A NiCa-based bifunctional material, its preparation method and application, and an integrated method for direct air carbon dioxide capture and in-situ conversion to produce methane.

By using NiCa-based bifunctional materials to efficiently capture and in-situ convert CO2 in the air at room temperature, the problems of low capture efficiency and low conversion yield in existing technologies are solved, realizing the integration of low-cost direct air carbon dioxide capture and in-situ methane production.

CN118949999BActive Publication Date: 2026-11-10SHANGHAI JIAOTONG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411009817.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2026-11-10
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

Existing technologies have low efficiency in capturing extremely low concentrations of CO2 from the air at room temperature, and the yield of methane conversion is low and the cost is high, making it difficult to achieve the integration of direct air carbon dioxide capture and in-situ conversion to produce methane.

Method used

The NiCa-based bifunctional material, with a chemical composition including calcium hydroxide and elemental nickel, was prepared by the sol-gel method. CO2 was captured by passing humid air through the material at room temperature, followed by in-situ methanation in a hydrogen atmosphere. Mg, Ce, and Zr elements were doped into the material to improve its stability.

Benefits of technology

It achieves highly efficient capture of extremely low concentrations of CO2 at room temperature, with a CO2 adsorption capacity of up to 8.96 mmol/g and a conversion rate of 95.97%. The in-situ conversion of CH4 yield is as high as 8.60 mmol/g, and the material cost is low with good cycle stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention provides a NiCa-based bifunctional material, its preparation method and application, and an integrated method for direct air carbon dioxide capture and in-situ conversion to methane, relating to the field of carbon capture technology. The invention provides a NiCa-based bifunctional material with a chemical composition comprising calcium hydroxide and elemental nickel, wherein the mass content of elemental nickel is 5-20%. Using calcium hydroxide as a CO2 adsorbent and nickel as a catalyst, this invention achieves a significantly higher adsorption capacity for extremely low concentrations of CO2 than existing K-based and Na-based adsorbents. The NiCa-based bifunctional material provided by this invention exhibits an adsorption capacity of up to 8.96 mmol / g for 400 ppm CO2 at room temperature, and a CH4 yield of up to 8.60 mmol / g from in-situ conversion. It achieves highly efficient capture of extremely low concentrations of CO2, high yield and selectivity of CH4 from in-situ conversion, and excellent performance in direct air carbon dioxide capture and in-situ conversion to methane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of carbon capture technology, specifically to a NiCa-based bifunctional material and its preparation method and application, and an integrated method for direct air carbon dioxide capture and in-situ conversion to produce methane. Background Technology

[0002] Carbon capture is mainly divided into two pathways based on the source of carbon dioxide: carbon capture and storage (CCS) and direct air capture (DAC). The former, also known as "flue gas capture," captures carbon from power plant and industrial waste gas, and currently has a higher level of technological maturity; the latter, where carbon dioxide originates from natural air, represents a new generation of carbon capture technology. Traditional CCUS (Carbon Capture, Utilization, and Storage) technology consists of two stages: CO2 capture and storage or conversion. In recent years, renewable electricity-to-hydrogen technology has developed rapidly, and the cost of hydrogen production has continued to decrease. If the energy required for CO2 desorption, purification, and conversion is utilized, and CO2 is not desorbed, through hydrogenation catalytic reaction, the regeneration of the adsorbent and the resource utilization of CO2 can be achieved simultaneously, realizing integrated carbon capture and utilization (ICCU), which will have significant energy-saving and consumption-reducing advantages.

[0003] Currently, research on ICCU technology mainly focuses on flue gas CO2 concentration (volume concentration of approximately 10-20%). Only four papers report on the application of ICCU technology to DAC. The adsorption-catalytic bifunctional materials used are all supported materials, with adsorbent components such as potassium (K) and sodium (Na) and ruthenium (Ru) catalyst supported on alumina (Al2O3). The material compositions are 22.1% K2CO3 / Al2O3 + 4% Ru / Al2O3 (VESELOVSKAYA JV, PARUNIN PD, NETSKINA OV, et al. A Novel Process for Renewable Methane Production: Combining Direct Air Capture by K2CO3 / Alumina Sorbent with CO2 Methanation over Ru / Alumina Catalyst[J]. Topics in Catalysis, 2018, 61(15): 1528-36.) and 5% Ru / 40% K2CO3 / K-β”-Al2O3 (LEE J, OTOMOJ. Low-Temperature Activated Direct Air Capture Methanation Using K-β”Alumina[J]. Industrial&Engineering Chemistry Research, 2023, 62(31):12096-108.), 0.5% Ru, 6.1% “Na2O” / Al2O3 (JEONG-POTTER C, FARRAUTO R. Feasibility Study of CombiningDirect Air Capture of CO2and Methanation at Isothermal Conditions with DualFunction Materials[J].Applied Catalysis B:Environmental,2021,282:119416.) and 1%Ru, 6.1% "Na2O" / Al2O3 (JEONG-POTTER C, ABDALLAH M, SANDERSON C, et al.Dual-function materials (Ru+Na2O / Al2O3) for direct air capture of CO2 and in situ catalytic methanation: The impact of realistic ambient conditions [J]. Applied Catalysis B: Environment and Energy, 2022, 307: 120990. The above materials can achieve a maximum adsorption capacity of 1.3 mmol / g for 400 ppm CO2 at room temperature, and a methane yield of 1.04 mmol / g, verifying the feasibility of the integrated direct air CO2 capture and in-situ conversion to methane (DAC-ICCU) technology. However, the CO2 capture capacity of the above materials at room temperature is low, and even with a high CO2 conversion rate, the yield of CH4 obtained by heating is still very low.

[0004] Chinese patent CN117046437A discloses a bifunctional material for integrating CO2 capture and fuel production in optical drives. The preparation reagents include calcium nitrate tetrahydrate, nickel nitrate hexahydrate, and aluminum nitrate nonahydrate, with citric acid as a chelating agent and deionized water as a solvent. This material is used for calcium cycle coupling in a methane dry reforming reaction. This bifunctional material is low-cost, produces little carbon, can convert greenhouse gases into syngas, achieving negative greenhouse gas emissions, and exhibits high CO2 conversion rates, CH4 conversion rates, CO yield, and H2 yield. The conversion reaction used in this bifunctional material is methane dry reforming. The capture process targets high-concentration CO2 in flue gas (20% CO2 concentration), and both the capture and conversion processes are at high temperatures (720°C). However, this bifunctional material is difficult to use for capturing extremely low concentrations of CO2 from the air at room temperature, resulting in low CO2 capture rates.

[0005] Chinese patent CN117839377A discloses an integrated capture and conversion system based on a bifunctional adsorption-catalytic material for carbon dioxide. The bifunctional material consists of three parts: an adsorbent, a catalyst, and a support. The adsorbent is an alkali metal, including one or more of K₂CO₃, Na₂CO₃, and MgO. The catalyst, which enables the hydrogenation conversion process, includes one or more of Ru, Ni, Co, and Pt. The support includes one or more of Al₂O₃, SiO₂, and CeO₂. The adsorbent and catalyst are uniformly dispersed on a support with a predetermined specific surface area and pore structure to enhance contact and mass transfer with the gas flow. However, the CO₂ capture capacity of this bifunctional adsorption-catalytic material is below 1 mmol / g, indicating a low CO₂ capture rate. Summary of the Invention

[0006] In view of this, the purpose of this invention is to provide a NiCa-based bifunctional material, its preparation method and application, and an integrated method for direct air carbon dioxide capture and in-situ conversion to produce methane. The NiCa-based bifunctional material provided by this invention, used in DAC-ICCU, can achieve highly efficient capture of extremely low concentrations of CO2, with high CO2 adsorption capacity and high CH4 yield.

[0007] To achieve the above-mentioned objectives, the present invention provides the following technical solution:

[0008] This invention provides a NiCa-based bifunctional material, the chemical composition of which includes calcium hydroxide and elemental nickel; the mass content of elemental nickel in the NiCa-based bifunctional material is 5-20%.

[0009] Preferably, the NiCa-based bifunctional material further includes a doped metal element, wherein the doped metal element includes one or more of Mg, Ce and Zr;

[0010] The molar ratio of calcium to doped metal elements in the NiCa-based bifunctional material is 5–15:1.

[0011] This invention provides a method for preparing the NiCa-based bifunctional material described above, comprising the following steps:

[0012] A mixture of calcium precursor, nickel precursor, citric acid and water was prepared to obtain a solution.

[0013] The mixture is then subjected to heat treatment to obtain a sol;

[0014] The sol was dried and then calcined to obtain NiCa-based calcined material;

[0015] The NiCa-based calcined material is reduced to obtain the NiCa-based bifunctional material.

[0016] Preferably, when the NiCa-based bifunctional material further includes a doped metal oxide, the mixture further includes a doped metal precursor; the doped metal precursor includes one or more of magnesium precursor, cerium precursor and zirconium precursor.

[0017] In the mixture, the molar ratio of metal ions to water is 1:30 to 80, and the molar ratio of metal ions to citric acid is 1:0.8 to 1.2.

[0018] Preferably, the temperature of the heat treatment is 80–90°C.

[0019] Preferably, the calcination temperature is 500–650°C, and the holding time is 3–5 hours.

[0020] Preferably, the reduction treatment temperature is 450–550°C, and the holding time is 0.5–2 h; the reducing agent used in the reduction treatment includes a hydrogen-containing atmosphere, wherein the volume fraction of hydrogen in the hydrogen-containing atmosphere is 10–100%.

[0021] This invention also provides the application of the NiCa-based bifunctional material described in the above technical solution or the NiCa-based bifunctional material prepared by the above technical solution in CO2 capture and / or CO2 conversion to methane.

[0022] This invention also provides an integrated method for direct air carbon dioxide capture and in-situ conversion to produce methane, comprising the following steps:

[0023] Moist air is introduced into the NiCa-based bifunctional material for direct air CO2 capture, followed by in-situ methanation in a hydrogen-containing atmosphere to obtain methane; the NiCa-based bifunctional material is the NiCa-based bifunctional material described in the above technical solution or the NiCa-based bifunctional material prepared by the preparation method described in the above technical solution.

[0024] Preferably, the temperature for direct air CO2 capture is room temperature;

[0025] The volume fraction of hydrogen in the hydrogen-containing atmosphere is 10-100%.

[0026] The in-situ methanation temperature is 400–600 °C.

[0027] This invention provides a NiCa-based bifunctional material, chemically composed of calcium hydroxide and elemental nickel; the mass content of elemental nickel in the NiCa-based bifunctional material is 5-20%. This invention uses Ca(OH)₂ as a CO₂ adsorbent and Ni as a catalyst. At room temperature and in humid air, the adsorption capacity of extremely low concentrations of CO₂ is significantly greater than that of existing K-based and Na-based adsorbents. The material exhibits good cycle stability and a fast adsorption rate. As shown in the test results of the examples, the NiCa-based bifunctional material provided by this invention can rapidly adsorb extremely low concentrations (400 ppm) of CO₂ in humid air at room temperature, with an adsorption capacity as high as 8.96 mmol / g, a CO₂ conversion rate as high as 95.97%, and an in-situ CH₄ yield as high as 8.60 mmol / g, with a CH₄ selectivity of 100% and no CO production. It can achieve highly efficient capture of extremely low concentrations of CO₂, high CH₄ yield from in-situ conversion, and high CH₄ selectivity. It demonstrates excellent performance in direct air carbon dioxide capture and in-situ conversion for methane production. Moreover, this invention does not use precious metals, resulting in low cost for the NiCa-based bifunctional material.

[0028] This invention utilizes Mg, Ce, and Zr doping as promoters to inhibit the agglomeration and deactivation of NiCa-based bifunctional materials, thereby further improving their recycling stability. As shown in the test results of the examples, doping NiCa bifunctional materials with MgO, CeO2, or ZrO2 can improve their cycling performance. Compared to standard NiCa bifunctional materials, the CO2 adsorption capacity of the doped NiCa-based bifunctional materials decreases slightly due to the reduced effective Ca content. However, the CO2 adsorption capacity of all three NiCa bifunctional materials (NiCaMg, NiCaCe, and NiCaZr) is higher than 7.4 mmol / g, and the CO2 conversion rate is higher than 95.4%, while the CH4 selectivity remains at 100%. Therefore, the bifunctional materials doped with metal oxides still exhibit excellent performance. In five cycles, the CO2 adsorption capacity decreased from 7.42 mmol / g to 7.29 mmol / g, and the CO2 conversion rate decreased from 97.11% to 94.39%, with a small degree of performance degradation, indicating that the doping of NiCaZr with ZrO2 significantly improves its cycle stability.

[0029] The method for preparing the NiCa-based bifunctional material provided by this invention is simple in process and operation, with a wide range of raw material sources, low cost, and suitable for industrial production. Attached Figure Description

[0030] Figure 1 A schematic diagram of an integrated apparatus for reduction treatment, direct air carbon dioxide capture, and in-situ conversion of methane;

[0031] Figure 2 The images show the XRD patterns of the NiCa-based calcined material (NiCaZr-calcined), NiCa-based bifunctional material (NiCaZr-pretreated), and the material after CO2 adsorption (NiCaZr-CO2) prepared in Example 4.

[0032] Figure 3 The figures show the real-time changes in the concentration and temperature of the gas components at the reactor outlet during the DAC (a-d) and in-situ methanation (e-h) processes. In the figures for a-d, the black curve represents the CO2 concentration at the reactor outlet, and the gray dashed line represents the CO2 inlet concentration. Detailed Implementation

[0033] This invention provides a NiCa-based bifunctional material, the chemical composition of which includes calcium hydroxide and elemental nickel; the mass content of elemental nickel in the NiCa-based bifunctional material is 5-20%.

[0034] In this invention, the NiCa-based bifunctional material preferably further includes a doped metal element, which preferably includes one or more of Mg, Ce, and Zr. When the doped metal element is a mixture of two or more, this invention does not have a particular limitation on the ratio of different doped metal elements, and any ratio is acceptable. In this invention, the doped metal element preferably exists in the form of a doped metal oxide. In this invention, the doped metal oxide preferably includes one or more of MgO, CeO2, and ZrO2.

[0035] In this invention, the molar ratio of calcium to doped metal element (denoted as M) in the NiCa-based bifunctional material is preferably 5 to 15:1, more preferably 6 to 12:1, and even more preferably 8 to 10:1.

[0036] In this invention, the mass content of elemental nickel in the NiCa-based bifunctional material is preferably 5-20%, more preferably 8-12%, and even more preferably 10%.

[0037] This invention also provides a method for preparing the NiCa-based bifunctional material described in the above technical solution, comprising the following steps:

[0038] A mixture of calcium precursor, nickel precursor, citric acid and water was prepared to obtain a solution.

[0039] The mixture is then subjected to heat treatment to obtain a sol;

[0040] The sol was dried and then calcined to obtain NiCa-based calcined material;

[0041] The NiCa-based calcined material is reduced to obtain the NiCa-based bifunctional material.

[0042] Unless otherwise specified, the materials and equipment used in this invention are all commercially available products in the field.

[0043] This invention involves mixing a calcium precursor, a nickel precursor, citric acid, and water to obtain a mixture.

[0044] In this invention, the calcium precursor preferably includes one or more of calcium nitrate, calcium oxalate, and calcium acetate.

[0045] In this invention, the nickel precursor preferably includes one or more of nickel nitrate and / or nickel acetate.

[0046] In this invention, when the NiCa-based bifunctional material further includes a doped metal oxide, the mixture also includes a doped metal precursor. The mixture is preferably obtained by mixing a calcium precursor, a nickel precursor, a doped metal precursor, citric acid, and water. In this invention, the doped metal precursor preferably includes one or more of a magnesium precursor, a cerium precursor, and a zirconium precursor; the nickel precursor preferably includes one or more of a magnesium nitrate, a magnesium oxalate, and a magnesium acetate; the cerium precursor preferably includes cerium nitrate and / or cerium acetate; and the zirconium precursor preferably includes one or more of a zirconium nitrate, a zirconium oxalate, and a zirconium acetate.

[0047] The present invention does not have any special limitations on the mixing, as long as the raw materials can be dissolved in water, such as by stirring; the mixing temperature is preferably room temperature.

[0048] In this invention, the molar ratio of metal ions to water in the mixture is preferably 1:30-80, more preferably 1:35-60, and even more preferably 1:40-50; the molar ratio of metal ions to citric acid in the mixture is preferably 1:0.8-1.2, more preferably 1:0.9-1.1, and even more preferably 1:1.

[0049] After obtaining the mixture, the present invention performs heat treatment on the mixture to obtain a sol.

[0050] In this invention, the heat treatment temperature is preferably 80-90°C, more preferably 80-85°C; the heat treatment is preferably carried out under stirring conditions, and this invention does not have a special limitation on the stirring time, as long as a transparent sol is obtained.

[0051] After obtaining the sol, the present invention dries and calcines the sol to obtain NiCa-based calcined material.

[0052] In this invention, the drying temperature is preferably 110-130°C, more preferably 120°C; the drying time is preferably 8-16 hours, more preferably 10-12 hours; and the drying is preferably carried out in an oven.

[0053] In this invention, the calcination temperature is preferably 500–650°C, more preferably 530–620°C, and even more preferably 550–600°C; the calcination holding time is preferably 3–5 h, more preferably 3.5–4.5 h, and even more preferably 4 h; the heating rate from room temperature to the calcination temperature is preferably 2.5–10°C / min, and even more preferably 5–8°C / min.

[0054] After obtaining the NiCa-based calcined material, the present invention performs a reduction treatment on the NiCa-based calcined material to obtain the NiCa-based bifunctional material.

[0055] In this invention, the temperature of the reduction treatment is preferably 450–550°C, more preferably 480–520°C, and even more preferably 500°C; the holding time of the reduction treatment is preferably 0.5–2 h, more preferably 1–1.5 h; the time for the temperature to rise from room temperature to the pretreatment temperature is preferably 25–45 min, more preferably 30–40 min, and even more preferably 30–35 min; the pressure of the reduction treatment is preferably atmospheric pressure; the reducing agent used in the reduction treatment preferably includes a hydrogen-containing atmosphere; the hydrogen-containing atmosphere preferably includes hydrogen-nitrogen; the volume fraction of hydrogen in the hydrogen-containing atmosphere is preferably 10–100%, more preferably 30–80%, and even more preferably 40–50%; the flow rate of the hydrogen-containing atmosphere is preferably 300–500 mL / min, more preferably 350–450 mL / min, and even more preferably 400 mL / min.

[0056] In this invention, the pretreatment preferably includes: heating, introducing a hydrogen-containing atmosphere, and purging activation. In this invention, during the reduction treatment, NiO is reduced to Ni, and CaCO3 is ultimately converted to Ca(OH)2.

[0057] After the pretreatment is completed, the present invention preferably further includes purging the system obtained by pretreatment with nitrogen gas until no hydrogen gas can be detected in the outflow gas flow to obtain the NiCa-based bifunctional material; the nitrogen gas flow rate is preferably 300-500 mL / min, more preferably 350-450 mL / min, and even more preferably 400 mL / min.

[0058] When the reducing agent is a hydrogen-containing atmosphere, after the pretreatment is completed, the present invention preferably further includes purging the system obtained by pretreatment with nitrogen until no hydrogen is detected in the outflow gas, thereby obtaining the NiCa-based bifunctional material; the nitrogen flow rate is preferably 300-500 mL / min, more preferably 350-450 mL / min, and even more preferably 400 mL / min.

[0059] This invention also provides the application of the NiCa-based bifunctional material described in the above-described technical solutions or the NiCa-based bifunctional material prepared by the above-described preparation method in CO2 capture and / or CO2 conversion to methane. In this invention, the concentration of CO2 in the CO2 capture and CO2 conversion to methane is preferably independently ≥400 ppm.

[0060] This invention also provides an integrated method for direct air carbon dioxide capture and in-situ conversion to produce methane, comprising the following steps:

[0061] Moist air is introduced into the NiCa-based bifunctional material for direct air CO2 capture, followed by in-situ methanation in a hydrogen-containing atmosphere to obtain methane; the NiCa-based bifunctional material is the NiCa-based bifunctional material described in the above technical solution or the NiCa-based bifunctional material prepared by the preparation method described in the above technical solution.

[0062] In embodiments of the present invention, the humid air is preferably simulated humid air, which preferably includes CO2, O2, N2, and water; the concentration of CO2 in the simulated humid air is preferably 400 ppm, and the volume fraction of oxygen is preferably 21%. In the present invention, the relative humidity of the air is preferably 30-90%, specifically preferably 30%, 50%, 70%, or 90%.

[0063] In this invention, the temperature for direct air CO2 capture is preferably room temperature (15-40°C); the air flow rate is preferably 300-500 mL / min, more preferably 350-450 mL / min, and even more preferably 400 mL / min; during the direct air CO2 capture process, Ca(OH)2 captures CO2 to generate CaCO3, and the air flow is stopped when the NiCa-based bifunctional material reaches adsorption saturation.

[0064] In this invention, the temperature of the in-situ methanation is preferably 400–600°C, more preferably 450–550°C, and even more preferably 450–500°C; the flow rate of the hydrogen-containing atmosphere is preferably 100–300 mL / min, more preferably 150–250 mL / min, and even more preferably 200 mL / min; the volume fraction of hydrogen in the hydrogen-containing atmosphere is preferably 10–100%, more preferably 30–80%, and even more preferably 40–50%; this invention does not specifically limit the time of the in-situ methanation, and the in-situ methanation is stopped when the CH4 concentration in the outflow gas is lower than 0.01 vol%; the pressure of the in-situ methanation is preferably atmospheric pressure; during the in-situ methanation process, the CO2 adsorbed under the action of the catalyst Ni reacts with H2 to obtain the target product CH4, and the adsorbent is regenerated into Ca(OH)2.

[0065] In this invention, the reduction treatment, direct air carbon dioxide capture, and in-situ methane conversion are preferably integrated in [the following context is missing from the original text]. Figure 1 The process is carried out in the apparatus shown below, in conjunction with... Figure 1A detailed description is provided. A NiCa-based calcined material is filled into a quartz tube reactor, with both ends fixed with quartz wool. Thermocouples are inserted into the NiCa-based calcined material to measure temperature. The quartz tube reactor is placed in a tube furnace, and a variable temperature mode is achieved by adjusting the temperature of the tube furnace (room temperature (15–40°C) for the direct air CO2 capture stage, and 400–600°C for the in-situ methane conversion stage). During the direct air CO2 capture process, the flow rates of two air streams are controlled to simulate relative humidity levels (30%, 50%, 70%, and 90%). One air stream passes through a water-filled gas washing bottle, while the other does not. Two non-dispersive infrared analyzers are used to monitor the gas composition in real time; one is used to monitor the extremely low CO2 concentration in the DAC step, and the other is used to monitor the concentrations of CO2, CH4, and CO in the in-situ methanation.

[0066] In this invention, the integrated method for direct air CO2 capture and in-situ conversion to prepare methane includes two main stages: direct air CO2 capture and in-situ methanation. The specific experimental operation process includes: introducing simulated air at room temperature and setting the relative humidity to simulate the air under real conditions. During this process, Ca(OH)2 captures CO2 to generate CaCO3. After the NiCa-based bifunctional material reaches adsorption saturation, the gas flow is stopped; pure N2 is introduced for purging; the reactor is heated and a second hydrogen-containing atmosphere is introduced. During this process, under the action of the catalyst Ni, the adsorbed CO2 reacts with H2 to obtain the target product CH4, and the adsorbent is regenerated into Ca(OH)2. The gas flow is continued until the CH4 concentration in the reactor effluent is lower than 0.01 wt%; pure N2 is introduced for purging until H2 is undetectable in the effluent. All the above operations are carried out at atmospheric pressure.

[0067] To further illustrate the present invention, the following detailed description, in conjunction with embodiments, provides an integrated method for the preparation and application of a NiCa-based bifunctional material, as well as an integrated method for the direct capture of carbon dioxide from the air and in-situ conversion to prepare methane. However, these descriptions should not be construed as limiting the scope of protection of the present invention.

[0068] Example 1

[0069] The sol-gel method was used for preparation: calcium nitrate and citric acid were added to deionized water and stirred at room temperature until completely dissolved and uniformly dispersed to obtain a mixed solution. Stirring was continued at 80°C until a transparent sol was formed. This sol was then dried in a 120°C oven for 12 hours to obtain a puffed solid. The puffed solid was placed in a muffle furnace and heated to 550°C at a rate of 5°C / min, then calcined for 4 hours to obtain a NiCa-based calcined material (abbreviated as NiCa-calcined). Wherein, Ni mass / (Ni mass + Ca(OH)2 mass) × 100% = 10%, and the total amount of deionized water and metal ions in the mixed solution (Ca...)...2+ +Ni 2+ The molar ratio of citric acid to the total amount of metal ions is 40:1, and the molar ratio of citric acid to the total amount of metal ions is 1:1.

[0070] Example 2

[0071] The sol-gel method was used for preparation: calcium nitrate, magnesium nitrate, and citric acid were added to deionized water and stirred at room temperature until completely dissolved and uniformly dispersed to obtain a mixed solution. Stirring was continued at 80°C until a transparent sol was formed. This sol was then dried in a 120°C oven for 12 hours to obtain a puffed solid. The puffed solid was placed in a muffle furnace and heated to 550°C at a rate of 5°C / min, then calcined for 4 hours to obtain a NiCa-based calcined material (abbreviated as NiCaMg-calcined). The mass percentage of Ni (Ni mass / (Ni mass + Ca(OH)2 mass + MgO mass)) × 100% = 10%, and the H2O content in the mixed solution was: (Ca...)... 2+ +Ni 2+ +Mg 2+ The molar ratio is 40:1, and the molar ratio of citric acid to the total amount of metal ions is 1:1.

[0072] Example 3

[0073] The sol-gel method was used for preparation: calcium nitrate, cerium nitrate, and citric acid were added to deionized water and stirred at room temperature until completely dissolved and uniformly dispersed to obtain a mixed solution. Stirring was continued at 80°C until a transparent sol was formed. This sol was then dried in a 120°C oven for 12 hours to obtain a puffed solid. The puffed solid was placed in a muffle furnace and heated to 550°C at a rate of 5°C / min, then calcined for 4 hours to obtain NiCa-based calcined material (abbreviated as NiCaCe-calcined). The mass percentage of Ni (Ni mass / (Ni mass + Ca(OH)2 mass + CeO2 mass)) × 100% = 10%, and the H2O content in the mixed solution was: (Ca...)... 2+ +Ni 2+ +Ce 4+ The molar ratio is 40:1, and the molar ratio of citric acid to the total amount of metal ions is 1:1.

[0074] Example 4

[0075] The sol-gel method was used for preparation: calcium nitrate, zirconium nitrate, and citric acid were added to deionized water and stirred at room temperature until completely dissolved and uniformly dispersed to obtain a mixed solution. Stirring was continued at 80°C until a transparent sol was formed. This sol was then dried in a 120°C oven for 12 hours to obtain a puffed solid. The puffed solid was placed in a muffle furnace and heated to 550°C at a rate of 5°C / min, then calcined for 4 hours to obtain a NiCa-based calcined material (abbreviated as NiCaZr-calcined). The mass percentage of Ni (Ni mass / (Ni mass + Ca(OH)2 mass + ZrO2 mass)) × 100% = 10%, and the H2O content in the mixed solution was: (Ca...)... 2+ +Ni 2+ +Zr 4+ The molar ratio is 40:1, and the molar ratio of citric acid to the total amount of metal ions is 1:1.

[0076] Example 5

[0077] use Figure 1 The apparatus integrates the reduction treatment, direct air CO2 capture, and in-situ methane conversion of the NiCa-based calcined materials prepared in Examples 1-4. The NiCa-based calcined materials are filled into a quartz tube reactor, with both ends fixed with quartz wool. Thermocouples are inserted into the material to measure temperature. The quartz tube reactor is placed in a tube furnace, and a variable temperature mode is achieved by adjusting the temperature of the tube furnace (25°C for the direct air CO2 capture stage and 450°C for the in-situ methane conversion stage). During the direct air CO2 capture process, the flow rates of two simulated air streams are controlled to simulate relative humidity levels (dry, 30%, 50%, 70%, and 90%). One air stream passes through a gas washing bottle, while the other does not. Two non-dispersive infrared analyzers are used to monitor the gas composition in real time; one is used to monitor the extremely low CO2 concentration in the DAC step, and the other is used to monitor the concentrations of CO2, CH4, and CO in the in-situ methanation. Simulated air composition: 400ppm CO2 + 21vol% O2 + N2.

[0078] The specific experimental procedure includes:

[0079] Step 1) Reduction treatment: Heat to 500℃ for 30 min, introduce 40 vol% H2-N2 at a flow rate of 400 mL / min, purge and activate for 1 h to obtain the NiCa-based bifunctional material; The NiCa-based bifunctional materials obtained by reduction treatment of the NiCa-based calcined materials prepared in Examples 1 to 4 are respectively named NiCa, NiCaMg, NiCaCe and NiCaZr;

[0080] Step 2) Purge with pure N2 at a flow rate of 400 mL / min until no H2 is detected in the outflow gas;

[0081] Step 3) DAC: Simulated air is introduced at room temperature, and the relative humidity is set to 90%. The air supply is stopped after the NiCa-based bifunctional material reaches adsorption saturation.

[0082] Step 4) Purge with pure N2 at a flow rate of 400 mL / min;

[0083] Step 5) In-situ methanation: The reactor is heated to 450°C, and 40 vol% H2-N2 is introduced at a flow rate of 200 mL / min. Under the action of catalyst Ni, the adsorbed CO2 reacts with H2 to obtain the target product CH4, and the adsorbent is regenerated into Ca(OH)2. The gas is continuously introduced until the CH4 concentration in the gas flow out of the reactor is less than 0.01 wt%.

[0084] Step 6) Purge with pure N2 at a flow rate of 400 mL / min until no H2 is detected in the outflow gas;

[0085] Step 7) Repeat steps 1) to 6) to perform a cycle performance test. Steps 1) to 6) are all performed under normal pressure.

[0086] The NiCa-based bifunctional materials obtained by reduction treatment of the NiCa-based calcined materials prepared in Examples 1-4 are respectively named NiCa, NiCaMg, NiCaCe and NiCaZr.

[0087] Figure 2 The XRD patterns of the NiCa-based calcined material (NiCaZr-calcined), NiCa-based bifunctional material (NiCaZr-pretreated), and NiCaZr after CO2 adsorption (NiCaZr-CO2) prepared in Example 4 show that the main components of the calcined NiCaZr are CaCO3, NiO, and ZrO2. Due to the low content and uniform dispersion of NiO and ZrO2, no characteristic peaks are observed in the XRD results. The pretreatment step enables NiCaZr to have active components—Ca(OH)2 and Ni—that can achieve carbon capture and methanation functions in the air. Zr species still exist in the form of oxide ZrO2. During the DAC process, Ca(OH)2 adsorbs CO2 from the air and converts it into CaCO3.

[0088] Figure 3 Table 1 shows the real-time changes in the concentration and temperature of the gas components at the reactor outlet during the DAC (a-d) and in-situ methanation (e-h) processes. In sections a-d, the black curve represents the CO2 concentration at the reactor outlet, and the gray dashed line represents the CO2 inlet concentration. The CO2 adsorption capacity, conversion rate, CH4 yield, and selectivity of the NiCa-based bifunctional material were calculated using the inlet and outlet concentrations, as shown in Table 1. The CO2 inlet concentration was obtained from a blank experiment (i.e., no material was added to the quartz tube reactor).

[0089] Table 1 Catalytic performance parameters of NiCa-based bifunctional materials used for the first time

[0090]

[0091]

[0092] NiCa exhibited excellent performance, with a CO2 adsorption capacity of 8.96 mmol / g and a CH4 production of 8.60 mmol / g. No CO2 was released during the heating phase, and CH4 was the only conversion product, with no CO generation. However, due to sintering and agglomeration of the material, after five cycles of DAC and in-situ methanation, the CO2 adsorption capacity of NiCa dropped sharply to 46% of that in the first cycle.

[0093] Doping NiCa bifunctional materials with MgO, CeO2, or ZrO2 can improve their cycling performance. Compared to standard NiCa bifunctional materials, the CO2 adsorption capacity of the doped NiCa-based bifunctional materials decreases slightly due to the reduced effective Ca content. However, the CO2 adsorption capacity of all three NiCa bifunctional materials (NiCaMg, NiCaCe, and NiCaZr) is higher than 7.4 mmol / g, and the CO2 conversion rate is higher than 95.4%, while the CH4 selectivity remains at 100%. Therefore, the bifunctional materials doped with metal oxides still exhibit excellent performance. In five cycles, the CO2 adsorption capacity decreased from 7.42 mmol / g to 7.29 mmol / g, and the CO2 conversion rate decreased from 97.11% to 94.39%, showing only a small performance degradation. This indicates that doping NiCaZr with ZrO2 significantly improves its cycling stability.

[0094] During the methanation process, CH4 is gradually generated as the temperature increases, with no CO2 release or CO generation, indicating that the NiCa-based bifunctional material provided by this invention has high CO2 conversion rate and CH4 selectivity, and has excellent catalytic conversion performance.

[0095] Comparative Example 1

[0096] Supported bifunctional materials were synthesized by impregnation method, using Al2O3 as support, Ru as catalyst, and Na2CO3 as adsorbent. The catalyst content in the supported bifunctional materials was 1 wt%, and the adsorbent content was 20 wt%.

[0097] The adsorbent metal precursor (Na₂CO₃) and Al₂O₃ were added to deionized water. The resulting adsorbent metal precursor mixture was stirred at room temperature for 12 h, then heated to 80 °C and stirred until the water evaporated naturally. The mixture was then dried in a 120 °C oven for 12 h to obtain a dry solid. After grinding, the solid was placed in a muffle furnace and calcined at 400 °C for 4 h at a heating rate of 5 °C / min to obtain the adsorbent-support material. The concentration of Na₂CO₃ in the adsorbent metal precursor mixture was 47.2 mmol / L, and the concentration of Al₂O₃ was 193.7 mmol / L.

[0098] The catalyst metal precursor (RuCl3·H2O) was added to deionized water to obtain a catalyst precursor solution. The solution was stirred at room temperature for 12 h, then heated to 80 °C and stirred until the water evaporated naturally. The solution was then dried in a 120 °C oven for 12 h to obtain a dry solid. After grinding, the solid was placed in a muffle furnace and calcined at 300 °C for 4 h at a heating rate of 5 °C / min to obtain a supported bifunctional material (denoted as Ru / Na / Al2O3). The concentration of RuCl3·H2O in the catalyst metal precursor salt mixture was 2.9 mmol / L.

[0099] Comparative Example 2

[0100] The supported bifunctional material was prepared according to the method of Example 1, the only difference from Comparative Example 1 being that the adsorbent metal precursor was K2CO3, resulting in the supported bifunctional material (denoted as Ru / K / Al2O3).

[0101] Comparative Example 3

[0102] The supported bifunctional material was prepared according to the method of Example 1, the only difference from Comparative Example 1 being that the adsorbent metal precursor was MgO and the first calcination temperature was 550℃, resulting in the supported bifunctional material (denoted as Ru / Mg / Al2O3).

[0103] Comparative Example 4

[0104] The supported bifunctional material was prepared according to the method of Example 1. The only difference from Comparative Example 1 is that the catalyst content in the supported bifunctional material is 10 wt%, the adsorbent metal precursor is CaO, the catalyst metal precursor is Ni(NO3)2·6H2O, the first calcination temperature is 550℃, and the second calcination temperature is 550℃, thus obtaining the supported bifunctional material (denoted as Ni / Ca / Al2O3).

[0105] Comparative Example 5

[0106] The catalytic performance of the supported bifunctional materials prepared in Comparative Examples 1-4 for direct air carbon dioxide capture and in-situ conversion to methane was tested according to the method in Example 5. The in-situ methanation temperature and the performance parameters of the supported bifunctional materials are shown in Table 2.

[0107] Table 2 Catalytic performance parameters of the supported bifunctional material in its first application

[0108]

[0109] As shown in Table 2, compared with the supported bifunctional materials prepared in Comparative Examples 1-4, the NiCa-based bifunctional materials prepared in this invention are used for direct air carbon dioxide capture and in-situ conversion of methane, and the CO2 adsorption capacity, CO2 conversion rate and CH4 yield are significantly improved, demonstrating excellent catalytic performance.

[0110] Comparative Example 6

[0111] The material composition of the materials used in the DAC-ICCU technology and the reaction conditions and catalytic performance parameters of the DAC-ICCU technology are reported in the literature, as shown in Table 3.

[0112] Literature [1]: VESELOVSKAYA JV, PARUNIN PD, NETSKINA OV, et al. ANovelProcess for Renewable Methane Production: Combining DirectAir Capture by K2CO3 / Alumina Sorbent with CO2Methanation over Ru / Alumina Catalyst[J]. Topics inCatalysis, 2018, 61(15):1528-36.

[0113] Literature [2]: LEE J, OTOMO J. Low-Temperature Activated Direct Air CaptureMethanation Using K-β” Alumina[J]. Industrial&Engineering Chemistry Research, 2023, 62(31):12096-108.

[0114] Literature [3]: JEONG-POTTER C, FARRAUTO R.Feasibility Study ofCombiningDirect Air Capture of CO2and Methanation at Isothermal Conditions with DualFunction Materials[J].Applied Catalysis B:Environmental,2021,282:119416.

[0115] Literature [4]: ​​JEONG-POTTER C, ABDALLAH M, SANDERSON C, et al. Dual functionmaterials (Ru+Na2O / Al2O3) for direct air capture ofCO2and in situ catalyticmethanation: The impact of realistic ambient conditions[J].Applied CatalysisB:Environment and Energy, 2022,307:120990.

[0116] Table 3. Composition of K-based and Na-based adsorbents and reaction conditions and catalytic performance parameters of DAC-ICCU technology.

[0117]

[0118] As shown in Table 3, compared with existing materials, the NiCa-based bifunctional material prepared in this invention exhibits significantly improved CO2 adsorption capacity and CH4 yield when used for direct air carbon dioxide capture and in-situ methane conversion, demonstrating superior performance. Furthermore, this invention does not use precious metals, resulting in low cost for the NiCa-based bifunctional material.

[0119] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. An integrated method for direct air carbon dioxide capture and in-situ conversion to produce methane, comprising the following steps: Moist air is introduced into the NiCa-based bifunctional material for direct air CO2 capture, followed by in-situ methanation in a hydrogen-containing atmosphere to obtain methane. The chemical composition of the NiCa-based bifunctional material includes calcium hydroxide and elemental nickel; the mass content of elemental nickel in the NiCa-based bifunctional material is 5-20%.

2. The integrated method according to claim 1, characterized in that, The NiCa-based bifunctional material further includes a doped metal element, which includes one or more of Mg, Ce and Zr. The molar ratio of calcium to doped metal elements in the NiCa-based bifunctional material is 5~15:

1.

3. The integrated method according to claim 1 or 2, characterized in that, The preparation method of the NiCa-based bifunctional material includes the following steps: A mixture of calcium precursor, nickel precursor, citric acid and water was prepared to obtain a solution. The mixture is then subjected to heat treatment to obtain a sol; The sol was dried and then calcined to obtain NiCa-based calcined material; The NiCa-based calcined material is reduced to obtain the NiCa-based bifunctional material.

4. The integrated method according to claim 3, characterized in that, When the NiCa-based bifunctional material further includes a doped metal oxide, the mixture further includes a doped metal precursor; the doped metal precursor includes one or more of magnesium precursor, cerium precursor and zirconium precursor; In the mixture, the molar ratio of metal ions to water is 1:30~80, and the molar ratio of metal ions to citric acid is 1:0.8~1.

2.

5. The integrated method according to claim 3, characterized in that, The heat treatment temperature is 80~90℃.

6. The integrated method according to claim 3, characterized in that, The calcination temperature is 500~650℃, and the holding time is 3~5h.

7. The integrated method according to claim 3, characterized in that, The reduction treatment is performed at a temperature of 450~550℃ for 0.5~2h. The reducing agent used in the reduction treatment includes a hydrogen-containing atmosphere, wherein the volume fraction of hydrogen in the hydrogen-containing atmosphere is 10~100%.

8. The integrated method according to claim 1, characterized in that, The temperature at which direct air CO2 is captured is room temperature; The volume fraction of hydrogen in the hydrogen-containing atmosphere is 10-100%. The in-situ methanation temperature is 400~600℃.

Citation Information

Patent Citations

  • Difunctional material for CD-ROM integrated CO2 capture and fuel production and preparation method of difunctional material

    CN117046437A

  • Collection and conversion integrated system based on carbon dioxide adsorption and catalysis bifunctional material

    CN117839377A

  • Catalyst for preparing high-purity hydrogen by biomass low-temperature gasification and preparation method thereof