White Portland cement clinker and preparation method thereof

Through the composition and modification of raw materials of a specific ratio, the problem of insufficient whiteness and mechanical properties of white cement is solved, and the whiteness and cost reduction are achieved, while the firing temperature is reduced.

CN118954984APending Publication Date: 2024-11-15HEBEI QIANBAO SPECIAL CEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411429677.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-14
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The whiteness value of existing white cement is low, has high production cost, and has a high firing temperature, making it difficult to improve both whiteness and mechanical properties at the same time.

Method used

The modification and calcination process are optimized by the composition of raw materials with a specific ratio, including limestone, modified high-magnesium waste stone, wollastonite, kaolin, wollastonite, bauxite, waste aluminum slag, borax and composite mineralizer. Reduce the firing temperature and improve whiteness and mechanical properties.

Benefits of technology

The whiteness and comprehensive performance of white silicate cement clinker is significantly improved, production costs are reduced, and the firing temperature is reduced without affecting the whiteness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of white cement, and particularly discloses a white Portland cement clinker and a preparation method thereof. The white Portland cement clinker is prepared from the following raw materials in parts by mass: 38 to 42 parts of limestone, 38 to 42 parts of modified high-magnesium waste rock, 8 to 11 parts of wollastonite, 3 to 5 parts of kaolin, 3 to 6 parts of pyrophyllite, 1 to 1.5 parts of bauxite, 1 to 1.5 parts of aluminum scrap slag, 1 to 1.5 parts of borax and 0.8 to 1.4 parts of compound mineralizer. According to the invention, inorganic chemical reaction modification is carried out on the high-magnesium waste rock, the surface appearance of the high-magnesium waste rock is changed, and the surface of the high-magnesium waste rock with the original appearance is coated with a layer of loose and porous substance, so that the specific surface area of the clinker is increased, and diffuse reflection on light is increased; through the raw materials in a specific ratio, a synergistic effect is formed among the raw materials, the cost of the raw materials is reduced, the whiteness and mechanical strength of the clinker are remarkably improved, and the clinker has a relatively good market application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of white cement, in particular to a white Portland cement clinker and a preparation method thereof. Background Art

[0002] White cement, full name white silicate cement, codenamed P·W, is a hydraulic cementitious material made by grinding silicate cement clinker with less iron oxide content, appropriate amount of gypsum and qualified mixed materials (limestone and kiln dust) together. White cement has the characteristics of high whiteness, bright color and high strength. It is generally used as a building decoration material in building decoration projects. It is mainly used for sculptures, floors, and the manufacture of terrazzo products. It can also be used to make white and colored concrete components and prepare colored mortar for decorative plastering. It is the largest-scale colored silicate cement. White silicate cement clinker refers to cement clinker with calcium silicate as the main component and less iron oxide content obtained by burning raw materials with appropriate ingredients until they are partially melted. The color of Portland cement is mainly determined by the iron oxide content in the clinker. Generally, Portland cement contains more iron oxide (3%~4%) and is gray; when the iron oxide content is 0.45%~0.7%, it is light green; white Portland cement is white due to the very small amount of coloring substances such as iron oxide (0.35%~0.4%), manganese oxide, titanium oxide, chromium oxide, and cobalt oxide. Therefore, white Portland cement clinker needs to use purer raw materials, such as pure kaolin, pure quartz sand, pure lime or chalk, and burn it at a higher temperature (1500℃~1600℃) to make clinker.

[0003] The mineral composition and production process of white cement are similar to those of ordinary Portland cement. However, the quality requirements of white cement are mainly reflected in strength and whiteness. There are many factors affecting the whiteness of cement clinker, including raw materials, fuel quality, raw material quality, clinker calcination, bleaching and cooling. How to obtain white cement with higher whiteness value and stronger mechanical properties while reducing the firing temperature and production cost is a problem that needs to be solved at present. Summary of the invention

[0004] In view of the above problems, the present invention provides a white Portland cement clinker and a preparation method thereof, which reduces the firing temperature and improves the whiteness of the white Portland cement clinker by limiting the raw material composition and ratio, and has good comprehensive performance.

[0005] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions: In a first aspect, the present invention provides a white silicate cement clinker, comprising the following raw materials in parts by weight: 38 to 42 parts of limestone, 38 to 42 parts of modified high-magnesium waste rock, 8 to 11 parts of wollastonite, 3 to 5 parts of kaolin, 3 to 6 parts of pyrophyllite, 1 to 1.5 parts of bauxite, 1 to 1.5 parts of waste aluminum slag, 1 to 1.5 parts of borax, and 0.8 to 1.4 parts of a composite mineralizer; The preparation method of the modified high-magnesium waste rock comprises the following steps: Add high-magnesium waste rock, phosphate and inorganic acid into water, stir and react until pH = 5.5~6, adjust the pH of the reaction system to weak alkalinity, continue the reaction for 30min~60min, and obtain modified high-magnesium waste rock.

[0006] Compared with the prior art, the white silicate cement clinker provided by the present invention uses limestone, modified high-magnesium waste rock and wollastonite as calcium materials, uses wollastonite, kaolin and pyrophyllite as siliceous materials, and uses bauxite and waste aluminum slag as aluminum materials. The raw materials in specific proportions have a matching and homogenizing effect, which can homogenize and reduce the Fe2O3 content in the raw material; the addition of a specific amount of borax can produce a synergistic effect with the magnesium oxide in the raw materials (such as high-magnesium waste rock), promote the formation of a liquid phase, slow down the heat release rate of the hydration reaction, and stabilize silicate minerals (C3S and C2S), significantly improving the whiteness of the white silicate cement clinker; the SiO2 content in the siliceous material is relatively high, which will reduce the wear resistance of the product and increase the firing temperature. The addition of a specific amount of composite mineralizer can significantly reduce the firing temperature without affecting the whiteness of the white silicate cement clinker. In addition, the associated element Ti in the raw materials (such as bauxite) can reduce the coordination of metal ions, dissolve more iron ions, and change the iron ions from four-coordinated to eight-coordinated, thereby improving the whiteness of white silicate cement clinker.

[0007] The present invention performs inorganic chemical reaction modification on high-magnesium waste rock, changes the surface morphology of the high-magnesium waste rock, covers the surface of the original morphology of the high-magnesium waste rock with a layer of loose and porous material, increases the specific surface area of ​​the white silicate cement clinker, increases the diffuse reflection of the white silicate cement clinker to light, and thus improves the whiteness of the white silicate cement clinker.

[0008] The present invention forms a synergistic effect between the raw materials through the raw material composition of a specific ratio, reduces the raw material cost, and at the same time significantly improves the whiteness of the white silicate cement clinker, and also effectively improves the mechanical properties of the white silicate cement clinker, and has good market application value.

[0009] Preferably, the raw materials of the white Portland cement clinker also include 0.1 to 0.2 parts of barite.

[0010] In the present invention, the main component of barite is BaSO4. During the clinker sintering process, barium salts preferentially participate in the reaction to form barium aluminoferrite and barium aluminate minerals, which dissolve more iron ions and convert the iron ions from four-coordinated to eight-coordinated, thereby improving the whiteness value of white silicate cement clinker.

[0011] Preferably, the composite mineralizer comprises CaF2, CaCl2, CuO and ZnO in a mass ratio of (4-5):(6-8):(0.8-1):(0.5-0.8).

[0012] The present invention uses a specific composite mineralizer to significantly reduce the firing temperature of clinker, promote the generation of C3S in clinker, and improve the whiteness and comprehensive performance of white silicate cement clinker. CaF2 participates in the calcination reaction of clinker, and the generated hydrofluoric acid has strong polarity, which can destroy the lattice of SiO2 in the raw material and reduce the activation energy of solid phase reaction; at the same time, it accelerates the decomposition of CaCO3 and alkali-containing minerals and promotes the solid phase reaction; it can also reduce the generation temperature and viscosity of the liquid phase, increase the amount of liquid phase, form an intermediate transition phase, so that C3S minerals can be formed at a faster reaction speed and at a lower temperature, and generate early strength minerals. The compounding of CaCl2 and CaF2 can reduce the content of free calcium oxide (f-CaO) in white silicate cement clinker and increase the whiteness of white silicate cement clinker. The addition of CuO improves the burnability of clinker, increases the content of C3S in white silicate cement clinker, reduces free calcium oxide, and improves the reflectivity of white silicate cement clinker. ZnO can promote more Fe to enter the mineral, thereby reducing the formation of C4AF and making the white Portland cement clinker significantly whiter.

[0013] Preferably, the chemical composition of the limestone meets the following mass content requirements: CaO ≥ 51%, SiO2 ≤ 3%, MgO ≤ 2.5%, Fe2O3 ≤ 0.15%.

[0014] Preferably, the chemical composition of the high-magnesium waste rock meets the following mass content requirements: CaO ≥ 52%, MgO 3.5%~4%, SiO2 ≤ 2%, Fe2O3 ≤ 0.15%.

[0015] Preferably, the chemical composition of the wollastonite meets the following mass content requirements: CaO 45%~50%, SiO240%~52%, MgO 2%~5%, Al2O32%~5%, Fe2O3≤0.18%.

[0016] Preferably, the chemical composition of the kaolin meets the following mass content requirements: Al2O3≥26%, Fe2O3≤0.5%.

[0017] Preferably, the chemical composition of the pyrophyllite meets the following mass content requirements: SiO2≥67%, Al2O3≥20%, Fe2O3≤0.18%.

[0018] Preferably, the chemical composition of the bauxite meets the following mass content requirements: Al2O3≥65%, SiO2≤10%, Fe2O3≤3%.

[0019] Preferably, the chemical composition of the waste aluminum slag meets the following mass content requirements: Al2O3≥72%, SiO2≤8%, Fe2O3≤1.1%.

[0020] Preferably, the chemical composition of the barite meets the following mass content requirements: BaSO4≥80%, Fe2O3≤1%.

[0021] The invention further improves the quality of raw materials, reduces the burning temperature and improves the whiteness and comprehensive performance of white silicate cement clinker by controlling the chemical component content of each raw material.

[0022] Preferably, during the preparation of the modified high-magnesium waste rock, the temperature of the reaction system is 40°C to 80°C.

[0023] Preferably, the phosphate is selected from at least one of sodium tripolyphosphate, sodium hexametaphosphate, sodium phosphate or sodium pyrophosphate.

[0024] Preferably, the inorganic acid is selected from at least one of hydrochloric acid, sulfuric acid or nitric acid.

[0025] Preferably, the mass volume of the high-magnesium waste rock, the phosphate, the inorganic acid and the water is 100g:(2~6)g:(20~26)g:(800~1000)mL.

[0026] Preferably, the weak alkalinity is pH=7.5~8.5.

[0027] For example, an inorganic base is used to adjust the pH of the reaction system to 7.5-8.5.

[0028] The present invention changes the surface condition of the high-magnesium waste rock by limiting the preparation conditions of the modified high-magnesium waste rock, covers the surface of the high-magnesium waste rock with a layer of looser porous material, increases the specific surface area of ​​the white silicate cement clinker, and increases the diffuse reflection of the white silicate cement clinker to light.

[0029] Preferably, the specific surface area of ​​the white Portland cement clinker is 340 m 2 / kg~380m 2 / kg.

[0030] Preferably, the lime saturation coefficient KH of the white Portland cement clinker is 0.88-0.93, the aluminum content IM is 2.4-2.6, and the silicon content SM is 5.1-5.5.

[0031] In a second aspect, the present invention provides a method for preparing white Portland cement clinker, comprising the following steps: S1, weighing various raw materials according to the designed proportion, mixing and grinding limestone, modified high-magnesium waste rock, wollastonite, kaolin, pyrophyllite, bauxite, waste aluminum slag, borax and composite mineralizer to obtain a mixed raw material; S2, calcining the mixed raw material at 1350° C.-1400° C., and then cooling it by spraying water under reducing gas to obtain white Portland cement clinker.

[0032] The preparation method of white silicate cement clinker provided by the present invention has simple process, each raw material is cheap and easy to obtain, and the firing temperature is low; a specific cooling method is adopted, and under the action of reducing gas, Fe2O3 with strong coloring ability in the clinker is reduced to FeO with lighter color, and under the condition of rapid cooling (water spraying), the aluminate phase does not have time to dissolve into the iron phase in large quantities, and a small amount of C6AF2 type calcium aluminoferrite with lighter color is generated, and a large amount of minerals in the clinker exist in the form of fine crystals after rapid cooling, which increases the diffuse scattering of light, thereby improving the whiteness of the white silicate cement clinker. In addition, the water spraying rapid cooling method will not reduce the strength of the white silicate cement clinker.

[0033] Preferably, in S1, barite is also added during the mixing and grinding.

[0034] Preferably, in S2, the calcination time is 30 min to 45 min.

[0035] Preferably, in S2, the reducing gas is selected from natural gas or hydrogen.

[0036] For example, in S2, after cooling to below 100°C, drying and grinding are required. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0038] Example 1 The present embodiment provides a white silicate cement clinker, which is composed of the following raw materials in parts by weight: 40 parts of limestone, 40 parts of modified high-magnesium waste rock, 9 parts of wollastonite, 4 parts of kaolin, 5 parts of pyrophyllite, 1.2 parts of bauxite, 1.2 parts of waste aluminum slag, 0.1 parts of barite, 1.2 parts of borax and 0.9 parts of composite mineralizer.

[0039] The mass content of the chemical components of each raw material is shown in Table 1. The composite mineralizer includes CaF2, CaCl2, CuO and ZnO in a mass ratio of 4.5:7:0.9:0.6.

[0040] Table 1 Mass content of chemical components of each raw material (%)

[0041] In the table, “ / ” means no measurement was performed.

[0042] The preparation method of the above-mentioned white Portland cement clinker comprises the following steps: Sa, add 100g high-magnesium waste rock, 4g sodium tripolyphosphate and 20g hydrochloric acid into 900mL water, stir and react at 60℃ until pH=5.8, then use sodium hydroxide to adjust the pH of the reaction system to 8, and continue to react at 60℃ for 45min to obtain modified high-magnesium waste rock.

[0043] Sb, weigh the raw materials according to the designed ratio, mix and grind limestone, modified high-magnesium waste rock, wollastonite, kaolin, pyrophyllite, bauxite, waste aluminum slag, barite, borax and composite mineralizer to obtain a mixed raw material.

[0044] Sc, the mixed raw material was calcined at 1380℃ and kept at this temperature for 38min; then it was cooled by spraying water under natural gas, cooled to below 100℃, dried and ground, and the specific surface area was 371m 2 / kg of white Portland cement clinker.

[0045] After testing, the lime saturation coefficient of white silicate cement clinker is KH=0.91, aluminum rate IM=2.5, and silicon rate SM=5.3.

[0046] Example 2 The present embodiment provides a white silicate cement clinker, which is composed of the following raw materials in parts by weight: 38 parts of limestone, 42 parts of modified high-magnesium waste rock, 8 parts of wollastonite, 3 parts of kaolin, 4 parts of pyrophyllite, 1.3 parts of bauxite, 1.3 parts of waste aluminum slag, 0.2 parts of barite, 1.3 parts of borax and 1 part of composite mineralizer.

[0047] The mass content of the chemical components of each raw material is shown in Table 1. The composite mineralizer includes CaF2, CaCl2, CuO and ZnO in a mass ratio of 5:6:0.8:0.7.

[0048] The preparation method of the above-mentioned white Portland cement clinker comprises the following steps: Sa, add 100g high-magnesium waste rock, 6g sodium hexametaphosphate and 26g sulfuric acid into 800mL water, stir and react at 50℃ until pH=5.5, then use sodium hydroxide to adjust the pH of the reaction system to 7.5, and continue to react at 50℃ for 50min to obtain modified high-magnesium waste rock.

[0049] Sb, weigh the raw materials according to the designed ratio, mix and grind limestone, modified high-magnesium waste rock, wollastonite, kaolin, pyrophyllite, bauxite, waste aluminum slag, barite, borax and composite mineralizer to obtain a mixed raw material.

[0050] Sc, the mixed raw material was calcined at 1370℃ and kept warm for 40min; then cooled by spraying water under hydrogen, cooled to below 100℃, dried and ground, and the specific surface area was 363m 2 / kg of white Portland cement clinker.

[0051] After testing, the lime saturation coefficient of white silicate cement clinker is KH=0.9, aluminum rate IM=2.5, and silicon rate SM=5.2.

[0052] Example 3 The present embodiment provides a white silicate cement clinker, which is composed of the following raw materials in parts by weight: 42 parts of limestone, 38 parts of modified high-magnesium waste rock, 10 parts of wollastonite, 5 parts of kaolin, 3 parts of pyrophyllite, 1 part of bauxite, 1.5 parts of waste aluminum slag, 0.1 parts of barite, 1.5 parts of borax and 0.8 parts of composite mineralizer.

[0053] The mass content of the chemical components of each raw material is shown in Table 1. The composite mineralizer includes CaF2, CaCl2, CuO and ZnO in a mass ratio of 4:8:1:0.5.

[0054] The preparation method of the above-mentioned white Portland cement clinker comprises the following steps: Sa, add 100g high-magnesium waste rock, 2g sodium phosphate and 23g nitric acid into 1L water, stir and react at 80℃ until pH=6, then use sodium hydroxide to adjust the pH of the reaction system to 8.5, and continue to react at 80℃ for 30min to obtain modified high-magnesium waste rock.

[0055] Sb, weigh the raw materials according to the designed ratio, mix and grind limestone, modified high-magnesium waste rock, wollastonite, kaolin, pyrophyllite, bauxite, waste aluminum slag, barite, borax and composite mineralizer to obtain a mixed raw material.

[0056] Sc, the mixed raw material was calcined at 1400℃ and kept warm for 30min; then cooled by spraying water under natural gas, cooled to below 100℃, dried and ground, and the specific surface area was 376m 2 / kg of white Portland cement clinker.

[0057] After testing, the lime saturation coefficient of white silicate cement clinker is KH=0.93, aluminum rate IM=2.6, and silicon rate SM=5.5.

[0058] Example 4 The present embodiment provides a white silicate cement clinker, which is composed of the following raw materials in parts by weight: 40 parts of limestone, 41 parts of modified high-magnesium waste rock, 11 parts of wollastonite, 4 parts of kaolin, 6 parts of pyrophyllite, 1.5 parts of bauxite, 1 part of waste aluminum slag, 1 part of borax and 1.4 parts of composite mineralizer.

[0059] The mass content of the chemical components of each raw material is shown in Table 1 (excluding barite). The composite mineralizer includes CaF2, CaCl2, CuO and ZnO in a mass ratio of 4.5:7:0.9:0.8.

[0060] The preparation method of the above-mentioned white Portland cement clinker comprises the following steps: Sa, add 100g high-magnesium waste rock, 3g sodium pyrophosphate and 20g hydrochloric acid into 900mL water, stir and react at 40℃ until pH=5.5, then use sodium hydroxide to adjust the pH of the reaction system to 7.5, and continue to react at 40℃ for 60min to obtain modified high-magnesium waste rock.

[0061] Sb, weigh the raw materials according to the designed ratio, mix and grind limestone, modified high-magnesium waste rock, wollastonite, kaolin, pyrophyllite, bauxite, waste aluminum slag, borax and composite mineralizer to obtain a mixed raw material.

[0062] Sc, the mixed raw material was calcined at 1350℃ and kept at this temperature for 45min; then it was cooled by spraying water under hydrogen, cooled to below 100℃, dried and ground, and the specific surface area was 344m 2 / kg of white Portland cement clinker.

[0063] After testing, the lime saturation coefficient of white silicate cement clinker is KH=0.88, aluminum rate IM=2.4, and silicon rate SM=5.1.

[0064] Comparative Example 1 This comparative example provides a white silicate cement clinker, which is similar to Example 1, except that the modified high-magnesium waste rock is replaced with high-magnesium waste rock of the same quality. The remaining conditions are the same as those in Example 1 and will not be repeated.

[0065] The preparation method of the white silicate cement clinker is similar to that of Example 1, except that step Sa is omitted and the modified high-magnesium waste rock in Sb is replaced with high-magnesium waste rock. The remaining conditions are the same as those of Example 1 and will not be described in detail.

[0066] According to the test, the specific surface area of ​​white Portland cement clinker is 323m2 / kg, lime saturation coefficient KH=0.85, aluminum rate IM=2.2, silicon rate SM=5.1.

[0067] Comparative Example 2 This comparative example provides a white silicate cement clinker, which is similar to Example 1, except that the modified high-magnesium waste rock is replaced with limestone of the same quality. The remaining conditions are the same as those of Example 1 and will not be described in detail.

[0068] The preparation method of the white silicate cement clinker is similar to that of Example 1, except that step Sa is omitted and the modified high-magnesium waste rock in Sb is replaced by limestone. The remaining conditions are the same as those of Example 1 and will not be described in detail.

[0069] According to the test, the specific surface area of ​​white Portland cement clinker is 312m 2 / kg, lime saturation coefficient KH=0.82, aluminum rate IM=2.0, silicon rate SM=5.0.

[0070] Comparative Example 3 This comparative example provides a white silicate cement clinker, which is similar to Example 1, except that borax is omitted. The remaining conditions are the same as those in Example 1 and will not be described in detail.

[0071] The preparation method of the white silicate cement clinker is similar to that of Example 1, except that borax is omitted from Sb. The remaining conditions are the same as those of Example 1 and will not be described in detail.

[0072] According to the test, the specific surface area of ​​white Portland cement clinker is 327m 2 / kg, lime saturation coefficient KH=0.86, aluminum rate IM=2.2, silicon rate SM=5.1.

[0073] Comparative Example 4 This comparative example provides a white silicate cement clinker, which is similar to Example 1, except that the composite mineralizer is replaced with CaF2 (single mineralizer) of the same mass. The remaining conditions are the same as those of Example 1 and will not be described in detail.

[0074] The preparation method of the white silicate cement clinker is similar to that of Example 1, except that the composite mineralizer is replaced by CaF2 in Sb. The remaining conditions are the same as those of Example 1 and will not be described in detail.

[0075] According to the test, the specific surface area of ​​white Portland cement clinker is 345m 2 / kg, lime saturation coefficient KH=0.85, aluminum rate IM=2.3, silicon rate SM=5.2.

[0076] Comparative Example 5 This comparative example provides a method for preparing white silicate cement clinker, which is similar to Example 1, except that sodium tripolyphosphate is omitted in Sa. The remaining conditions are the same as those in Example 1 and will not be described in detail. (The raw material composition of the white silicate cement clinker is the same as that in Example 1 and will not be described in detail.) According to the test, the specific surface area of ​​white Portland cement clinker is 341m 2 / kg, lime saturation coefficient KH=0.87, aluminum rate IM=2.4, silicon rate SM=5.2.

[0077] Verification test The whiteness of the white Portland cement clinker provided in Examples 1 to 4 and Comparative Examples 1 to 5 was tested, and white cement was prepared according to the following ratio: 68% white Portland cement clinker, 28% limestone powder, and 4% mold gypsum. The strength of the prepared white cement was tested according to GB / T 2015-2017 "White Portland Cement", and the test results are shown in Table 2.

[0078] Table 2 Clinker whiteness and strength results of white cement

[0079] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A white Portland cement clinker, characterized in that: The raw materials include the following parts by weight: 38 to 42 parts of limestone, 38 to 42 parts of modified high-magnesium waste rock, 8 to 11 parts of wollastonite, 3 to 5 parts of kaolin, 3 to 6 parts of pyrophyllite, 1 to 1.5 parts of bauxite, 1 to 1.5 parts of waste aluminum slag, 1 to 1.5 parts of borax and 0.8 to 1.4 parts of composite mineralizer; The preparation method of the modified high-magnesium waste rock comprises the following steps: High-magnesium waste rock, phosphate and inorganic acid are added to water, stirred and reacted until the pH reaches 5.5~6, the pH of the reaction system is adjusted to be weakly alkaline, and the reaction is continued for 30min~60min to obtain modified high-magnesium waste rock.

2. The white Portland cement clinker according to claim 1, wherein The raw materials of the white Portland cement clinker also include 0.1 to 0.2 parts of barite.

3. The white Portland cement clinker according to claim 1 or 2, characterized in that The composite mineralizer includes CaF2, CaCl2, CuO and ZnO in a mass ratio of (4-5):(6-8):(0.8-1):(0.5-0.8).

4. The white Portland cement clinker according to claim 2, wherein The chemical composition of the limestone meets the following mass content requirements: CaO ≥ 51%, SiO2 ≤ 3%, MgO ≤ 2.5%, Fe2O3 ≤ 0.15%; The chemical composition of the high-magnesium waste rock meets the following mass content requirements: CaO ≥ 52%, MgO 3.5% to 4%, SiO2 ≤ 2%, Fe2O3 ≤ 0.15%; The chemical composition of the wollastonite meets the following mass content requirements: CaO 45%~50%, SiO2 40%~52%, MgO 2%~5%, Al2O3 2%~5%, Fe2O3≤0.18%; The chemical composition of the kaolin meets the following mass content requirements: Al2O3≥26%, Fe2O3≤0.5%; The chemical composition of the pyrophyllite meets the following mass content requirements: SiO2≥67%, Al2O3≥20%, Fe2O3≤0.18%; The chemical composition of the bauxite meets the following mass content requirements: Al2O3 ≥ 65%, SiO2 ≤ 10%, Fe2O3 ≤ 3%; The chemical composition of the waste aluminum slag meets the following mass content requirements: Al2O3 ≥ 72%, SiO2 ≤ 8%, Fe2O3 ≤ 1.1%; The chemical composition of the barite meets the following mass content requirements: BaSO4≥80%, Fe2O3≤1%.

5. The white Portland cement clinker according to claim 1, wherein The phosphate is selected from at least one of sodium tripolyphosphate, sodium hexametaphosphate, sodium phosphate or sodium pyrophosphate; The inorganic acid is selected from at least one of hydrochloric acid, sulfuric acid or nitric acid; The mass volume of the high-magnesium waste rock, the phosphate, the inorganic acid and the water is 100g:(2-6)g:(20-26)g:(800-1000)mL.

6. The white Portland cement clinker according to claim 1 or 5, characterized in that During the preparation of the modified high-magnesium waste rock, the temperature of the reaction system is 40°C to 80°C; The weak alkalinity is pH=7.5~8.

5.

7. The white Portland cement clinker according to claim 1, characterized in that The specific surface area of ​​the white Portland cement clinker is 340m 2 / kg~380m 2 / kg.

8. The white Portland cement clinker according to claim 1, wherein The white Portland cement clinker has a lime saturation coefficient KH of 0.88-0.93, an aluminum ratio IM of 2.4-2.6, and a silicon ratio SM of 5.1-5.

5.

9. The method for preparing white Portland cement clinker according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, weighing various raw materials according to the designed ratio, mixing and grinding limestone, modified high-magnesium waste rock, wollastonite, kaolin, pyrophyllite, bauxite, waste aluminum slag, borax and composite mineralizer to obtain a mixed raw meal; S2, calcining the mixed raw material at 1350° C. to 1400° C., and then cooling it by spraying water under reducing gas to obtain white Portland cement clinker.

10. The method for preparing white Portland cement clinker according to claim 9, wherein: In S1, barite needs to be added during the mixing and grinding; In S2, the calcination time is 30 min to 45 min; In S2, the reducing gas is selected from natural gas or hydrogen.