Catalyst for selective hydrogenation of acetylene in synthesis gas as well as preparation method and application of catalyst
By supporting copper and nickel on the γ-Al2O3 support and using sodium borohydride and hydrogen to form an amorphous copper-nickel-boron combination, catalyst deactivation and ethylene over-addition in the synthesis gas are solved during the selective hydrogenation of acetylene in the synthesis gas. The hydrogen problem has achieved efficient acetylene hydrogenation and low side reaction generation, and is suitable for industrial applications.
Patent Information
- Application Number
- CN202411025903.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The existing catalysts are inactivated due to high content of CO and H2 during the selective hydrogenation of acetylene in synthesis gas, and it is difficult to effectively inhibit the excessive hydrogenation of ethylene, resulting in an increase in ethane generation, affecting reaction selectivity and catalyst life.
Using copper and nickel-supported γ-Al2O3 catalyst support, amorphous copper-nickel-boron combination is formed through low-temperature liquid phase reduction of sodium borohydride and hydrogen-strengthening reduction. It is used to selective hydrogenation of acetylene in synthesis gas, and the reaction conditions are controlled to ensure Acetylene is completely hydrogenated and ethylene is not hydrogenated as much as possible.
Acetylene selective hydrogenation in high CO and H2 environments is achieved, the catalyst has high activity, selectivity and durability, the acetylene hydrogenation conversion rate exceeds 98%, and the ethylene selectivity exceeds 95%, and it is shown in industrial applications. Stability and low side reaction generation.
Smart Images

Figure SMS_2 
Figure SMS_3 
Figure SMS_5
Abstract
Description
Technical Field
[0001] The invention relates to the field of acetylene selective hydrogenation, and in particular to a catalyst for selective hydrogenation of acetylene in synthesis gas, and a preparation method and application thereof. Background Art
[0002] The exhaust gas of calcium carbide furnace is discharged through torch combustion, which is not only a huge waste of energy, but also causes serious environmental pollution. Therefore, in recent years, the comprehensive utilization projects of calcium carbide furnace exhaust gas have gradually increased, and methanol, ethylene glycol, etc. are produced through calcium carbide furnace exhaust gas. At present, there are industrial devices for producing ethylene glycol at the level of 200,000 tons. Under the background of dual carbon, the comprehensive utilization of calcium carbide furnace exhaust gas is the general trend. The tail gas of calcium carbide furnace contains 75-85% CO. After the conversion reaction, the synthesis gas contains about 45% H2, about 45% CO, about 2% C2H4, and about 0.2% acetylene. When pressure swing adsorption (PSA) is used to separate and purify CO, the acetylene contained in the gas will react with the CO adsorbent cuprous chloride to generate explosive acetylene copper, which will cause safety hazards and affect the separation effect and service life of the adsorbent. Therefore, the acetylene in it needs to be purified. There is currently no industrialized catalyst of this type in China, and the emerging market urgently needs to develop a catalyst for selective hydrogenation of acetylene in synthesis gas.
[0003] Using CO2 to oxidize ethane to produce ethylene can upgrade ethane to high-value-added ethylene and convert CO2 into CO. This reaction is not only economical, but also realizes the resource utilization of CO2. The product gas of CO2 oxidation of ethane to produce ethylene contains about 0.3% acetylene, which can cause polyethylene catalyst poisoning; acetylene exists in CO and H2. When pressure swing adsorption (PSA) separates and purifies CO, acetylene affects the use of adsorbents, just like separating CO from calcium carbide furnace tail gas. Therefore, acetylene in the product gas of CO2 oxidation of ethane to produce ethylene also needs to be removed. In addition to about 25% ethylene, this product gas also contains about 25% CO and about 20% H2, which belongs to the synthesis gas atmosphere. To hydrogenate acetylene to ethylene is also the selective hydrogenation of acetylene in the synthesis gas.
[0004] In the new hydrogen production project, methane and CO2 are reformed to produce hydrogen, and CO is generated at the same time. The generated mixed gas contains about 20% hydrogen, about 30% CO, and about 0.1% acetylene. The acetylene needs to be removed before the conversion process. The atmosphere is also a synthesis gas atmosphere to remove acetylene.
[0005] In summary, the purification of acetylene in synthesis gas is a new topic raised by the high-quality development of the chemical industry. It has realistic market demand, and both economic and social benefits coexist. By developing a catalyst for the selective hydrogenation of acetylene in synthesis gas, the needs of industry and social development can be met, and contributions can be made to the dual-carbon goals. The selective hydrogenation catalyst of acetylene is a key technology in the ethylene industry. There are many types of industrial products at home and abroad. It mainly uses precious metal palladium as an active component and silver as an auxiliary agent to regulate the excessive hydrogenation activity of palladium metal, so as to achieve the purpose of taking both activity and selectivity into account. In the ethylene gas flow, the precious metal catalyst selectively hydrogenates acetylene and hydrogen to produce ethylene, while ethylene does not continue to hydrogenate to produce ethane. In order to fully hydrogenate acetylene and hydrogenate ethylene as little as possible, the hydrogen involved in the reaction should not be high. Generally, the amount added is 2 to 4 times that of acetylene. When the hydrogen content is high, the amount of ethane produced increases. In order to inhibit the hydrogenation of ethylene, a small amount of CO is also added to the reaction gas, usually at 300-3000ppm, to inhibit the catalyst activity through competitive adsorption of CO on the catalyst surface and improve the ethylene selectivity of the reaction. CO is a reversible poisoning component of the catalyst. When the content is high, the activity decreases and the selectivity increases, and vice versa. Therefore, CO is also called a regulator for the selective hydrogenation of acetylene. In the selective hydrogenation of acetylene in synthesis gas, CO is a reversible poisoning component of the precious metal catalyst, and its content is usually greater than 10%. To make the acetylene hydrogenation reaction occur, the reaction temperature must be greatly increased. In addition, there is more than 10% H2 in the synthesis gas, which makes ethylene hydrogenation easier to occur. After the reaction is exothermic, the reaction is strengthened and the temperature rises. When using traditional precious metal catalysts, the catalyst is quickly deactivated due to the adsorption of CO. In general, compared with the selective hydrogenation of acetylene in the ethylene industry, the selective hydrogenation of acetylene in synthesis gas is more difficult to develop catalysts due to the presence of high content of CO and H2. At present, there are no reports of industrial applications at home and abroad. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a catalyst for selective hydrogenation of acetylene in synthesis gas and its preparation method and application in view of the deficiencies in the prior art. The catalyst is used for selective hydrogenation of acetylene in synthesis gas, has good acetylene selective hydrogenation activity, high selectivity and good catalyst durability.
[0007] In order to solve the above technical problems, the present invention is implemented through the following technical solutions:
[0008] Provided is a catalyst for selective hydrogenation of acetylene in synthesis gas, comprising a catalyst carrier and active components copper and nickel loaded on the carrier, wherein the copper loading is 1-2.5wt%, the nickel loading is 0.5-1.5wt%, and zero-valent boron, zero-valent metal copper and zero-valent nickel in the catalyst form an amorphous copper-nickel-boron alloy.
[0009] According to the above scheme, the catalyst carrier is γ-Al2O3, SiO2, preferably γ-Al2O3.
[0010] According to the above scheme, the catalyst carrier is γ-Al2O3 with a specific surface area of 100 to 250 m 2 / g, bulk density 0.5±0.1g / ml, average pore diameter 5~25nm, pore volume 0.5~1.5ml / g.
[0011] According to the above scheme, the catalyst is obtained by subjecting a catalyst precursor containing a divalent copper salt, a divalent nickel salt and a carrier to sodium borohydride low-temperature liquid phase reduction and hydrogen reduction strengthening.
[0012] A method for preparing the catalyst for selective hydrogenation of acetylene in synthesis gas is provided, wherein a catalyst precursor containing a divalent copper salt, a divalent nickel salt and a carrier is sequentially subjected to sodium borohydride low-temperature liquid phase reduction and hydrogen reduction enhancement to prepare the catalyst for selective hydrogenation of acetylene in synthesis gas.
[0013] According to the above scheme, the preparation method is specifically as follows: after preparing a catalyst precursor containing a divalent copper salt, a divalent nickel salt and a carrier and drying it, it is first subjected to low-temperature liquid phase reduction with sodium borohydride to form a boride metal mixture; after drying in an inert atmosphere, it is subjected to hydrogen reduction enhancement to obtain a stable boride metal mixture, i.e., the acetylene selective hydrogenation catalyst in synthesis gas of the present invention.
[0014] According to the above scheme, a catalyst precursor containing a divalent copper salt, a divalent nickel salt and a carrier is prepared by an equal volume impregnation method. The carrier includes but is not limited to a γ-Al2O3 carrier, SiO2, and preferably γ-Al2O3.
[0015] According to the above scheme, the copper salt is copper acetate, and the nickel salt is nickel acetate. After the copper salt and nickel salt solution are impregnated into the carrier, the solution is allowed to stand for a period of time, such as 4 hours, and then dried, such as at 120° C. for 3 hours.
[0016] According to the above scheme, the sodium borohydride reduction is carried out by using an ethanol solution of sodium borohydride, which is placed in an ice-water mixed water bath, and the temperature of the sodium borohydride ethanol solution is maintained at 0-10°C. Further, the catalyst precursor is immersed in the solution for reduction for 3-6 hours, preferably 3-5 hours, and the amount of sodium borohydride is 1-3.5wt% of the weight of the carrier; during the reduction process, stirring is intermittent, such as stirring the solution for 3-5 minutes every half an hour, so that the undissolved sodium borohydride continues to dissolve, and the solution concentration is evenly distributed, so as to better reduce. During the sodium borohydride reduction, when the spherical catalyst particles completely turn black, and the blue or green inside the particles also turn black or gray, pour the ethanol solution on the catalyst particles, and keep the catalyst particles immersed in the solution without contact with air.
[0017] According to the above scheme, the amount of ethanol used in the sodium borohydride reduction is 1.5 to 2.5 times the weight of the catalyst carrier.
[0018] According to the above scheme, sodium borohydride is subjected to low-temperature liquid phase reduction, washed to remove sodium salt impurities, dried under an inert atmosphere, and then reduced with hydrogen.
[0019] According to the above scheme, the washing is to wash the catalyst particles with deionized water at 0-10°C to wash the sodium salt generated by the reaction, each washing lasts 5-20 minutes, and the washing is continuous for 5-10 times. The amount of water used for each washing is 1.5-2.5 times the weight of the carrier.
[0020] According to the above scheme, the drying of the catalyst under an inert atmosphere means that the washed catalyst is heated and dried in a tubular furnace filled with an inert atmosphere such as nitrogen, or in a reaction furnace filled with an inert atmosphere such as nitrogen, with a heating temperature of 120°C and a heating time of 3 to 5 hours. The heated catalyst is cooled naturally, taken out of the tubular furnace, and loaded into a reaction tube according to the amount of catalyst required for the reaction. Alternatively, after drying in the reaction tube, it is directly switched to hydrogen for reduction enhancement.
[0021] According to the above scheme, the hydrogen reduction enhancement is to reduce the dried catalyst at 300-400°C for 3-5h, and then naturally cool it to the reaction temperature to prepare a catalyst for selective hydrogenation of acetylene in synthesis gas for standby use. When used, the reaction gas can be directly introduced for reaction. The space velocity of hydrogen used in hydrogen reduction enhancement can be 500-3000h -1 airspeed.
[0022] According to the above scheme, during the low-temperature liquid phase reduction and water washing and drying process of sodium borohydride, contact with air is avoided as much as possible; the catalyst precursor is immersed in an ethanol solution of liquid sodium borohydride for reaction, and after the reaction, the ethanol on the upper part of the particles is poured out and washed with water. During the washing, the catalyst particles are immersed in deionized water and do not contact with air. When drying, the washed catalyst is transferred to a tubular furnace or a reaction tube, and an inert gas such as nitrogen is continuously passed through the tubular furnace or the reaction tube to replace the air in the tubular furnace or the reaction tube, so that the catalyst is in an inert gas atmosphere, and dried in the inert atmosphere, such as drying at 120°C for 3 hours. After natural cooling, a black particle catalyst is formed.
[0023] A method for selectively hydrogenating acetylene in synthesis gas by using the catalyst is provided, wherein the catalyst used for selectively hydrogenating acetylene in synthesis gas is used as a catalyst to catalyze the selective hydrogenation of acetylene in synthesis gas.
[0024] According to the above scheme, the content of imported acetylene in the synthesis gas is not higher than 0.3% (v / v), and the contents of CO and H2 are both greater than 10%. Such synthesis gases in industry include yellow phosphorus tail gas, calcium carbide furnace tail gas, and waste coal gas.
[0025] According to the above scheme, when the catalyst reacts, the reaction pressure is not higher than 0.3MPa, the temperature is 90-120℃, and the space velocity is 2000-3000h -1 The catalyst can convert acetylene into ethylene in a syngas atmosphere with almost no ethane produced.
[0026] Beneficial effects of the present invention:
[0027] In the hydrogenation of acetylene in a synthesis gas atmosphere, a common acetylene hydrogenation catalyst will be poisoned by the high content of CO and lose its hydrogenation activity, or the high content of H2 will cause the acetylene to be over-hydrogenated to generate ethane. The catalyst of the present invention is suitable for the hydrogenation of acetylene in synthesis gas, and is used for the selective hydrogenation of acetylene in a synthesis gas atmosphere. It has the ability to resist CO poisoning, and ethylene will not be over-hydrogenated. It has excellent hydrogenation performance, high catalytic acetylene hydrogenation activity, high selectivity, good catalyst durability, long service life, acetylene hydrogenation conversion rate>98%, ethylene selectivity>95%, and when the imported ethylene content is high and greater than 10%, the overall ethylene loss is less than 0.3% (ethylene content 10-30%), and it is an excellent catalyst for the selective hydrogenation of acetylene in a synthesis gas atmosphere.
[0028] The catalyst preparation process of the present invention first uses a carrier to load transition metal copper and nickel, uses an ethanol solution of sodium borohydride to perform low-temperature liquid phase reduction, dries the catalyst in an inert atmosphere, and then strengthens the reduction of the catalyst in a hydrogen atmosphere at high temperature. The direct reduction of hydrogen obtains zero-valent metals of copper and nickel. The present invention first uses sodium borohydride to perform low-temperature liquid phase reduction to form a borided metal mixture, and then the hydrogen-enhanced reduction obtains a copper-nickel-boron combination similar to an alloy form, wherein the copper and nickel exist in an amorphous form (amorphous copper-nickel-boron combination), and through the introduction of boron, the obtained catalyst has completely different catalytic performance and catalytic effect. The present invention first uses sodium borohydride to perform low-temperature liquid phase reduction and then hydrogen-enhanced reduction to provide a catalyst, and the selectivity of acetylene hydrogenation is good and the conversion rate is high. After the catalyst is unloaded, it can be exposed to air at room temperature, has good stability, is easy to transport in industrial use, and has industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a gas chromatographic analysis of the reaction outlet gas in Example 1. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below in conjunction with the embodiments, but the present invention is not limited thereto.
[0031] Embodiment 1:
[0032] (1) Weigh 2.36 g of copper acetate with 1 crystal water and 0.64 g of nickel acetate with 4 crystal waters, add 20 g of deionized water and 10 g of concentrated ammonia water, and stir until completely dissolved.
[0033] (2) Take 30g of γ-Al2O3 beads were impregnated with an equal volume of a mixed solution of copper acetate and nickel acetate, left at room temperature for 4h, and then dried at 120℃ for 3h.
[0034] (3) Take 50g of anhydrous ethanol, add 0.5g of sodium borohydride, stir for 3 minutes, place in an ice water bath, cool the sodium borohydride ethanol solution to below 10°C, pour the dried room temperature catalyst precursor particles into the ethanol solution, and the dissolved sodium borohydride reacts with copper acetate and nickel acetate, and bubbles escape. Stir the solution to dissolve the undissolved sodium borohydride in the solution and make the solution concentration uniform. Stir once every half an hour, and stir for 3 minutes each time.
[0035] (4) The catalyst particles are reacted in an ethanol solution of sodium borohydride for 3 to 5 hours. The catalyst particles are cut open and the inside of the particles turns black or gray, indicating that the catalyst liquid phase reduction is complete.
[0036] (5) Pour out the ethanol on the top of the particles, immediately add 50g of 0-10℃ deionized water, stir the deionized water, and dissolve the sodium salts such as sodium borate and sodium acetate generated by the reaction into the deionized water; after washing for 5 minutes, pour out the water on the top of the particles, add 50g of 0-10℃ deionized water for the second time, and stir and wash for 5 minutes. After repeating the washing 5 times, the catalyst particles are immersed in the deionized water.
[0037] (6) Replace the reaction tube with nitrogen. Continue to pass nitrogen into the reaction tube from the lower end of the reaction tube. Use a medicine spoon to transfer the catalyst immersed in water to the reaction tube. After the catalyst is loaded, seal the reaction tube with nitrogen and install it on the reaction device. Pass the nitrogen replacement system, heat it to 120°C within half an hour, and pass nitrogen to dry for 3 hours. The nitrogen space velocity is 1000h -1 .
[0038] (7) Switch nitrogen to pure hydrogen, raise the temperature to 300°C within 1 hour, and the hydrogen space velocity is 1000h -1 After 3 h of enhanced reduction, the temperature was lowered to the reaction temperature of 120°C.
[0039] (8) Switch hydrogen to feed gas, the feed gas composition is 20% CO + 20% H2 + 20% C2H4 + 0.32% C2H2 + residual N2, the reactor inlet pressure is 0.2 MPa, and the space velocity is 2000 h -1 The reaction was carried out to analyze the contents of ethylene, acetylene, ethane and other hydrocarbons in the inlet and outlet. The analysis results are shown in Table 1. From the data in the table, it can be seen that all acetylene was hydrogenated, the inlet ethylene increased by 0.31%, and the inlet ethane increased by 60ppm. Figure 1 In the chromatogram, there are 4 hydrocarbon peaks after 7 minutes. According to the peak area normalization method, the total area of the peaks is less than 0.1%. These impurities are hydrocarbons with C4 and higher carbon content generated by acetylene polymerization. They are called green oil in the acetylene industry, but the amount of them is very small.
[0040] Table 1 Effect of selective hydrogenation of acetylene in synthesis gas
[0041]
[0042]
[0043] Embodiment 2:
[0044] (1) Weigh 1.5 g of copper acetate with 1 crystal water and 1.28 g of nickel acetate with 4 crystal waters, add 20 g of deionized water and 10 g of concentrated ammonia water, and stir until completely dissolved.
[0045] (2) Take 30g of γ-Al2O3 beads were impregnated with an equal volume of a mixed solution of copper acetate and nickel acetate, left at room temperature for 4h, and then dried at 120℃ for 3h.
[0046] (3) Take 50g of anhydrous ethanol, add 1g of sodium borohydride, stir for 3 minutes, place in an ice water bath, cool the ethanol solution to 3°C, pour the dried room temperature catalyst particles into the ethanol solution, the dissolved sodium borohydride reacts with copper acetate and nickel acetate, bubbles escape, stir the solution to make the undissolved sodium borohydride in the solution continue to dissolve, and make the solution concentration uniform. Stir once every half an hour, and stir for 3 minutes each time.
[0047] (4) The catalyst particles react in the ethanol solution for 5 hours. When the catalyst particles are cut open, the color inside the particles turns black or gray, and the catalyst liquid phase reduction is complete.
[0048] (5) Pour out the ethanol on the top of the particles, immediately add 50g of 0-10℃ deionized water, stir the deionized water, and dissolve the sodium salts such as sodium borate and sodium acetate generated by the reaction into the deionized water; after washing for 5 minutes, pour out the water on the top of the particles, add 50g of 0-10℃ deionized water for the second time, and stir and wash for 5 minutes. After repeating the washing 5 times, the catalyst particles are immersed in the deionized water.
[0049] (6) Replace the reaction tube with nitrogen. Continue to pass nitrogen into the reaction tube from the lower end of the reaction tube. Use a medicine spoon to transfer the catalyst immersed in water to the reaction tube. After the catalyst is loaded, seal the reaction tube with nitrogen and install it on the reaction device. Pass the nitrogen replacement system, heat it to 120°C within half an hour, and pass nitrogen to dry for 3 hours. The nitrogen space velocity is 1000h -1 .
[0050] (7) Switch nitrogen to pure hydrogen, raise the temperature to 300°C within 1 hour, and the hydrogen space velocity is 500h -1 After 3 h of enhanced reduction, the temperature was lowered to the reaction temperature of 120°C.
[0051] (8) Switch hydrogen to feed gas, the feed gas composition is 20% CO + 20% H2 + 20% C2H4 + 0.305% C2H2 + residual N2, the reactor inlet pressure is 0.2 MPa, and the space velocity is 2000 h -1 The reaction was carried out and the contents of ethylene, acetylene, ethane and other hydrocarbons at the inlet and outlet were analyzed. The analysis results are shown in Table 2 below. From the data in Table 2, it can be seen that all acetylene was hydrogenated, the outlet ethylene increased by 0.3%, and the outlet ethane increased by 30ppm. In the outlet chromatogram, there are four main hydrocarbon peaks after 7 minutes. According to the area normalization method, the total area of the peaks is less than 0.1%.
[0052] Table 2 Effect of selective hydrogenation of acetylene in synthesis gas
[0053]
[0054] The catalyst prepared according to Example 1 was subjected to an original particle size life test in the laboratory. The cumulative operating time was 100 hours. The catalyst activity and selectivity remained stable. The experimental data are shown in Table 3.
[0055] Table 3 Experimental data on catalyst life for selective hydrogenation of acetylene in synthesis gas
[0056]
[0057] Note: The total peak area of impurity peaks is the sum of the peak area proportions of all impurity peaks when measured by the area normalization method.
[0058] As can be seen from Table 3, the catalyst of the present invention has stable properties, few side reactions, and has a promising prospect for industrial application.
[0059] Comparative Example 1:
[0060] (1) Weigh 1.5 g of copper acetate with 1 crystal water and 1.28 g of nickel acetate with 4 crystal waters, add 20 g of deionized water and 10 g of concentrated ammonia water, and stir until completely dissolved.
[0061] (2) Take 30g of γ-Al2O3 beads were impregnated with an equal volume of a mixed solution of copper acetate and nickel acetate, left at room temperature for 4h, and then dried at 120℃ for 3h.
[0062] (3) The dried catalyst was loaded into the reaction tube and loaded into the reaction device. The reaction tube and its reaction system were replaced with nitrogen. The temperature was raised to 120°C within half an hour and nitrogen was passed through for drying for 3 hours. The nitrogen space velocity was 1000 h -1 .
[0063] (4) Switch nitrogen to pure hydrogen, raise the temperature to 300°C within 1 hour, and the hydrogen space velocity is 500h -1 After reduction for 3 h, the temperature was lowered to the reaction temperature of 120°C.
[0064] (5) Switch hydrogen to feed gas, the feed gas composition is 20% CO + 20% H2 + 20% C2H4 + 0.305% C2H2 + residual N2, the reactor inlet pressure is 0.2 MPa, and the space velocity is 2000 h -1 The reaction was carried out to analyze the contents of imported and exported ethylene, acetylene, ethane and other hydrocarbons. The analysis results are shown in Table 4 below. As can be seen from the data in Table 4, all acetylene was hydrogenated, and a large amount of ethylene was also hydrogenated to ethane, and the export ethane increased with the increase of reaction time. During the reaction, acetylene was over-hydrogenated, and a large amount of ethylene was hydrogenated. The reaction heat caused the reaction temperature to rise, which was further aggravated by over-hydrogenation, and the temperature rose, and the amount of green oil generated increased. At the outlet temperature measuring point of the reactor, it can be seen that the temperature rose significantly. This reaction phenomenon is similar to the catalyst overheating accident in industrial practice. As can be seen from the comparative example, for the selective hydrogenation reaction of acetylene in synthesis gas, the copper-nickel catalyst directly obtained by high-temperature reduction of hydrogen is not suitable for acetylene hydrogenation of synthesis gas.
[0065] Table 4 Experimental data of comparative catalysts for selective hydrogenation of acetylene in synthesis gas
[0066]
[0067] Note: The total peak area of impurity peaks is the sum of the peak area proportions of all impurity peaks when measured by the area normalization method.
[0068] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the appended claims of the present invention.
Claims
1. A catalyst for selective hydrogenation of acetylene in synthesis gas, characterized in that: The catalyst comprises a catalyst carrier and active components copper and nickel loaded on the carrier, wherein the copper loading is 1-2.5wt%, the nickel loading is 0.5-1.5wt%, and the zero-valent boron, zero-valent metal copper and zero-valent nickel in the catalyst form an amorphous copper-nickel-boron alloy.
2. The catalyst according to claim 1, characterized in that: The catalyst carrier is γ-Al2O3 or SiO2.
3. The catalyst according to claim 1, characterized in that: The catalyst carrier is γ-Al2O3 with a specific surface area of 100 to 250 m 2 / g, bulk density 0.5±0.1g / ml, average pore diameter 5~25nm, pore volume 0.5~1.5ml / g.
4. The method for preparing the catalyst for selective hydrogenation of acetylene in synthesis gas according to claim 1, characterized in that: A catalyst precursor containing a divalent copper salt, a divalent nickel salt and a carrier is sequentially subjected to sodium borohydride low-temperature liquid phase reduction and hydrogen reduction enhancement to prepare a catalyst for selective hydrogenation of acetylene in synthesis gas.
5. The method for preparing the catalyst for selective hydrogenation of acetylene in synthesis gas according to claim 4, characterized in that: After preparing and drying a catalyst precursor containing a divalent copper salt, a divalent nickel salt and a carrier, sodium borohydride is first used for low-temperature liquid phase reduction to form a boride metal mixture; after drying in an inert atmosphere, hydrogen reduction is strengthened to obtain a stable boride metal mixture, i.e., a catalyst for selective hydrogenation of acetylene in synthesis gas.
6. The preparation method according to claim 5, characterized in that: The sodium borohydride reduction is carried out by placing a sodium borohydride ethanol solution in an ice-water mixed water bath, maintaining the temperature of the sodium borohydride ethanol solution at 0-10° C., and immersing the catalyst precursor in the solution for reduction for 3-6 hours.
7. The preparation method according to claim 5, characterized in that: Sodium borohydride is subjected to low temperature liquid phase reduction, washed to remove sodium salt impurities, dried, and then subjected to hydrogen reduction enhancement; The hydrogen reduction enhancement is to reduce the dried catalyst at 300-400° C. for 3-5 hours, and then naturally cool it to the reaction temperature to prepare a catalyst for selective hydrogenation of acetylene in synthesis gas.
8. A method for selective hydrogenation of acetylene in synthesis gas using the catalyst according to claim 1, characterized in that: The selective hydrogenation of acetylene in the synthesis gas is catalyzed by using a catalyst used for the selective hydrogenation of acetylene in the synthesis gas.
9. The method according to claim 8, characterized in that: The imported acetylene content in the synthesis gas is not higher than 0.3% (v / v), and the CO and H2 contents are both greater than 10%.
10. The method according to claim 8, characterized in that: During the catalyst reaction, the reaction pressure is not higher than 0.3MPa, the temperature is 90-120℃, and the air velocity is 2000-3000h -1 .
Citation Information
Patent Citations
Method for preparing alpha-phenethyl alcohol by catalyzing acetophenone hydrogenation with supported amorphous alloy
CN110368946A
Copper-based catalyst for acetylene selective hydrogenation and preparation method thereof
CN111437852A
Non-crystal catalyst for hydrogenating benzene and its preparing process
CN1298760A