Method for treating calcified high-phosphorus-manganese acid vanadium liquid
By using a specially formulated vanadium precipitant agent and ammonium carbonate solution in high-phosphorus permanganic acid vanadium solution, the separation of vanadium manganese and phosphorus and the preparation of high-purity vanadium pentoxide is achieved, and the difficulty of manganese separation and acid consumption in the prior art are solved. The problem of high volume simplifies wastewater treatment and improves the purity of vanadium liquid.
Patent Information
- Application Number
- CN202411186759.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-15
AI Technical Summary
In the high-phosphorus, high-manganese vanadium slag calcium method, high phosphorus content leads to large vanadium loss. The existing vanadium extraction process cannot effectively separate manganese, resulting in manganese being present in wastewater or entering waste slag, and the acid consumption of conventional vanadium deposition process is high And inefficient.
The vanadium precipitant agent is prepared by water, triethanolamine and triethylamine, and the pH value is adjusted within the range of 5-7 for stirring and filtration. The manganese compound is leached with ammonium carbon solution, and high-purity vanadium pentoxide is obtained by cooling and crystallization and calcination. , realize the separation of vanadium, manganese, phosphorus and phosphorus.
Effectively separate vanadium-manganese phosphorus, obtain more than 99.5% high-purity vanadium pentoxide, and simplify wastewater treatment to avoid the generation of useless wastewater. Manganese compounds can be used to smelter manganese-containing alloys.
Smart Images

Figure CN118954591A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of vanadium slag treatment, and in particular to a method for treating calcified high-phosphorus-manganese acidic vanadium liquid. Background Art
[0002] In the high-phosphorus and high-manganese vanadium slag calcium method of vanadium extraction, due to the high phosphorus content and manganese content in the calcified acid leaching solution, both phosphorus removal and vanadium precipitation will lead to large vanadium losses. In addition, due to the high phosphorus content in the acidic vanadium solution, the removal method is generally to add ordinary slag to the raw materials for dilution, control the phosphorus content of the clinker and then leaching. The process is complicated, and the conventional vanadium precipitation pH value is generally 2-2.2, but when the phosphorus content exceeds 0.03g / L, it is necessary to control the pH value to 1.0-1.5 for vanadium precipitation, but this not only increases the acid consumption, but also affects the vanadium precipitation rate. In addition, the existing vanadium extraction process cannot separate manganese, which causes manganese to remain in the wastewater or enter the waste slag through further lime neutralization. Summary of the invention
[0003] In view of this, in order to overcome at least one aspect of the above problems, an embodiment of the present invention provides a method for treating calcified high-phosphorus manganese acid vanadium liquid, comprising the following steps: The vanadium precipitant is prepared with water, triethanolamine and triethylamine; The vanadium precipitating agent is added to the calcified high-phosphorus manganese acidic vanadium solution, and the pH value is adjusted, followed by stirring and filtering to obtain a first filter residue containing vanadium, manganese and phosphorus elements; Leaching the first filter residue with an ammonium carbonate solution to obtain a manganese compound and a first filtrate; Dephosphorizing the first filtrate and then cooling and crystallizing it to obtain ammonium metavanadate; The ammonium metavanadate is calcined to obtain vanadium pentoxide.
[0004] In some embodiments, the vanadium precipitant is prepared with water, triethanolamine and triethylamine, further comprising: The vanadium precipitant is prepared according to the volume ratio of water: triethanolamine: triethylamine of 5~10:3~5:0.5~1.
[0005] In some embodiments, the method further comprises: The high phosphorus manganese vanadium slag is roasted after adding calcium salt; The calcified high-phosphorus-manganese acid vanadium solution is acid-leached using a leaching agent at a pH value of 2.6-3.2, wherein the vanadium content is 20-35 g / L, the phosphorus content is 0.2-1.5 g / L, and the manganese content is 5-10 g / L.
[0006] In some embodiments, the vanadium precipitating agent is added to the calcified high-phosphorus manganese acidic vanadium solution and the pH value is adjusted, followed by stirring and filtering to obtain a first filter residue including vanadium, manganese and phosphorus elements, further comprising: Add the vanadium precipitator dropwise into the calcified high phosphorus manganese acid vanadium solution while stirring, and when the pH is 5-7, stop adding the vanadium precipitator dropwise, and continue stirring for 30-60 minutes; The first filter residue and the second filtrate containing vanadium, manganese and phosphorus elements are obtained by filtration.
[0007] In some embodiments, the method further comprises: The second filtrate is filtered after adjusting the pH value to 9-9.5 using lime or lime water; The pH value of the third filtrate obtained by filtration is adjusted and returned to be used as a leaching agent for calcified high-phosphorus manganese-vanadium slag clinker.
[0008] In some embodiments, leaching the first filter residue with an ammonium carbonate solution to obtain a manganese compound and a first filtrate further comprises: Leaching the first filter residue with an ammonium carbonate solution at 40-50° C. for 30-60 min; Adding an oxidant, wherein the ratio of the volume of the oxidant to the volume of the ammonium carbonate solution is 0.5-1 mL: 100 mL; The stirring was continued for 30-60 min to obtain a manganese compound and a first filtrate.
[0009] In some embodiments, leaching the first filter residue with an ammonium carbonate solution to obtain a manganese compound and a first filtrate further comprises: Leaching the first filter residue with an ammonium bicarbonate solution at 70-80° C. for 30-60 min; Adding an oxidant, wherein the ratio of the volume of the oxidant to the volume of the ammonium carbonate solution is 0.5-1 mL: 100 mL; The stirring was continued for 30-60 min to obtain a manganese compound and a first filtrate.
[0010] In some embodiments, the content of ammonium ions in the ammonium carbonate solution is 20-25 g / L.
[0011] In some embodiments, removing phosphorus from the first filtrate and then cooling and crystallizing to obtain ammonium metavanadate further comprises: Dephosphorizing the first filtrate and then cooling and crystallizing it to obtain ammonium metavanadate and vanadium precipitation liquid; Ammonium bicarbonate or ammonium carbonate with an ammonium ion content of 20-25 g / L is added to the solution after vanadium precipitation to prepare an ammonium carbonate solution.
[0012] In some embodiments, removing phosphorus from the first filtrate and then cooling and crystallizing to obtain ammonium metavanadate further comprises: The first filtrate is filtered after adding calcium oxide to remove phosphorus to obtain a filtered first solution, wherein the filtration temperature is 40-50°C.
[0013] The present invention has one of the following beneficial technical effects: the present invention uses high-phosphorus and manganese acidic vanadium liquid as raw material, adopts a new type of vanadium precipitation agent to precipitate vanadium, manganese and phosphorus, and does not bring in other cations that affect wastewater reuse, such as sodium ions; then extracts vanadium and phosphorus from the precipitated slag, manganese remains in the slag, and vanadium and phosphorus enter the alkaline solution, and dephosphorization treatment is carried out in the alkaline solution, thereby achieving effective separation of vanadium, manganese and phosphorus, and the obtained vanadium liquid is precipitated with ammonium to prepare high-purity vanadium pentoxide of more than 99.5%. The separated manganese compound can also be used as a raw material to smelt manganese-containing alloys. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments can be obtained based on these drawings without paying creative work.
[0015] Figure 1 A schematic flow chart of a method for treating calcified high-phosphorus manganese acid vanadium liquid provided by an embodiment of the present invention; Figure 2 A flowchart of a method for treating calcified high-phosphorus manganese acid vanadium liquid provided by an embodiment of the present invention; Figure 3 This is a schematic diagram of the contents of three types of calcified high-phosphorus manganese acid vanadium liquids provided by the present invention. DETAILED DESCRIPTION
[0016] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.
[0017] It should be noted that all expressions using "first" and "second" in the embodiments of the present invention are for distinguishing two non-identical entities with the same name or non-identical parameters. It can be seen that "first" and "second" are only for the convenience of expression and should not be understood as limitations on the embodiments of the present invention. The subsequent embodiments will not explain this one by one.
[0018] According to one aspect of the present invention, an embodiment of the present invention provides a method for treating plastic calcification high phosphorus manganese acid vanadium liquid, such as Figure 1 As shown, it may include the steps of: The vanadium precipitant is prepared with water, triethanolamine and triethylamine; The vanadium precipitating agent is added to the calcified high-phosphorus manganese acidic vanadium solution, and the pH value is adjusted, followed by stirring and filtering to obtain a first filter residue containing vanadium, manganese and phosphorus elements; Leaching the first filter residue with an ammonium carbonate solution to obtain a manganese compound and a first filtrate; Dephosphorizing the first filtrate and then cooling and crystallizing it to obtain ammonium metavanadate; The ammonium metavanadate is calcined to obtain vanadium pentoxide.
[0019] Normally, if the phosphorus content in the acidic vanadium liquid is too high, it is difficult to remove the phosphorus. Generally, ordinary slag is added to the raw materials for dilution, and the phosphorus content of the clinker is controlled before leaching. The conventional pH value of vanadium precipitation is generally 2-2.2. If the phosphorus content exceeds 0.03g / L, vanadium precipitation becomes difficult. There is a patented method to control the pH value of vanadium precipitation at 1.0-1.5, which not only increases the acid consumption, but also affects the vanadium precipitation rate.
[0020] The present invention uses high-phosphorus and manganese acidic vanadium liquid as raw material, adopts a new type of vanadium precipitation agent to precipitate vanadium, manganese and phosphorus, and does not bring in other cations that affect wastewater reuse, such as sodium ions; then extracts vanadium and phosphorus from the precipitated slag, manganese remains in the slag, and vanadium and phosphorus enter an alkaline solution, and dephosphorization treatment is performed in the alkaline solution, thereby effectively separating vanadium, manganese and phosphorus, and the obtained vanadium liquid partial ammonium vanadium precipitation can prepare high-purity vanadium pentoxide of more than 99.5%. Moreover, the wastewater after vanadium, phosphorus and manganese precipitation can be reused after simple treatment, and no excess wastewater is generated. The separated manganese compound can also be used as a raw material to smelt manganese-containing alloys.
[0021] In some embodiments, the vanadium precipitant is prepared with water, triethanolamine and triethylamine, further comprising: The vanadium precipitant is prepared according to the volume ratio of water: triethanolamine: triethylamine of 5~10:3~5:0.5~1.
[0022] In some embodiments, it also includes: The high phosphorus manganese vanadium slag is roasted after adding calcium salt; The calcified high-phosphorus-manganese acid vanadium solution is acid-leached using a leaching agent at a pH value of 2.6-3.2, wherein the vanadium content is 20-35 g / L, the phosphorus content is 0.2-1.5 g / L, and the manganese content is 5-10 g / L.
[0023] In some embodiments, the vanadium precipitating agent is added to the calcified high-phosphorus manganese acidic vanadium solution and the pH value is adjusted, followed by stirring and filtering to obtain a first filter residue including vanadium, manganese and phosphorus elements, further comprising: Add the vanadium precipitator dropwise into the calcified high phosphorus manganese acid vanadium solution while stirring, and when the pH is 5-7, stop adding the vanadium precipitator dropwise, and continue stirring for 30-60 minutes; Filtration to obtain a first filter residue and a second filtrate containing vanadium, manganese and phosphorus elements; In some embodiments, it also includes: The second filtrate is filtered after adjusting the pH value to 9-9.5 using lime or lime water; The pH value of the third filtrate obtained by filtration is adjusted and returned to be used as a leaching agent for calcified high-phosphorus manganese-vanadium slag clinker.
[0024] In some embodiments, leaching the first filter residue with an ammonium carbonate solution to obtain a manganese compound and a first filtrate further comprises: Leaching the first filter residue with an ammonium carbonate solution at 40-50° C. for 30-60 min; Adding an oxidant, wherein the ratio of the volume of the oxidant to the volume of the ammonium carbonate solution is 0.5-1 mL: 100 mL; The stirring was continued for 30-60 min to obtain a manganese compound and a first filtrate.
[0025] In some embodiments, leaching the first filter residue with an ammonium carbonate solution to obtain a manganese compound and a first filtrate further comprises: Leaching the first filter residue with an ammonium bicarbonate solution at 70-80° C. for 30-60 min; Adding an oxidant, wherein the ratio of the volume of the oxidant to the volume of the ammonium carbonate solution is 0.5-1 mL: 100 mL; The stirring was continued for 30-60 min to obtain a manganese compound and a first filtrate.
[0026] In some embodiments, the content of ammonium ions in the ammonium carbonate solution is 20-25 g / L.
[0027] In some embodiments, removing phosphorus from the first filtrate and then cooling and crystallizing to obtain ammonium metavanadate further comprises: Dephosphorizing the first filtrate and then cooling and crystallizing it to obtain ammonium metavanadate and vanadium precipitation liquid; Ammonium bicarbonate or ammonium carbonate with an ammonium ion content of 20-25 g / L is added to the solution after vanadium precipitation to prepare an ammonium carbonate solution.
[0028] In some embodiments, removing phosphorus from the first filtrate and then cooling and crystallizing to obtain ammonium metavanadate further comprises: The first filtrate is filtered after adding calcium oxide to remove phosphorus to obtain a filtered first solution, wherein the filtration temperature is 40-50°C.
[0029] Specifically, Figure 2As shown, firstly, a vanadium precipitant is prepared according to the ratio of water: triethanolamine: triethylamine of 10:5:1, and the mixture is sealed in a polyethylene bottle for storage for later use; then a certain amount of calcified high phosphorus manganese acid vanadium liquid is measured, and the vanadium precipitant is added dropwise while stirring, and the pH value is adjusted to 5-7, and the addition is stopped, and stirring is continued for 30-60 minutes; the first filter residue including vanadium, manganese and phosphorus elements is leached with a bicarbonate ammonium solution with an ammonium ion concentration of 20-25g / L, and the leaching conditions are that the volume and wet weight ratio of the two is 4-5:1, and the temperature is 40-50°C or 70-80℃, and add a certain oxidant after leaching for 30-60min, the volume of hydrogen peroxide added is 0.5-1mL:100mL of ammonium carbonate solution, and stirring is continued for 30-60min; filter to obtain manganese compound and the first filtrate, add calcium oxide to the first filtrate for phosphorus removal, the phosphorus removal temperature is 80℃, and the filtration temperature is 40-50℃; then stir and cool to 5-10℃ to crystallize and precipitate ammonium; add ammonium bicarbonate or ammonium carbonate with ammonium ions of 20-25g / L to the liquid after vanadium precipitation to prepare ammonium carbonate solution.
[0030] Among them, since the triethanolammonium contained in the first filter residue will release reducing substances such as carbon monoxide and formaldehyde when heated, the above reducing substances will reduce vanadium, thereby affecting the leaching effect of vanadium by ammonium carbonate. Therefore, adding an oxidant can eliminate the effect of vanadium reduction.
[0031] Example 1 Ammonium bicarbonate leaching of the first filter residue containing vanadium, manganese and phosphorus elements like Figure 3 As shown, 200 mL of calcified high-phosphorus manganese acid vanadium solution 1 is measured, and a vanadium precipitating agent is added dropwise while stirring to adjust the pH value to 5; the addition is stopped and stirring is continued for 30 minutes; the first filter residue and the second filtrate are obtained by filtration, and the second filtrate is reused after simple treatment; the first filter residue is leached with an ammonium bicarbonate solution with an ammonium ion concentration of 20 g / L and a wet weight ratio of 4:1, and leached at 40°C. After leaching for 30 minutes, hydrogen peroxide is added, and the volume of hydrogen peroxide added is 0.5 mL:100 mL. Stirring is continued for 30 minutes; the manganese compound and the first filtrate are obtained, and the first filtrate is dephosphorized at a dephosphorization temperature of 80°C and a filtration temperature of 40°C; the partial ammonium is crystallized and precipitated by stirring and cooling at 5°C; ammonium bicarbonate with an ammonium ion concentration of 20 g / L is added to the solution after vanadium precipitation to prepare an ammonium bicarbonate solution, which is then returned to the first filter residue for leaching. The volume of the second filtrate is 185 mL, of which vanadium is 0.20 g / L; the composition of the manganese compound is MnO: 93.5%, V: 0.56%, MgO: 2.1%, CaO: 0.90%; V obtained by calcining ammonium metavanadate 2 O 5 Content 99.7%, including Mn content 0.015%, P content <0.01%, Na 2 O+K 2 O0.273%.
[0032] The first filter residue containing vanadium, manganese and phosphorus elements is leached by ammonium carbonate solution Measure 200mL of calcified high-phosphorus manganese acid vanadium solution 1, add vanadium precipitation agent dropwise while stirring, and adjust the pH value to 5; stop adding dropwise, continue stirring for 30 minutes; filter to obtain the first filter residue and the second filtrate, and the second filtrate is reused after simple treatment; the first filter residue is leached with ammonium carbonate solution with an ammonium ion concentration of 20g / L and the wet weight of the filter residue in a ratio of 4:1, leaching at 70℃, adding hydrogen peroxide after leaching for 30min, the volume of hydrogen peroxide added is 0.5mL:100mL, and stirring is continued for 30min; filter to obtain manganese compound and the first filtrate, the first filtrate is dephosphorized, the dephosphorization temperature is 80℃, and the filtration temperature is 40℃; then stir and cool to 5℃ to crystallize and precipitate partial ammonium; ammonium carbonate with an ammonium ion concentration of 20g / L is added to the liquid after vanadium precipitation to prepare a carbonate ammonium solution. The volume of the second filtrate is 185 mL, of which vanadium is 0.20 g / L; the composition of the manganese compound is MnO: 93.6%, V: 0.56%, MgO: 2.13%, CaO: 0.91%; V obtained by calcining ammonium metavanadate 2 O 5 Content 99.72%, including Mn content 0.010%, P content <0.01%, Na 2 O+K 2 O0.260%.
[0033] Example 2 Ammonium bicarbonate leaching of the first filter residue containing vanadium, manganese and phosphorus elements Measure 1000mL of calcified high-phosphorus manganese acid vanadium solution 2, add vanadium precipitation agent dropwise while stirring, and adjust the pH value to 6; stop dropping, continue stirring for 45 minutes; filter to obtain the first filter residue and the second filtrate, and the second filtrate is reused after simple treatment; the first filter residue is leached with ammonium bicarbonate solution with an ammonium ion concentration of 23g / L and a wet weight ratio of 4.5:1, leached at 45℃, and hydrogen peroxide is added after leaching for 40min, the volume of hydrogen peroxide added is 0.7mL:100mL, and stirring is continued for 40min; filter to obtain manganese compound and the first filtrate, the first filtrate is dephosphorized, the dephosphorization temperature is 80℃, and the filtration temperature is 45℃; then stir and cool to 8℃ to crystallize and precipitate partial ammonium; ammonium bicarbonate with an ammonium ion concentration of 23g / L is added to the liquid after vanadium precipitation to prepare ammonium carbonate solution. The volume of the second filtrate is 925 mL, of which vanadium is 0.17 g / L; the composition of the manganese compound is MnO: 94.1%, V: 0.54%, MgO: 2.2%, CaO: 0.91%; V obtained by calcining ammonium metavanadate 2 O 5 Content 99.68%, including Mn content 0.012%, P content <0.01%, Na 2 O+K2 O0.254%.
[0034] Ammonium carbonate leaching of the first filter residue containing vanadium, manganese and phosphorus elements Measure 1000mL of calcified high-phosphorus manganese acid vanadium solution 2, add vanadium precipitation agent dropwise while stirring, and adjust the pH value to 6; stop dropping, continue stirring for 45 minutes; filter to obtain the first filter residue and the second filtrate, and reuse the second filtrate after simple treatment; the first filter residue is leached with ammonium carbonate solution with an ammonium ion concentration of 23g / L and the wet weight of the filter residue in a ratio of 4.5:1, leaching at 75℃, adding a certain oxidant after leaching for 40min, the volume of hydrogen peroxide added is 0.7mL:100mL, and stirring is continued for 40min; filter to obtain manganese compound and the first filtrate, the first filtrate is dephosphorized, the dephosphorization temperature is 80℃, and the filtration temperature is 45℃; then stir and cool to 8℃ to crystallize and precipitate partial ammonium; ammonium carbonate with an ammonium ion concentration of 23g / L is added to the liquid after vanadium precipitation to prepare a carbonate ammonium solution. The volume of the second filtrate is 925 mL, of which vanadium is 0.17 g / L; the composition of manganese compound is MnO: 94.4%, V 0.46%, MgO: 2.23%, CaO: 0.91%; V obtained by calcining ammonium metavanadate 2 O 5 Content 99.80%, of which Mn content <0.010%, P content <0.01%, Na 2 O+K 2 O 0.180%.
[0035] Example 3 Ammonium bicarbonate leaching of the first filter residue containing vanadium, manganese and phosphorus elements Measure 2000mL of calcified high-phosphorus manganese acid vanadium solution 3, add vanadium precipitation agent dropwise while stirring, and adjust the pH value to 7; stop dropping, continue stirring for 60min; filter to obtain the first filter residue and the second filtrate, and reuse the second filtrate after simple treatment; the first filter residue is leached with ammonium bicarbonate solution with an ammonium ion concentration of 25g / L and a wet weight ratio of 5:1, leaching at 50℃, adding hydrogen peroxide after leaching for 60min, the volume of hydrogen peroxide added and the volume of ammonium bicarbonate solution are 1mL:100mL, and stirring is continued for 60min; filter to obtain manganese compound and the first filtrate, dephosphorize the first filtrate, the dephosphorization temperature is 80℃, and the filtration temperature is 50℃; then stir and cool to 10℃ to crystallize and precipitate partial ammonium; add ammonium bicarbonate with an ammonium ion concentration of 25g / L to the liquid after vanadium precipitation to prepare a carbonate ammonium solution. The volume of the second filtrate is 1850 mL, of which vanadium is 0.12 g / L; the composition of the manganese compound is MnO: 94.3%, V0.48%, MgO: 2.1%, CaO: 0.90%; V obtained by calcining ammonium metavanadate 2 O 5Content 99.7%, including Mn content 0.011%, P content <0.01%, Na 2 O+K 2 O0.263%.
[0036] Ammonium carbonate leaching of the first filter residue containing vanadium, manganese and phosphorus elements Measure 2000mL of calcified high-phosphorus manganese acid vanadium solution 3, add vanadium precipitation agent dropwise while stirring, and adjust the pH value to 7; stop dropping, continue stirring for 60min; filter to obtain the first filter residue and the second filtrate, and reuse the second filtrate after simple treatment; the first filter residue is leached with ammonium carbonate solution with an ammonium ion concentration of 25g / L and the wet weight of the filter residue in a ratio of 5:1, leaching at 80℃, adding hydrogen peroxide after leaching for 60min, the volume of hydrogen peroxide added and the volume of ammonium carbonate solution are 1mL:100mL, and stirring is continued for 60min; filter to obtain manganese compound and the first filtrate, dephosphorize the first filtrate, the dephosphorization temperature is 80℃, and the filtration temperature is 50℃; then stir and cool to 10℃ to crystallize and precipitate partial ammonium; add ammonium carbonate with an ammonium ion concentration of 25g / L to the liquid after vanadium precipitation to prepare a carbonate ammonium solution. The volume of the second filtrate is 1850 mL, of which vanadium is 0.12 g / L; the composition of the manganese compound is MnO: 95.6%, V: 0.26%, MgO: 2.13%, CaO: 0.90%; V obtained by calcining ammonium metavanadate 2 O 5 Content 99.82%, of which Mn content <0.010%, P content <0.01%, Na 2 O+K 2 O0.160%.
[0037] The present invention uses high-phosphorus and manganese acidic vanadium liquid as raw material, adopts a new type of vanadium precipitation agent to precipitate vanadium, manganese and phosphorus, and does not bring in other cations that affect wastewater reuse, such as sodium ions; then extracts vanadium and phosphorus from the precipitated slag, manganese remains in the slag, and vanadium and phosphorus enter an alkaline solution, and dephosphorization treatment is performed in the alkaline solution, thereby effectively separating vanadium, manganese and phosphorus, and the obtained vanadium liquid partial ammonium vanadium precipitation can prepare high-purity vanadium pentoxide of more than 99.5%. Moreover, the wastewater after vanadium, phosphorus and manganese precipitation can be reused after simple treatment, and no excess wastewater is generated. The separated manganese compound can also be used as a raw material to smelt manganese-containing alloys.
[0038] The above are exemplary embodiments disclosed in the present invention, but it should be noted that various changes and modifications may be made without departing from the scope disclosed in the embodiments of the present invention as defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.
[0039] It should be understood that, as used herein, the singular forms "a", "an" are intended to include the plural forms as well, unless the context clearly supports an exception. It should also be understood that, as used herein, "and / or" refers to any and all possible combinations including one or more of the associated listed items.
[0040] The serial numbers of the embodiments disclosed in the above embodiments of the present invention are only for description and do not represent the advantages or disadvantages of the embodiments.
[0041] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the above embodiments of the present invention, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.
Claims
1. A method for treating calcified high-phosphorus manganese acid vanadium liquid, characterized in that: The following steps are involved: The vanadium precipitant is prepared with water, triethanolamine and triethylamine; The vanadium precipitating agent is added to the calcified high-phosphorus manganese acidic vanadium solution, and the pH value is adjusted, followed by stirring and filtering to obtain a first filter residue containing vanadium, manganese and phosphorus elements; Leaching the first filter residue with an ammonium carbonate solution to obtain a manganese compound and a first filtrate; Dephosphorizing the first filtrate and then cooling and crystallizing it to obtain ammonium metavanadate; The ammonium metavanadate is calcined to obtain vanadium pentoxide.
2. The method according to claim 1, characterized in that The vanadium precipitant is prepared with water, triethanolamine and triethylamine, and further comprises: The vanadium precipitant is prepared according to the volume ratio of water: triethanolamine: triethylamine of 5~10:3~5:0.5~1.
3. The method according to claim 1, characterized in that Also includes: The high phosphorus manganese vanadium slag is roasted after adding calcium salt; The calcified high-phosphorus-manganese acid vanadium solution is acid-leached using a leaching agent at a pH value of 2.6-3.2, wherein the vanadium content is 20-35 g / L, the phosphorus content is 0.2-1.5 g / L, and the manganese content is 5-10 g / L.
4. The method according to claim 3, further comprising: adding the vanadium precipitating agent to the calcified high-phosphorus manganese acidic vanadium solution and adjusting the pH value, stirring, filtering to obtain a first filter residue containing vanadium, manganese and phosphorus elements; and Add the vanadium precipitator dropwise into the calcified high phosphorus manganese acid vanadium solution while stirring, and when the pH is 5-7, stop adding the vanadium precipitator dropwise, and continue stirring for 30-60 minutes; The first filter residue and the second filtrate containing vanadium, manganese and phosphorus elements are obtained by filtration.
5. The method according to claim 4, characterized in that Also includes: The second filtrate is filtered after adjusting the pH value to 9-9.5 using lime or lime water; The pH value of the third filtrate obtained by filtration is adjusted and returned to be used as a leaching agent for calcified high-phosphorus manganese-vanadium slag clinker.
6. The method according to claim 1, characterized in that Leaching the first filter residue with an ammonium carbonate solution to obtain a manganese compound and a first filtrate further comprises: Leaching the first filter residue with an ammonium carbonate solution at 40-50° C. for 30-60 min; Adding an oxidant, wherein the ratio of the volume of the oxidant to the volume of the ammonium carbonate solution is 0.5-1 mL: 100 mL; The stirring was continued for 30-60 min to obtain a manganese compound and a first filtrate.
7. The method according to claim 1, characterized in that Leaching the first filter residue with an ammonium carbonate solution to obtain a manganese compound and a first filtrate further comprises: Leaching the first filter residue with an ammonium bicarbonate solution at 70-80° C. for 30-60 min; Adding an oxidant, wherein the ratio of the volume of the oxidant to the volume of the ammonium carbonate solution is 0.5-1 mL: 100 mL; The stirring was continued for 30-60 min to obtain a manganese compound and a first filtrate.
8. The method according to claim 6 or 7, characterized in that The content of ammonium ions in the ammonium carbonate solution is 20-25g / L.
9. The method according to claim 1, characterized in that The first filtrate is dephosphorized and then cooled and crystallized to obtain ammonium metavanadate, further comprising: Dephosphorizing the first filtrate and then cooling and crystallizing it to obtain ammonium metavanadate and vanadium precipitation liquid; Ammonium bicarbonate or ammonium carbonate with an ammonium ion content of 20-25 g / L is added to the solution after vanadium precipitation to prepare an ammonium carbonate solution.
10. The method according to claim 1, characterized in that The first filtrate is dephosphorized and then cooled and crystallized to obtain ammonium metavanadate, further comprising: Calcium oxide is added to the first filtrate to remove phosphorus and then filtered to obtain a filtered vanadium solution, wherein the filtering temperature is 40-50°C.