Gadolinium-doped modified lithium-rich manganese-based positive electrode material and preparation method thereof
By doping the rare earth element gadolinium, adjusting the layer spacing and structure of the lithium-rich manganese-based positive electrode material, the problems of low efficiency and poor circulation stability in the prior art were solved for the first time, and the improvement of battery rate performance and material structure were achieved. The stability of the synthesis process simplifies the synthesis process.
Patent Information
- Application Number
- CN202411010122.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
The application of existing lithium-rich manganese-based positive electrode materials in lithium-ion batteries has problems such as low efficiency, poor cycle stability and poor rate performance for the first time. The existing doping modification methods are costly and large doping amounts for the materials. The structural impact is obvious, and the performance improvement is not significant.
By doping the rare earth element gadolinium, spray pyrolysis method and high-temperature calcination, etc., the gadolinium-doped lithium-manganese-based positive electrode material is prepared, the material layer spacing is adjusted, the lithium ion diffusion performance is improved, and the lattice oxygen is stabilized through the Gd-O bond. , reduce the content of manganese ions to simplify the synthesis process.
The cycle stability and rate performance of the battery have been significantly improved, and the efficiency of the Coulomb is improved for the first time, and the stability of the material structure is enhanced. The capacity retention rate of the battery 1C current cycle for 400 cycles at 2-4.8V voltage reaches 95.79%, and reduces the battery during the cycle process. polarization in.
Smart Images

Figure CN118954622A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery cathode materials, and specifically relates to a gadolinium-doped modified lithium-rich manganese-based cathode material and a preparation method thereof. Technical Background
[0002] Since lithium-rich manganese-based cathode materials exhibit significantly high specific capacity, high energy density, and high working voltage compared to other cathode materials, they have received extensive attention and have become one of the most promising next-generation lithium-ion battery cathodes. However, due to the presence of an anion redox process, oxygen is inevitably released during the charge and discharge process, leading to a series of problems. Specifically, the application of lithium-rich manganese-based cathode materials in lithium-ion batteries mainly has three problems: low initial Coulombic efficiency (during the activation process of Li2MnO3, there is a net release of Li2O, and the oxygen evolution is an irreversible process, which will cause irreversible changes in the material structure, making the released lithium ions unable to be embedded in the subsequent discharge process), capacity decay during cycling, and rapid voltage decay (structural changes, transition metal dissolution, and side reactions between the active material and the electrolyte during cycling will all lead to capacity decay), and poor rate performance (low electronic and ionic conductivities, which is also related to the migration of transition metals to the lithium layer to block the lithium ion diffusion channels). These directly affect its practical application. The element doping modification method is simple, controllable, and easy to repeat. Moreover, it can significantly improve the material performance, and it is one of the common methods to improve the structural stability and electrochemical performance of lithium-rich manganese-based cathode materials. By doping different elements, the initial Coulombic efficiency, rate performance, and cycling stability of lithium-rich manganese-based cathode materials can be improved.
[0003] There are many existing element doping modification methods. Among them, a patent with the application number "202311418791.50" discloses a cation and anion co-doped modified lithium-rich manganese-based cathode material of F, S2, and Na+, with the chemical formula Li 1.2- x Na x Ni 0.2 Mn 0.6 O 2-y-2z F y S z , 0.02 < x < 0.1, 0.02 < y < 0.1, 0.02 < z < 0.1. A patent with the application number "202310472838.X" discloses a fluorine-aluminum double-doped lithium-rich manganese-based cathode material, with the structural formula Li 1.2 Mn 0.54 Co 0.13 Ni 0.13-x O 2-6 xAl x F 6x , x = 0.02 - 0.06.
[0004] In summary, in the existing doping modification methods, the cost of the elements used is relatively high. At the same time, the cost is increased due to the large amount of element doping. At the same time, the large amount of doping will affect the material structure, so the performance improvement is not obvious, among which the first coulombic efficiency and cycle stability are not ideal. Summary of the invention
[0005] The present invention provides a gadolinium-doped modified lithium-rich manganese-based positive electrode material and a preparation method thereof, in order to solve the problems in the prior art that the doping amount is large and the cost is high, and at the same time, the large doping amount has an impact on the material structure, the performance improvement is not obvious, and the first coulomb efficiency and cycle stability are not ideal. To achieve the above purpose, the technical solution provided by the present invention is: a method for preparing a gadolinium-doped lithium-rich manganese-based positive electrode material, the specific steps are as follows:
[0006] Step 1: According to the general formula Li 1.2 Ni 0.13 Co 0.13 Mn 0.51-0.539 G 0.001-0.03 O2, lithium acetate, manganese acetate, cobalt acetate, and nickel acetate are added to deionized water and mixed evenly, a gadolinium source is added, monohydrated citric acid is added as a complexing agent to complex cations to obtain a salt solution, and the solution is stirred evenly;
[0007] Step 2, preparing precursor powder by spray pyrolysis of the uniformly mixed solution;
[0008] Step 3, placing the precursor powder in a muffle furnace for high-temperature calcination to obtain a powder;
[0009] Step 4: Add conductive activated carbon to the powder and ball-mill in anhydrous ethanol;
[0010] Step 5: Place the ball-milled material in a blast oven to dry, and allow to stand to obtain gadolinium-doped lithium-rich manganese-based positive electrode material powder.
[0011] Furthermore, in the salt solution of step 1, the total concentration of metal ions is 0.15 mol / L, and the concentration of citric acid is 0.30-0.45 mol / L.
[0012] Furthermore, the stirring rate of the above step 1 is 400-600 R / Min, and the stirring time is 1-3 hours.
[0013] Furthermore, the gadolinium source in the above step 1 is gadolinium acetate or gadolinium chloride.
[0014] Furthermore, the temperatures of the inlet and outlet during the spraying process in the above step 2 are set to 200-230° C. and 100-120° C. respectively, and the peristaltic speed is 10-15 rpm.
[0015] Furthermore, the high temperature calcination treatment in step three is specifically to increase the temperature by 3 degrees per minute to 1000 degrees, keep the temperature for 20 minutes, and naturally cool down to room temperature.
[0016] Furthermore, in the above step 4, the mass ratio of powder to activated carbon is 6-8:1, the ball milling rate is 400-500R / Min, the mass ratio of ball milling beads to material is 100-120:1, and the time is 4-5 hours.
[0017] Furthermore, in the above step 5, the drying temperature is 60-80° C., and the drying time is 6-8 hours.
[0018] Furthermore, a gadolinium-doped lithium-rich manganese-based positive electrode material is prepared according to the above preparation method.
[0019] Compared with the prior art, the advantages of the present invention are:
[0020] 1. The present invention improves the conductivity and kinetic properties of lithium-rich manganese-based positive electrode materials by micro-regulating the rare earth element gadolinium. The doping of gadolinium ions will widen the interlayer spacing of lithium-rich manganese-based positive electrode layered materials, improve the lithium ion diffusion performance, and reduce the material impedance, thereby improving the battery rate performance; during the cycle process, the doping of gadolinium stabilizes the material structure and slows down the undesirable phase transition from the surface to the inside, reducing the polarization of the battery during the cycle, making the structure more stable, and greatly improving the overall cycle stability of the battery. The button battery finally prepared shows excellent cycle stability. Within the voltage range of 2-4.8V, the capacity retention rate of 1C current cycles 400 times reaches 95.79%.
[0021] 2. The doping amount of gadolinium in the present invention is less than that in the previous doping modification method, and has little effect on the original structure of the material. The gadolinium ions doped into the bulk phase combine with oxygen ions to produce a stronger Gd-O bond energy, which is not easy to break, and can anchor the lattice oxygen, further stabilizing the lattice oxygen and inhibiting the escape of oxygen during the first charge and discharge process. Therefore, a trace amount of doping can improve the first coulomb efficiency, effectively improving the first coulomb efficiency of the battery.
[0022] 3. The lithium-rich manganese-based positive electrode material of the present invention reduces the content of manganese ions while introducing a small amount of gadolinium ions. This is because there is a competitive relationship between trace doping of gadolinium ions to replace manganese positions, and reducing manganese can successfully dope gadolinium ions into the lithium-rich manganese-based positive electrode material. Therefore, the synthesis steps of the present invention are simple, and the preparation of the lithium-rich manganese-based positive electrode material can be achieved using conventional equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A comparison chart of the first charge and discharge capacity of 0.5% Gd doping and the comparative example;
[0024] Figure 2This is a comparison chart of the first charge and discharge capacity of 2% Gd doping and the comparative example;
[0025] Figure 3 0.1c 50 cycle performance diagram of 2% Gd doping and comparative example;
[0026] Figure 4 1c 400 cycle performance diagram of 0.5% Gd doping and comparative example;
[0027] Figure 5 1c 400 cycle performance diagram of 2% Gd doping and comparative example;
[0028] Figure 6 The rate performance diagram of 0.5% Gd doping and comparative example;
[0029] Figure 7 It is the rate performance diagram of 2% Gd doping and comparative example;
[0030] Figure 8 Graph showing the cycle performance of the comparative example and embodiment 3;
[0031] Fig. 9 Graph showing the cycle performance of the comparative example and embodiment 4;
[0032] Fig.10 EIS comparison diagram of comparative example, 0.5% Gd doping, and 2.0% Gd doping;
[0033] Fig.11 XRD patterns of 0.5% Gd-doped, 2.0% Gd-doped and control samples;
[0034] Fig.12 SEM images of 0.5% Gd-doped, 2.0% Gd-doped and control samples;
[0035] Fig.13 O1s XPS graphs of 0.5% Gd-doped, 2.0% Gd-doped and control samples. Specific implementation methods
[0037] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0038] The chemical formula of the lithium-rich manganese-based positive electrode material prepared by the present invention is Li 1.2 Co 0.13 Ni 0.13 Mn 0.54-x G x O, 0.001 <x<0.03。
[0039] Example 1: A Gadolinium-doped modified lithium-rich manganese-based positive electrode material Li 1.2 Ni 0.13 Co 0.13 Mn 0.535 G 0.005 The preparation method of O2 comprises the following steps:
[0040] Step 1: Weigh acetate containing Li, Ni, Co, Gd and Mn elements according to the molar ratio shown in the chemical formula, dissolve them in deionized water to prepare a mixed salt solution with a concentration of 0.15 mol / L; add citric acid as a complexing agent with a concentration of 0.3 mol / L; place the mixed solution in a magnetic stirrer, set the speed to 600 r / min, and stir for 1 hour.
[0041] Step 2: The mixed solution is granulated into a precursor by a spray dryer, with a liquid feeding rate of 10 ml / min, an air inlet temperature of 230° C., an air outlet temperature of 100-120° C., and a creeping speed of 15 rpm.
[0042] Step 3: The precursor obtained by spraying is loaded into an alumina crucible, and the temperature is raised to 1000° C. at a rate of 3° C. / min in a box furnace, kept at that temperature for 20 min, and naturally cooled to room temperature to obtain a powder.
[0043] Step 4: Mix the powder with super p powder in a ratio of 8:1, add anhydrous ethanol for wet ball milling, the mass ratio of ball milling beads to powder is 100:1, the ball milling rate is 400R / Min, and the time is 4 hours.
[0044] Step 5: Place the ball-milled solution in a blast oven to dry, and let stand to obtain a lithium-rich manganese-based positive electrode material Li 1.2 Ni 0.13 Co 0.13 Mn 0.535 G 0.005 O2.
[0045] Example 2: A Gadolinium-doped modified lithium-rich manganese-based positive electrode material Li 1.2 Ni 0.13 Co 0.13 Mn 0.52 G 0.02 The preparation method of O2 comprises the following steps:
[0046] The preparation method is basically the same as that of Example 1, except that the Mn element added in step 1 is 0.52 and the Gd element content is 0.02.
[0047] Example 3: A Gadolinium-doped modified lithium-rich manganese-based positive electrode material Li 1.2 Ni 0.13 Co 0.13 Mn0.54 G 0.005 The preparation method of O2 comprises the following steps:
[0048] Step 1: According to the molar ratio shown in the chemical formula, acetate containing Li, Ni, Co, and Mn elements and gadolinium chloride as the Gd source are weighed and dissolved in deionized water to prepare a mixed salt solution with a concentration of 0.15 mol / L; citric acid is added as a complexing agent with a concentration of 0.45 mol / L; the mixed solution is placed in a magnetic stirrer, the speed is set to 400 r / min, and stirred for 3 hours.
[0049] Step 2: The mixed solution is granulated into a precursor by a spray dryer, with a liquid feeding rate of 15 ml / min, an air inlet temperature of 230° C., an air outlet temperature of 100-120° C., and a creeping speed of 10 rpm.
[0050] Step 3: The precursor obtained by spraying is loaded into an alumina crucible, and the temperature is raised to 1000° C. at a rate of 3° C. / min in a box furnace, kept at that temperature for 20 min, and naturally cooled to room temperature to obtain a powder.
[0051] Step 4: Mix the prepared powder with super p powder in a ratio of 6:1, add them into anhydrous ethanol and wet ball mill them. The mass ratio of ball milling beads to powder is 120:1, the ball milling rate is 500R / Min, and the time is 5 hours.
[0052] Step 5: Place the ball-milled solution into a blast oven for drying, dry at 60°C for 8 hours, and then let stand to obtain a lithium-rich manganese-based positive electrode material Li 1.2 Ni 0.13 Co 0.13 Mn 0.54 G 0.005 O2.
[0053] Example 4: A Gadolinium-doped modified lithium-rich manganese-based positive electrode material Li 1.2 Ni 0.13 Co 0.13 Mn 0.535 G 0.005 The preparation method of O2 comprises the following steps: The preparation method is basically the same as that of Example 1, except that the Gd salt added in step 1 is gadolinium chloride.
[0054] Comparative Example: Preparation of Li-rich manganese-based positive electrode material Li 1.2 Ni 0.13 Co 0.13 Mn 0.54 O2
[0055] The preparation method is basically the same as that of Example 4, except that the Gd element is not added in step 1.
[0056] The dried lithium-rich manganese-based positive electrode materials obtained in the above Examples 1-4 and the comparative example were filtered through a 300-mesh screen, and the filtered powder was mixed with the CMC aqueous solution at a mass ratio of 57:250. Stir for 2 hours, ultrasonic for 2 hours, and stir for 2 hours. The stirred slurry was coated on aluminum foil, dried at 110°C for 20 hours, cut and dried at 115°C for 10 hours, and placed in a glove box to prepare button batteries. Tests were carried out, and the test results are as follows:
[0057] like Figure 1 As shown, at a voltage of 2-4.8V and a current of 0.1C, the first discharge capacity of the comparative example is 262.5mAh / g, and the first coulombic efficiency is 70.78%, while that of Example 1 is 289.31mAh / g, and the first coulombic efficiency is 81.76%. The first coulombic efficiency and discharge capacity of the example are higher than those of the comparative example, because the doped gadolinium ions form bonds with oxygen, inhibiting the irreversible reaction of lattice oxygen.
[0058] like Figure 2 As shown, under the same test current and voltage, the first discharge specific capacity of Example 2 is 248.50 mAh / g, and the first coulombic efficiency is 79.39%. The gadolinium-oxygen bond energy is stronger and is not easily destroyed during the charge and discharge process. The gadolinium doping amount increases, and more bonds are formed with oxygen, resulting in part of the lattice oxygen not participating in the reaction, which reduces the charge specific capacity and further reduces the discharge specific capacity.
[0059] like Figure 4 As shown, Example 1 cycles 400 times at 1C current and 2-4.8V voltage, and the capacity retention rate is 86.12%, which is much higher than 13.77% of the comparative example, indicating that gadolinium ions are doped into the material, stabilizing the layered structure of the material and inhibiting subsequent adverse phase changes.
[0060] like Figure 3 , Figure 5 As shown, the capacity retention rate of Example 2 after 50 cycles at 0.1C current and 2-4.8V voltage is 101.62%, which is much higher than 74.79% of the comparative example. (The reason for exceeding 100% is the continuous activation of the battery) The capacity retention rate of Example 2 after 400 cycles at 1C current and 2-4.8V voltage is 95.79%, which is 13.77% higher than the comparative example and also higher than Example 1 (86.12%), indicating that the introduction of gadolinium ions has a significant effect on stabilizing the structure of lithium-rich manganese-based positive electrode materials and the cycle stability of the battery.
[0061] like Figure 6As shown, they are rate performance diagrams of the comparative example and embodiment 1, wherein the specific capacities of the comparative example 0.1C, 0.5C, 1C, 2C, and 5C are 246.43mAh / g, 189.66mAh / g, 161.47mAh / g, 135.51mAh / g, and 102.36mAh / g, respectively, and those of embodiment 1 are 283.57mAh / g, 229.9mAh / g, 200.79mAh / g, 169.62mAh / g, and 139.81mAh / g, respectively. The discharge specific capacity of embodiment 1 at different times is higher than that of the comparative example.
[0062] like Figure 7 As shown, they are rate performance diagrams of the comparative example and Example 2, wherein the specific capacities of Example 2 at 0.1C, 0.5C, 1C, 2C, and 5C are 243.44mAh / g, 195.17mAh / g, 170.82mAh / g, 148.43mAh / g, and 120.79mAh / g, respectively. The high current discharge specific capacity of Example 2 is higher than that of the comparative example because gadolinium ion doping improves the band structure of the lithium-rich manganese-based positive electrode material, reduces impedance, and improves its conductivity and ion diffusion capacity (see Fig.10 ).
[0063] like Figure 8 As shown, it is the cycle performance diagram of Example 1 and Example 3. It can be seen that when doping a trace amount of gadolinium, it is necessary to reduce the corresponding manganese content, because a small amount of gadolinium doping, during the solid phase sintering process, there is a competition between ions entering the bulk phase lattice. If the manganese content is not reduced, the element ratio of the designed material will not be achieved. It can also be seen from the performance that the first discharge specific capacity and 400 cycle stability of Example 1 are higher than those of Example 3.
[0064] like Fig. 9 As shown, after changing the salt of gadolinium ion to gadolinium chloride, the performance of Example 4 prepared is almost the same as that of Example 1 prepared with gadolinium acetate.
[0065] like Fig.10 As shown, the EIS graphs of the comparative example, Example 1, and Example 2, the semicircle in the high frequency region is related to the charge transfer resistance (Rct), and the oblique line in the low frequency region is the Warburg impedance, corresponding to the diffusion of lithium ions inside the electrode. The radius of the semicircle in the high frequency region of Experimental Examples 1 and 2 is smaller than that of the comparative example, and the slope in the low frequency region is also greater than that of the comparative example, indicating that gadolinium ion doping improves the mobility of lithium ions in the lithium-rich manganese-based positive electrode material and improves its conductivity.
[0066] like Fig.11As shown, the SEM images of the comparative example, Example 1, and Example 2 in the original state and after 400 cycles, compared with the original state, gadolinium doping refines the particle size of the lithium-rich manganese-based positive electrode material, inhibits the agglomeration phenomenon, and increases its contact area with the electrolyte, which is beneficial to ion migration. After 400 cycles, the agglomeration phenomenon of the comparative example is aggravated, while the particles of Example 1 and Example 2 are still evenly dispersed.
[0067] like Fig.12 As shown, the XRD diagrams of the comparative example, Example 1, and Example 2, most of the main diffraction peaks indicate that the material has an a-NaFeO2 structure of the R3m space group of a hexagonal layered material (LiMO2 component), and there is no obvious impurity peak, indicating that gadolinium doping will not affect the material structure of the lithium-rich manganese-based positive electrode material. The difference is that the (003) peak at 18°-19° shifts to the low-angle region with the doping of gadolinium, which indicates that the gadolinium ions are successfully doped into the lattice of the lithium-rich manganese-based positive electrode material and cause the c-axis to expand. This is conducive to the migration of lithium ions in the lithium layer, thereby improving the rate performance.
[0068] like Fig.13 As shown, it is the O1s graph of the XPS test of the comparative example, Example 1, and Example 2. The peaks at 529.5 and 531.5 eV correspond to lattice oxygen (O2-) and oxygen vacancies, respectively. After 400 cycles, the lattice oxygen peak of the comparative example weakened, while the peak at 529.5 eV of Example 1 and Example 2 remained almost the same as the intensity before the cycle, indicating that the doping of gadolinium ions is beneficial to stabilize the lattice oxygen and improve the redox reversibility of oxygen during the cycle. The cycle performance of the above examples and comparative examples is listed in Table 1. The capacity performance at different rates is listed in Table 2.
[0069] Table 1
[0070]
[0071] Table 2
[0072]
[0073] In summary, embodiment 1 is the best embodiment.
[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may be modified and varied in various forms. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a gadolinium-doped lithium-rich manganese-based positive electrode material, characterized in that: The specific steps are as follows: Step 1: According to the general formula Li 1.2 Ni 0.13 Co 0.13 Mn 0.54-x G 0.001-0.03 O2, lithium acetate, manganese acetate, cobalt acetate, and nickel acetate are added to deionized water and mixed evenly, a gadolinium source is added, monohydrated citric acid is added as a complexing agent to complex cations to obtain a salt solution, and the solution is stirred evenly; Step 2, preparing precursor powder by spray pyrolysis of the uniformly mixed solution; Step 3, placing the precursor powder in a muffle furnace for high-temperature calcination to obtain a powder; Step 4: Add conductive activated carbon to the powder and ball-mill in anhydrous ethanol; Step 5: Place the ball-milled material in a blast oven to dry, and allow to stand to obtain gadolinium-doped lithium-rich manganese-based positive electrode material powder.
2. The method for preparing a gadolinium-doped lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In the salt solution of step 1, the total concentration of metal ions is 0.15 mol / L, and the concentration of citric acid is 0.30-0.45 mol / L.
3. The method for preparing a gadolinium-doped lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The stirring rate of step 1 is 400-600 R / Min, and the stirring time is 1-3 hours.
4. The method for preparing a gadolinium-doped lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The gadolinium source in step 1 is gadolinium acetate or gadolinium chloride.
5. A method for preparing a gadolinium-doped lithium-rich manganese-based positive electrode material according to any one of claims 1 to 4, characterized in that: In the step 2, the inlet and outlet temperatures during the spraying process are set to 200-230°C and 100-120°C, respectively, and the peristaltic speed is 10-15 rpm.
6. The method for preparing a gadolinium-doped lithium-rich manganese-based positive electrode material according to claim 5, characterized in that: The high temperature calcination treatment in step three is specifically to increase the temperature by 3 degrees per minute to 1000 degrees, keep the temperature for 20 minutes, and naturally cool down to room temperature.
7. A method for preparing a gadolinium-doped lithium-rich manganese-based positive electrode material according to claim 6, characterized in that: In the step 4, the mass ratio of powder to activated carbon is 6-8:1, the ball milling rate is 400-500R / Min, the mass ratio of ball milling beads to material is 100-120:1, and the time is 4-5 hours.
8. The method for preparing a gadolinium-doped lithium-rich manganese-based positive electrode material according to claim 7, characterized in that: The drying temperature in step 5 is 60-80° C. and the drying time is 6-8 hours.
9. The gadolinium-doped lithium-rich manganese-based positive electrode material obtained by the preparation method according to claim 1.
Citation Information
Cited By
Doped lithium-rich manganese oxide positive electrode material and preparation method and application thereof
CN119361676A