Silver niobate-based anti-ferroelectric ceramic with high energy storage density under low electric field and preparation method of silver niobate-based anti-ferroelectric ceramic
Through Bi3+/Ca2+ co-doping and solid phase reaction method, the problems of AgNbO3 ceramics are solved instability in the room temperature structure and insufficient breakdown electric field, and silver niobate-based antiferrometer with high energy storage density and high efficiency under low electric field are achieved. Electric ceramic preparation improves its performance in high energy storage applications.
Patent Information
- Application Number
- CN202411166013.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
AgNbO3 antiferroelectric ceramics have a ferrous electrical phase structure at room temperature, which leads to severe lag in the electrical hysteresis loop, which limits its development in applications of high energy storage efficiency. At the same time, high driving electric field can easily lead to ceramic breakdown failure, and it is necessary to improve the ceramics. Breakdown electric field and saturation polarization intensity.
Silver niobate antiferroelectric ceramics were modified by A-position Bi3+/Ca2+ co-doping, stabilizing its antiferroelectric structure to room temperature, enhancing saturation polarization strength and dielectric breakdown strength, and synthesizing by solid phase reaction method, and preparing Silver niobate-based antiferroelectric ceramics with high energy storage density at low electric fields.
The structural stability, saturation polarization strength and breakdown field strength of the ceramic are significantly improved, and a high effective energy density of 4.4J/cm3 and a 63% energy storage efficiency are achieved under a low electric field of 205kV/cm, and the process is simple. , does not contain toxic substances.
Smart Images

Figure CN119049882A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of dielectric energy storage ceramic materials, and in particular relates to a silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field and a preparation method thereof. Background Art
[0002] Dielectric capacitors are widely used in the field of high-power pulse devices due to their ultra-fast charge and discharge rates and ultra-high power density. However, the low energy density is the main reason that limits their use in terminal products with miniaturization and integration development requirements. 3 Although antiferroelectric ceramics have a high energy density, their effective energy density is relatively low compared to traditional lead-based antiferroelectric ceramic materials. This is mainly due to the fact that AgNbO 3 At room temperature, it has a ferroelectric phase structure, which will cause its hysteresis loop to lag severely, which is not conducive to obtaining high energy storage efficiency. It is necessary to try to adjust its antiferroelectric phase that is stable at high temperature to room temperature, so as to enhance the stability of its antiferroelectric structure. In addition, the ultra-high energy storage density reported so far is based on ultra-high driving electric fields (mainly between 400 and 800 kV / cm), but ultra-high driving electric fields are prone to ceramic breakdown failure, so while trying to increase the ceramic breakdown electric field, it is necessary to synergistically improve the saturation polarization strength of the ceramic. Summary of the invention
[0003] In order to solve the above technical problems, the present invention proposes a silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field and a preparation method thereof. 3+ / Ca 2+ Silver niobate antiferroelectric ceramics were modified by co-doping, and the M 2a and M 2b Phase stability to room temperature, significantly enhanced saturation polarization intensity D m and dielectric breakdown strength, increasing the forward reversal electric field E F and the reverse electric field E B , and effectively reduces E F and E B The difference between them greatly improves the energy storage capacity.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] One of the technical solutions of the present invention:
[0006] A silver niobate (AgNbO) with high energy storage density under low electric field 3 )-based antiferroelectric ceramics, whose general chemical formula is Ag (1-5x) Bi x Ca x NbO3 where \(0 \lt x \lt 0.02\).
[0007] The silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field in the present invention 3 is a lead-free antiferroelectric ceramic. The ceramic is a pure phase without the generation of impurity phases.
[0008] The second technical solution of the present invention:
[0009] The present invention also provides a preparation method of the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field. According to the chemical formula \(Ag_{1 - x}Bi_{x}Ca_{0.5}NbO_{3}\), (1-5x) Bi x Ca x NbO 3 where \(0 \lt x \lt 0.02\), raw materials \(Ag_{2}O\), \(Nb_{2}O_{5}\), 2 O, \(Nb\) 2 O 5 Bi 2 O 3 and \(CaCO_{3}\) 3 are weighed according to the stoichiometric ratio. Additionally, \(5x / 2\) mol of \(Ag_{2}O\) and \(x / 2\) mol of \(Bi_{2}O_{3}\) 2 O and \(x / 2\) mol Bi 2 O 3 are added to make up for the material loss caused by the volatilization of volatile elements during high-temperature sintering. The silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field is synthesized by the solid-phase reaction method.
[0010] Preferably, the preparation method of the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field includes the following steps:
[0011] According to the chemical formula \(Ag_{1 - x}Bi_{x}Ca_{0.5}NbO_{3}\), (1-5x) Bi x Ca x NbO 3 where \(0 \lt x \lt 0.02\), raw materials \(Ag_{2}O\), \(Nb_{2}O_{5}\), 2 O, \(Nb\) 2 O 5 Bi 2 O 3 and \(CaCO_{3}\) 3 are weighed according to the stoichiometric ratio. Additionally, \(5x / 2\) mol of \(Ag_{2}O\) and \(x / 2\) mol of \(Bi_{2}O_{3}\) 2 O and \(x / 2\) mol Bi 2 O 3 are added. The above raw materials are wet ball-milled, dried and sieved after ball-milling to obtain powder;
[0012] The powder is pre-sintered in an atmosphere with flowing \(O_{2}\) 2 to obtain pre-sintered powder;
[0013] The pre-burned powder is crushed, dried and sieved to obtain a powder with uniform particle size;
[0014] The powder material with uniform particle size is granulated and formed to obtain a ceramic green body;
[0015] The ceramic green body is subjected to debinding and sintering treatment to obtain the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field.
[0016] Preferably, in the method for preparing the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field, during wet ball milling, the mass ratio of raw material, grinding balls and ball milling medium is 1:(5-10):(1-1.5).
[0017] Preferably, in the method for preparing the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field, the ball milling medium is anhydrous ethanol, and the grinding ball is ZrO 2 Grinding ball.
[0018] Preferably, in the method for preparing the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field, the ball milling time during wet ball milling is 24 hours, and the ball milling speed is 250-350 rpm.
[0019] Preferably, in the method for preparing the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field, the drying temperature is 80-120° C., and the drying time is 12-36 h; more preferably, drying at 100° C. for 24 h.
[0020] Preferably, in the method for preparing the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field, the pre-sintering temperature is 850-900° C., the holding time is 3-6 hours, the heating rate is 5° C. / min, 2 The flow rate is 0.5L / min.
[0021] Preferably, in the preparation method of the silver niobate-based antiferroelectric ceramic with high energy storage density under the low electric field, the method of crushing the pre-burned powder is: placing the pre-burned powder in a nylon ball mill and performing wet planetary ball milling crushing, the ball milling time is 24 hours, the rotation speed during the ball milling crushing is 250-350rpm, and the powder particle size after ball milling is between 200 and 500nm.
[0022] Preferably, in the method for preparing the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field, when the dried pre-sintered powder is sieved, the mesh number of the sieve is between 200 and 300 meshes.
[0023] Preferably, in the method for preparing the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field, polyvinyl alcohol (PVA) aqueous solution is added during granulation; and the molding method is isostatic pressing.
[0024] Preferably, in the method for preparing the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field, the concentration of the PVA aqueous solution is 5-7wt%. If the concentration of the PVA aqueous solution is too low, the formed particles will have a higher porosity, which will reduce the hardness of the particles; if the concentration of the PVA aqueous solution is too high, for example, when the concentration of the PVA aqueous solution is 10wt%, the PVA is difficult to completely dissolve, and there is undissolved PVA in the solution, which will affect the uniformity and hardness of the ceramic.
[0025] Preferably, in the method for preparing the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field, the isostatic pressing pressure is 180-250 MPa, and the holding time is 1-3 min.
[0026] Preferably, in the preparation method of silver niobate-based antiferroelectric ceramics with high energy storage density under the low electric field, the debinding temperature is 500-600°C, and the debinding time is 1-2h; the debinding temperature and time have a significant impact on the ceramic properties. Incomplete debinding will cause internal cracks, delamination or cracking during the sintering process. At the same time, the residual carbon will affect the density of the sintered dielectric layer and the continuity of the internal electrode, thereby affecting the effective energy storage density, energy storage efficiency and reliability of the ceramic.
[0027] The sintering temperature is 1075-1090°C, the holding time is 3-6h, the heating rate during sintering is 5°C / min, 2 The flow rate is 0.5L / min. Sintering temperature and time are two key factors affecting the performance of ceramics. Sintering temperature has a significant effect on the performance of ceramics. Appropriate sintering temperature can increase the bulk density, flexural strength and hardness of ceramics, and reduce water absorption and porosity. Excessively high sintering temperature may cause abnormal growth of grains, thus affecting the performance of the material. Sintering time also has an important influence on the performance of ceramics. Appropriate sintering time can ensure that the ceramics achieve the ideal density and strength. If the sintering time is insufficient, the ceramics may not be fully densified, resulting in lower density and strength; and if the sintering time is too long, it may cause excessive growth of grains, affecting the microstructure and properties of the material. In addition to sintering temperature and time, the heating rate is also an important factor affecting the sintering results. During the sintering process, the microstructure and phase composition of the ceramics will change, and these changes are closely related to the sintering temperature, time and heating rate. In the early stage of sintering, the main manifestation is the formation and rapid growth of necks between particles. In the middle and late stages of sintering, the necks between particles grow further, and the shape of the pores gradually changes from irregular to nearly cylindrical, eventually forming dense ceramics.
[0028] More preferably, the preparation method of the silver niobate-based antiferroelectric ceramic with a high energy storage density under a low electric field is as follows:
[0029] (1)配料混合:根据化学通式Ag (1-5x) Bi x Ca x NbO 3 ,0<x<0.02,按化学计量比称取原料Ag 2 O、Nb 2 O 5 、Bi 2 O 3 和CaCO 3 ,额外添加5x / 2mol Ag 2 O和x / 2mol Bi 2 O 3 ,将称取的原料加入尼龙球磨罐中,进行湿式行星球磨,球磨后再进行干燥和过筛,得到混合均匀的粉体,其中原料、磨球与球磨介质的质量比为1:(5~10):(1~1.5),球磨介质为无水乙醇,磨球为ZrO 2 磨球,球磨时间为24h,球磨转速为250~350rpm,干燥的温度为80~120℃,干燥的时间为12~36h;
[0030] (2)有氧预烧:将上述混合均匀的粉体在通有流动O 2 气氛的管式烧结炉中进行850~900℃的高温预烧,保温时间为3~6h,升温速率为5℃ / min,O 2 流量为0.5L / min,得到预烧粉;
[0031] (3)二次破碎:将预烧粉置于尼龙球磨罐,进行湿式行星球磨破碎,球磨破碎时间为24h,球磨破碎的转速为250~350rpm;
[0032] (4)干燥:将球磨破碎后的预烧粉在鼓风干燥箱中于80~120℃下干燥12~36h,此步骤是为了使球磨破碎后的预烧粉充分干燥;
[0033] (5)过筛:将充分干燥的预烧粉过筛,筛网目数介于200~300目,得到粒度均匀的粉料;
[0034] (6) Granulation and molding: Add a PVA (polyvinyl alcohol) aqueous solution to the above powder, add deionized water, heat and stir until dry, grind to obtain the powder required for steel mold pressing, and then use the steel mold and cold isostatic press to press and mold to obtain a ceramic green body (which is a round piece with a diameter of 10 mm). The concentration of the PVA aqueous solution is 5 to 7 wt%, the pressing pressure is 180 to 250 MPa, and the pressure holding time is 1 to 3 min;
[0035] (7) Debinding and sintering: Place the ceramic green body in a flowing O 2 The tube sintering furnace is used for debinding at 500-600℃ for 1-2h. After debinding, it is sintered into porcelain at a high temperature of 1075-1090℃ for 3-6h. The heating rate during sintering is 5℃ / min. 2 The flow rate is 0.5 L / min, and a dense ceramic is obtained, that is, a silver niobate-based antiferroelectric ceramic with high energy storage density under a low electric field.
[0036] A position Bi 3+ Doping can significantly enhance the AgNbO 3 The antiferroelectric structure stability of antiferroelectric ceramics effectively reduces the forward and reverse reversal electric fields (E F and E B ), and Bi 3+ Doping can promote the orbital hybridization effect between Bi 6s and O 2p orbitals, inducing a further increase in the saturation polarization intensity, thereby improving the energy storage density and efficiency. 2+ Doping can effectively refine the grains, which is conducive to further improving the breakdown field strength. 3+ The enhancement effect of doping on the phase structure stability, saturation polarization intensity, and energy storage efficiency of antiferroelectric ceramics, as well as the Ca 2+ The doping has an advantageous effect on improving the breakdown field strength. In the present invention, Bi 3+ / Ca 2+ The co-doping and volatile element compensation strategy successfully prepared a nanostructured ... 3 AgNbO with high effective energy density 3 Based antiferroelectric ceramics.
[0037] The third technical solution of the present invention:
[0038] The present invention also provides the use of the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field in the preparation of dielectric energy storage capacitors.
[0039] The fourth technical solution of the present invention:
[0040] The present invention also provides a method for preparing a dielectric energy storage capacitor, comprising grinding and flattening the two surfaces of the silver niobate-based antiferroelectric ceramic with high energy storage density under a low electric field in the thickness direction (i.e., perpendicular to the diameter direction of the ceramic sheet) to form a ceramic sheet of equal thickness, printing silver paste on the surface of the ceramic sheet of equal thickness, and obtaining the dielectric energy storage capacitor after drying and electrode sintering.
[0041] In the present invention, after grinding, it is necessary to ensure that the thickness between the two surfaces perpendicular to the diameter direction of the ceramic sheet is equal and the two surfaces are parallel to each other, otherwise the results obtained from the electrical performance test are inaccurate.
[0042] Preferably, in the method for preparing the dielectric energy storage capacitor, the electrode diameter of the ceramic sheet with equal thickness is 2 to 4 mm and is circular.
[0043] Preferably, in the method for preparing the dielectric energy storage capacitor, the electrode sintering temperature is 500-600° C., and the holding time is 15-30 min.
[0044] Compared with the prior art, the present invention has the following advantages and technical effects:
[0045] (1) The A-site Bi provided by the present invention 3+ / Ca 2+ The co-doping strategy can effectively transform silver niobate antiferroelectric ceramics into high-temperature stable M 2a and M 2b The antiferroelectric phase is stable to room temperature, which significantly enhances the structural stability of silver niobate antiferroelectric ceramics at room temperature.
[0046] (2) The silver niobate-based antiferroelectric ceramic provided by the present invention has high saturation polarization intensity, high breakdown field strength, and small hysteresis loop hysteresis, and can obtain up to 4.4 J / cm under low electric field conditions of 205 kV / cm 3 The effective energy storage density and energy storage efficiency of 63% are achieved.
[0047] (3) The silver niobate-based antiferroelectric ceramic provided by the present invention is prepared by a high-temperature solid phase method, which has a simple and efficient process. The obtained ceramic does not contain volatile toxic substances such as Pb and is environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0049] Figure 1Figure 2 is the XRD spectra and lattice parameters of antiferroelectric ceramics of AN (x=0, comparative example 1), ABCN1 (x=0.006, example 1) and ABCN2 (x=0.019, example 2), wherein (a) is the XRD spectrum of AN, ABCN1 and ABCN2, (b) and (c) are partial enlarged views of (a), and (d) and (e) are the variation curves of lattice parameters a, b and c with components.
[0050] Figure 2 Surface morphology SEM photos and average grain sizes of antiferroelectric ceramics of AN (Comparative Example 1), ABCN1 (Example 1) and ABCN2 (Example 2), where (a), (b) and (c) are SEM photos of AN, ABCN1 and ABCN2, respectively, and (d), (e) and (f) are average grain sizes of AN, ABCN1 and ABCN2, respectively.
[0051] Figure 3 Dielectric temperature spectra of dielectric energy storage capacitors made of antiferroelectric ceramics AN (Comparative Example 1), ABCN1 (Example 1) and ABCN2 (Example 2), where (a) is AN, (b) is ABCN1, and (c) is ABCN2.
[0052] Figure 4 Ferroelectric hysteresis loops of dielectric energy storage capacitors made of antiferroelectric ceramics AN (Comparative Example 1), ABCN1 (Example 1) and ABCN2 (Example 2), where (a) is AN, (b) is ABCN1, and (c) is ABCN2. DETAILED DESCRIPTION
[0053] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0054] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0055] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. Although this invention has been described only with reference to preferred methods and materials, any methods and materials similar or equivalent to those described herein can also be used in the practice or testing of this invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In case of conflict with any incorporated document, the content of this specification shall prevail.
[0056] Without departing from the scope or spirit of the present invention, various modifications and variations can be made to the specific embodiments of the description of the present invention, which will be apparent to those skilled in the art. Other embodiments obtained from the description of the present invention will be apparent to those skilled in the art. The description of the present invention and the examples are merely exemplary.
[0057] Regarding the use of "comprising", "including", "having", "containing", etc. herein, they are all open-ended terms, meaning including but not limited to.
[0058] All raw materials used in the examples of the present invention are obtained by purchasing from the market.
[0059] In some embodiments of the present invention, there is provided a silver niobate (AgNbO 3 )-based antiferroelectric ceramic having a high energy storage density under a low electric field, and its chemical general formula is Ag (1-5x) Bi x Ca x NbO 3 , 0 < x < 0.02.
[0060] In some embodiments of the present invention, there is also provided a preparation method of the above silver niobate-based antiferroelectric ceramic having a high energy storage density under a low electric field:
[0061] (1)配料混合:根据化学通式Ag (1-5x) Bi x Ca x NbO 3 , 0 < x < 0.02,按化学计量比称取原料Ag 2 O、Nb 2 O 5 、Bi 2 O 3 和CaCO 3 ,额外添加5x / 2mol Ag 2 O和x / 2mol Bi 2 O 3The weighed raw materials are added into a nylon ball mill, and wet planetary ball milling is performed. After ball milling, the raw materials are dried and sieved to obtain a uniformly mixed powder, wherein the mass ratio of raw materials, grinding balls and ball milling medium is 1:(5-10):(1-1.5), the ball milling medium is anhydrous ethanol, and the grinding balls are ZrO 2 grinding balls, the ball milling time is 24 hours, the ball milling speed is 250-350 rpm, the drying temperature is 80-120°C, and the drying time is 12-36 hours. For example, the mass ratio of raw materials, grinding balls and ball milling media can be 1:5:1.5, 1:10:1, 1:7:1, 1:6:1.2, 1:8:1.1 or 1:10:1.5. Good ball milling efficiency can be achieved within the above ranges;
[0062] (2) Oxygen pre-calcination: The uniformly mixed powders are calcined in a stream of flowing oxygen. 2 The high temperature pre-sintering is carried out at 850-900℃ in a tubular sintering furnace with an atmosphere of 3-6h and a heating rate of 5℃ / min. 2 The flow rate is 0.5L / min, and a pre-burned powder is obtained. For example, the pre-burning temperature can be 850°C, 855°C, 856°C, 857°C, 858°C, 859°C, 860°C, 870°C, 875°C, 880°C, 885°C, 890°C, 895°C or 900°C, and the pre-burning time can be 3h, 3.2h, 3.5h, 4h, 4.5h, 5h or 6h. Within the above pre-burning temperature and time range, organic impurities in the raw materials can be effectively removed, the solid phase reaction can be promoted, a relatively pure main crystal phase can be obtained, and the microstructure and properties of the final sintered body can be affected;
[0063] (3) Secondary crushing: The calcined powder is placed in a nylon ball mill and subjected to wet planetary ball milling. The ball milling time is 24 hours and the speed of the ball milling is 250-350 rpm.
[0064] (4) Drying: The pre-burned powder after ball milling is dried in a blast drying oven at 80-120°C for 12-36 hours. This step is to fully dry the pre-burned powder after ball milling;
[0065] (5) Sieving: Sieve the fully dried pre-burned powder through a sieve with a mesh size of 200 to 300 to obtain a powder with uniform particle size;
[0066] (6) Granulation and molding: PVA aqueous solution is added to the above powder, and deionized water is added, heated and stirred until dry, and the powder required for steel mold pressing is obtained after grinding, and then pressed and molded using a steel mold and a cold isostatic press to obtain a ceramic green body (which is a round piece with a diameter of 10 mm). The concentration of the PVA aqueous solution is 5-7wt%, the pressing pressure is 180-250MPa, and the holding time is 1-3min. Within the above pressure range, a green body with a higher density can be obtained. The high-density green body is easier to form a uniform microstructure during the sintering process, the grains are finer, and the porosity is reduced, thereby improving the mechanical strength, hardness and energy storage efficiency of the ceramic;
[0067] (7) Debinding and sintering: Place the ceramic green body in a flowing O 2 The tube sintering furnace is used for debinding at 500-600℃ for 1-2h. After debinding, it is sintered into porcelain at a high temperature of 1075-1090℃ for 3-6h. The heating rate during sintering is 5℃ / min. 2 The flow rate is 0.5 L / min, and a dense ceramic is obtained, that is, a silver niobate-based antiferroelectric ceramic with high energy storage density under a low electric field.
[0068] In some embodiments of the present invention, there is also provided the use of the above-mentioned silver niobate-based antiferroelectric ceramics with high energy storage density under low electric field in the preparation of dielectric energy storage capacitors.
[0069] In some embodiments of the present invention, a method for preparing the above-mentioned dielectric energy storage capacitor is also provided: the two surfaces of the above-mentioned silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field are polished and flattened to form a ceramic sheet of equal thickness, silver paste is printed on the surface of the ceramic sheet of equal thickness, and after drying and electrode sintering, wherein the electrode sintering temperature is 500-600°C, the insulation time is 15-30 minutes, and the diameter of the silver electrode is 2-4 mm, to obtain the dielectric energy storage capacitor.
[0070] The technical solution of the present invention is further illustrated by the following embodiments.
[0071] Example 1
[0072] Ag 0.97 Bi 0.006 Ca 0.006 NbO 3 Preparation of (ABCN1) ceramics
[0073] Ag 2 O、Nb 2 O 5 、Bi 2 O 3 and CaCO 3As raw materials, it was weighed according to the stoichiometric ratio, and 0.015 mol Ag was added during weighing. 2 O and 0.003 mol Bi 2 O 3 , in order to make up for the material loss caused by the volatilization of volatile elements during high temperature sintering. Then, anhydrous ethanol was used as the ball milling medium. 2 The powder was mixed by planetary ball milling in a nylon ball mill with grinding balls for 24 h at a speed of 300 rpm. The mass ratio of raw materials, grinding balls and ball milling media was 1:7:1. The powder after ball milling was dried at 100 °C for 24 h. After the powder was dried, it was placed in a corundum ark and passed with flowing O 2 The sintering temperature was 880℃ for 4h in a tubular sintering furnace with a heating rate of 5℃ / min. 2 The flow rate is 0.5L / min to obtain pre-burned powder. After cooling, the pre-burned powder is placed in a nylon ball mill and subjected to wet planetary ball milling. Anhydrous ethanol is used as the ball milling medium, and the pre-burned powder is ball milled for 24 hours at a speed of 300rpm. The pre-burned powder after ball milling is dried in a blast drying oven at 100°C for 24 hours, and the dried pre-burned powder is sieved with a mesh size of 200 mesh. After the above drying and sieving treatment, 5wt% PVA solution is added to the above powder for granulation. The amount of PVA added relative to the mass of the powder is 1.5%, and deionized water is added. Heat and stir until dry. After grinding, the powder required for steel mold pressing is obtained, and then the steel mold and cold isostatic press are used for pressing. The isostatic pressure is 200MPa, and the holding time is 1min. It is pressed into a disc (i.e., ceramic green body) with a diameter of 10mm and a thickness of 1mm. Finally, the obtained disc-shaped ceramic green body is placed in a flowing O 2 The sintering furnace was heated to 600℃ for 2h and then heated to 1080℃ for 6h. The heating rate was 5℃ / min. 2 The flow rate was 0.5 L / min, and a dense silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field was obtained, which was recorded as ABCN1.
[0074] Example 2
[0075] Ag 0.905 Bi 0.019 Ca 0.019 NbO 3 Preparation of (ABCN2) ceramics
[0076] Ag 2 O、Nb 2 O 5 、Bi 2 O 3 and CaCO 3As raw materials, it was weighed according to the stoichiometric ratio, and 0.0475 mol Ag was added during weighing. 2 O and 0.0095 mol Bi 2 O 3 , in order to make up for the material loss caused by the volatilization of volatile elements during high temperature sintering. Then, anhydrous ethanol was used as the ball milling medium. 2 The powder was mixed by planetary ball milling in a nylon ball mill with grinding balls for 24 h at a speed of 300 rpm. The mass ratio of raw materials, grinding balls and ball milling media was 1:5:1.5. The powder after ball milling was dried at 120 °C for 12 h. After the powder was dried, it was placed in a corundum ark and passed through a flowing O 2 The sintering temperature was 880℃ for 6h in a tubular sintering furnace with a heating rate of 5℃ / min. 2 The flow rate is 0.5L / min to obtain pre-burned powder. After cooling, the pre-burned powder is placed in a nylon ball mill and subjected to wet planetary ball milling. Anhydrous ethanol is used as the ball milling medium, and the pre-burned powder is ball milled for 24 hours at a speed of 300rpm. The pre-burned powder after ball milling is dried in a blast drying oven at 120°C for 12 hours, and the dried pre-burned powder is sieved with a mesh size of 250. After the above drying and sieving treatments, 6wt% PVA solution is added to the above powder for granulation. The amount of PVA added relative to the mass of the powder is 1.5%, and deionized water is added. Heat and stir until dry. After grinding, the powder required for steel mold pressing is obtained, and then the steel mold and cold isostatic press are used for pressing. The isostatic pressure is 180MPa, and the holding time is 3min. It is pressed into a disc (i.e., ceramic green body) with a diameter of 10mm and a thickness of 1mm. Finally, the obtained disc-shaped ceramic green body is placed in a flowing O 2 The sintering was carried out in a tubular sintering furnace with an atmosphere of 600 °C for debinding for 2 h, and then the temperature was continuously raised to 1075 °C for sintering for 6 h. The heating rate during sintering was 5 °C / min. 2 The flow rate was 0.5 L / min, and a dense silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field was obtained, which was recorded as ABCN2.
[0077] Comparative Example 1
[0078] AgNbO 3 (AN) Preparation of Ceramics
[0079] Ag 2 O and Nb 2 O 5 As raw materials, they were weighed according to the stoichiometric ratio, and then anhydrous ethanol was used as the ball milling medium. 2 The powder was mixed by planetary ball milling in a nylon ball mill with grinding balls for 24 h at a speed of 300 rpm. After the powder was dried, it was placed in a corundum ark and 2The powder was calcined at 850°C for 6 hours in a tubular sintering furnace with a low atmosphere. After cooling, the calcined powder was milled for 24 hours at a speed of 300 rpm using anhydrous ethanol as a ball milling medium. After drying and sieving, 5 wt% PVA solution was added to the fine calcined powder for granulation, and then molded under an isostatic pressure of 180 MPa to form a disc with a diameter of 10 mm and a thickness of about 1 mm. The holding time was 1 minute. Finally, the obtained round green body was placed in a flowing O 2 The AN ceramic sheet was obtained by debinding at 600°C for 2 h in a tubular sintering furnace with a high temperature and low atmosphere, and then continuing to heat up to 1090°C for 6 h.
[0080] Comparative Example 2
[0081] Same as Example 1, except that no additional 0.015 mol Ag was added 2 O and 0.003 mol Bi 2 O 3 .
[0082] Since no additional Ag was added in this comparative example 2 O and Bi 2 O 3 Although ceramics can be successfully fired, the volatilization of Bi and Ag during the high-temperature sintering process will cause a large number of oxygen vacancies and lattice defects in the ceramic body, resulting in increased dielectric loss and enhanced domain reversal hysteresis, affecting the improvement of ceramic energy storage density and energy storage efficiency.
[0083] Comparative Example 3
[0084] Same as Example 1, except that the concentration of the PVA solution is 10 wt %.
[0085] Since the concentration of the PVA solution in this comparative example is relatively high, there is undissolved PVA in the solution, and local holes will be generated after the ceramic is fired, affecting the uniformity and density of the ceramic. When a higher electric field is applied, local dielectric breakdown is obvious.
[0086] The physical phases of the antiferroelectric ceramics prepared in Example 1, Example 2 and Comparative Example 1 were characterized respectively. Figure 1 The XRD patterns and unit cell parameters of the antiferroelectric ceramics AN (Comparative Example 1), ABCN1 (Example 1) and ABCN2 (Example 2) show that the prepared ceramics are all pure phases without the generation of impurities. 3+ / Ca 2+ With the increase of doping amount, the unit cell parameters of the ceramics changed significantly and the diffraction peak shifted significantly.
[0087] The microscopic morphologies of the antiferroelectric ceramics prepared in Example 1, Example 2 and Comparative Example 1 were characterized respectively. Figure 2The SEM photos of the antiferroelectric ceramics of AN (Comparative Example 1), ABCN1 (Example 1) and ABCN2 (Example 2) show that the ceramics prepared in each embodiment of the present invention have clear grain boundaries, dense structures and no obvious holes. 3+ / Ca 2+ With the introduction of , the average grain size is reduced from 2.4μm of AN ceramic to 1.2μm of ABCN1 ceramic, and the grains are obviously refined. Grain refinement is beneficial to the improvement of the breakdown field strength of ceramics.
[0088] The two surfaces of the antiferroelectric ceramics prepared in Example 1, Example 2 and Comparative Example 1 in the thickness direction were polished to form ceramic sheets of equal thickness, and silver paste was printed on the surface. After drying and electrode sintering, the electrode sintering temperature was 500°C and the insulation time was 30 minutes to obtain a dielectric energy storage capacitor, and subsequent performance tests were carried out.
[0089] The dielectric properties of the dielectric energy storage capacitors prepared from antiferroelectric ceramics in Example 1, Example 2 and Comparative Example 1 were characterized respectively, and the dielectric data were collected using an Agilent E4980A LCR tester. The thickness of the ceramic sheet was about 900 μm, and the diameter of the silver electrode was 4 mm. Figure 3 The dielectric temperature spectra of AN (Comparative Example 1), ABCN1 (Example 1) and ABCN2 (Example 2) antiferroelectric ceramics show that as Bi 3+ / Ca 2+ With the gradual increase of content, the phase transition temperature changes significantly, and the dipole freezing temperature T f Gradually adjusted to below room temperature, making AN ceramics stable at high temperatures 2a and M 2b The antiferroelectric phase is successfully stabilized to room temperature, and the ABCN1 ceramics are in the M 2a Phase, ABCN2 ceramics are in M 2b Mutually
[0090] The energy storage performance of the dielectric energy storage capacitors prepared from the antiferroelectric ceramics in Example 1, Example 2 and Comparative Example 1 were characterized respectively. Figure 4 The room temperature ferroelectric hysteresis loops of AN (Comparative Example 1), ABCN1 (Example 1) and ABCN2 (Example 2) antiferroelectric ceramics are shown in Figure 1. The ferroelectric data are obtained by testing with aixACCT TF Analyzer 2000 ferroelectric analyzer. The thickness of the ceramic sheet is about 200 μm and the diameter of the silver electrode is 2 mm. The results show that Bi 3+ / Ca 2+ The introduction of niobate has led to the following changes in the properties of silver niobate antiferroelectric ceramics: (1) The antiferroelectric properties are enhanced, and the forward reversal electric field E FThe electric field E increased from 144.9 kV / cm for AN ceramic to 189.3 kV / cm for ABCN1 ceramic. B The voltage of AN ceramic increases from 52.1 kV / cm to 122.6 kV / cm of ABCN1 ceramic, and E F and E B The difference between them is reduced from 92.8 kV / cm for AN ceramic to 66.7 kV / cm for ABCN1 ceramic. (2) The saturation polarization intensity is enhanced from 26.0 μC / cm for AN ceramic to 66.7 kV / cm for ABCN1 ceramic. 2 Enhanced to 45.1μC / cm of ABCN1 ceramic 2 (3) The dielectric breakdown field strength increases from 165 kV / cm for AN ceramics to 210 kV / cm for ABCN2 ceramics, and the dielectric breakdown field strength for ABCN1 ceramics is 205 kV / cm. Since ABCN2 ceramics do not completely undergo antiferroelectric-ferroelectric phase transition under a driving electric field of 210 kV / cm, their saturation polarization value is only 26.7 μC / cm. 2 , the energy storage density is small, and finally, at room temperature, it is in M 2a The ABCN1 antiferroelectric ceramics can achieve a high conductivity of 4.4 J / cm at a low electric field of 205 kV / cm. 3 The effective energy density and energy storage efficiency of 63% are
[0091] The effective energy density (W) of the ceramics obtained in Examples 1 to 4 and Comparative Example 1 rec ) and energy storage efficiency (η) are shown in Table 1.
[0092] Table 1
[0093] sample <![CDATA[W rec (J / cm 3 )]]> η(%) AN 1.3 37.7 ABCN1 4.4 63.0 ABCN2 2.4 77.5
[0094] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field, characterized in that: Its chemical formula is Ag (1-5x) Bi x Ca x NbO3,0 <x<0.02。 2. A method for preparing the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field as claimed in claim 1, characterized in that: According to the chemical general formula Ag (1-5x) Bi x Ca x NbO3, where 0 < x < 0.02, weigh the raw materials Ag2O, Nb2O5, Bi2O3 and CaCO3 according to the stoichiometric ratio, and additionally add 5x / 2 mol of Ag2O and x / 2 mol of Bi2O3, and synthesize the silver niobate-based antiferroelectric ceramic with a high energy storage density under a low electric field by the solid-state reaction method.
3. The method for preparing silver niobate-based antiferroelectric ceramics with high energy storage density under low electric field according to claim 2, characterized in that: The following steps are involved: According to the chemical formula Ag (1-5x) Bi x Ca x NbO3, where 0 < x < 0.02, weigh the raw materials Ag2O, Nb2O5, Bi2O3 and CaCO3 according to the stoichiometric ratio, and additionally add 5x / 2 mol of Ag2O and x / 2 mol of Bi2O3. Wet ball mill the above raw materials, dry and screen them after the ball milling to obtain a powder. Pre-calcining the powder in a flowing O2 atmosphere to obtain pre-calcined powder; The pre-burned powder is crushed, dried and sieved to obtain a powder with uniform particle size; The powder material with uniform particle size is granulated and formed to obtain a ceramic green body; The ceramic green body is subjected to debinding and sintering treatment to obtain the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field.
4. The method for preparing silver niobate-based antiferroelectric ceramics with high energy storage density under low electric field according to claim 3, characterized in that: During wet ball milling, the mass ratio of raw material, grinding ball and ball milling medium is 1:(5-10):(1-1.5); the ball milling medium is anhydrous ethanol, and the grinding ball is ZrO2 grinding ball.
5. The method for preparing silver niobate-based antiferroelectric ceramics with high energy storage density under low electric field according to claim 3, characterized in that: The pre-burning temperature is 850-900° C., and the heat preservation time is 3-6 hours.
6. The method for preparing silver niobate-based antiferroelectric ceramics with high energy storage density under low electric field according to claim 3, characterized in that: A polyvinyl alcohol aqueous solution is added during the granulation; and the molding method is isostatic pressing.
7. The method for preparing silver niobate-based antiferroelectric ceramics with high energy storage density under low electric field according to claim 3, characterized in that: The debinding temperature is 500-600°C, and the debinding time is 1-2h; The sintering temperature is 1075-1090° C., and the heat preservation time is 3-6 hours.
8. Use of the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field as claimed in claim 1 in the preparation of dielectric energy storage capacitors.
9. A method for preparing a dielectric energy storage capacitor, characterized in that: The two surfaces of the silver niobate-based antiferroelectric ceramic with high energy storage density under low electric field as claimed in claim 1 are polished and flattened in the thickness direction to form a ceramic sheet of equal thickness, and silver paste is printed on the surface of the ceramic sheet of equal thickness. After drying and electrode sintering, the dielectric energy storage capacitor is obtained.
10. The method for preparing a dielectric energy storage capacitor according to claim 9, characterized in that: The electrode sintering temperature is 500-600° C., and the heat preservation time is 15-30 minutes.