Antibacterial and durable ceramic glaze, ceramics having the glaze and preparation method thereof
By using potassium feldspar, quartz, nano silver oxide and calcium fluoride in ceramic glaze, and through the coordination of kaolin coordination and modified nano zinc oxide, combined with wet ball milling and sintering treatment, ceramic glaze is solved The problem of insufficient antibacterial properties and acid and alkali resistance stability has achieved coordinated improvements in the durability and ease of cleanliness of ceramic glaze.
Patent Information
- Application Number
- CN202411250135.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-06
AI Technical Summary
The existing ceramic glaze has shortcomings in antibacterial properties, durability, easy cleaning function and acid and alkali resistance stability, which is difficult to coordinate and improve, limiting the efficiency of the product.
Potassium feldspar, quartz, porcelain stone, nano silver oxide and calcium fluoride are used as matrix materials, and antibacterial and long-lasting ceramic glaze is prepared through kaolin coordination and coordination of modified nano zinc oxide, combined with wet ball milling and sintering treatment. Use regulators to improve the overall performance of ceramic products.
It significantly improves the antibacterial durability, easy cleaning function and acid-base resistance of ceramic glaze, and improves the overall performance and use efficiency of the product.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramics, and in particular to an antibacterial and durable ceramic glaze, a ceramic having the glaze and a preparation method thereof. Background Art
[0002] Generally speaking, the so-called ceramic glaze is a uniform glassy thin layer covering the surface of the ceramic body. For ceramic products, ceramic glaze can improve the performance and play a decorative role. During the preparation process, the ceramic glaze needs to be fully melted, dried after water quenching, and then crushed to obtain ceramic frit.
[0003] Existing ceramic glazes are used in ceramics, and the product's antibacterial performance is poor and durable, and the product's easy-to-clean function is poor. The product's antibacterial durability and easy-to-clean function are difficult to coordinate and improve, and the product's acid and alkali stability is poor, which further limits the product's use efficiency. Summary of the invention
[0004] In view of the defects of the prior art, the purpose of the present invention is to provide an antibacterial and long-lasting ceramic glaze, a ceramic having the glaze and a preparation method, so as to solve the problems raised in the above background technology.
[0005] The present invention solves the technical problem by adopting the following technical solution:
[0006] The present invention provides an antibacterial and durable ceramic glaze, comprising the following raw materials in parts by weight:
[0007] 35-40 parts of potassium feldspar, 10-15 parts of kaolin coordinator, 10-15 parts of quartz, 10-15 parts of porcelain stone, 4-7 parts of modified nano zinc oxide, 4-7 parts of nano silver oxide, and 3-5 parts of calcium fluoride.
[0008] Preferably, the preparation method of the kaolin coordinator is:
[0009] S01: Blending kaolin with a sufficient amount of 5% by mass sodium alginate solution to obtain kaolin solution;
[0010] S02: stirring and mixing the glass fiber and the sodium silicate solution in a weight ratio of 2:5, and then washing and drying to obtain the glass fiber adjusted with sodium silicate;
[0011] 3-5 parts of nano-silicon dioxide, 2-4 parts of lanthanum oxide, 4-6 parts of 5-7% by mass sodium dodecylbenzene sulfonate solution, and 1-2 parts of glass fiber adjusted with sodium silicate are fully blended to obtain a coordination solution;
[0012] S03: kaolin liquid and coordination liquid are mixed and ball-milled in a weight ratio of 5:3, with a ball-milling speed of 1000-1500 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a kaolin coordination agent.
[0013] Preferably, the mass fraction of the sodium silicate solution is 4-6%.
[0014] Preferably, the preparation method of the modified nano zinc oxide is:
[0015] S11: treating the nano zinc oxide with protons, with an irradiation power of 350-400W for 10-15 minutes, and then obtaining irradiated nano zinc oxide after the irradiation is completed;
[0016] S12: 5-8 parts of irradiated nano zinc oxide, 1-3 parts of nano silica sol, 2-5 parts of calcium sulfate whiskers, 4-7 parts of chitosan solution, and 1-3 parts of dopamine hydrochloride solution are mixed and fully ball-milled at a ball-milling speed of 1500 r / min for 1-2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain modified nano zinc oxide.
[0017] Preferably, the mass fraction of the chitosan solution is 2-5%; the mass fraction of the dopamine hydrochloride solution is 4-7%.
[0018] The present invention also provides a method for preparing ceramics, using the antibacterial and durable ceramic glaze, comprising the following steps:
[0019] Step 1: 25-30 parts of pyrophyllite, 20-25 parts of calcium feldspar, 10-15 parts of silicon carbide, 2-5 parts of magnesium silicate and 3-5 parts of spodumene are fully mixed, and then pressed at a pressure of 50 MPa to obtain a green body;
[0020] Step 2: spraying the regulating liquid on the surface of the green body until the surface of the green body is infiltrated to form an infiltrated body;
[0021] Step 3: wet-milling the raw materials of the antibacterial and durable ceramic glaze into a glaze slurry at a wet-milling speed of 1000 r / min for 2 h;
[0022] Step 4: applying the glaze slurry to the impregnated body, after the application is completed, sintering and improving treatment are performed, and after the treatment is completed, a ceramic with antibacterial and long-lasting ceramic glaze is obtained.
[0023] Preferably, the amount of glaze slurry applied is 200-220 g / m 2 ; The sintering temperature of the sintering improvement treatment is 1200-1250℃, and the sintering time is 1-2h.
[0024] Preferably, the preparation method of the regulating liquid is:
[0025] The flaky talc powder is first subjected to ultrasonic modification treatment in a sufficient amount of yttrium nitrate solution, and after the ultrasonic treatment is finished, the flaky talc powder is washed with water, filtered and dried to obtain dry flaky talc powder;
[0026] 1-3 parts of silane coupling agent KH550, 2-5 parts of sodium lignin sulfonate solution, 1-2 parts of citric acid and 2-4 parts of wood ash are mixed to obtain a conditioning agent; dry flaky talcum powder and the conditioning agent are mixed in a weight ratio of 2:5 to obtain a conditioning liquid.
[0027] Preferably, the mass fraction of the yttrium nitrate solution is 3-6%; the mass fraction of the sodium lignin sulfonate solution is 4-7%; the ultrasonic power of the ultrasonic modification treatment is 350-400W, and the ultrasonic time is 30-40min.
[0028] The invention also provides a ceramic prepared by the ceramic preparation method.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1. The antibacterial and durable ceramic glaze of the present invention uses potassium feldspar, quartz, porcelain stone, nano silver oxide and calcium fluoride as the matrix materials, and the antibacterial durability and easy-cleaning function of the obtained ceramic glaze product are coordinated and improved by adding kaolin coordinator and modified nano zinc oxide, and the acid and alkali stability of the product are significantly improved. At the same time, the ceramic of the present invention uses pyrophyllite, calcium feldspar, silicon carbide, magnesium silicate and spodumene to be fully pressed and formed, and then the liquid agent is adjusted to infiltrate the surface of the green body, and the ceramic glaze is coordinated and glazed, so that the performance of the obtained ceramic product is further improved;
[0031] 2. Kaolin coordinator: kaolin is first mixed with a sufficient amount of 5% by mass sodium alginate solution to obtain kaolin liquid, glass fiber and sodium silicate solution are coordinated and improved to obtain glass fiber adjusted by sodium silicate, nano-silicon dioxide, lanthanum oxide, 5-7% by mass sodium dodecylbenzene sulfonate solution and glass fiber adjusted by sodium silicate are fully blended to obtain a coordination liquid, the coordination liquid and kaolin liquid are coordinated and ball milled to improve, kaolin with a lamellar structure is coordinated with nano-silicon dioxide and other raw materials, and through the coordinated effect between the raw materials, the antibacterial durability and easy-to-clean performance of the product are coordinated and improved, and the acid and alkali stability of the product is significantly improved;
[0032] 3. Modified nano zinc oxide uses nano zinc dioxide to be irradiated with protons to stimulate the active performance of nano zinc dioxide, and then the irradiated nano zinc oxide, nano silica sol, calcium sulfate whiskers, chitosan solution, and dopamine hydrochloride solution are fully blended and ball-milled. The whisker structure is coordinated with nano zinc dioxide and other raw materials. Through the synergistic effect between the raw materials, the antibacterial durability of the product is further enhanced, and the antibacterial durability and easy-to-clean coordination are optimized. At the same time, the acid and alkali stability of the product is further improved;
[0033] 4. The regulating liquid adopts flaky talcum powder to be ultrasonically modified in a sufficient amount of yttrium nitrate solution to optimize the activity of the flaky talcum powder. At the same time, silane coupling agent KH550, sodium lignin sulfonate solution, citric acid and wood ash are fully blended to obtain a conditioning agent. The raw materials in the conditioning agent are blended and adjusted with each other to jointly optimize the flaky talcum powder. The flaky talcum powder is used as an intermediate carrier structure to further combine the green body and the glaze layer, thereby improving the overall strength performance of the ceramic product, and then the antibacterial durability and easy-to-clean performance of the product are coordinated and improved, and the acid and alkali stability of the product are significantly improved. DETAILED DESCRIPTION
[0034] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The antibacterial and durable ceramic glaze of this embodiment includes the following raw materials in parts by weight:
[0036] 35-40 parts of potassium feldspar, 10-15 parts of kaolin coordinator, 10-15 parts of quartz, 10-15 parts of porcelain stone, 4-7 parts of modified nano zinc oxide, 4-7 parts of nano silver oxide, and 3-5 parts of calcium fluoride.
[0037] The preparation method of the kaolin coordinating agent of this embodiment is:
[0038] S01: Blending kaolin with a sufficient amount of 5% by mass sodium alginate solution to obtain kaolin solution;
[0039] S02: stirring and mixing the glass fiber and the sodium silicate solution in a weight ratio of 2:5, and then washing and drying to obtain the glass fiber adjusted with sodium silicate;
[0040] 3-5 parts of nano-silicon dioxide, 2-4 parts of lanthanum oxide, 4-6 parts of 5-7% by mass sodium dodecylbenzene sulfonate solution, and 1-2 parts of glass fiber adjusted with sodium silicate are fully blended to obtain a coordination solution;
[0041] S03: kaolin liquid and coordination liquid are mixed and ball-milled in a weight ratio of 5:3, with a ball-milling speed of 1000-1500 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a kaolin coordination agent.
[0042] The mass fraction of the sodium silicate solution in this embodiment is 4-6%.
[0043] The preparation method of the modified nano zinc oxide of this embodiment is:
[0044] S11: treating the nano zinc oxide with protons, with an irradiation power of 350-400W for 10-15 minutes, and then obtaining irradiated nano zinc oxide after the irradiation is completed;
[0045] S12: 5-8 parts of irradiated nano zinc oxide, 1-3 parts of nano silica sol, 2-5 parts of calcium sulfate whiskers, 4-7 parts of chitosan solution, and 1-3 parts of dopamine hydrochloride solution are mixed and fully ball-milled at a ball-milling speed of 1500 r / min for 1-2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain modified nano zinc oxide.
[0046] The mass fraction of the chitosan solution in this embodiment is 2-5%; the mass fraction of the dopamine hydrochloride solution is 4-7%.
[0047] A method for preparing ceramics in this embodiment, using the antibacterial durable ceramic glaze, comprises the following steps:
[0048] Step 1: 25-30 parts of pyrophyllite, 20-25 parts of calcium feldspar, 10-15 parts of silicon carbide, 2-5 parts of magnesium silicate and 3-5 parts of spodumene are fully mixed, and then pressed at a pressure of 50 MPa to obtain a green body;
[0049] Step 2: spraying the regulating liquid on the surface of the green body until the surface of the green body is infiltrated to form an infiltrated body;
[0050] Step 3: wet-milling the raw materials of the antibacterial and durable ceramic glaze into a glaze slurry at a wet-milling speed of 1000 r / min for 2 h;
[0051] Step 4: applying the glaze slurry to the impregnated body, after the application is completed, sintering and improving treatment are performed, and after the treatment is completed, a ceramic with antibacterial and long-lasting ceramic glaze is obtained.
[0052] The amount of glaze slurry applied in this embodiment is 200-220g / m 2 ; The sintering temperature of the sintering improvement treatment is 1200-1250℃, and the sintering time is 1-2h.
[0053] The preparation method of the regulating liquid of this embodiment is:
[0054] The flaky talc powder is first subjected to ultrasonic modification treatment in a sufficient amount of yttrium nitrate solution, and after the ultrasonic treatment is finished, the flaky talc powder is washed with water, filtered and dried to obtain dry flaky talc powder;
[0055] 1-3 parts of silane coupling agent KH550, 2-5 parts of sodium lignin sulfonate solution, 1-2 parts of citric acid and 2-4 parts of wood ash are mixed to obtain a conditioning agent; dry flaky talcum powder and the conditioning agent are mixed in a weight ratio of 2:5 to obtain a conditioning liquid.
[0056] The mass fraction of the yttrium nitrate solution in this embodiment is 3-6%; the mass fraction of the sodium lignin sulfonate solution is 4-7%; the ultrasonic power of the ultrasonic modification treatment is 350-400W, and the ultrasonic time is 30-40min.
[0057] A ceramic of this embodiment is prepared by the ceramic preparation method.
[0058] Example 1: An antibacterial and durable ceramic glaze comprising the following raw materials in parts by weight:
[0059] 35 parts of potassium feldspar, 10 parts of kaolin coordinator, 10 parts of quartz, 10 parts of porcelain stone, 4 parts of modified nano zinc oxide, 4 parts of nano silver oxide, and 3 parts of calcium fluoride.
[0060] The preparation method of the kaolin coordinating agent of this embodiment is:
[0061] S01: Blending kaolin with a sufficient amount of 5% by mass sodium alginate solution to obtain kaolin solution;
[0062] S02: stirring and mixing the glass fiber and the sodium silicate solution in a weight ratio of 2:5, and then washing and drying to obtain the glass fiber adjusted with sodium silicate;
[0063] 3 parts of nano-silicon dioxide, 2 parts of lanthanum oxide, 4 parts of 5% by mass sodium dodecylbenzene sulfonate solution, and 1 part of glass fiber adjusted with sodium silicate are fully blended to obtain a coordination solution;
[0064] S03: kaolin liquid and coordination liquid are mixed and ball-milled in a weight ratio of 5:3, with a ball-milling speed of 1000 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a kaolin coordination agent.
[0065] The mass fraction of the sodium silicate solution in this embodiment is 4%.
[0066] The preparation method of the modified nano zinc oxide of this embodiment is:
[0067] S11: treating the nano zinc oxide with protons, with an irradiation power of 350 W for 10 minutes, and then completing the irradiation to obtain irradiated nano zinc oxide;
[0068] S12: 5 parts of irradiated nano zinc oxide, 1 part of nano silica sol, 2 parts of calcium sulfate whiskers, 4 parts of chitosan solution and 1 part of dopamine hydrochloride solution are mixed and fully ball-milled at a ball-milling speed of 1500 r / min for 1 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain modified nano zinc oxide.
[0069] The mass fraction of the chitosan solution in this embodiment is 2%; the mass fraction of the dopamine hydrochloride solution is 4%.
[0070] This embodiment also provides a method for preparing ceramics, using the antibacterial and durable ceramic glaze, the preparation method comprising the following steps:
[0071] Step 1: 25 parts of pyrophyllite, 20 parts of anorthite, 10 parts of silicon carbide, 2 parts of magnesium silicate and 3 parts of spodumene are fully mixed, and then pressed at a pressure of 50 MPa to obtain a green body;
[0072] Step 2: spraying the regulating liquid on the surface of the green body until the surface of the green body is infiltrated to form an infiltrated body;
[0073] Step 3: wet-milling the raw materials of the antibacterial and durable ceramic glaze into a glaze slurry at a wet-milling speed of 1000 r / min for 2 h;
[0074] Step 4: applying the glaze slurry to the impregnated body, after the application is completed, sintering and improving treatment are performed, and after the treatment is completed, a ceramic with antibacterial and long-lasting ceramic glaze is obtained.
[0075] The amount of glaze slurry applied in this embodiment is 200g / m 2 ; The sintering temperature of the sintering improvement treatment is 1200℃ and the sintering time is 1h.
[0076] The preparation method of the regulating liquid of this embodiment is:
[0077] The flaky talc powder is first subjected to ultrasonic modification treatment in a sufficient amount of yttrium nitrate solution, and after the ultrasonic treatment is finished, the flaky talc powder is washed with water, filtered and dried to obtain dry flaky talc powder;
[0078] 1 part of silane coupling agent KH550, 2 parts of sodium lignin sulfonate solution, 1 part of citric acid and 2 parts of wood ash are mixed to obtain a conditioning agent; dry flaky talcum powder and the conditioning agent are mixed in a weight ratio of 2:5 to obtain a conditioning liquid.
[0079] The mass fraction of the yttrium nitrate solution in this embodiment is 3%; the mass fraction of the sodium lignin sulfonate solution is 4%; the ultrasonic power of the ultrasonic modification treatment is 350W, and the ultrasonic time is 30 minutes.
[0080] This embodiment also provides a ceramic prepared by the ceramic preparation method.
[0081] Example 2: An antibacterial and durable ceramic glaze comprising the following raw materials in parts by weight:
[0082] 40 parts of potassium feldspar, 15 parts of kaolin coordinator, 15 parts of quartz, 15 parts of porcelain stone, 7 parts of modified nano zinc oxide, 7 parts of nano silver oxide, and 5 parts of calcium fluoride.
[0083] The preparation method of the kaolin coordinating agent of this embodiment is:
[0084] S01: Blending kaolin with a sufficient amount of 5% by mass sodium alginate solution to obtain kaolin solution;
[0085] S02: stirring and mixing the glass fiber and the sodium silicate solution in a weight ratio of 2:5, and then washing and drying to obtain the glass fiber adjusted with sodium silicate;
[0086] 5 parts of nano-silicon dioxide, 4 parts of lanthanum oxide, 6 parts of 7% by mass sodium dodecylbenzene sulfonate solution, and 2 parts of glass fiber adjusted with sodium silicate are fully blended to obtain a coordination solution;
[0087] S03: kaolin liquid and coordination liquid are mixed and ball-milled in a weight ratio of 5:3, with a ball-milling speed of 1500 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a kaolin coordination agent.
[0088] The mass fraction of the sodium silicate solution in this embodiment is 6%.
[0089] The preparation method of the modified nano zinc oxide of this embodiment is:
[0090] S11: treating the nano zinc oxide with proton irradiation, with an irradiation power of 400 W for 15 minutes, and then completing the irradiation to obtain irradiated nano zinc oxide;
[0091] S12: 8 parts of irradiated nano zinc oxide, 3 parts of nano silica sol, 5 parts of calcium sulfate whiskers, 7 parts of chitosan solution and 3 parts of dopamine hydrochloride solution are mixed and fully ball-milled at a ball-milling speed of 1500 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain modified nano zinc oxide.
[0092] The mass fraction of the chitosan solution in this embodiment is 5%; the mass fraction of the dopamine hydrochloride solution is 7%.
[0093] This embodiment also provides a method for preparing ceramics, using the antibacterial and durable ceramic glaze, comprising the following steps:
[0094] Step 1: 30 parts of pyrophyllite, 25 parts of anorthite, 15 parts of silicon carbide, 5 parts of magnesium silicate and 5 parts of spodumene are fully mixed, and then pressed at a pressure of 50 MPa to obtain a green body;
[0095] Step 2: spraying the regulating liquid on the surface of the green body until the surface of the green body is infiltrated to form an infiltrated body;
[0096] Step 3: wet-milling the raw materials of the antibacterial and durable ceramic glaze into a glaze slurry at a wet-milling speed of 1000 r / min for 2 h;
[0097] Step 4: applying the glaze slurry to the impregnated body, after the application is completed, sintering and improving treatment are performed, and after the treatment is completed, a ceramic with antibacterial and long-lasting ceramic glaze is obtained.
[0098] The amount of glaze slurry applied in this embodiment is 220g / m 2 ; The sintering temperature of the sintering improvement treatment is 1250℃ and the sintering time is 2h.
[0099] The preparation method of the regulating liquid of this embodiment is:
[0100] The flaky talc powder is first subjected to ultrasonic modification treatment in a sufficient amount of yttrium nitrate solution, and after the ultrasonic treatment is finished, the flaky talc powder is washed with water, filtered and dried to obtain dry flaky talc powder;
[0101] 3 parts of silane coupling agent KH550, 5 parts of sodium lignin sulfonate solution, 2 parts of citric acid and 4 parts of wood ash are mixed to obtain a conditioning agent; dry flaky talcum powder and the conditioning agent are mixed in a weight ratio of 2:5 to obtain a conditioning liquid.
[0102] The mass fraction of the yttrium nitrate solution in this embodiment is 6%; the mass fraction of the sodium lignin sulfonate solution is 7%; the ultrasonic power of the ultrasonic modification treatment is 400 W, and the ultrasonic time is 40 min.
[0103] This embodiment also provides a ceramic prepared by the ceramic preparation method.
[0104] Example 3: An antibacterial and durable ceramic glaze comprising the following raw materials in parts by weight:
[0105] 37.5 parts of potassium feldspar, 12.5 parts of kaolin coordinator, 12.5 parts of quartz, 12.5 parts of porcelain stone, 5.5 parts of modified nano zinc oxide, 5.5 parts of nano silver oxide, and 4 parts of calcium fluoride.
[0106] The preparation method of the kaolin coordinating agent of this embodiment is:
[0107] S01: Blending kaolin with a sufficient amount of 5% by mass sodium alginate solution to obtain kaolin solution;
[0108] S02: stirring and mixing the glass fiber and the sodium silicate solution in a weight ratio of 2:5, and then washing and drying to obtain the glass fiber adjusted with sodium silicate;
[0109] 4 parts of nano-silicon dioxide, 3 parts of lanthanum oxide, 5 parts of 6% by mass sodium dodecylbenzene sulfonate solution, and 1.5 parts of glass fiber adjusted with sodium silicate are fully blended to obtain a coordination solution;
[0110] S03: kaolin liquid and coordination liquid are mixed and ball-milled in a weight ratio of 5:3 at a ball-milling speed of 1250 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a kaolin coordination agent.
[0111] The mass fraction of the sodium silicate solution in this embodiment is 5%.
[0112] The preparation method of the modified nano zinc oxide of this embodiment is:
[0113] S11: treating the nano zinc oxide with protons, with an irradiation power of 370 W for 12.5 min, and then completing the irradiation to obtain irradiated nano zinc oxide;
[0114] S12: 6.5 parts of irradiated nano zinc oxide, 2 parts of nano silica sol, 3.5 parts of calcium sulfate whiskers, 5.5 parts of chitosan solution and 2 parts of dopamine hydrochloride solution are mixed and fully ball-milled at a ball-milling speed of 1500 r / min for 1.5 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain modified nano zinc oxide.
[0115] The mass fraction of the chitosan solution in this embodiment is 3.5%; the mass fraction of the dopamine hydrochloride solution is 5.5%.
[0116] This embodiment also provides a method for preparing ceramics, using the antibacterial and durable ceramic glaze, comprising the following steps:
[0117] Step 1: 27.5 parts of pyrophyllite, 22.5 parts of anorthite, 12.5 parts of silicon carbide, 3.5 parts of magnesium silicate and 4 parts of spodumene are fully mixed, and then pressed at a pressure of 50 MPa to obtain a green body;
[0118] Step 2: spraying the regulating liquid on the surface of the green body until the surface of the green body is infiltrated to form an infiltrated body;
[0119] Step 3: wet-milling the raw materials of the antibacterial and durable ceramic glaze into a glaze slurry at a wet-milling speed of 1000 r / min for 2 h;
[0120] Step 4: applying the glaze slurry to the impregnated body, after the application is completed, sintering and improving treatment are performed, and after the treatment is completed, a ceramic with antibacterial and long-lasting ceramic glaze is obtained.
[0121] The amount of glaze slurry applied in this example is 210 g / m 2 ; The sintering temperature of the sintering improvement treatment is 1225℃, and the sintering time is 1.5h.
[0122] The preparation method of the regulating liquid of this embodiment is:
[0123] The flaky talc powder is first subjected to ultrasonic modification treatment in a sufficient amount of yttrium nitrate solution, and after the ultrasonic treatment is finished, the flaky talc powder is washed with water, filtered and dried to obtain dry flaky talc powder;
[0124] 2 parts of silane coupling agent KH550, 3.5 parts of sodium lignin sulfonate solution, 1.5 parts of citric acid and 3 parts of wood ash are mixed to obtain a conditioning agent; dry flaky talcum powder and the conditioning agent are mixed in a weight ratio of 2:5 to obtain a conditioning liquid.
[0125] The mass fraction of the yttrium nitrate solution in this embodiment is 4.5%; the mass fraction of the sodium lignin sulfonate solution is 5.5%; the ultrasonic power of the ultrasonic modification treatment is 370W, and the ultrasonic time is 35min.
[0126] This embodiment also provides a ceramic prepared by the ceramic preparation method.
[0127] Comparative Example 1:
[0128] The difference from Example 3 is that no kaolin coordinator is added.
[0129] Comparative Example 2:
[0130] The difference from Example 3 is that the preparation method of the kaolin coordinator does not use coordinating liquid treatment.
[0131] Comparative Example 3:
[0132] The difference from Example 3 is that the glass fiber adjusted by sodium silicate is not added into the coordination liquid.
[0133] Comparative Example 4:
[0134] The difference from Example 3 is that no nano silicon dioxide or lanthanum oxide is added to the coordination solution.
[0135] Comparative Example 5:
[0136] The difference from Example 3 is that no kaolin liquid is added in the preparation of the kaolin coordinator.
[0137] Comparative Example 6:
[0138] The difference from Example 3 is that no modified nano zinc oxide is added.
[0139] Comparative Example 7:
[0140] The difference from Example 3 is that no calcium sulfate whiskers are added to the modified nano zinc oxide.
[0141] Comparative Example 8:
[0142] The difference from Example 3 is that no dopamine hydrochloride solution or nano silica sol is added to the modified nano zinc oxide.
[0143] Comparative Example 9:
[0144] The difference from Example 3 is that no conditioning liquid treatment was used.
[0145] Comparative Example 10:
[0146] The difference from Example 3 is that no dry flaky talc is added to the conditioning liquid.
[0147] Comparative Example 11:
[0148] The difference from Example 3 is that no silane coupling agent KH550 or wood ash is added to the regulating liquid.
[0149] The ceramic products of Examples 1-3 and Comparative Examples 1-11 were tested for their antibacterial durability and cleanability under normal conditions. The test results are shown in Table 1.
[0150] Table 1: Antimicrobial persistence and easy-to-clean test results
[0151]
[0152] From Table 1, we can conclude that:
[0153] The product of Example 3 of the present invention has significant antibacterial persistence performance under normal conditions, and the easy-to-clean performance effect and antibacterial persistence of the product can be improved in a coordinated manner;
[0154] The present invention does not add any of the following: kaolin coordinator, modified nano zinc oxide, or conditioning liquid treatment, and the performance of the product deteriorates significantly. The kaolin coordinator, modified nano zinc oxide, and conditioning liquid treatment are used, and the three are coordinated and coordinated to enhance the synergy, and the performance effect of the product is significant.
[0155] The preparation method of the kaolin coordinator does not use the coordinating liquid treatment, the glass fiber adjusted by sodium silicate is not added to the coordinating liquid, the nano silicon dioxide and lanthanum oxide are not added to the coordinating liquid, and the kaolin liquid is not added in the preparation of the kaolin coordinator. The performance of the product has a tendency to deteriorate. The kaolin coordinator obtained by the method of the present invention has the most obvious product performance effect;
[0156] No calcium sulfate whiskers were added to the modified nano zinc oxide, no dopamine hydrochloride solution and nano silica sol were added to the modified nano zinc oxide, no dry flaky talcum powder was added to the regulating liquid, and no silane coupling agent KH550 and wood ash were added to the regulating liquid. The performance of the products showed a trend of deterioration to varying degrees. Only the modified nano zinc oxide and regulating liquid obtained by the method of the present invention had the most significant performance effect of the product. The effects of other methods were not as obvious as those of the present invention.
[0157] The ceramic products of Examples 1-3 and Comparative Examples 1-11 were placed in 2% hydrochloric acid mist for 12 hours and then placed in 5% sodium hydroxide alkaline mist for 12 hours to test the acid and alkali stability of the products. The test results are shown in Table 2.
[0158] Table 2: Acid and alkali resistance stability test results
[0159]
[0160] As can be seen from Table 2, the present invention adopts kaolin coordinator, modified nano zinc oxide and regulating liquid for treatment, and the three are coordinated and matched, and the acid and alkali resistance of the product is remarkable. The performance of the kaolin coordinator, modified nano zinc oxide and regulating liquid obtained by different methods all tends to deteriorate to varying degrees. Only the raw material product obtained by the method of the present invention has the most remarkable performance effect.
[0161] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0162] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. An antibacterial and durable ceramic glaze, characterized in that: It includes the following raw materials in parts by weight: Potassium feldspar 35-40 parts, kaolin coordinator 10-15 parts, quartz 10-15 parts, porcelain stone 10-15 parts, modified nano zinc oxide 4-7 parts, nano silver oxide 4-7 parts, calcium fluoride 3-5 parts; The preparation method of the kaolin coordinating agent is: S01: Blending kaolin with a sufficient amount of 5% by mass sodium alginate solution to obtain kaolin solution; S02: stirring and mixing the glass fiber and the sodium silicate solution in a weight ratio of 2:5, and then washing and drying to obtain the glass fiber adjusted with sodium silicate; 3-5 parts of nano-silicon dioxide, 2-4 parts of lanthanum oxide, 4-6 parts of 5-7% by mass sodium dodecylbenzene sulfonate solution, and 1-2 parts of glass fiber adjusted with sodium silicate are fully blended to obtain a coordination solution; S03: kaolin liquid and coordination liquid are mixed and ball-milled in a weight ratio of 5:3, with a ball-milling speed of 1000-1500r / min for 2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a kaolin coordination agent; The preparation method of the modified nano zinc oxide is: S11: treating the nano zinc oxide with protons, with an irradiation power of 350-400W for 10-15 minutes, and then obtaining irradiated nano zinc oxide after the irradiation is completed; S12: 5-8 parts of irradiated nano zinc oxide, 1-3 parts of nano silica sol, 2-5 parts of calcium sulfate whiskers, 4-7 parts of chitosan solution, and 1-3 parts of dopamine hydrochloride solution are mixed and fully ball-milled at a ball-milling speed of 1500 r / min for 1-2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain modified nano zinc oxide.
2. The antibacterial long-lasting ceramic glaze according to claim 1, characterized in that: The mass fraction of the sodium silicate solution is 4-6%.
3. The antibacterial long-lasting ceramic glaze according to claim 1, characterized in that: The mass fraction of the chitosan solution is 2-5%; the mass fraction of the dopamine hydrochloride solution is 4-7%.
4. A method for preparing ceramics, using the antibacterial and durable ceramic glaze according to claim 1, characterized in that: The following steps are involved: Step 1: 25-30 parts of pyrophyllite, 20-25 parts of calcium feldspar, 10-15 parts of silicon carbide, 2-5 parts of magnesium silicate and 3-5 parts of spodumene are fully mixed, and then pressed at a pressure of 50 MPa to obtain a green body; Step 2: spraying the regulating liquid on the surface of the green body until the surface of the green body is infiltrated to form an infiltrated body; Step 3: wet-milling the raw materials of the antibacterial and durable ceramic glaze into a glaze slurry at a wet-milling speed of 1000 r / min for 2 h; Step 4: applying the glaze slurry to the impregnated body, and then performing sintering and improvement treatment. After the treatment is completed, a ceramic with antibacterial and durable ceramic glaze is obtained; The preparation method of the regulating liquid is as follows: The flaky talc powder is first subjected to ultrasonic modification treatment in a sufficient amount of yttrium nitrate solution, and after the ultrasonic treatment is finished, the flaky talc powder is washed with water, filtered and dried to obtain dry flaky talc powder; 1-3 parts of silane coupling agent KH550, 2-5 parts of sodium lignin sulfonate solution, 1-2 parts of citric acid and 2-4 parts of wood ash are mixed to obtain a conditioning agent; dry flaky talcum powder and the conditioning agent are mixed in a weight ratio of 2:5 to obtain a conditioning liquid.
5. The method for preparing ceramics according to claim 4, characterized in that: The amount of glaze applied is 200-220g / m 2 ; The sintering temperature of the sintering improvement treatment is 1200-1250℃, and the sintering time is 1-2h.
6. The method for preparing ceramics according to claim 4, characterized in that: The mass fraction of the yttrium nitrate solution is 3-6%; the mass fraction of the sodium lignin sulfonate solution is 4-7%; the ultrasonic power of the ultrasonic modification treatment is 350-400W, and the ultrasonic time is 30-40min.
7. A ceramic prepared by the method for preparing a ceramic according to any one of claims 4 to 6.