid or semi-solid. Such a stack may also be a stack in which at least one layer (e.g., all layers) of the positive electrode layer, the solid electrolyte layer, and the negative electrode layer is formed of a solid.
[0091] (Solid-state battery manufacturing device) The manufacturing device of the present embodiment is a manufacturing device for a solid battery (e.g., an all-solid battery). Hereinafter, the manufacturing device is sometimes referred to as a "manufacturing device (D)". According to the manufacturing device (D), the manufacturing method (M) can be easily implemented. However, the manufacturing method (M) can also be implemented by a device other than the manufacturing device (D). In addition, the matters described for the manufacturing method (M) can also be applied to the manufacturing device (D), so repeated descriptions are sometimes omitted. In addition, the matters described for the manufacturing device (D) can also be applied to the manufacturing method (M).
[0092] The manufacturing device (D) is a manufacturing device for a solid battery. The manufacturing device (D) implements a process of dividing a stack including a power generation element. The manufacturing device (D) includes a first mold for placing the stack, a second mold, and a driving mechanism for reversibly approaching the first mold and the second mold. The power generation element includes a positive electrode layer, a negative electrode layer, and a solid electrolyte layer arranged between the positive electrode layer and the negative electrode layer. The stack has a main surface SA1 and a main surface SA2. The solid electrolyte layer has a main surface SB1 on the side of the main surface SA1 and a main surface SB2 on the side of the main surface SA2. The first mold, the second mold, and the stack can apply the description related to the first mold, the second mold, and the stack in the manufacturing method (M).
[0093] In the manufacturing device (D), the stack is placed on the placement surface of the first mold in a manner that the main surface SA1 is closer to the first mold than the main surface SA2, and the blade of the second mold is brought close to the first mold from the main surface SA2 side, thereby dividing the stack (dividing step). In this dividing step, the dividing of the stack is performed by driving the blade and the first mold to approach each other within a range where at least a portion (P) of the blade does not pass through the main surface SA1 of the stack.
[0094] According to the manufacturing device (D), the manufacturing method (M) can be implemented. Therefore, according to the manufacturing device (D), a solid battery that is not prone to short circuit between the positive electrode layer and the negative electrode layer can be manufactured with a good yield. That is, according to the manufacturing device (D), a solid battery with high characteristics can be manufactured with a good yield.
[0095] In the splitting step, the driving mechanism moves the first mold and / or the second mold. Usually, the second mold is the upper mold, and the driving mechanism moves only the second mold.
[0096] The first die and the second die may be the same as the known lower die and upper die (die and punch) used for shearing of metal sheets and the like.
[0097] The first mold has a placement surface on which the laminate is placed. The end of the placement surface functions as a shoulder (blade) opposite to the blade of the second mold. When the blade of the second mold approaches the placement surface of the first mold, the laminate is divided by being clamped by the shoulder of the first mold and the blade of the second mold.
[0098] As long as the mold can be moved, it is not limited to the driving mechanism. The driving mechanism can also use the driving mechanism used in the previous shearing device (or extrusion machine). The driving mechanism can be a mechanical driving mechanism (such as an electric driving mechanism) or a hydraulic driving mechanism (such as an oil pressure driving mechanism). Or the driving mechanism can also be a pneumatic driving mechanism. That is, the driving mechanism can also make the first mold and the second mold reversibly approach each other through air pressure.
[0099] The driving mechanism may be any one of an electric linear actuator, a hydraulic linear actuator, and a pneumatic linear actuator (cylinder). They may use a known actuator or a commercially available actuator. Among them, a pneumatic linear actuator (cylinder) is preferred in that the device can be miniaturized and lightweight.
[0100] In the splitting step, the position (closest position) reached by the blade of the second mold may be the position exemplified in the manufacturing method (M). For example, in the splitting step performed in the manufacturing device (D), the driving mechanism brings the blade of the second mold close to the first mold in a manner that satisfies at least one of the above conditions (1) to (4). For example, the driving mechanism may also split the laminate by bringing the blade of the second mold close to the first mold within a range where at least a portion (P) of the blade of the second mold does not reach the position of the main surface SB1 of the solid electrolyte layer.
[0101] Furthermore, in the dividing step performed in the manufacturing apparatus (D), the driving mechanism may bring the blade of the second die closer to the first die so as to satisfy any one of the above conditions (5) to (7).
[0102] The method for stopping the blade of the second mold at the closest position is not particularly limited. The blade of the second mold may be stopped at the desired closest position by setting the drive mechanism. Alternatively, the blade of the second mold may be stopped at the desired closest position by adjusting the position of the drive mechanism. Alternatively, a stopper may be used, which abuts against the second mold (or a part of the drive mechanism) to stop the movement of the second mold when the blade of the second mold reaches the closest position.
[0103] It is preferable that the ratio L1 / L0 of the length L1 of at least a portion (P) of the blade portion of the second die and the length L0 of the blade portion satisfy the above relationship.
[0104] In the manufacturing device (D), the moving range of the blade of the second mold can also be adjusted based on the measured value of the distance (interlayer distance) between one main surface of the stack (e.g., main surface SA1 or main surface SA2) and the main surface of the layer constituting the stack (e.g., main surface SB1 or main surface SB2). Through this adjustment, the blade of the second mold can be accurately moved within a desired range. The adjustment of the moving range of the blade of the second mold can also be performed by at least one method selected from setting a drive mechanism, adjusting the position of the drive mechanism, and using a stopper.
[0105] In the manufacturing apparatus (D), it is preferred that the stack is divided without short-circuiting the positive electrode layer and the negative electrode layer. Specifically, it is preferred that at least one of the above conditions (a) to (c) is satisfied.
[0106] The distance G (the distance G described later) between the blade of the second mold and the shoulder of the first mold is not particularly limited, as long as it is a distance (interval) that can implement the splitting process. The distance G can also be less than 200 μm, less than 100 μm, less than 50 μm, less than 20 μm, less than 10 μm, or less than 0 μm. The distance G can also be greater than -50 μm, greater than -10 μm, or greater than 0 μm. The distance G can also be in the range of -50 to 100 μm, in the range of -10 to 50 μm, in the range of 0 to 50 μm, in the range of 0 to 20 μm, or in the range of 0 to 10 μm.
[0107] The manufacturing device (D) may also include a fixing mechanism for fixing the laminate to the placement surface of the first mold. The fixing mechanism is not limited as long as it can fix the laminate. For example, the fixing mechanism may also use a known fixing mechanism used in a shearing device. Examples of the fixing mechanism include a member for fixing (e.g., a pressing plate), a vacuum chuck, etc.
[0108] The first die is preferably sized so that the entire portion of the stack adjacent to the split position is placed on the first die. The blade of the second die is preferably sized to abut the entire width of the split position in the stack.
[0109] The angle α of the cross section of the blade of the second die (the cross section perpendicular to the direction in which the blade extends) may be a right angle or an acute angle. The angle α may be greater than 60° or greater than 70°, or may be in the range of 80 to 90° (e.g., 85 to 90°).
[0110] The manufacturing device (D) may also include a measuring device for measuring the electrical characteristics between the main surface SA1 and the main surface SA2 of the stack. In addition, as described above, the electrical characteristics between the main surface SA1 and the main surface SA2 of the stack may also be measured when the stack is placed on the placement surface of the first mold. The description related to the manufacturing method (M) may also be applied to the type of electrical characteristics and the timing of measurement. The measuring device is selected according to the type of electrical characteristics to be measured. Examples of the measuring device include a resistance meter and a voltmeter.
[0111] The first mold and the second mold may be electrically insulated from each other. By electrically insulating them, it is easy to measure the electrical characteristics between the main surface SA1 and the main surface SA2 of the stacked body.
[0112] The manufacturing device (D) includes a delivery mechanism for moving the laminate on the first mold as required. In addition, the manufacturing device (D) may also include a control device for controlling mechanisms such as a driving mechanism and a delivery mechanism. The delivery mechanism and the control device are not particularly limited, and the mechanisms and control devices used in the known shearing devices and extrusion devices can be used, or they can be modified to be suitable for the present embodiment. The control device (D) includes, for example, a storage device for storing a program for performing necessary processes such as a splitting process and a computing processing device for executing the program.
[0113] The manufacturing device (D) may also include a member for receiving the divided laminated body (laminated body protruding from the first mold), a conveying mechanism for conveying the divided laminated body, etc. as needed. In addition, the manufacturing device (D) may also include an adjustment mechanism for adjusting the position of the driving mechanism as needed. By adjusting the position of the driving mechanism by the adjustment mechanism, the distance G between the first mold and the second mold and / or the closest position of the blade of the second mold can be adjusted.
[0114] Hereinafter, examples of embodiments of the present invention will be specifically described with reference to the accompanying drawings. The manufacturing method and manufacturing apparatus described below can be applied to the description of the above-mentioned embodiments, and can also be changed based on the above-mentioned description. The processes and components of the manufacturing method and manufacturing apparatus described below that are not necessary for the manufacturing method and manufacturing apparatus of the present invention can also be omitted. In addition, the matters described below can also be applied to the above-mentioned embodiments. In addition, the following figures are schematic figures, which are different from the actual scale. In the following figures, in order to make it easier to observe the drawings, a part of the components is sometimes omitted for illustration.
[0115] (Implementation Method 1) In Embodiment 1, an example of the first manufacturing method (M) and an example of the manufacturing device (D) used therein are described. In addition, in the following example, a method for manufacturing an all-solid-state battery including a laminate having a structure such as a positive electrode collector / positive electrode layer / solid electrolyte layer / negative electrode layer / negative electrode collector is described. However, an all-solid-state battery including a laminate having a structure other than this and a solid battery other than an all-solid-state battery can also be manufactured in the same manner.
[0116] In the manufacturing method of embodiment 1, first, Figure 1 As shown, a laminate 100 is prepared. The laminate 100 includes a power generation element 110, a positive electrode collector 121, and a negative electrode collector 122. The power generation element 110 includes a positive electrode layer 111 and a negative electrode layer 112 and a solid electrolyte layer 113 disposed therebetween. The laminate 100 can be formed by the above method.
[0117] The laminated body 100 has a principal surface 100SA1 and a principal surface 100SA2 on the opposite side to the principal surface 100SA1. The solid electrolyte layer 113 has a principal surface 113SB1 on the principal surface 100SA1 side and a principal surface 113SB2 on the principal surface 100SA2 side.
[0118] Next, as shown in FIG. 2 , the stacked body 100 is placed on the first mold (lower mold) 210 in such a manner that the main surface 100SA1 is closer to the first mold 210 than the main surface 100SA2. Specifically, the stacked body 100 is placed on the first mold 210 in such a manner that the placement surface 210p of the first mold 210 is close to the main surface 100SA1. Then, the stacked body 100 is clamped and fixed by the first mold 210 and the pressing member (fixing mechanism) 211. Specifically, the adjacent portion ( Figure 3 The portion of the laminate 100 protruding from the first mold 210 ( Figure 3 The protrusion 100b) is not fixed.
[0119] The first mold 210 has a shoulder (corner) 210a extending in a straight line. The second mold (upper mold) 220 includes a blade 220a. The blade 220a has the shape of an angle extending in a straight line. In the example shown in embodiment 1, the shoulder 210a and the blade 220a extend parallel to each other. In addition, the blade 220a extends parallel to the placement surface 210p. In addition, their shapes can be changed according to the shape of the dividing position 100d, etc. The first mold 210 and the second mold 220 are electrically insulated. In addition, the first mold 210 and the pressing member 211 are electrically insulated.
[0120] Figure 3 Schematic representation of the view from above Figure 2A The configuration of the stacked body 100 and the first mold 210. Figure 3 An example of the configuration of the second mold 220 is also shown. Figure 3 , the direction in which the split position 100d extends is represented as the width direction WD, and the width of the stack 100 in the width direction WD is represented as the width W. The pressing member 211 preferably presses and fixes the stack 100 over the entire width (width W) of the split position 100d. However, as long as the stack 100 can be split, only a portion of the entire width may be pressed and fixed. As shown in FIG. 2 , the blade 220a is preferably in a shape that contacts the stack 100 over the entire width of the stack 100.
[0121] Figure 3 Indicates the direction PD described later. Figure 3Indicates the length (total length) L0 of the blade 220a of the second mold 220. In addition, as described above, the blade 220a refers to the corner portion of the second mold 220 that contacts the stacked body 100 in order to split the stacked body 100 in the splitting step. In Embodiment 1, the case where the entire blade 220a moves within the range of a predetermined position is described. That is, in Embodiment 1, the case where L1 / L0=1 is described.
[0122] The stacked body 100 is divided along a linear dividing position 100d. Figure 2A In the example shown, the first mold 210 and the pressing member 211 are arranged so that their respective linear shoulders 210a and 211a are along the dividing position 100d. Figure 2A As shown, the end surface 210s of the first mold 210 and the end surface 211s of the pressing member 211 may also be in the same plane. Alternatively, the end surface 211s may be located at a position on the first mold 210 and at a position away from the end surface 210s.
[0123] Then, if Figure 2B As shown, the stacked body 100 is divided by bringing the blade 220a of the second mold 220 close to the first mold 210 from the main surface 100SA2 side. In the dividing step, the blade 220a is brought close to the first mold 210 within a range where the blade 220a does not pass through the main surface 100SA1 (the position of the placement surface 210p), thereby dividing the stacked body 100. Figure 2B The moving direction SD of the second mold 220 is indicated by an arrow.
[0124] A direction parallel to the placement surface 210p of the first mold 210 and perpendicular to the shoulder 210a of the first mold 210 is referred to as direction PD. In addition, a direction perpendicular to the surface of the laminated body 100 placed on the first mold 210 is referred to as direction ND. Figure 2B In the example shown, the direction SD and the direction ND are substantially parallel.
[0125] The distance G (the distance in the direction PD) between the blade 220a of the second mold and the shoulder 210a of the first mold 210 can be any distance that allows the splitting process to be implemented. The distance G may also be within the above range. In addition, the distance G sets the direction away from the first mold 210 as positive. A negative distance G means that the first mold 210 and the second mold 220 partially overlap when the two are observed from one side (above) of the second mold 220. The distance G can also be considered as the minimum value of the coordinates of the blade 220a on the coordinate axis, which is the coordinate axis along the direction PD, and the position of the shoulder 210a is set as the origin, and the direction in which the stack 100 protrudes from the placement surface 210p of the first mold 210 is set as positive. In addition, the maximum value Gmax of the coordinates of the blade 220a on the coordinate axis and the average value Gave of the coordinates can also be within the range illustrated for the distance G. The coordinate axis is the coordinate axis along the direction PD, and the position of the shoulder 210a is set as the origin and the direction in which the stack 100 protrudes from the placement surface 210p of the first mold 210 is set as positive.
[0126] In the manufacturing method and manufacturing apparatus of Embodiment 1, the laminate 100 can be divided even if the blade 220a does not pass through the shoulder 210a of the first die 210. Therefore, unlike conventional shearing devices, the distance G can be made 0 μm or less. By reducing the distance G, more appropriate division can be performed.
[0127] Figure 2B FIG. 2 shows an example of a state when the blade 220a reaches a position (closest position) closest to the placement surface 210p of the first mold 210 in the splitting process. Figure 2B In the example shown, the closest position is between the position of the main surface 113SB1 and the position of the main surface 113SB2 of the solid electrolyte layer. In the prior art, it is considered that the blade 220a needs to be moved downward from the placement surface 210p. However, according to the results of the study, it is known that the stacked body 100 can be divided even if the blade 220a is not moved downward from the placement surface 210p (or the main surface 100SA1).
[0128] Here, the position of the blade 220a refers to the coordinate position (height position) of the blade 220a when the moving direction SD of the second die 220 (blade 220a) is used as the coordinate axis in the dividing step.
[0129] Figure 4 An example is shown in which the closest position of the blade portion 220 a is located between the placement surface 210 p (or the main surface 100SA1 ) and the main surface 113SB1 of the solid electrolyte layer 113 . Figure 4 It indicates the state when the blade 220a is at the closest position. Figure 4As shown, the blade portion 220 a may be closer to the placement surface 210 p (or the main surface 100SA1 ) than the main surface 113SB1 of the solid electrolyte layer 113 .
[0130] As described above, the stacked body 100 can be divided. After the stacked body 100 is divided into the final size, the lead tabs are connected and the stacked body is sealed in an outer package as necessary. In this way, a solid battery can be manufactured.
[0131] In Embodiment 1, the stacked body 100 is described as including the positive electrode current collector 121 and the negative electrode current collector 122. However, the stacked body 100 may not include one or both of the positive electrode current collector 121 and the negative electrode current collector 122. In this case, the current collector may be formed as needed after the stacked body 100 is divided.
[0132] Figure 5 An example of a manufacturing apparatus 200 including a first mold 210 , a pressing member 211 , and a second mold 220 is shown. Figure 5 The manufacturing device 200 includes a first mold 210, a pressing member 211, a second mold 220, a driving mechanism 231, 250, a roller 240 (feeding mechanism), a position adjustment mechanism 251 and a measuring device 260. The driving mechanism 231 moves the pressing member 211, thereby fixing and releasing the stack 100. The roller 240 feeds the stack 100 and moves it to an appropriate position. The position adjustment mechanism 251 enables the driving mechanism 250 to move along the direction SD and fix it. The position adjustment mechanism 251 can adjust the closest position. For example, the interlayer distance of the stack and / or the thickness of the stack can also be measured, and the closest position can be adjusted based on the measured value.
[0133] If the closest position does not need to be changed or can be adjusted only by the drive mechanism 250, the position adjustment mechanism 251 may not be provided. The closest position can also be changed by moving the placement surface 210p of the first mold 210.
[0134] The driving mechanism 250 causes the second mold 220 to move along Figure 5 The driving mechanism 250 (manufacturing device 200) lowers the second mold 220 and brings the blade 220a closer to the first mold 210 from the main surface 100SA2 side, thereby performing the splitting process (see Figure 2A and Figure 2B ). As described above, the driving mechanism 250 (manufacturing device 200 ) moves the blade 220 a to a predetermined position, thereby dividing the stacked body 100 .
[0135] The measurement device 260 measures the electrical characteristics of the stacked body 100 . Figure 5 This shows an example of a case where the pressing member 211 and the first mold 210 are conductive. The measuring device 260 is connected to the pressing member 211 and the first mold 210, and measures the electrical properties of the stacked body 100 through them. Alternatively, the electrical properties of the stacked body 100 may be measured by bringing a probe or the like into contact with the stacked body 100.
[0136] Figure 6 An example of the structure of the periphery of the driving mechanism 250 when the driving mechanism 250 is an air cylinder is shown. Figure 6 The device of one example includes gas flow paths 252a and 252b connected to the driving mechanism 250 and speed controllers 253a and 253b provided in between. The second mold 220 moves up and down by the gas flowing in the gas flow paths 252a and 252b.
[0137] Figure 6 An angle α showing a cross section of the blade 220a of the second die 220 is an example of an acute angle. The angle α is an angle of the blade 220a in a cross section perpendicular to the direction in which the blade 220a extends.
[0138] In addition, in the above description, an example of dividing only one side of the stack at a time is described. However, it is also possible to divide multiple sides of the stack by moving the second mold once. For example, the two second molds are configured so that their shoulders form an L shape. Similarly, the first mold and the pressing member are also configured to correspond to the second mold. At this time, the two second molds are configured to have different positions in the direction ND (i.e., they are configured to have different heights). By using these second molds, the first mold, and the pressing member, it is also possible to divide the two sides of the stack by moving the second mold once. By the same method, it is also possible to divide three or four sides of the stack by moving the second mold once. In addition, as long as the sides do not intersect each other, they can be divided at the same time even if the positions in the direction ND are not different. Industrial Applicability
[0139] The present invention can be used for a solid battery, a method for manufacturing a solid battery, and a device for manufacturing a solid battery. The preferred embodiments of the present invention are described, but such disclosure should not be interpreted in a limiting sense. Various modifications and changes will be apparent to those skilled in the art of the present invention upon reading the above disclosure. Therefore, the appended claims should be interpreted as including all modifications and changes without departing from the true spirit and scope of the present invention. Description of Reference Numerals
[0140] 100: Laminated body 100d: Split position 100SA1, 100SA2, 113SB1, 113SB2: Main surface 110: Power generation element 111: Positive electrode layer 112: Negative electrode layer 113: Solid electrolyte layer 200: Manufacturing device 210: First mold 210p: Placement surface 220: Second mold 220a: Blade 250: Driving mechanism 260: Measuring device
Claims
1. A method for manufacturing a solid battery, the solid battery using a stacked body including a power generation element, the method for manufacturing a solid battery being characterized by: The power generation element includes a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer. The laminate has a main surface SA1 and a main surface SA2 opposite to the main surface SA1. The solid electrolyte layer has a main surface SB1 on the main surface SA1 side and a main surface SB2 on the main surface SA2 side. The manufacturing method comprises: a placing step of placing the laminate on a placing surface of the first mold in such a manner that the main surface SA1 is closer to the first mold than the main surface SA2; as well as a dividing step of dividing the stacked body by bringing the blade of the second die closer to the first die from the main surface SA2 side, In the dividing step, the stacked body is divided by bringing the blade and the first mold closer together within a range where at least a portion of the blade does not pass through the main surface SA1 .
2. The manufacturing method according to claim 1, characterized in that: In the dividing step, the stacked body is divided by bringing the blade and the first mold closer together within a range where the at least a portion of the blade does not reach the main surface SA1 .
3. The manufacturing method according to claim 1, characterized in that: In the dividing step, the stacked body is divided by bringing the blade and the first die closer together within a range where the at least a portion of the blade does not reach the main surface SB1 .
4. The manufacturing method according to claim 1, characterized in that: In the dividing step, the stacked body is divided by bringing the blade and the first die closer together within a range where the at least a portion of the blade does not reach the main surface SB2 .
5. The manufacturing method according to claim 1, characterized in that: In the dividing step, the blade and the first mold are brought close to each other so that at least a portion of the blade reaches a position closer to the placement surface than the main surface SB2.
6. The manufacturing method according to claim 1, characterized in that: The dividing step is performed in a state where the positive electrode layer and the negative electrode layer are not short-circuited.
7. The manufacturing method according to any one of claims 1 to 5, characterized in that: In the dividing step, the stacked body is divided while the stacked body is fixed to the placement surface.
8. The manufacturing method according to claim 1, characterized in that: The stack further comprises at least one metal layer.
9. A solid battery manufacturing device that implements a step of dividing a stacked body including a power generation element, wherein the solid battery manufacturing device is characterized in that: The solid battery manufacturing device includes a first mold for placing the stacked body, a second mold, and a driving mechanism for reversibly bringing the first mold and the second mold close to each other. The power generation element includes a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer. The laminate has a main surface SA1 and a main surface SA2. The solid electrolyte layer has a main surface SB1 on the main surface SA1 side and a main surface SB2 on the main surface SA2 side. The stacked body is placed on the placement surface of the first mold in a state in which the main surface SA1 is closer to the first mold than the main surface SA2, and the driving mechanism brings the blade and the first mold close to each other in a state in which the blade of the second mold approaches the first mold from the main surface SA2 side, thereby dividing the stacked body. The division of the stacked body is performed by the drive mechanism bringing the blade and the first mold closer together within a range where at least a portion of the blade does not pass through the main surface SA1.
10. The manufacturing device according to claim 9, characterized in that: The distance between the blade and the shoulder of the first mold in a direction parallel to the placement surface is in a range of -50 μm to 100 μm.