High-precision wave plate assembly processing technology

Through double-sided polishing and slitting glueing processes, the problems of surface roughness and surface shape changes in wave plate assembly processing are solved, and high-precision and efficient wave plate assembly processing are achieved, which is suitable for mass production, significantly improving yield and production efficiency .

CN118954975APending Publication Date: 2024-11-15SUZHOU GULAI OPTICAL TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411051390.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing wave plate assembly processing technology has problems such as surface roughness, surface shape changes, difficulty in controlling the thickness of the glue layer and low processing efficiency, resulting in poor optical communication performance and mass production problems.

Method used

The quartz wave plate and glass components are treated with double-sided polishing, and the adhesive thickness is controlled to be less than 5μm. After cutting the finished product, secondary glue and coating are performed, and the coating temperature is controlled to be less than 70℃. High-precision component processing is achieved through polishing and cutting.

Benefits of technology

It improves the accuracy and yield of wave plate components, is suitable for mass production, improves processing efficiency, avoids the reliability failure of glue layer and changes in surface shape, and realizes the mass production of high-precision wave plate components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954975A_ABST
    Figure CN118954975A_ABST
Patent Text Reader

Abstract

The invention discloses a processing technology of a high-precision wave plate assembly. The processing technology comprises the following steps: taking a quartz wave plate, a first glass element and a second glass element which meet technological requirements as processing raw materials for later use; carrying out double-sided polishing treatment on the quartz wave plate, the first glass element and the second glass element; sequentially gluing the plurality of quartz wave plates and the polished surface of the first glass element according to the specification requirement of a final product to obtain a first processing body; the first machined body is longitudinally cut into flat sheets with the preset thickness, and the two faces of each flat sheet are polished to obtain a second machined body; carrying out secondary gluing on the second processing body and a second glass element to form a gluing assembly, and carrying out polishing treatment to obtain a third processing body; coating the third processing body to obtain a fourth processing body; cutting to obtain a finished product. According to the invention, the batch production of the high-precision wave plate assembly can be realized, the production efficiency can be greatly improved, and the yield can be obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of optical element processing, and in particular to a high-precision wave plate component processing technology. Background Art

[0002] Wave plate components are usually formed by combining multiple quartz glass plates that are glued together and stacked together. The polarization axes of adjacent wave plates can be deflected at a certain angle according to different requirements, thereby meeting different optical communication needs. The current process of wave plate component processing is: several single wave plates are processed to the finished product thickness, then cut into small pieces, and then assembled with other glass components by side splicing and gluing. This processing method has the following defects: 1. Since the side is cut and processed, the surface is rough and uneven after processing, resulting in a gluing gap of more than 20μm; 2. Since the wave plate is very thin, the thickness of the general optical communication band application is only about 9μm, and the surface shape will change during the gluing process, resulting in poor performance of the final output light; 3. When the wave plate is spliced ​​with the glass element, the thickness of the glue layer cannot be accurately controlled, which makes it easy for the adjacent two wave plates to be non-coplanar and poor in flatness, resulting in the appearance of empty glue bubbles when gluing and assembling with the previous splitter element; 4. Since this processing technology requires small-sized wave plates to be assembled with glass elements piece by piece, the processing efficiency is low and it is not convenient for mass production. Summary of the invention

[0003] In order to overcome the deficiencies of the prior art, the purpose of the present invention is to provide a high-precision wave plate component processing technology, which has the advantages of improving the accuracy and yield of the wave plate component, being suitable for mass production and having high processing efficiency.

[0004] The purpose of the present invention is achieved by the following technical solutions:

[0005] According to an embodiment of the present disclosure, a high-precision wave plate assembly processing process is provided, comprising:

[0006] Taking the quartz wave plate, the first glass element and the second glass element that meet the process requirements as processing raw materials for standby;

[0007] Performing double-sided polishing on the quartz wave plate, the first glass element, and the second glass element until the surface flatness reaches a predetermined process parameter;

[0008] According to the specification requirements of the final product, a plurality of quartz wave plates and the polished surface of the first glass element are sequentially glued to obtain a first processed body, wherein the thickness of each glue layer produced by the gluing is controlled to be less than 5 μm;

[0009] Cutting the first processed body into flat sheets of a predetermined thickness along the longitudinal direction, and polishing both sides of each of the flat sheets to obtain a second processed body, wherein the dimensional accuracy after polishing is controlled to be less than 0.5 μm;

[0010] The second processed body and the second glass element are glued together for a second time to form a glued assembly, and both sides of the glued assembly are polished to control the dimensional accuracy, thereby obtaining a third processed body;

[0011] Performing a coating process on the third processed body according to preset process parameters to obtain a fourth processed body, wherein the coating temperature is controlled to be less than 70° C.;

[0012] The fourth processed body is cut into a specified size according to the finished product specification requirements to obtain a finished product.

[0013] In some exemplary embodiments, the optical axis direction of the quartz wave plate is selected to be 45°, and the optical axis direction is determined by an X-ray crystal orientation instrument; the first glass element and the second glass element are both made of H-K9L glass material.

[0014] In some exemplary embodiments, during the polishing process, polyurethane and polishing powder are used as polishing media to prepare a polishing liquid, and the specific gravity of the polishing liquid is 1.015 and the pH is 7-8.

[0015] In some exemplary embodiments, the quartz wave plate, the first glass element, and the second glass element are double-sided polished to a surface flatness of 1 μm and a smoothness of 40-20.

[0016] In some exemplary embodiments, the number of glued sheets of the first processed body is controlled to be 6-9 sheets.

[0017] In some exemplary embodiments, the dimensional accuracy of the second processed body after polishing is controlled by measuring the retardation using an ellipsometer.

[0018] In some exemplary embodiments, the polishing of both sides of the glued assembly to control the delay performance specifically includes:

[0019] Taking the side of the glued assembly opposite to the second glass element as the reference surface, the second glass element is polished after the light glue is applied;

[0020] The second glass element after polishing is used as the reference surface, and the surface of the glued assembly is polished after the optical glue is applied.

[0021] In some exemplary embodiments, when the second glass element is polished, the parallelism is controlled to be less than 3 seconds; when the quartz wave plate is polished, the dimensional accuracy after polishing is controlled to be less than 0.5 μm, and the thickness of the obtained third processed body is 0.8 mm, and the dimensional accuracy after polishing is controlled by the delay performance.

[0022] In some exemplary embodiments, the quartz wave plate and the first glass element are glued together with UT-20 glue to obtain a first processed body, and the second processed body and the second glass element are glued together with Norland 61 glue to form a glued assembly.

[0023] In some exemplary embodiments, the cutting process of the fourth processed body is performed by a dicing saw.

[0024] In summary, compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention provides a high-precision wave plate component processing technology. The first processing body is formed by gluing and then the first processing body is cut, so that the processing requirements of multiple finished products can be met at one time, and the production efficiency is improved. The overall precision of the wave plate component is higher through polishing. The coating temperature is controlled to be less than 70°C during coating, which can effectively avoid the reliability failure of the glue layer and the surface shape change caused by high temperature. Through the above process, the batch production of high-precision wave plate components can be realized, the production efficiency can be greatly improved, and the yield rate can be significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The process flow chart of an embodiment of the present invention.

[0027] Figure 2 Schematic diagram of the structure of the first processing body in an embodiment of the present invention.

[0028] Figure 3 It is a schematic structural diagram of the first processed body when being cut in an embodiment of the present invention.

[0029] Figure 4 Schematic diagram of the structure of the glued assembly in an embodiment of the present invention.

[0030] Figure 5 It is a schematic structural diagram of the fourth processed body when being cut in an embodiment of the present invention.

[0031] The numbers and letters in the figure represent the corresponding component names:

[0032] 10. Quartz wave plate; 20. First glass element; 30. Second glass element; 40. First cutting line; 50. Second processed body; 60. Second cutting line. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] like Figures 1 to 5 As shown, an embodiment of the present invention provides a high-precision wave plate component processing process, including: S100, taking the quartz wave plate 10, the first glass element 20 and the second glass element 30 that meet the process requirements as processing raw materials for standby use.

[0036] Specifically, the optical axis direction of the quartz wave plate 10 is selected to be 45°, and the optical axis direction is determined by an X-ray crystal orientation instrument. The first glass element 20 and the second glass element 30 are both made of H-K9L glass material, and the quartz wave plate 10, the first glass element 20 and the second glass element 30 need to be pre-cut into corresponding sizes according to process requirements.

[0037] S200, performing double-sided polishing on the quartz wave plate 10, the first glass element 20 and the second glass element 30 until the surface flatness reaches a predetermined process parameter.

[0038] Specifically, during the polishing process, polyurethane and polishing powder are used as polishing media to prepare a polishing liquid. The specific gravity of the polishing liquid is 1.015, the pH is 7-8, the polyurethane material is LP66 polyurethane polishing leather, and the polishing powder is 2800 polishing powder. After polishing, the surface flatness is controlled to reach 1μm. Generally, there is no special requirement for the smoothness, which can usually be controlled to 40-20.

[0039] S300, according to the specification requirements of the final product, a plurality of quartz wave plates 10 and the polished surface of the first glass element 20 are sequentially glued to obtain a first processed body, wherein the thickness of each glue layer produced by the gluing is controlled to be less than 5 μm.

[0040] Specifically, the quartz wave plate 10 and the first glass element 20 are glued together using UT-20 glue. UT-20 has a low viscosity and can achieve an extremely narrow gluing gap. Usually, the number of glued sheets of the first processed body is controlled to be 6-9 sheets, which can be adjusted according to the specifications of the final product.

[0041] S400, cutting the first processed body into flat sheets of a predetermined thickness along the longitudinal direction, and polishing both sides of each of the flat sheets to obtain a second processed body 50, wherein the dimensional accuracy after polishing is controlled to be less than 0.5 μm.

[0042] Specifically, the first processed body can be cut by a J5060 inner circle cutting machine, and the cutting position and direction are as follows: Figure 3 As shown in the first cutting line 40 in the figure, the thickness of each flat sheet can be set to 1-1.5mm, preferably 1.3mm; during polishing, polyurethane and polishing powder are also used as polishing media to prepare the polishing liquid, the specific gravity of the polishing liquid is 1.015, the pH is 7-8, the polyurethane material is LP66 polyurethane polishing leather, and the polishing powder is 2800 polishing powder. The dimensional accuracy of the second processed body 50 after polishing is controlled by measuring the delay degree by an ellipsometer.

[0043] S500, performing secondary gluing of the second processed body 50 and the second glass element 30 to form a glued assembly, and performing polishing treatment on both sides of the glued assembly to control dimensional accuracy, thereby obtaining a third processed body.

[0044] like Figure 4 As shown, Figure 4 The schematic structural diagram of the glued assembly is shown, in which the second glass element 30 is glued to one side of the second processed body 50 in the longitudinal direction, wherein the second processed body 50 and the second glass element 30 are glued for a second time with Norland 61 glue to form a glued assembly.

[0045] Polishing both sides of the glued assembly to control the delay performance specifically includes:

[0046] S501, taking the side of the bonding assembly opposite to the second glass element 30 as the reference plane, polishing the second glass element 30 after the optical glue is applied, and controlling the parallelism to be less than 3 seconds during the polishing process.

[0047] S502, taking the polished second glass element 30 as the reference plane, polishing the surface of the glued assembly after the optical glue is applied, and when polishing the glued assembly, controlling the dimensional accuracy after polishing to be less than 0.5 μm, and the thickness of the obtained third processed body is 0.8 mm, and the dimensional accuracy after polishing is controlled by the delay performance, for example, by measuring the delay through an ellipsometer.

[0048] Among them, during polishing in steps S501 and S502, polyurethane and polishing powder are also used as polishing media to prepare the polishing liquid. The specific gravity of the polishing liquid is 1.015, the pH is 7-8, the polyurethane material is LP66 polyurethane polishing leather, and the polishing powder is 2800 polishing powder. The dimensional accuracy after polishing can also be controlled by measuring the delay degree by an ellipsometer.

[0049] S600, performing coating treatment on the third processed body according to preset process parameters to obtain a fourth processed body, wherein the coating temperature is controlled to be less than 70°C.

[0050] Specifically, the coating process is as follows: after wiping the third processed body clean, place it in the coating chamber of the coating equipment, evacuate it and use physical vapor deposition to evaporate the film material, control the temperature to be less than 70°C during coating, and use tantalum dioxide and silicon dioxide as the film materials. The coated wave plate assembly can effectively reduce reflected light and improve product quality.

[0051] S700, cutting the fourth processed body into a specified size according to the finished product specification requirements to obtain a finished product. For example, the fourth processed body may be cut by a DISCO321 dicing cutting machine. The specific cutting position and direction are as follows: Figure 5 As shown in the second cutting line 60 in FIG.

[0052] The present invention provides a high-precision wave plate component processing technology. The first processing body is formed by gluing and then the first processing body is cut, so that the processing requirements of multiple finished products can be met at one time, and the production efficiency is improved. The overall precision of the wave plate component is higher through polishing. The coating temperature is controlled to be less than 70°C during coating, which can effectively avoid the reliability failure of the glue layer and the surface shape change caused by high temperature. Through the above process, the batch production of high-precision wave plate components can be realized, the production efficiency can be greatly improved, and the yield rate can be significantly improved.

[0053] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which are equivalent modifications and improvements made to the above embodiments based on the essential technology of the present invention, and all of them belong to the protection scope of the present invention.

Claims

1. A high-precision wave plate component processing process, characterized in that: include: Taking the quartz wave plate, the first glass element and the second glass element that meet the process requirements as processing raw materials for standby; Performing double-sided polishing on the quartz wave plate, the first glass element, and the second glass element until the surface flatness reaches a predetermined process parameter; According to the specification requirements of the final product, a plurality of quartz wave plates and the polished surface of the first glass element are sequentially glued to obtain a first processed body, wherein the thickness of each glue layer produced by the gluing is controlled to be less than 5 μm; Cutting the first processed body into flat sheets of a predetermined thickness along the longitudinal direction, and polishing both sides of each of the flat sheets to obtain a second processed body, wherein the dimensional accuracy after polishing is controlled to be less than 0.5 μm; The second processed body and the second glass element are glued together for a second time to form a glued assembly, and both sides of the glued assembly are polished to control the dimensional accuracy, thereby obtaining a third processed body; Performing a coating process on the third processed body according to preset process parameters to obtain a fourth processed body, wherein the coating temperature is controlled to be less than 70° C.; The fourth processed body is cut into a specified size according to the finished product specification requirements to obtain a finished product.

2. The high-precision wave plate assembly processing technology according to claim 1 is characterized in that: The optical axis direction of the quartz wave plate is selected to be 45°, and the optical axis direction is determined by an X-ray crystal orientation instrument; the first glass element and the second glass element are both made of H-K9L glass material.

3. The high-precision wave plate assembly processing process according to claim 1 or 2, characterized in that: When performing the polishing treatment, polyurethane and polishing powder are used as polishing media to prepare the polishing liquid, and the specific gravity of the polishing liquid is 1.015 and the pH is 7-8.

4. The high-precision wave plate assembly processing process according to claim 3 is characterized in that: The quartz wave plate, the first glass element and the second glass element are double-sided polished until the surface flatness reaches 1 μm and the smoothness is 40-20.

5. The high-precision wave plate assembly processing technology according to claim 1 is characterized in that: The number of glued sheets of the first processed body is controlled to be 6-9 sheets.

6. The high-precision wave plate assembly processing technology according to claim 1 is characterized in that: The dimensional accuracy of the second processed body after polishing is controlled by measuring the retardation with an ellipsometer.

7. The high-precision wave plate assembly processing technology according to claim 1 is characterized in that: The polishing of both sides of the glued component to control the delay performance specifically includes: Taking the side of the glued assembly opposite to the second glass element as the reference surface, the second glass element is polished after the light glue is applied; The second glass element after polishing is used as the reference surface, and the surface of the glued assembly is polished after the optical glue is applied.

8. The high-precision wave plate assembly processing process according to claim 7, characterized in that: When the second glass element is polished, the parallelism is controlled to be less than 3 seconds; when the quartz wave plate is polished, the dimensional accuracy after polishing is controlled to be less than 0.5μm, and the thickness of the obtained third processed body is 0.8mm, and the dimensional accuracy after polishing is controlled by the delay performance.

9. The high-precision wave plate assembly processing process according to claim 1, characterized in that: The quartz wave plate and the first glass element are glued together with UT-20 glue to obtain a first processed body, and the second processed body and the second glass element are glued together with Norland 61 glue to form a glued assembly.

10. The high-precision wave plate assembly processing technology according to claim 1, characterized in that: The fourth processed body is cut by a dicing saw.

Citation Information

Patent Citations

  • ITO and wave plate combined device

    CN105223637A

  • Glued wave plate

    CN212965498U

  • Method for producing prism

    JP2006337641A

  • Dual-source optical wavelength processor

    US20050276537A1