Gadolinium-doped high-energy-storage relaxation antiferroelectric sodium niobate-based ceramic material as well as preparation method and application thereof
By introducing Gd3+ ions into sodium niobate-based ceramics, the problems of complex composition and difficult preparation of sodium niobate-based relaxor antiferroelectric ceramics are solved, and their breakdown field strength and energy storage performance are improved, making them suitable for multilayer ceramic capacitors and high-power pulse capacitors.
Patent Information
- Application Number
- CN202410995935.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-24
AI Technical Summary
Existing sodium niobate-based relaxor antiferroelectric ceramics suffer from problems such as complex composition, difficult preparation, and Bi volatilization in practical applications, resulting in high production costs and affecting the stability and reliability of capacitors. Furthermore, their energy storage performance needs to be improved.
By introducing rare earth ions Gd3+ with small ionic radii into sodium niobate, the tolerance factor is reduced, the antiferroelectricity and relaxation behavior are enhanced, and the breakdown field strength is increased by reducing the grain size. Gadolinium-doped high-energy-storage-soothing, relaxable antiferroelectric sodium niobate-based ceramic materials are prepared using simple preparation methods such as wet ball milling, calcination, plasticizing and sintering processes.
It significantly improves the breakdown field strength, energy storage density, and energy storage efficiency of sodium niobate ceramic materials, making it suitable for multilayer ceramic capacitors and high-power pulse capacitors. It features high saturation polarization, low residual polarization, and high breakdown strength, making it suitable for extreme environments.
Smart Images

Figure CN118955130A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional ceramics, and in particular relates to a gadolinium-doped high-energy-storage relaxation antiferroelectric sodium niobate-based ceramic material and a preparation method and application thereof. Background Art
[0002] With the continuous increase in energy demand, the continuous consumption of fossil fuels and the escalation of environmental problems, improving the utilization efficiency of traditional energy and expanding the scope and application of new energy have become hot issues that researchers are paying more and more attention to in recent years. Compared with other energy storage materials, ceramic capacitors play an extremely important role in modern power and electronic systems due to their high power density, fast charge and discharge speed, and good cycle stability.
[0003] Antiferroelectric ceramic capacitors are one of the most promising ceramic capacitors. They have the advantages of low remanent polarization, high saturation polarization and high breakdown field. However, the current mainstream antiferroelectric ceramic capacitors contain a large amount of lead, which poses a threat to the ecological environment and human health. Therefore, it is necessary to develop lead-free ceramic capacitors with high energy storage performance and fast discharge performance. NaNbO3 (NN) is a typical lead-free antiferroelectric ceramic at room temperature. Due to its rich phase structure, large saturation polarization and small density, it is considered to be a potential dielectric energy storage material. However, unmodified sodium niobate ceramics have the disadvantages of large remanent polarization and low breakdown field. Therefore, how to improve the energy storage properties of sodium niobate-based ceramic materials has become a research hotspot in recent years.
[0004] At present, a lot of work is focused on improving the comprehensive energy storage properties of sodium niobate by solid solution with other strong relaxation components, mainly including two aspects: on the one hand, with BiFeO3, (Bi 0.5 Na 0.5 )TiO3 and other components solid solution to form relaxor antiferroelectric ceramics; on the other hand, with (Bi 0.5 Li 0.5 )TiO3 and other components are solid-dissolved to form relaxor ferroelectric ceramics. Relatively speaking, the modified sodium niobate-based relaxor antiferroelectric ceramics will have a higher energy storage density.
[0005] However, in practical applications, sodium niobate-based relaxor antiferroelectric ceramics often have problems such as complex components, difficult preparation, and volatilization of Bi elements, which greatly increases the production cost and has a negative impact on the stability and reliability of capacitors. Therefore, it is of great significance to develop sodium niobate-based relaxor antiferroelectric ceramics with simple components and no serious volatile elements. Summary of the invention
[0006] In view of the above technical problems, the present invention provides a gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material and its preparation method and application. 3+ On the one hand, it reduces the tolerance factor, which is conducive to enhancing its antiferroelectricity. On the other hand, it increases the disorder of the local structure of sodium niobate and enhances its relaxation behavior. 3+ The introduction of ions reduces the grain size and significantly improves the breakdown field strength of sodium niobate ceramic materials.
[0007] In a first aspect, the present invention provides a gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material, wherein the chemical composition of the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material is Na 1-3x G x NbO3; wherein 0.04<x<0.12, preferably 0.06≤x≤0.10, and more preferably 0.08.
[0008] Preferably, the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material has a breakdown electric field of 371-582 kV / cm and an energy storage density of 2.16-6.77 J / cm 3 , the energy storage efficiency is 32.8~83.8%; Preferably, the breakdown electric field is 534-582 kV / cm, and the energy storage density is 5.94-6.77 J / cm 3 , the energy storage efficiency is 81.0~83.8%.
[0009] In a second aspect, the present invention provides a method for preparing the above-mentioned gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material, the preparation method comprising the following steps: (1) Sodium carbonate, niobium pentoxide, and gadolinium oxide raw materials are mixed according to the chemical composition Na 1-3x G x The stoichiometric ratio of NbO3 is weighed, and the raw materials are mixed and calcined to obtain a ceramic raw material mixed powder; (2) mixing the ceramic raw material mixed powder with a binder, granulating, screening and molding to obtain a ceramic green body; (3) Extruding and sintering the ceramic green body to obtain the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material.
[0010] Preferably, the sodium carbonate, niobium pentoxide and gadolinium oxide raw materials are weighed using an electronic balance with an accuracy of 0.001 g; wherein the purity of sodium carbonate is 99.8%, the purity of niobium pentoxide is 99.93%, and the purity of gadolinium oxide is 99.99%.
[0011] Preferably, the raw materials are mixed by wet ball milling; the ball milling media are zirconia balls, zirconia columns and anhydrous ethanol, preferably the zirconia balls have a particle size of 6 mm, the zirconia columns have a size of 10 mm in diameter × 10 mm in height, and the number of each is half; the ball milling speed is 200 to 240 rpm; and the ball milling time is 4 to 6 hours.
[0012] Preferably, the calcination temperature is 1100-1200° C. and the calcination time is 4-5 hours.
[0013] Preferably, the binder is a polyvinyl alcohol aqueous solution with a concentration of 6-7wt.%; the amount of the binder added is 5-7wt% of the mass of the ceramic raw material powder, preferably 6-7wt%; The temperature of the plastic discharge is 700-800°C, and the time is 1-2 hours; preferably, the temperature of the plastic discharge is 800°C, and the time is 2 hours.
[0014] Preferably, the sintering temperature is 1200-1320°C, preferably 1260-1320°C, the sintering time is 2-4 hours, preferably 2-3 hours, and the sintering heating rate is 1-3°C / min, preferably 2°C / min.
[0015] In a third aspect, the present invention provides an application of the above-mentioned gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material in the preparation of energy storage ceramic components; wherein the energy storage ceramic component comprises: the above-mentioned gadolinium-doped high energy storage sodium niobate-based ceramic material, and electrodes distributed on the surface of the sodium niobate-based ceramic material.
[0016] In a fourth aspect, the present invention provides an application of the above-mentioned gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material in the preparation of multilayer ceramic capacitors and high-power pulse capacitors.
[0017] Beneficial Effects The gadolinium-doped high-energy storage sodium niobate-based ceramic material prepared in the present invention has the characteristics of high saturation polarization intensity, low residual polarization intensity, high breakdown strength, high energy storage density and efficiency; The preparation process provided in the present invention is simple, can work in extreme environments, and is suitable for the preparation and application of multilayer capacitors. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 X-ray diffraction patterns of the sodium niobate-based ceramic materials prepared in Examples 1-3 and Comparative Examples 1-2; Figure 2-6 Surface microscopic morphology of the sodium niobate-based ceramic materials prepared in Examples 1-3 and Comparative Examples 1-2; Figure 7-11The dielectric temperature spectra of the sodium niobate-based ceramic materials prepared in Examples 1-3 and Comparative Examples 1-2; Figure 12-14 This is a unipolar hysteresis loop diagram of the sodium niobate-based ceramic material prepared in Examples 1-3 of the present invention; Figure 15-16 This is a unipolar hysteresis loop diagram of the sodium niobate-based ceramic material prepared in Comparative Example 1-2 of the present invention; Fig.17 This is a graph showing the changes in energy storage density and energy storage efficiency of the sodium niobate-based ceramic materials prepared in Examples 1-3 and Comparative Examples 1-2. DETAILED DESCRIPTION
[0019] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.
[0020] First, the present invention provides a gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material. The chemical composition of the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material is Na 1-3x G x NbO3; wherein 0.04<x<0.12, preferably 0.06≤x≤0.10, and more preferably 0.08.
[0021] The present invention introduces a small ion radius rare earth ion Gd into sodium niobate. 3+ On the one hand, it reduces the material tolerance factor, which is conducive to enhancing its antiferroelectricity. On the other hand, it increases the disorder of the local structure of sodium niobate and enhances its relaxation behavior. 3+ The introduction of ions reduces the grain size and significantly improves the breakdown field strength of sodium niobate ceramic materials.
[0022] It should be noted that: (1) in terms of modification method, it is different from solid solution in pure sodium niobate (La 0.2 Nd 0.2 Sm 0.2 G 0.2 Bi 0.2 )(Mg 2 / 3 Nb 1 / 3 )O3 and other high entropy components and no vacancies are introduced. The modification method in this patent is to dope the A-site with a single element rare earth. 3+ Replace monovalent Na at A + In order to maintain charge balance, vacancies will be generated at the A position, which is conducive to stabilizing antiferroelectricity; (2) In terms of mechanism of action, the improvement of energy storage characteristics in conventional technical solutions mainly relies on the high entropy material's natural large lattice disorder, which is conducive to reducing the electric domain size, and the "hysteresis diffusion" effect helps to inhibit grain growth and obtain a smaller grain size. However, this patent mainly introduces Gd into the A position.3+ Radius smaller than Na + , which is beneficial to reduce the overall tolerance factor of ceramics, thereby stabilizing the AFE structure. 3+ and Na + The difference in ionic radius also causes local structural heterogeneity in the ceramic, reducing the size of the electric domain, which is helpful for inducing relaxation behavior and reducing P r It produces a promoting effect and at the same time introduces a cation vacancy at the A position to stabilize its antiferroelectricity.
[0023] The ceramic material obtained by introducing a specific content of Gd (0.04<x<0.12) into NaNbO3 has excellent temperature stability, energy storage characteristics (energy storage density and energy storage efficiency) and electrical properties, and is expected to be used in pulse power energy storage elements. If the value of x is too large, the dielectric constant will be significantly reduced, thereby reducing the maximum polarization intensity, and it is difficult to obtain excellent energy storage characteristics; if the value of x is too small, the hysteresis loop will show the shape of an antiferroelectric double hysteresis loop, with a large residual polarization intensity, which will reduce the energy storage density and efficiency.
[0024] In some embodiments, the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material has a breakdown electric field of 371 to 582 kV / cm and an energy storage density of 2.16 to 6.77 J / cm 3 , the energy storage efficiency is 32.8-83.8%; preferably, the breakdown electric field is 534-582 kV / cm, and the energy storage density is 5.94-6.77 J / cm 3 , the energy storage efficiency is 81.0~83.8%.
[0025] The following is an exemplary description of the preparation method of the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material provided by the present invention. The preparation method may include the following steps: First, sodium carbonate, niobium pentoxide, and gadolinium oxide are mixed according to the chemical composition Na 1-3x G x The stoichiometric ratio of NbO3 is weighed, and the raw materials are mixed and calcined to obtain a ceramic raw material mixed powder; Then, the ceramic raw material mixed powder is mixed with a binder, and granulated, sieved, and formed to obtain a ceramic green body; Finally, the ceramic green body is subjected to plastic removal and sintering to obtain the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material.
[0026] In some embodiments, the sodium carbonate, niobium pentoxide, and gadolinium oxide raw materials are weighed using an electronic balance with an accuracy of 0.001 g; wherein the purity of sodium carbonate is 99.8%, the purity of niobium pentoxide is 99.93%, and the purity of gadolinium oxide is 99.99%.
[0027] In some embodiments, the raw materials can be mixed by wet ball milling; the ball milling media can be zirconia balls, zirconia columns and anhydrous ethanol, preferably the zirconia balls have a particle size of 6 mm, the zirconia columns have a size of 10 mm in diameter × 10 mm in height, and the number of each is half; the ball milling speed can be 200 to 240 rpm; and the ball milling time can be 4 to 6 hours.
[0028] In some embodiments, the calcination temperature may be 1100-1200° C. and the calcination time may be 4-5 hours.
[0029] In some embodiments, the calcined ceramic raw material powder can also be finely ground; wherein, the fine grinding can use small-size (such as 1 mm) zirconium oxide balls and anhydrous ethanol as the medium, and the fine grinding time can be 6 hours.
[0030] In some embodiments, the particle size of the ceramic raw material mixed powder can be controlled to be 200 nm-1 μm.
[0031] In some embodiments, the binder may be a polyvinyl alcohol aqueous solution with a concentration of 6 to 7 wt. %; the binder may be added in an amount of 5 to 7 wt. % of the ceramic raw material powder, preferably 6 to 7 wt. %.
[0032] In some embodiments, the sieve may have a mesh size of 20-60, preferably 40 mesh.
[0033] In some embodiments, the temperature of the plastic discharge can be 700-800°C, and the time can be 1-2 hours; preferably, the plastic discharge temperature is 800°C, and the time is 2 hours.
[0034] In some embodiments, the sintering temperature may be 1200-1320°C, preferably 1260-1320°C, the sintering time may be 2-4 hours, preferably 2-3 hours, and the sintering heating rate may be 1-3°C / min, preferably 2°C / min.
[0035] The gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material obtained by the preparation method provided by the present invention can be used to prepare energy storage ceramic components. The energy storage ceramic components include: the gadolinium-doped high energy storage sodium niobate-based ceramic material and electrodes distributed on the surface of the sodium niobate-based ceramic material.
[0036] At the same time, the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material provided by the present invention can also be used to prepare multilayer ceramic capacitors (Multi-Layer Ceramic Capacitor, MLCC) and high-power pulse capacitors.
[0037] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention all belong to the scope of protection of the present invention. The specific process parameters of the following examples are also only examples within a suitable range, that is, those skilled in the art can make selections within a suitable range through the description of this article, and are not limited to the specific values exemplified below. If not specifically stated, the technical means used in the embodiments are conventional means well known to those skilled in the art.
[0038] Example 1
[0039] The preparation method of the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material provided in this embodiment comprises the following steps: (1) According to the molecular formula Na 1-3x G x NbO3 (x = 0.06) is used for batching calculation; the raw materials used include: sodium carbonate with a purity of 99.8% and a molecular weight of 84.007; niobium pentoxide with a purity of 99.93% and a molecular weight of 265.810; gadolinium oxide with a purity of 99.99% and a molecular weight of 362.5. An electronic balance is used for weighing, and the weighing accuracy is 0.001g; The weighed raw materials are mixed and put into a nylon can, anhydrous ethanol is added to the can to a level not higher than 2 / 3 of the can height, and the nylon can is placed on a planetary ball mill with zirconium oxide balls and zirconium oxide columns as media for mixing for 6 hours (the zirconium oxide balls used have a particle size of 6 mm, and the zirconium oxide columns have a size of 10 mm in diameter × 10 mm in height, and the number of each is half); then the raw materials are poured out and dried in a baking oven, and then sieved with a 40-mesh nylon sieve, and the sieved mixed powder is pressed into a cylinder with a size of 65 mm in diameter × 20 mm in height on a press; in an atmospheric atmosphere, the mixture is synthesized at 1100-1200° C. for 5 hours, and then the 40-mesh sieve is smashed, and the obtained powder is placed in a stirred mill with zirconium oxide balls with a diameter of 1 mm and anhydrous ethanol as media for grinding for 6 hours, and dried in a baking oven to obtain a ceramic raw material mixed powder; (2) adding a polyvinyl alcohol aqueous solution with a concentration of 7 wt.% to the obtained ceramic raw material mixed powder, wherein the amount of the polyvinyl alcohol aqueous solution added is 6.5% of the mass of the ceramic raw material mixed powder, and then granulating the mixture uniformly, passing through a 40-mesh sieve, and pressing the mixture into a cylindrical ceramic green body with a size of 13 mm in diameter and 1 mm in height; (3) The obtained cylindrical ceramic green body is molded, and the molded green body is sintered in an alumina crucible at a sintering temperature of 1300° C. for 2 hours. After naturally cooling to room temperature, the sample is taken out to obtain the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material.
[0040] Example 2
[0041] The preparation method of the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material provided in this embodiment refers to that in Example 1, the main difference is that: the molecular formula Na 1-3x G x In NbO3, x=0.08.
[0042] Example 3
[0043] The preparation method of the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material provided in this embodiment refers to that in Example 1, the main difference is that: the molecular formula Na 1-3x G x In NbO3, x=0.10.
[0044] Comparative Example 1
[0045] The preparation method of the ceramic material provided in this comparative example is similar to that in Example 1, except that: (1) the molecular formula Na 1-3x G x In NbO3, x=0.04; (2) the sintering temperature is 1320°C.
[0046] Comparative Example 2
[0047] The preparation method of the ceramic material provided in this comparative example is similar to that in Example 1, except that: (1) the molecular formula Na 1-3x G x In NbO3, x=0.12; (2) the sintering temperature is 1280°C.
[0048] Figure 1 The X-ray diffraction diagrams of the sodium niobate-based ceramic materials prepared in Examples 1-3 and Comparative Examples 1-2 are shown in FIG. 1. As can be seen from the diagrams, the sodium niobate-based ceramic materials prepared in Examples 1-3 and Comparative Examples 1-2 have no impurity phase.
[0049] The surface morphology of the ceramic was taken after chrome plating. Figure 2-6 The surface microscopic morphology of the sodium niobate-based ceramic materials prepared in Example 1-3 and Comparative Example 1-2 is shown in FIG. As can be seen from the figure, the surface of the sodium niobate-based ceramic materials prepared in Example 1-3 and Comparative Example 1-2 is dense.
[0050] The ceramics were ground and polished on both sides, and silver-plated electrodes were applied to test the electrical properties. Figure 7-11 The dielectric temperature spectra of the sodium niobate-based ceramic materials prepared in Examples 1-3 and Comparative Examples 1-2 are shown in the figure. As can be seen from the figure, with the addition of gadolinium, the dielectric peak moves toward the low temperature direction, gradually moves to below -100°C, and frequency dispersion occurs, indicating the emergence of relaxation behavior, and with the increase of gadolinium content, the dielectric constant of the sodium niobate-based ceramic at room temperature gradually decreases.
[0051] Figure 12-14 The unipolar hysteresis loop diagram of the sodium niobate-based ceramic material prepared in Examples 1-3 of the present invention. It can be seen from the figure that with the increase of Gd content, the hysteresis loop gradually transforms into a narrow relaxation type hysteresis loop. The breakdown electric fields of the sodium niobate-based ceramic materials prepared in Examples 1-3 are 536 kV / cm, 582 kV / cm and 565 kV / cm, respectively, and the maximum energy storage density is 5.94 J / cm 3 、6.77J / cm 3 and 6.55 J / cm 3 The energy storage efficiencies are 81.0%, 82.7% and 83.8% respectively.
[0052] Figure 15-16 The unipolar hysteresis loop diagram of the sodium niobate-based ceramic material prepared in Comparative Examples 1-2 of the present invention. It can be seen from the figure that the breakdown electric fields of the sodium niobate-based ceramic materials prepared in Comparative Examples 1-2 are 371 kV / cm and 465 kV / cm, respectively, and the maximum energy storage density is 2.16 J / cm 3 and 4.32 J / cm 3 The energy storage density of the two comparative examples is less than 5J / cm 3 , the energy storage efficiencies are 32.8% and 76.2% respectively.
[0053] Fig.17 The energy storage density and energy storage efficiency of the sodium niobate-based ceramic materials prepared in Examples 1-3 and Comparative Examples 1-2 are shown in the figure. As can be seen from the figure, the energy storage density of the sodium niobate-based ceramics prepared in Comparative Examples 1-2 with too low and too high gadolinium contents is significantly weaker than the energy storage density of the sodium niobate-based ceramics prepared in Examples 1-3 with moderate gadolinium contents. Therefore, the design of gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic materials can achieve high energy storage characteristics, and the gadolinium content has a certain moderate range.
[0054] Table 1 below shows the composition and properties of the sodium niobate-based ceramic materials prepared in Examples 1-3 and Comparative Examples 1-2 of the present invention: x Breakdown electric field Energy storage density Energy storage efficiency Example 1 0.06 536kV / cm <![CDATA[5.94J / cm 3 ]]> 81.0% Example 2 0.08 582kV / cm <![CDATA[6.77J / cm 3 ]]> 82.7% Example 3 0.10 565kV / cm <![CDATA[6.55J / cm 3 ]]> 83.8% Comparative Example 1 0.04 371kV / cm <![CDATA[2.16J / cm 3 ]]> 32.8% Comparative Example 2 0.12 465kV / cm <![CDATA[4.32J / cm 3 ]]> 76.2%
[0055] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.
Claims
1. A gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material, characterized in that: The chemical composition of the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material is Na 1-3x G x NbO3; wherein 0.04<x<0.12, preferably 0.06≤x≤0.10, and more preferably 0.
08.
2. The gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material according to claim 1, characterized in that: The gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material has a breakdown electric field of 371-582 kV / cm and an energy storage density of 2.16-6.77 J / cm 3 , the energy storage efficiency is 32.8~83.8%; Preferably, the breakdown electric field is 534-582 kV / cm, and the energy storage density is 5.94-6.77 J / cm 3 , the energy storage efficiency is 81.0~83.8%.
3. A method for preparing the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material according to claim 1 or 2, characterized in that: The preparation method comprises the following steps: (1) Sodium carbonate, niobium pentoxide, and gadolinium oxide raw materials are mixed according to the chemical composition Na 1-3x G x The stoichiometric ratio of NbO3 is weighed, and the raw materials are mixed and calcined to obtain a ceramic raw material mixed powder; (2) mixing the ceramic raw material mixed powder with a binder, granulating, screening and molding to obtain a ceramic green body; (3) Extruding and sintering the ceramic green body to obtain the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material.
4. The preparation method according to claim 3, characterized in that: The sodium carbonate, niobium pentoxide and gadolinium oxide raw materials are weighed using an electronic balance with an accuracy of 0.001 g; wherein the purity of sodium carbonate is 99.8%, the purity of niobium pentoxide is 99.93%, and the purity of gadolinium oxide is 99.99%.
5. The preparation method according to claim 3 or 4, characterized in that: The raw materials are mixed by wet ball milling; the ball milling media are zirconia balls, zirconia columns and anhydrous ethanol, preferably the zirconia balls have a particle size of 6 mm, the zirconia columns have a size of 10 mm in diameter × 10 mm in height, and the number of each is half; the ball milling speed is 200-240 rpm; and the ball milling time is 4-6 hours.
6. The preparation method according to any one of claims 3 to 5, characterized in that: The calcination temperature is 1100-1200° C. and the calcination time is 4-5 hours.
7. The preparation method according to any one of claims 3 to 6, characterized in that: The binder is a polyvinyl alcohol aqueous solution with a concentration of 6-7wt.%; the amount of the binder added is 5-7wt% of the mass of the ceramic raw material powder, preferably 6-7wt%; The temperature of the plastic discharge is 700-800°C, and the time is 1-2 hours; preferably, the temperature of the plastic discharge is 800°C, and the time is 2 hours.
8. The preparation method according to any one of claims 3 to 7, characterized in that: The sintering temperature is 1200-1320° C., preferably 1260-1320° C., the sintering time is 2-4 hours, preferably 2-3 hours, and the sintering heating rate is 1-3° C. / min, preferably 2° C. / min.
9. Use of the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material according to claim 1 or 2 in the preparation of energy storage ceramic components, characterized in that: The energy storage ceramic element comprises: the gadolinium-doped high energy storage sodium niobate-based ceramic material according to claim 1 or 2, and electrodes distributed on the surface of the sodium niobate-based ceramic material.
10. Use of the gadolinium-doped high energy storage relaxation antiferroelectric sodium niobate-based ceramic material according to claim 1 or 2 in the preparation of multilayer ceramic capacitors and high power pulse capacitors.
Citation Information
Patent Citations
High energy storage density ceramic capacitor dielectric medium and preparation method thereof
CN110511018A
Sodium niobate-based lead-free relaxation antiferroelectric energy storage ceramic capacitor and preparation method thereof
CN116313515A
High-energy-storage sodium niobate-based high-entropy ceramic material as well as preparation method and application thereof
CN117819964A
Dielectric Ceramic Material and Multilayer Ceramic Capacitor Using the Same
US20130250482A1