Shell assembly and electronic equipment
By using a combination of laminated fiber layer and polyurethane resin layer in the back cover of the mobile phone, using the design of high-strength fiber yarn and hot melt adhesive layer, the problem that the polyurethane resin material cannot provide sufficient strength and puncture resistance is solved, and the problem of the polyurethane resin material cannot provide sufficient strength and puncture resistance is achieved. Improves strength and puncture resistance while maintaining a light and light design.
Patent Information
- Application Number
- CN202410909873.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-05
AI Technical Summary
The existing polyurethane resin materials cannot provide sufficient strength and puncture resistance to thinned mobile phone back covers, and cannot meet the usage requirements.
The housing assembly of the laminated fiber layer and polyurethane resin layer is made of fiber yarns with tensile modulus greater than 60Gpa to provide support strength, and bond to the base layer through a hot melt adhesive layer to control hot melting. The viscosity and melting point of the glue layer are used to improve bond strength.
The thinned back cover has sufficient strength and puncture resistance to meet the requirements of use while maintaining a thin and light design.
Smart Images

Figure CN118952808A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the technical field of electronic equipment, and in particular to a housing assembly and an electronic device. Background Art
[0002] With the development of mobile phone terminals and plastic back cover industry, creating lightweight, high-strength and thin back covers has become a unified pursuit of the industry. At present, the back cover composition includes polyurethane resin (PU) material, but the polyurethane material itself does not provide supporting strength, and cannot provide sufficient strength and puncture resistance for the thinned back cover, and cannot meet the use requirements. Therefore, how to make the thinned back cover have sufficient strength and puncture resistance has become a problem that needs to be solved urgently. Summary of the invention
[0003] The embodiments of the present application provide a housing assembly and an electronic device. The back cover of the electronic device has sufficient strength and puncture resistance after being thinned to meet the use requirements.
[0004] The first aspect of the present application provides a shell component, which includes a stacked base layer and a cortex layer, wherein the cortex layer includes a stacked fiber layer and a polyurethane resin layer, the fiber layer is located between the base layer and the polyurethane resin layer, and the fiber layer is made of fiber yarn with a tensile modulus greater than 60 GPa.
[0005] In this implementation, the fiber layer is made of fiber yarn with a tensile modulus greater than 60 Gpa, so that the fiber layer has a certain strength, can enhance the strength of the cortical layer, and play a role in supporting the polyurethane resin layer. In addition, while the fiber layer provides support strength, the thickness of the fiber layer is thin, so that the thickness of the cortical layer is thin, so that the thickness of the shell component is thin, thereby achieving a thinning design. Therefore, the shell component is applied to the back cover, and the back cover can provide sufficient strength and puncture resistance while achieving a thinning design, which can meet the use requirements.
[0006] In some possible implementations, the tensile breaking strength of the cortical layer may be greater than 100 N / cm, so that the cortical layer provides a certain supporting strength and puncture resistance, so that the thinned shell assembly has sufficient strength, and the shell assembly can be designed to be thinned.
[0007] In some possible implementations, the fiber layer is made of fiber yarns of the same material, or the fiber layer is made of fiber yarns of different materials. The fiber layer made of one or more fiber yarns can provide a certain support strength, so that the cortex layer can provide support strength, thereby ensuring that the thinned shell component provides sufficient strength and puncture resistance.
[0008] In some possible implementations, the fiber layer is a woven fabric, and the tensile strength of the woven fabric is greater than or equal to 100D and less than or equal to 150D. By limiting the tensile strength of the woven fabric to between 100D and 150D, not only can the fiber layer provide a certain support strength, but also the thickness of the fiber layer can be controlled within a reasonable range to achieve a thinning design of the shell component.
[0009] In some possible implementations, the fiber layer is a unidirectional fabric, and the weight of the unidirectional fabric is greater than or equal to 100D and less than or equal to 250D. By limiting the weight of the unidirectional fabric to between 100D and 250D, not only can the fiber layer provide a certain support strength, but also the thickness of the fiber layer can be controlled within a reasonable range to achieve a thinning design of the shell component.
[0010] In some possible implementations, the fiber yarn includes at least one of the following fibers: glass fiber, high modulus glass fiber, poly(p-phenylene benzobisoxazole) fiber, polyimide fiber, and aramid fiber. These fibers can be used to obtain fiber yarns with a tensile modulus greater than 60 GPa, so that the fiber layer can provide a certain support strength and achieve a thinning design of the shell component.
[0011] In some possible implementations, the shell assembly further includes a hot melt adhesive layer, the hot melt adhesive layer is located between the base layer and the fiber layer, and the base layer and the cortex layer are bonded together through the hot melt adhesive layer. Thus, the cortex layer is bonded to the base layer through the hot melt adhesive layer, and the process is simple.
[0012] In some possible implementations, the viscosity of the hot melt adhesive layer is greater than or equal to 900 cps and less than or equal to 1100 cps. Since the specific surface area of the fiber layer is small, by controlling the viscosity of the hot melt adhesive layer to 900 cps to 1100 cps, the hot melt adhesive has high fluidity, so that when the hot melt adhesive layer is dissolved, it can penetrate more into the fiber layer, making the hot melt adhesive layer and the fiber layer more firmly connected.
[0013] In some possible implementations, the melting point of the hot melt adhesive layer is greater than or equal to 80° C. and less than or equal to 90° C. By controlling the melting point of the hot melt adhesive layer to be between 80° C. and 90° C., the difficulty of dissolving the hot melt adhesive layer can be reduced, and the hot melt adhesive layer can be changed from solid to liquid more quickly, thereby reducing the difficulty of connecting the hot melt adhesive layer to the fiber layer. In addition, it can also prevent the fiber layer from being deformed or damaged by heat due to excessive temperature of the hot melt adhesive layer.
[0014] In some possible implementations, the molecular weight of the hot melt adhesive layer is greater than or equal to 5W and less than or equal to 5.5W. By controlling the molecular weight of the hot melt adhesive layer to 5W to 5.5W, the molecular weight of the hot melt adhesive is lowered, which can improve the viscosity and fluidity of the hot melt adhesive layer, making the hot melt adhesive layer easier to flow and quickly solidify. At the same time, the bonding strength between the hot melt adhesive layer and the fiber layer can also be improved.
[0015] In some possible implementations, the hot melt adhesive layer is a polyurethane hot melt adhesive layer or an epoxy resin hot melt adhesive layer. The polyurethane hot melt adhesive layer or the epoxy resin hot melt adhesive layer can allow the base layer and the cortex layer to be firmly connected.
[0016] In some possible implementations, the material of the base layer includes at least one of the following materials: glass fiber epoxy composite material, aramid fiber composite material, poly(p-phenylene benzobisoxazole) fiber composite material, polyimide fiber composite material, polycarbonate composite material or poly(methyl methacrylate) composite material. The base layer formed by the above materials has the characteristics of high strength and high modulus. The above materials are used for the shell components, which have high strength and are light and thin.
[0017] A second aspect of the present application provides an electronic device, which includes a middle frame, a display screen and a back cover, wherein the back cover and the display screen are respectively connected to two opposite sides of the middle frame, and the back cover includes the shell assembly of any one of the first aspects.
[0018] The third aspect of the present application provides a composite material, which is used as a cortical layer of a shell component, and the composite material includes a fiber layer and a polyurethane resin layer stacked, wherein the fiber layer is used to be arranged between the base layer of the shell component and the polyurethane resin layer, and the fiber layer is made of fiber yarn with a tensile modulus greater than 60Gpa.
[0019] In some possible implementations, the tensile breaking strength of the cortical layer may be greater than 100 N / cm.
[0020] In some possible implementations, the fiber layers are made of fiber yarns made of the same material, or the fiber layers are made of fiber yarns made of multiple different materials.
[0021] In some possible implementations, the fiber layer is a woven fabric, and the weight of the woven fabric is greater than or equal to 100D and less than or equal to 150D.
[0022] In some possible implementations, the fiber layer is a unidirectional fabric, and the tensile strength of the unidirectional fabric is greater than or equal to 100D and less than or equal to 250D.
[0023] In some possible implementations, the fiber yarn includes at least one of the following fibers: glass fiber, high modulus glass fiber, poly(p-phenylene benzobisoxazole) fiber, polyimide fiber, and aramid fiber.
[0024] The fourth aspect of the present application provides a method for preparing a shell assembly, which comprises: forming a base layer and a cortex layer respectively, the cortex layer comprising a stacked fiber layer and a polyurethane resin layer; and laminating the base layer to a side of the fiber layer away from the polyurethane resin layer.
[0025] In some possible implementations, laminating the base layer to the side of the fiber layer facing away from the polyurethane resin layer includes:
[0026] The fiber layer is bonded to the base layer via a hot melt adhesive layer.
[0027] In some possible implementations, forming the cortical layer includes:
[0028] Providing a polyurethane resin laminate and a fiber layer, wherein the polyurethane resin laminate comprises a polyurethane resin layer and a release paper which are stacked;
[0029] The polyurethane resin layer is laminated to one side of the fiber layer to form a cortical layer.
[0030] In some possible implementations, after the polyurethane resin layer and the fiber layer are bonded to form the cortex layer, the method further includes:
[0031] A pattern is formed on a side of the polyurethane resin layer away from the fiber layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a cross-sectional schematic diagram of a back cover in the related art;
[0033] Figure 2 An exploded schematic diagram of an electronic device provided in an embodiment of the present application;
[0034] Figure 3 A cross-sectional schematic diagram of a housing assembly provided in an embodiment of the present application;
[0035] Figure 4 A schematic diagram of a process for preparing a housing assembly provided in an embodiment of the present application;
[0036] Figure 5 A schematic diagram of a process for preparing a cortical layer provided in an embodiment of the present application;
[0037] Figure 6 A schematic diagram of the preparation process of a polyurethane resin laminate provided in an embodiment of the present application.
[0038] Description of reference numerals:
[0039] 100. Electronic equipment;
[0040] 110. display screen; 111. optical aperture area;
[0041] 120, middle frame; 121, middle plate; 122, frame;
[0042] 130. rear cover; 131. through hole;
[0043] 140, battery; 150, circuit board; 160, front camera module; 170, rear camera module;
[0044] 200, housing assembly;
[0045] 10. Basal layer;
[0046] 20. Cortical layer;
[0047] 21, polyurethane resin layer; 211, first polyurethane resin coating; 212, second polyurethane resin coating; 213, third polyurethane resin coating;
[0048] 22. fiber layer; 221. fiber yarn;
[0049] 30. Hot melt adhesive layer;
[0050] 300. Release paper. DETAILED DESCRIPTION
[0051] Figure 1 Schematic diagram of a cross-section of a back cover in the related art. Figure 1 As shown, the back cover 600 of the electronic device includes a cortex layer 620 and a base layer 610, and the cortex layer 620 is located on the side of the base layer 610 away from the battery. The cortex layer 620 includes a polyurethane resin layer 621 and a polyester fabric layer 622, the polyurethane resin layer 621 is made of polyurethane resin (PU) material, and the polyester fabric layer 622 is connected to the base layer 610. The cortex layer 620 gives the electronic device a leather appearance and feel, improving the texture.
[0052] Since the polyurethane resin material does not provide support strength, in order to ensure the safety of the battery, in one embodiment, a cortex layer 620 with a thickness of 0.3mm-0.4mm and a base layer 610 with a thickness greater than 0.5mm are used, so that the back cover 600 provides sufficient strength and puncture resistance to meet the use requirements. However, the thickness of the back cover 600 in this embodiment is greater than 0.7mm, resulting in a relatively thick back cover 600, and a thinning design cannot be achieved.
[0053] It can be seen that in order to reduce the thickness of the back cover 600, the thickness of the cortical layer 620 and / or the base layer 610 can be reduced, so that the thickness of the back cover 600 is reduced, that is, the thickness of the back cover 600 is reduced to less than 0.7 mm. However, after the thickness of the base layer 610 is reduced, the improved strength and puncture resistance of the back cover 600 are also reduced, and cannot meet the use requirements. Therefore, how to make the thinned back cover 600 provide sufficient strength and puncture resistance has become a problem that needs to be solved urgently.
[0054] In view of this, the embodiment of the present application provides a shell component and an electronic device, wherein the shell component is made of a composite material, so that the shell component has a leather appearance and effect, and improves the texture of the electronic device having the shell component. The composite material is composed of a fiber layer and a polyurethane resin layer, and the fiber layer can provide a certain support strength and play a role in supporting the polyurethane resin layer. Therefore, after the shell component is thinned, the composite material can provide a certain support strength, so that the shell component provides sufficient strength and puncture resistance to meet the use requirements.
[0055] The embodiment of the present application provides an electronic device, which may be a tablet computer, a mobile phone, an e-reader, a remote control, a personal computer (PC), a laptop, a personal digital assistant (PDA), a vehicle-mounted device, an Internet TV, a wearable device, a TV, and other products with a display interface, as well as smart display wearable products such as smart watches and smart bracelets. The embodiment of the present application does not impose any special restrictions on the form of the above electronic devices.
[0056] For the convenience of explanation, the following embodiments are all described by taking a mobile phone as an example of the electronic device. The mobile phone can be a foldable mobile phone, or a candy bar mobile phone, or a slider mobile phone. The following specific description is given by taking a candy bar mobile phone as an example.
[0057] Figure 2 An exploded schematic diagram of an electronic device provided in an embodiment of the present application.
[0058] See also Figure 2 As shown, the electronic device 100 includes a middle frame 120, a display screen 110 and a back cover 130 (or a back shell), the middle frame 120 is located between the display screen 110 and the back cover 130, and the back cover 130 and the display screen 110 are respectively connected to opposite sides of the middle frame 120.
[0059] The display screen 110 is used to display images, and the display screen 110 may also be integrated with a touch function.
[0060] Continue to see Figure 2As shown, the middle frame 120 may include a middle plate 121 and a frame 122 surrounding the outer edge of the middle plate 121. The inner wall of the frame 122 may be connected to the outer edge of the middle plate 121 to form an integral structure. The material of the middle plate 121 may be aluminum or aluminum alloy, or the material of the middle plate 121 may be stainless steel.
[0061] Continue to see Figure 2 As shown, the electronic device 100 may further include a battery 140 and a circuit board 150, which may be disposed on the middle plate 121, and the battery 140 and the circuit board 150 may be disposed on a side of the middle plate 121 facing the back cover 130. Alternatively, in some embodiments, the battery 140 and the circuit board 150 may also be disposed on a side of the middle plate 121 facing the display screen 110. Alternatively, in some embodiments, the battery 140 is located on a side of the middle plate 121 facing the back cover 130, and the circuit board 150 is located on a side of the middle plate 121 facing the display screen 110.
[0062] Continuing to refer to FIG. 2 , the electronic device 100 may further include a front camera module 160 and a rear camera module 170. The display screen 110 is provided with an optical hole area 111 that cooperates with the front camera module 160, and the front camera module 160 realizes functions such as shooting or taking pictures through the optical hole area 111. The rear cover 130 is provided with a through hole 131, and a part of the rear camera module 170 is located between the middle frame 120 and the rear cover 130, and the other part is located outside the electronic device 100 through the through hole 131.
[0063] The back cover 130 is connected to the middle frame 120 to form a receiving cavity for accommodating electronic components such as the circuit board 150, the battery 140, the front camera module 160 and the rear camera module 170, thereby preventing external moisture and dust from invading the receiving cavity and avoiding affecting the performance of the above-mentioned electronic components.
[0064] Continue to see Figure 2 As shown, the back cover 130 includes a housing assembly 200 . The orthographic projection of the battery 140 in the thickness direction Z of the electronic device 100 is located inside the orthographic projection of the housing assembly 200 in the thickness direction Z of the electronic device 100 , that is, the housing assembly 200 covers the battery 140 .
[0065] The material of the housing assembly 200 includes a polyurethane leather material having a polyurethane resin material, so that the housing assembly 200 has a leather appearance and feel, thereby improving the texture of the back cover 130. In addition, the polyurethane leather material supports the polyurethane resin material through a fiber material with a certain supporting strength, so that the polyurethane leather material can provide a certain supporting strength, so that the housing assembly 200 can improve sufficient strength and puncture resistance after thinning, and then the back cover 130 can improve sufficient strength and puncture resistance after thinning, ensuring the safety of the battery 140.
[0066] It should be noted that, in addition to the shell assembly 200 , the back cover 130 may also include other parts. For example, in some embodiments, the back cover 130 may also include an edge assembly (not shown in the figure) surrounding the shell assembly 200 .
[0067] In the embodiment of the present application, there is no limitation on the thickness of the housing assembly 200. For example, the thickness of the housing assembly 200 may be less than or equal to 0.65 mm. For example, the thickness of the housing assembly 200 may be 0.65 mm, 0.6 mm, 0.55 mm, 0.5 mm, etc.
[0068] Figure 3 A schematic cross-sectional view of a housing assembly provided in an embodiment of the present application.
[0069] See also Figure 3 As shown, the shell component 200 includes a stacked base layer 10 and a cortex layer 20. Among them, the cortex layer 20 includes a stacked fiber layer 22 and a polyurethane resin layer 21. The polyurethane resin layer 21 is made of polyurethane resin material, and the polyurethane resin layer 21 is used to make the shell component 200 have a leather appearance and feel, so that the shell component 200 is applied to the back cover 130, and the back cover 130 has a leather texture. The fiber layer 22 is located between the base layer 10 and the polyurethane resin layer 21. The fiber layer 22 is made of fiber yarn 221 with a tensile modulus greater than 60Gpa, so that the fiber layer 22 can provide a certain support strength while supporting the polyurethane resin layer 21, thereby playing a reinforcing role, and then the cortex layer 20 can also provide a certain strength and puncture resistance.
[0070] It can be understood that the cortical layer 20 is made of a composite material that can provide support strength and puncture resistance, and the composite material is composed of a fiber layer 22 and a polyurethane resin layer 21 that are stacked.
[0071] When the shell assembly 200 is designed to be thinned, the thickness of the base layer 10 is reduced, and the support strength and puncture resistance that the base layer 10 can provide are also reduced. However, the fiber layer 22 can provide a certain support strength, so that the cortical layer 20 can provide a certain support strength to make up for the part of the shell assembly 200 whose strength is reduced due to the reduction in the thickness of the base layer 10, so that the shell assembly 200 can provide sufficient strength and puncture resistance after being thinned, and can meet the use requirements. In addition, while the fiber layer 22 provides a certain support strength, the thickness of the fiber layer 22 can still be thinned, so that the cortical layer 20 can provide a certain strength and puncture resistance while being thinned. Therefore, the shell assembly 200 is applied to the back cover 130, and the back cover 130 can provide sufficient strength and puncture resistance while realizing the thinning design, and can meet the use requirements.
[0072] In order to make the back cover 130 have a richer appearance, in some embodiments, a pattern is generally formed on the surface of the polyurethane resin layer 21 away from the fiber layer 22. In some embodiments, it can be achieved by mechanical lamination through a release paper 300 with a texture effect. Of course, it can also be achieved by other methods, such as by roller coating or printing.
[0073] In some possible implementations, the tensile breaking strength of the cortical layer 20 can be greater than 100 N / cm, so that the cortical layer 20 provides a certain supporting strength and puncture resistance, so that the thinned shell assembly 200 has sufficient strength, and the shell assembly 200 can be designed to be thinned.
[0074] It can be understood that when the tensile breaking strength of the cortical layer 20 can be greater than 100 N / cm, the cortical layer 20 can not only provide a certain supporting strength and puncture resistance, but also control the thickness of the cortical layer 20 within a reasonable range to achieve a thinning design of the shell assembly 200.
[0075] There is no limitation on the specific value of the tensile strength at break of the cortical layer 20. For example, the tensile strength at break of the cortical layer 20 may be 101 N / cm, 105 N / cm, 110 N / cm, 115 N / cm, 115.95 N / cm or 120 N / cm.
[0076] In the embodiment of the present application, there is no limitation on the specific thickness of the cortical layer 20. For example, the thickness of the cortical layer 20 may be 0.2 mm.
[0077] In the embodiment of the present application, there is no limitation on the specific thickness of the polyurethane resin layer 21. For example, the thickness of the polyurethane resin layer 21 may be 0.1 mm.
[0078] In the embodiment of the present application, there is no limitation on the specific thickness of the fiber layer 22. For example, the thickness of the fiber layer 22 may be 0.1 mm.
[0079] In the embodiment of the present application, the fiber yarn 221 refers to a yarn made of fiber, and the tensile modulus of the yarn is greater than 60 GPa.
[0080] The fiber yarn 221 can be made of one or more fibers selected from glass fiber, high modulus glass fiber, poly(p-phenylene benzobisoxazole) fiber (PBO fiber), polyimide fiber (PI fiber), and aramid fiber. The fiber yarn 221 having a tensile modulus greater than 60 GPa can be obtained through these fibers, so that the fiber layer 22 can provide a certain supporting strength, thereby realizing a thinning design of the housing assembly 200.
[0081] There is no limitation on the specific value of the tensile modulus of the fiber yarn 221. The tensile modulus of the fiber yarn 221 may be 61 GPa, 69 GPa, 70 GPa, 74.6 GPa, 90 GPa, etc.
[0082] In the embodiment of the present application, the fiber layer 22 is made of a plurality of fiber yarns 221. The fiber layer 22 can be made of a fiber yarn 221 of the same material, or the fiber layer 22 can be made of a plurality of fiber yarns 221 of different materials. The fiber layer 22 made of one or more fiber yarns 221 can provide a certain support strength, so that the cortex layer 20 can provide support strength and puncture resistance, thereby ensuring that the thinned shell assembly 200 provides sufficient strength and puncture resistance.
[0083] There is no limitation on the type of the fiber layer 22 made of the plurality of fiber yarns 221. Several types of the fiber layer 22 are described below.
[0084] In some possible implementations, the fiber layer 22 may be a woven fabric (or a woven fabric), which is a mesh structure composed of warp and weft threads interwoven (e.g. Figure 3 As shown in the figure, the warp and weft are interlaced and woven perpendicularly to each other. That is, a part of the multiple fiber yarns 221 is used as warp and another part is used as weft. Alternatively, it can also be understood that multiple fiber yarns 221 are arranged crosswise. The woven cloth can be formed by knitting or weaving.
[0085] It should be noted that Figure 3 The structure of the woven cloth shown is a schematic diagram, and the specific structure of the woven cloth can also be other structures, which will not be described here one by one.
[0086] In some embodiments, the weight of the woven cloth may be greater than or equal to 100 D and less than or equal to 150 D. By limiting the weight of the woven cloth to between 100 D and 150 D, not only can the fiber layer 22 provide a certain support strength, but also the thickness of the fiber layer 22 can be controlled within a reasonable range to achieve a thinning design of the housing assembly 200.
[0087] There is no limitation on the specific tensile strength of the woven fabric. For example, the tensile strength of the woven fabric can be 100D, 105D, 110D, 120D, 130D, 140D or 150D, etc.
[0088] In some other possible implementations, the fiber layer 22 may also be a unidirectional cloth (or unidirectional fabric). Unidirectional cloth (UD cloth for short) is composed of a series of parallel core lines, the planes between the core lines are parallel to each other, one of which is a base line, and the other core lines are perpendicular to it.
[0089] In some embodiments, the load factor of the unidirectional fabric may be greater than or equal to 100 D and less than or equal to 250 D. By limiting the load factor of the unidirectional fabric to between 100 D and 250 D, not only can the fiber layer 22 provide a certain support strength, but also the thickness of the fiber layer 22 can be controlled within a reasonable range to achieve a thinning design of the housing assembly 200.
[0090] There is no limitation on the specific load factor of the unidirectional fabric. For example, the load factor of the unidirectional fabric can be 100D, 105D, 110D, 120D, 130D, 140D, 150D, 155D, 160D, 170D, 180D, 190D, 200D, 210D, 230D or 250D, etc.
[0091] In order to attach the cortical layer 20 to the base layer 10, see Figure 3 As shown, the shell assembly 200 may further include a hot melt adhesive layer 30, which is located between the base layer 10 and the fiber layer 22, and the hot melt adhesive layer 30 is connected to the fiber layer 22 and the base layer 10, respectively, so that the base layer 10 and the cortical layer 20 are bonded through the hot melt adhesive layer 30. Thus, the cortical layer 20 is bonded to the base layer 10 through the hot melt adhesive layer 30, and the process is simple.
[0092] There is no limitation on the specific type of the hot melt adhesive layer 30. The hot melt adhesive layer 30 may be a polyurethane hot melt adhesive layer or an epoxy resin hot melt adhesive layer, etc., which can firmly connect the base layer 10 and the cortex layer 20.
[0093] There is no limitation on the thickness of the hot melt adhesive layer 30. For example, the hot melt adhesive layer 30 may be 80 μm. Of course, the thickness of the hot melt adhesive layer 30 may also be other values.
[0094] In order to make the connection between the base layer 10 and the fiber layer 22 more firmly, the performance of the hot melt adhesive layer 30 can be improved by controlling one or more parameters of the hot melt adhesive layer 30 such as viscosity, melting point, molecular weight, etc.
[0095] In some possible implementations, the viscosity of the hot melt adhesive layer 30 may be greater than or equal to 900 cps and less than or equal to 1100 cps. Since the specific surface area of the fiber layer 22 is small, by controlling the viscosity of the hot melt adhesive layer 30 to be between 900 cps and 1100 cps, the hot melt adhesive has high fluidity, so that when the hot melt adhesive layer 30 is dissolved, it can penetrate more into the fiber layer 22, so that the hot melt adhesive layer 30 and the fiber layer 22 are more firmly connected.
[0096] There is no limitation on the specific value of the viscosity of the hot melt adhesive layer 30. The viscosity of the hot melt adhesive layer 30 may be 900 cps, 950 cps, 980 cps, 1000 cps, 1050 cps, 1100 cps, etc.
[0097] In some possible implementations, the melting point of the hot melt adhesive layer 30 may be greater than or equal to 80° C. and less than or equal to 90° C. By controlling the melting point of the hot melt adhesive layer 30 to be between 80° C. and 90° C., the difficulty of the hot melt adhesive layer 30 being dissolved can be reduced, and the hot melt adhesive layer 30 can be changed from a solid state to a liquid state more quickly, thereby reducing the difficulty of connecting the hot melt adhesive layer 30 to the fiber layer 22. In addition, it can also prevent the fiber layer 22 from being deformed or damaged by heat due to excessive temperature of the hot melt adhesive layer 30.
[0098] There is no limitation on the specific value of the melting point of the hot melt adhesive layer 30. The melting point of the hot melt adhesive layer 30 may be 80°C, 81°C, 81.5°C, 83°C, 86°C, 89.65°C, etc.
[0099] In some possible implementations, the molecular weight of the hot melt adhesive layer 30 may be greater than or equal to 5W and less than or equal to 5.5W. By controlling the molecular weight of the hot melt adhesive layer 30 to be between 5W and 5.5W, the molecular weight of the hot melt adhesive is lowered, and the viscosity and fluidity of the hot melt adhesive layer 30 can be improved, so that the hot melt adhesive layer 30 is easier to flow and solidifies quickly. In addition, the bonding strength between the hot melt adhesive layer 30 and the fiber layer 22 can also be improved.
[0100] There is no limitation on the specific value of the molecular weight of the hot melt adhesive layer 30. The molecular weight of the hot melt adhesive layer 30 may be 5W, 5.1W, 5.13W, 5.2W, 5.3W, 5.35W, 5.45W, 5.49W, etc.
[0101] In the embodiment of the present application, there is no limitation on the specific material of the base layer 10. The material of the base layer 10 may include one or more materials such as glass fiber epoxy composite material, aramid fiber composite material, poly(p-phenylene benzobisoxazole) fiber composite material, polyimide fiber composite material, polycarbonate (PC) composite material or polymethyl methacrylate (PMMA) composite material. The base layer 10 formed by the above materials has the characteristics of high strength and high modulus. The above materials are used for the housing assembly 200, which has high strength and thin material.
[0102] In the embodiment of the present application, there is no limitation on the specific thickness of the base layer 10. For example, the thickness of the base layer 10 may be 0.4 mm. Of course, the thickness of the base layer 10 may also be other values.
[0103] In summary, since the fiber layer 22 can be made of fiber yarn 221 made of one or more of glass fiber, high modulus glass fiber, polyphenylene benzobisoxazole fiber, polyimide fiber and aramid fiber, and the base layer 10 can be made of one or more of glass fiber epoxy composite material, aramid fiber composite material, polyphenylene benzobisoxazole fiber composite material, polyimide fiber composite material, polycarbonate composite material or polymethyl methacrylate composite material, the fiber layer 22 made of different fiber materials can be freely combined with the base layer 10 made of different materials. In addition, the fiber layer 22 can be a woven cloth or a unidirectional cloth, and can also be freely combined with the base layer 10 made of different materials (for example, the first to fourth embodiments below). Similarly, different types of hot melt adhesive layers 30 can also be freely combined with fiber layers 22 of different materials and base layers 10 of different materials.
[0104] Figure 4 A schematic flow chart of a method for preparing a shell assembly provided in an embodiment of the present application.
[0105] See also Figure 4 As shown, the embodiment of the present application also provides a method for preparing a housing assembly 200, the method comprising the following steps:
[0106] S10 , forming a base layer 10 and a cortex layer 20 , respectively. The cortex layer 20 includes a fiber layer 22 and a polyurethane resin layer 21 which are stacked.
[0107] The material of the base layer 10 may include one or more of the following materials: glass fiber epoxy composite material, aramid fiber composite material, poly(p-phenylene benzobisoxazole) fiber composite material, polyimide fiber composite material, polycarbonate composite material or polymethyl methacrylate composite material. These materials are used to make the base layer 10 of corresponding thickness.
[0108] The fiber layer 22 is made of a plurality of fiber yarns 221, and the tensile modulus of each fiber yarn 221 is greater than 60 GPa. The fiber layer 22 can be a woven fabric or a unidirectional fabric. The fiber yarn 221 can be made of one or more fibers such as glass fiber, high modulus glass fiber, poly(p-phenylene benzobisoxazole) fiber, polyimide fiber, and aramid fiber.
[0109] Figure 5 A schematic diagram of a method for preparing a cortical layer provided in an embodiment of the present application, Figure 6 A schematic diagram of the preparation process of a polyurethane resin laminate provided in an embodiment of the present application.
[0110] In some embodiments, see Figure 5 As shown, the cortical layer 20 can be formed by the following steps:
[0111] S101 , providing a polyurethane resin laminate and a fiber layer 22 , wherein the polyurethane resin laminate comprises a polyurethane resin layer 21 and a release paper 300 which are stacked.
[0112] Specifically, see Figure 6 As shown, a first polyurethane resin coating 211 of a first thickness is scraped on one side of the release paper 300 and dried. Then, a second polyurethane resin coating 212 of a second thickness is scraped on the surface of the first polyurethane resin coating 211 away from the release paper 300 and dried. Then, a third polyurethane resin coating 213 of a third thickness is scraped on the surface of the second polyurethane resin coating 212 away from the first polyurethane resin coating 211 and dried to form a polyurethane resin laminate.
[0113] The first thickness, the second thickness and the third thickness may be different, or at least two of the first thickness, the second thickness and the third thickness may be the same.
[0114] S102 , laminating the polyurethane resin layer 21 on one side of the fiber layer 22 to form the cortical layer 20 .
[0115] Specifically, the fiber layer 22 is bonded to the polyurethane resin layer 21 in the polyurethane resin laminate, and the release paper 300 is removed to form the cortex layer 20 .
[0116] S103 , after the polyurethane resin layer 21 and the fiber layer 22 are attached to form the cortical layer 20 , the process may further include: forming a pattern on a side of the polyurethane resin layer 21 away from the fiber layer 22 .
[0117] Specifically, the surface of the polyurethane resin layer 21 away from the fiber layer 22 can be surface treated by rolling or printing, so that a pattern is formed on the side of the polyurethane resin layer 21 away from the fiber layer 22, so that the surface of the polyurethane resin layer 21 can form a structure similar to the surface of leather.
[0118] It should be noted that in addition to forming patterns by processes such as rolling or printing, in some embodiments, a texture structure can also be provided on the side of the release paper 300 that contacts the first polyurethane resin coating 211 , and the texture structure is used to form a pattern on the surface of the polyurethane resin layer 21 .
[0119] S20 , attaching the base layer 10 to the side of the fiber layer 22 facing away from the polyurethane resin layer 21 .
[0120] The fiber layer 22 can be attached to the base layer 10 via the hot melt adhesive layer 30. Specifically, the hot melt adhesive layer 30 can be placed between the fiber layer 22 and the base layer 10, and then the hot melt adhesive layer 30 is firmly connected to the fiber layer 22 and the base layer 10 by hot pressing.
[0121] The housing assembly provided in the embodiment of the present application is described below in conjunction with specific embodiments.
[0122] Embodiment 1:
[0123] The shell assembly 200 provided in this embodiment may include a stacked base layer 10, a hot melt adhesive layer 30 and a cortex layer 20. The hot melt adhesive layer 30 is a polyurethane hot melt adhesive layer 30. The base layer 10 is made of a glass fiber composite material, and the thickness of the base layer 10 may be 0.4 mm. The cortex layer 20 includes a polyurethane resin layer 21 and a fiber layer 22, the thickness of the polyurethane resin layer 21 may be 0.1 mm, and the fiber layer 22 may be made of a fiber yarn 221 made of E-grade glass fiber, and the thickness of the fiber layer 22 may be 0.1 mm.
[0124] When the housing assembly 200 is applied to the back cover 130, the thickness of the back cover 130 is 0.65 mm. According to the puncture test standard GB / T10004-2008, the puncture force of the back cover 130 is 110N, and the puncture strength of the back cover 130 is 169N / mm. It can be seen that after the back cover 130 is thinned, sufficient strength and puncture resistance can be improved to ensure the safety of the battery 140.
[0125] Embodiment 2:
[0126] The shell assembly 200 provided in this embodiment may include a stacked base layer 10, a hot melt adhesive layer 30 and a cortex layer 20. The hot melt adhesive layer 30 is a polyurethane hot melt adhesive layer 30. The base layer 10 is made of a glass fiber composite material, and the thickness of the base layer 10 may be 0.3 mm. The cortex layer 20 includes a polyurethane resin layer 21 and a fiber layer 22, the thickness of the polyurethane resin layer 21 may be 0.1 mm, and the fiber layer 22 may be made of a fiber yarn 221 made of S-grade glass fiber, and the thickness of the fiber layer 22 may be 0.1 mm.
[0127] When the housing assembly 200 is applied to the back cover 130, the thickness of the back cover 130 can be 0.65 mm. According to the puncture test standard GB / T10004-2008, the puncture force of the back cover 130 is 130 N, and the puncture strength of the back cover 130 is 200 N / mm. It can be seen that after the back cover 130 is thinned, sufficient strength and puncture resistance can be improved to ensure the safety of the battery 140.
[0128] Embodiment three:
[0129] The shell assembly 200 provided in this embodiment may include a stacked base layer 10, a hot melt adhesive layer 30 and a cortical layer 20. The hot melt adhesive layer 30 is a polyurethane hot melt adhesive layer 30. The base layer 10 is made of a glass fiber composite material, and the thickness of the base layer 10 may be 0.25 mm. The cortical layer 20 includes a polyurethane resin layer 21 and a fiber layer 22, the thickness of the polyurethane resin layer 21 may be 0.1 mm, and the fiber layer 22 may be made of a fiber yarn 221 made of poly(p-phenylene benzobisoxazole) fiber (PBO fiber), and the thickness of the fiber layer 22 may be 0.1 mm.
[0130] When the housing assembly 200 is applied to the back cover 130, the thickness of the back cover 130 can be 0.55 mm. According to the puncture test standard GB / T10004-2008, the puncture force of the back cover 130 is 150 N, and the puncture strength of the back cover 130 is 272.73 N / mm. It can be seen that after the back cover 130 is thinned, sufficient strength and puncture resistance can be improved to ensure the safety of the battery 140.
[0131] Embodiment 4:
[0132] The shell assembly 200 provided in this embodiment may include a stacked base layer 10, a hot melt adhesive layer 30 and a cortical layer 20. The hot melt adhesive layer 30 is a polyurethane hot melt adhesive layer 30. The base layer 10 is made of a poly(p-phenylene benzobisoxazole) composite material, and the thickness of the base layer 10 may be 0.25 mm. The cortical layer 20 includes a polyurethane resin layer 21 and a fiber layer 22, the thickness of the polyurethane resin layer 21 may be 0.1 mm, and the fiber layer 22 may be made of a fiber yarn 221 made of polyimide fiber (PI fiber), and the thickness of the fiber layer 22 may be 0.1 mm.
[0133] When the housing assembly 200 is applied to the back cover 130, the thickness of the back cover 130 can be 0.55 mm. According to the puncture test standard GB / T10004-2008, the puncture force of the back cover 130 is 170 N, and the puncture strength of the back cover 130 is 309 N / mm. It can be seen that after the back cover 130 is thinned, sufficient strength and puncture resistance can be improved to ensure the safety of the battery 140.
[0134] It should be noted that the combination of the fiber layer 22 made of different materials and the base layer 10 made of different materials is not limited to the above four embodiments, and may also be other combinations, which will not be described one by one here.
[0135] In the related art, the back cover 600 includes a cortex layer 620 and a base layer 610, and the cortex layer 620 includes a polyurethane resin layer 621 and a polyester fabric layer 622. The polyurethane resin layer 621 is made of polyurethane resin (PU). The polyester fabric layer 622 is connected to the base layer 610, and the base layer 610 is made of a glass fiber composite material. The thickness of the back cover 600 is 0.7 mm. According to the GB / T10004-2008 puncture test standard, the puncture force of the back cover 600 is 100 N, and the puncture strength of the back cover 600 is 142 N / mm.
[0136] In summary, the puncture strength of the back cover 130 provided in the first to fourth embodiments is greater than the puncture strength of the back cover 600 in the related art, and the thickness is less than the thickness of the back cover 600 in the related art. In addition, by changing the material constituting the fiber yarn 221, the thickness of the back cover 130 can be further reduced, and the puncture strength can be further improved. Therefore, the housing assembly 200 provided in the embodiment of the present application is applied to the back cover 130, and the back cover 130 can provide sufficient strength and puncture resistance after being thinned.
[0137] In the description of the embodiments of the present application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, or it can be an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present application can be understood according to specific circumstances.
[0138] In the embodiments of the present application, the devices or elements referred to or implied must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the embodiments of the present application. In the description of the embodiments of the present application, the meaning of "multiple" is two or more, unless otherwise precisely and specifically specified.
[0139] The terms "first", "second", "third", "fourth", etc. (if any) in the specification and claims of the embodiments of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0140] The term "plurality" in this article refers to two or more than two. The term "and / or" in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the previous and next associated objects are in an "or" relationship; in a formula, the character " / " indicates that the previous and next associated objects are in a "division" relationship.
[0141] It should be understood that the various numerical numbers involved in the embodiments of the present application are only used for the convenience of description and are not used to limit the scope of the embodiments of the present application.
[0142] It can be understood that in the embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
Claims
1. A housing assembly, characterized in that: It includes basal layer and cortical layer arranged in layers; The cortical layer comprises a fiber layer and a polyurethane resin layer which are stacked, wherein the fiber layer is located between the base layer and the polyurethane resin layer, and the fiber layer is made of fiber yarns with a tensile modulus greater than 60 GPa.
2. The housing assembly according to claim 1, characterized in that: The tensile breaking strength of the cortical layer is greater than 100 N / cm.
3. The housing assembly according to claim 1 or 2, characterized in that: The fiber layer is made of the fiber yarns made of the same material, or the fiber layer is made of a plurality of fiber yarns made of different materials.
4. The housing assembly according to any one of claims 1 to 3, characterized in that: The fiber layer is a woven cloth, and the weight of the woven cloth is greater than or equal to 100D and less than or equal to 150D.
5. The housing assembly according to any one of claims 1 to 3, characterized in that: The fiber layer is a unidirectional fabric, and the weight of the unidirectional fabric is greater than or equal to 100D and less than or equal to 250D.
6. The housing assembly according to any one of claims 1 to 5, characterized in that: The fiber yarn comprises at least one of the following fibers: glass fiber, high modulus glass fiber, poly(p-phenylene benzobisoxazole) fiber, polyimide fiber, and aramid fiber.
7. The housing assembly according to any one of claims 1 to 6, characterized in that: The shell component also includes a hot melt adhesive layer, which is located between the base layer and the fiber layer. The base layer and the cortex layer are bonded together through the hot melt adhesive layer.
8. The housing assembly according to claim 7, characterized in that: The viscosity of the hot melt adhesive layer is greater than or equal to 900 cps and less than or equal to 1100 cps.
9. The housing assembly according to claim 7 or 8, characterized in that: The melting point of the hot melt adhesive layer is greater than or equal to 80° C. and less than or equal to 90° C.
10. The housing assembly according to any one of claims 7 to 9, characterized in that: The molecular weight of the hot melt adhesive layer is greater than or equal to 5W and less than or equal to 5.5W.
11. The housing assembly according to any one of claims 7 to 10, characterized in that: The hot melt adhesive layer is a polyurethane hot melt adhesive layer or an epoxy resin hot melt adhesive layer.
12. The housing assembly according to any one of claims 1 to 11, characterized in that: The material of the base layer includes at least one of the following materials: glass fiber epoxy composite material, aramid fiber composite material, poly(p-phenylene benzobisoxazole) fiber composite material, polyimide fiber composite material, polycarbonate composite material or polymethyl methacrylate composite material.
13. An electronic device, characterized in that: It comprises a middle frame, a display screen and a back cover, wherein the back cover and the display screen are respectively connected to two opposite sides of the middle frame, and the back cover comprises the shell assembly according to any one of claims 1 to 12.
Citation Information
Patent Citations
Shell assembly, preparation method thereof and electronic equipment
CN114536904A
Shell assembly and electronic equipment
CN114727521A
Protective shell and electronic equipment
CN117119717A
Shell assembly, preparation method of shell assembly and electronic equipment
CN117677099A
Composite material as well as shell and electronic equipment applying same