Modified two-dimensional vermiculite film as well as preparation method and application thereof

By subjecting two-dimensional vermiculite films to rapid heavy ion irradiation, the ion transport channels are increased, solving the problem of high ion transport resistance in salinity gradient power generation and achieving a significant increase in output power.

CN118954526AActive Publication Date: 2024-11-15SHANDONG UNIV

Patent Information

Application Number
CN202411154234.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-15
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

In salinity gradient power generation, two-dimensional vermiculite thin films suffer from high ion transport resistance and low ion flux due to their tortuous transport channels, resulting in insufficient output power.

Method used

Two-dimensional vermiculite films are treated with rapid heavy ion irradiation to increase ion transport channels and change the ion transport path to a non-torsional transport path.

Benefits of technology

The output power of salinity gradient power generation was increased from 0.2–0.7 W/m² to 0.5–3.0 W/m², significantly improving ion flux and output power.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954526A_ABST
    Figure CN118954526A_ABST
Patent Text Reader

Abstract

The invention discloses a modified two-dimensional vermiculite film as well as a preparation method and application thereof, and belongs to the technical field of salinity gradient energy power generation. The method comprises the following steps: S1, treating vermiculite with a saturated sodium chloride solution, a Li C < l > solution and a H2O2 solution in sequence, then mixing the treated vermiculite with water, ultrasonically stripping nanosheets, centrifugally removing impurities, and centrifugally collecting a suspension liquid, namely a vermiculite nanosheet dispersion liquid; s2, carrying out suction filtration on the vermiculite nanosheet dispersion liquid on the surface of the porous substrate, and drying to obtain a self-supported two-dimensional vermiculite film; and S3, carrying out fast heavy ion irradiation treatment on the self-supported two-dimensional vermiculite film to obtain the modified two-dimensional vermiculite film. The ion irradiation modification technology is utilized, and a through ion transmission channel is added in the two-dimensional vermiculite film, so that the ion transmission resistance is reduced, and the ion flux is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of salt difference energy power generation, and specifically relates to a modified two-dimensional vermiculite membrane and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Two-dimensional inorganic layered materials have unique structural characteristics such as weak interactions between layers, strong covalent bonds within the layers, and molecular-level nano-layer thickness. This makes this type of material theoretically and practically feasible in terms of swelling, exfoliation, nanosheet functionalization, and the design and assembly of new nano-layered functional materials, and becomes an important precursor or basic unit for the design, assembly and preparation of two-dimensional nanomaterials. Among them, vermiculite has become an important object for studying nanosheet exfoliation due to its unique layered structure and expansibility. The development of liquid phase exfoliation technology has made the exfoliation of nanosheets more efficient. Vermiculite can be exfoliated into single-layer or few-layer nanosheets by ultrasonic treatment in a specific solvent. Materials assembled from vermiculite nanosheets have shown broad application prospects in the fields of energy conversion, adsorption separation, catalysis, and biosensing.

[0004] Salt difference energy refers to the chemical potential difference between seawater and freshwater or between two seawaters with different salt concentrations. It is ocean energy in the form of chemical energy. When vermiculite is used for salt difference energy power generation (referred to as salt difference power generation), the tortuous transmission channels inside the vermiculite greatly increase the ion transmission resistance, resulting in very low ion flux, which leads to extremely low output power of salt difference energy power generation.

[0005] Ion beam technology has been widely used in the modification of semiconductors, metals, insulators and other materials. Ion beam technology uses ions with a certain energy (eV to GeV) to interact with atoms and extranuclear electrons in the material, which can not only make the ions stay inside the material as foreign atoms, but also cause certain damage and defects inside the material. Summary of the invention

[0006] In order to overcome the deficiencies of the prior art, the purpose of the present invention is to provide a modified two-dimensional vermiculite membrane and a preparation method and application thereof, by treating the two-dimensional vermiculite film with rapid heavy ion irradiation to increase the ion transmission channel, thereby being able to increase the output power of salt difference power generation by several times.

[0007] In order to achieve the above object, the technical solution of the present invention is:

[0008] In a first aspect, the present invention provides a method for preparing a modified two-dimensional vermiculite film, comprising the following steps:

[0009] S1, treating vermiculite with a saturated sodium chloride solution, a 2-3M LiCl solution and a H2O2 solution in sequence, then mixing the treated vermiculite with water, exfoliating the nanosheets by ultrasonic treatment for 2-3 hours, centrifuging to remove impurities, centrifuging at a speed of 4000-4500 r / min for 2-50 minutes, and collecting the suspension to obtain a vermiculite nanosheet dispersion;

[0010] S2, filtering the vermiculite nanosheet dispersion obtained in S1 onto the surface of a porous substrate, and drying at 60 to 80° C. to obtain a self-supporting two-dimensional vermiculite film with a thickness of 4 to 100 μm;

[0011] S3, subjecting the self-supporting two-dimensional vermiculite film obtained in S2 to rapid heavy ion irradiation to obtain a modified two-dimensional vermiculite film;

[0012] In fast heavy ion irradiation, the heavy ions are Xe 31+ ; Irradiation ion energy is 0.1-4MeV / u; irradiation dose is 10 8 -10 12 i ons / cm 2 .

[0013] Optionally, in S1, 1 to 30 grams of vermiculite is soaked in 10 to 300 milliliters of saturated NaCl solution, refluxed at 110 to 120° C. for 20 to 28 hours, and then the vermiculite is washed with deionized water and ethanol until no chloride ions are detected to obtain a first powder; the first powder is mixed with 10 to 300 milliliters of LiCl solution, heated and refluxed at 110 to 120° C. for 20 to 28 hours, and then the vermiculite is washed with deionized water and ethanol until no chloride ions are detected to obtain a second powder; the second powder is mixed with 100-150 milliliters of H2O2 solution, and refluxed at 110 to 120° C. for 20 to 28 hours to obtain treated vermiculite.

[0014] Optionally, in S1, the centrifugal impurity removal method includes: removing unpeeled small vermiculite particles by centrifugation at a rotation speed of 4000-4500 r / min.

[0015] Optionally, in S1, the size of the vermiculite nanosheets dispersed in the vermiculite nanosheet dispersion liquid includes: 0.1-1 μm; and the concentration of the vermiculite nanosheets in the vermiculite nanosheet dispersion liquid is 1-10 mg / mL.

[0016] Optionally, in S2, the specifications of the porous substrate include: membrane thickness 10 to 30 microns, porosity 30 to 50%.

[0017] Optionally, in S2, the porous substrate may be: Celgard 2400 substrate, Celgard 2500 substrate or Celgard 3501 substrate.

[0018] Optionally, in S2, the substrate is peeled off after drying to obtain a self-supporting two-dimensional vermiculite film.

[0019] Optionally, in S3, the self-supporting two-dimensional vermiculite film is perpendicular to the direction of the irradiation beam, and the area of ​​the self-supporting two-dimensional vermiculite film is larger than the area of ​​the irradiation beam.

[0020] In a second aspect, the present invention provides a modified two-dimensional vermiculite membrane prepared by the above-mentioned method for preparing the modified two-dimensional vermiculite membrane.

[0021] In a third aspect, the present invention provides an application of the modified two-dimensional vermiculite membrane in salinity difference power generation, in which the modified two-dimensional vermiculite membrane provides an ion transmission channel between the electrolyte high concentration side and the electrolyte low concentration side.

[0022] Optionally, the NaCl concentration on the electrolyte high concentration side is 1.0-5.0M, and the NaCl concentration on the electrolyte low concentration side is 0.01-0.5M.

[0023] The beneficial effects of the present invention are:

[0024] 1. In order to solve the problem of higher ion transmission resistance and lower ion flux caused by the tortuous transmission channel of the two-dimensional vermiculite film, the present invention adopts ion irradiation modification technology and utilizes its energy loss mechanism to increase a through ion transmission channel inside the two-dimensional vermiculite film, thereby changing the tortuous transmission path of the ions into a non-tortuous transmission path, reducing the ion transmission resistance and increasing the ion flux.

[0025] 2. The modified two-dimensional vermiculite membrane of the present invention is applied to salt difference power generation, and the output power of the osmotic energy is increased from 0.2 to 0.7 W / m before modification. 2 Increased to 0.5~3.0W / m 2 The output power of salt difference power generation has been increased several times, showing great application potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0027] Figure 1 1 is an atomic force microscope (AFM) photograph of the two-dimensional vermiculite nanosheets obtained by peeling in Example 1 of the present invention; wherein (A) is the AFM image, and (B) is the height measured in the range of straight line ab.

[0028] Figure 2 These are digital photos and electron microscope cross-sectional photos of the self-supporting two-dimensional vermiculite membrane in Example 1 of the present invention, wherein (A) is a digital photo and (B) is an electron microscope photo.

[0029] Figure 3 It is a schematic diagram of the ion implantation system and its working principle in Example 1 of the present invention.

[0030] Figure 4 3 are atomic force microscope (AFM) photos of the two-dimensional vermiculite film before and after irradiation in Example 1 of the present invention; wherein (A) is a photo of the self-supporting two-dimensional vermiculite film before irradiation, and (B) is a photo of the self-supporting two-dimensional vermiculite film after irradiation.

[0031] Figure 5 It is a schematic diagram of a salt difference power generation performance testing device in Example 2 of the present invention.

[0032] Figure 6 It is a statistical diagram of the output power of salt difference power generation of unmodified and modified two-dimensional vermiculite membranes under different irradiation doses in Example 1 of the present invention.

[0033] Figure 7 It is a schematic diagram of the modification principle of the two-dimensional vermiculite membrane in a specific embodiment of the present invention.

[0034] Among them, 1. aperture; 2. ion pre-accelerator; 3. ion separation and mass analyzer; 4. ion accelerator; 5. center of gravity deflector; 6. scanner; 7. target chamber; 8. source meter; 9. DC resistance box; 10. low salt solution pool; 11. high salt solution pool; 12. membrane material; 13. ion transmission channel; 14. two-dimensional vermiculite film. DETAILED DESCRIPTION

[0035] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0036] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0037] Example 1

[0038] A method for preparing a modified two-dimensional vermiculite film comprises the following steps:

[0039] S1. Immerse 10 g of vermiculite with a particle size of 2.5 ± 5 mm in 150 ml of saturated NaCl solution, transfer to a round-bottom flask, and reflux at 110 ° C for 24 hours, then wash the vermiculite with deionized water and ethanol until no chloride ions are detected; then transfer the washed vermiculite to a 2M LiCl solution, heat and reflux at 110 ° C for 24 hours, then wash the vermiculite again with deionized water and ethanol until no chloride ions are detected; transfer the obtained substance to 150 mL of a mass flask. The method comprises the following steps: adding the solid obtained after the treatment with the H2O2 solution to a H2O2 solution with a concentration of 30 to 31%, stirring and mixing, and refluxing at 110° C. for 24 hours; adding the solid obtained after the treatment with the H2O2 solution to deionized water for ultrasonic treatment for 2 hours, during which the vermiculite nanosheets are gradually peeled off; centrifuging the mixture after ultrasonic treatment at 4000 rpm to remove the remaining unpeeled vermiculite small particles; and then centrifuging the mixture again at 4000 rpm for 10 minutes to retain the upper suspension, which is the vermiculite nanosheet dispersion.

[0040] It was detected that the concentration of the vermiculite nanosheet dispersion obtained by the above method was 5 mg / mL.

[0041] The vermiculite nanosheets in the obtained vermiculite nanosheet dispersion were observed using an atomic force microscope (AFM). Figure 1 As shown, Figure 1 (A) is the AFM image. Figure 1 (B) is along Figure 1 From the height measured by the straight lines ab in (A), it can be seen that the thickness of the single-layer vermiculite nanosheet is 1.5nm and the size is 0.5-1μm.

[0042] S2. The obtained vermiculite nanosheet dispersion was filtered onto a Celgard 2400 substrate, dried in an oven at 60° C., and then peeled off from the substrate to obtain a self-supporting two-dimensional vermiculite film. The thickness of the self-supporting two-dimensional vermiculite film was detected to be 7 μm.

[0043] The digital photos of the obtained free-standing two-dimensional vermiculite film are shown in Figure 2 As shown in (A), the diameter of the membrane is 44 mm; the electron microscope photo of the cross section of the self-supporting two-dimensional vermiculite film is shown in Figure 2 As shown in (B), the film surface is smooth and defect-free, and the thickness is 7.6 μm.

[0044] S3, cutting the obtained self-supporting two-dimensional vermiculite film so that the area of ​​the vermiculite film is greater than the area of ​​the irradiation beam, and then subjecting the vermiculite film to fast heavy ion irradiation treatment, providing high-energy heavy ions through an accelerator, inducing strong electronic excitation and thermal spike response of the film material, forming continuous track damage, so as to achieve the modification of the vermiculite film and obtain a modified two-dimensional vermiculite film; in the fast heavy ion irradiation treatment, the heavy ions are Xe 31+; irradiation ion energy is 4MeV / u; irradiation dose is 10 8 ~10 12 ions / cm 2 The self-supporting two-dimensional vermiculite film obtained by S2 was treated with 0 and 1.6ⅹ10 9 8ⅹ10 9 4 x 10 10 6ⅹ10 10 1 x 10 11 and 2 x 10 11 ions / cm 2 A total of 7 different irradiation doses were used.

[0045] The free-standing two-dimensional vermiculite film before irradiation was observed by atomic force microscopy (AFM). Figure 4 As shown in (A), 2×10 11 ions / cm 2 The two-dimensional vermiculite film treated with irradiation dose was observed by atomic force microscopy (AFM). Figure 4 As shown in (B), it can be seen that after irradiation, the roughness of the film material increases significantly.

[0046] The equipment structure used for fast heavy ion irradiation treatment is as follows Figure 3 As shown, it includes: an aperture 1, an ion pre-accelerator 2, an ion separation and mass analyzer 3, an ion accelerator 4, a center of gravity deflector 5, a scanner 6 and a target chamber 7; after the ion source emits ions, the ions pass through the ion pre-accelerator 2 and the aperture 1 and enter the ion separation and mass analyzer 3, the heavy ions are screened out, transported into the ion accelerator 4, and then pass through the center of gravity deflector 5 and the scanner 6 to reach the target chamber 7, and the self-supporting two-dimensional vermiculite film to be modified set in the target chamber 7 is irradiated and modified.

[0047] Example 2

[0048] The modified two-dimensional vermiculite membrane prepared in Example 1 is used for the collection of salt difference energy of high-salinity wastewater, namely, salt difference power generation.

[0049] Schematic diagram of the membrane material salt difference power generation performance test device Figure 5 As shown, it includes: a source meter 8, a DC resistance box 9, a low-salinity solution pool 10 loaded with low-salinity wastewater, and a high-salinity solution pool 11 loaded with high-salinity wastewater. Electrodes are immersed in the low-salinity wastewater and the high-salinity wastewater respectively. The electrodes connect the source meter 8, the DC resistance box 9, the low-salinity wastewater and the high-salinity wastewater into a loop. The modified two-dimensional vermiculite film is used as a membrane material 12 and is sandwiched between the two electrolytic cells to electrically connect the two electrolytic cells.

[0050] The test equipment is shown in Table 1.

[0051] Table 1 Test equipment

[0052]

[0053] The test conditions are: the experimental solution temperature is 25°C.

[0054] The electrode materials are: Ag / AgCl electrode and Ag / AgCl reference electrode with salt bridge.

[0055] 5M NaCl solution is used for high-salinity wastewater, and 0.5M NaCl solution is used for low-salinity wastewater; other water used is high-resistance pure water with a resistance value of 18.20 megohms.

[0056] The test contents include: 1. ion selectivity of membrane materials (i.e. modified two-dimensional vermiculite membranes), 2. salt difference power generation conversion efficiency of membrane materials and 3. output power density of salt difference power generation conversion devices.

[0057] 1. The test methods for ion selectivity of membrane materials include:

[0058] (1) Cut the sealing film into a 3 cm × 5 cm rectangle and fold it in half;

[0059] (2) Use a specific puncher to punch a hole with an area of ​​4.9 mm in the center of the folded sealing film. 2 holes;

[0060] (3) Place the membrane material to be tested at the center of the sealing film to expose the set area;

[0061] (4) Set the temperature of the heating stage to 65°C and place the slide on the heating stage;

[0062] (5) Pick up the heated slide and gently press it against the edge of the center of the sealing film (note: the slide should not touch the center of the sealing film to prevent the hole from deforming due to heating);

[0063] (6) Repeating the above steps (1) to (6) multiple times can complete the packaging of the membrane material;

[0064] (7) The sealed membrane material is loaded into an electrolytic cell to assemble into a device, and the Ag / AgCl reference electrode with a salt bridge is placed on both sides of the solution cell, and connected to a digital source meter 8 through an external circuit to form a loop;

[0065] (8) Add 5M NaCl aqueous solution to one side of the high-salt solution pool 11 of the solution pool, add 0.5M NaCl aqueous solution to one side of the low-salt solution pool 10, connect the positive electrode of the source meter 8 to the side of the 5M NaCl aqueous solution, and connect the negative electrode of the source meter 8 to the side of the 0.5M NaCl aqueous solution; do not connect the DC resistance box 9 or adjust its resistance to 0, and use the Ag / AgCl reference electrode with a salt bridge to perform IV curve test, the scanning range is -1V to +1V, the voltage step interval is 0.05V, and a total of 41 data points;

[0066] (9) Record the open circuit voltage V obtained by the Ag / AgCl reference electrode test OC , calculate the ion selectivity of the membrane material; where V OC The value is the average of three measurements.

[0067] (10) Based on the literature, the ion selectivity of membrane materials (t + ) is calculated by the following equation:

[0068]

[0069] Among them, V OC The open circuit voltage obtained for the Ag / AgCl electrode with salt bridge test;

[0070] F=96500C·mol -1 , is the Faraday constant; R = 8.314 J / (mol·K); T = 298 K; C H =0.50M;

[0071] C L =0.01M.

[0072] 2. The salt difference power generation conversion efficiency of the membrane material is calculated by the following equation:

[0073]

[0074] Among them, t + is the calculated ion selectivity.

[0075] 3. The test methods for the output power density of salt difference power generation conversion devices include:

[0076] (1) The sealed membrane material is loaded into an electrolytic cell to assemble into a device, and Ag / AgCl electrodes without salt bridges are placed on both sides of the solution cell, and a resistance box and a source meter are connected through an external circuit to form a loop;

[0077] (2) Add 5M NaCl aqueous solution to one side of the high-salt solution pool 11 of the solution pool, add 0.5M NaCl aqueous solution to one side of the low-salt solution pool 10, connect the positive electrode of the source meter 8 to the side of the 5M NaCl aqueous solution, and connect the negative electrode of the source meter 8 to the side of the 0.5M NaCl aqueous solution; set the resistance value of the DC resistance box 9 to 0Ω, and use the Ag / AgCl electrode without a salt bridge to perform IV curve test, the scanning range is -1V to +1V, the voltage step interval is 0.05V, and a total of 41 data points;

[0078] (3) Record the open circuit voltage V obtained from the test OC and short-circuit current I SC The value of the device internal resistance r = V OC / I SC Set the input voltage to 0V, adjust the resistance box to R=r, use the Ag / AgCl electrode without salt bridge to perform IT curve test, and set the test time to 1s; record the current I value of the first point of the IT curve;

[0079] (4) Within the resistance range of R = r ± 20Ω, adjust the resistance of the resistor box by 20Ω at a time, perform an IT curve test, and record the current I value obtained in the test;

[0080] (5) Repeat the operation of step (4) to expand the range of R to 10Ω~106Ω, a total of 20 points, and then calculate the maximum output power density of the salt difference power generation conversion device; wherein, the current I value is the average value of the three measurement results.

[0081] (6) Maximum output power density of salt difference power generation conversion device (P max ) is calculated by the following equation:

[0082]

[0083] Where I is the current value of the first point obtained by IT curve test under different resistance values ​​(R), and S is the membrane test area. The relationship between different external resistances and power density is obtained by plotting the maximum power density P max (W / m 2 ).

[0084] Afterwards, the unmodified two-dimensional vermiculite membrane of the same size was used as the membrane material to carry out the test in Example 2, and the experimental data of the membrane material before modification were obtained. The obtained data are shown in Table 2.

[0085] Table 2 Experimental data before and after modification

[0086] <![CDATA[V oc (mV)]]> I(μA) Before modification 47 75(R=600Ω) After modification 51 234(R=200Ω)

[0087] The calculation results show that among the seven irradiation doses taken in Example 1, the cation selectivity of the original vermiculite membrane (irradiation dose is 0) is 0.9, the conversion efficiency is 0.32, and the output power of the osmotic energy is 0.7 W / m 2 , the modified vermiculite membrane (irradiation dose is 2×10 11 ions / cm 2 ) has a cation selectivity of 0.93, a conversion efficiency of 0.37, and an output power of osmotic energy of 2.1 W / m 2 .

[0088] In summary, if Figure 7 As shown, the rapid heavy ion irradiation treatment of the two-dimensional vermiculite film 14 proposed in the present invention increases the ion transmission channel 13 inside the two-dimensional vermiculite film 14, changes the ion transmission path, and enables the ions to be transmitted along the ion transmission channel 13 with a shorter path, rather than the tortuous ion transmission channel 13, thereby increasing the output power of salt difference power generation by several times, showing great application potential.

[0089] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a modified two-dimensional vermiculite membrane, characterized in that: The following steps are involved: S1, treating vermiculite with a saturated sodium chloride solution, a 2-3M LiCl solution and a H2O2 solution in sequence, then mixing the treated vermiculite with water, exfoliating the nanosheets by ultrasonic treatment for 2-3 hours, centrifuging to remove impurities, centrifuging at a speed of 4000-4500 r / min for 5-20 minutes, and collecting the suspension to obtain a vermiculite nanosheet dispersion; S2, filtering the vermiculite nanosheet dispersion obtained in S1 onto the surface of a porous substrate, and drying at 60 to 80° C. to obtain a self-supporting two-dimensional vermiculite film with a thickness of 4 to 100 μm; S3, subjecting the self-supporting two-dimensional vermiculite film obtained in S2 to rapid heavy ion irradiation to obtain a modified two-dimensional vermiculite film; In fast heavy ion irradiation, the heavy ions are Xe 31+ ; Irradiation ion energy is 0.1-4MeV / u; irradiation dose is 10 8 -10 12 ions / cm 2 .

2. The method for preparing the modified two-dimensional vermiculite film according to claim 1, characterized in that: In S1, 1-30 g of vermiculite is soaked in 10-300 ml of saturated NaCl solution, refluxed at 110-120° C. for 20-28 h, and then the vermiculite is washed with deionized water and ethanol until no chloride ions are detected, thereby obtaining a first powder; the first powder is mixed with 10-300 ml of LiCl solution, heated and refluxed at 110-120° C. for 20-28 h, and then the vermiculite is washed with deionized water and ethanol until no chloride ions are detected, thereby obtaining a second powder; the second powder is mixed with 100-150 ml of H2O2 solution, and refluxed at 110-120° C. for 20-28 h, thereby obtaining treated vermiculite.

3. The method for preparing the modified two-dimensional vermiculite film according to claim 1, characterized in that: In S1, the centrifugal impurity removal method includes: removing unpeeled small vermiculite particles by centrifugation at a speed of 4000 to 4500 r / min; Optionally, in S1, the size of the vermiculite nanosheets dispersed in the vermiculite nanosheet dispersion liquid includes: 0.1-1 μm; and the concentration of the vermiculite nanosheets in the vermiculite nanosheet dispersion liquid is 1-10 mg / mL.

4. The method for preparing the modified two-dimensional vermiculite film according to claim 1, characterized in that: In S2, the specifications of the porous substrate include: membrane thickness 10-30 μm, porosity 30-50%.

5. The method for preparing the modified two-dimensional vermiculite membrane according to claim 1, characterized in that: The porous substrate may be selected from: Celgard 2400 substrate, Celgard 2500 substrate or Celgard 3501 substrate.

6. The method for preparing the modified two-dimensional vermiculite membrane according to claim 1, characterized in that: In S2, the substrate is peeled off after drying to obtain a self-supporting two-dimensional vermiculite film.

7. The method for preparing the modified two-dimensional vermiculite membrane according to claim 1, characterized in that: The self-supporting two-dimensional vermiculite film is perpendicular to the direction of the irradiation beam, and the area of ​​the self-supporting two-dimensional vermiculite film is larger than the area of ​​the irradiation beam.

8. A modified two-dimensional vermiculite membrane prepared by the method for preparing a modified two-dimensional vermiculite membrane according to any one of claims 1 to 7.

9. An application of the modified two-dimensional vermiculite membrane as claimed in claim 8 in salt difference power generation, characterized in that: The modified two-dimensional vermiculite membrane provides ion transport channels between the electrolyte high concentration side and the electrolyte low concentration side.

10. The use of the modified two-dimensional vermiculite membrane in salt difference power generation according to claim 9, characterized in that: The NaCl concentration on the electrolyte high concentration side is 0.5 to 5.0 M, and the NaCl concentration on the electrolyte low concentration side is 0.01 to 0.49 M.

Citation Information

Patent Citations

  • Two-dimensional layered vermiculite membrane, production and application

    CN110449037A

  • Polymer electrolyte film material and preparation method thereof

    CN112397780A

  • Ultrathin vermiculite composite film, preparation method and application thereof

    CN116943455A

  • Vermiculite nanosheet and preparation method therefor

    WO2023070867A1

Cited By

  • Two-dimensional glass composite film based on irradiation treatment as well as preparation method and application of two-dimensional glass composite film