Processing method of national storage retired single-base gunpowder
Through water-coated crushing and fatty acid acid acid chloride modification treatment, combined with polyazide glycidyl ether binder, the storage stability and safety of the decommissioned single-based gunpowder are solved, and its safety and stability in storage and use are improved. .
Patent Information
- Application Number
- CN202411015553.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-26
AI Technical Summary
Decommissioned single-based gunpowder has poor stability, insufficient mechanical strength and sensitivity to electrostatic sparks and mechanical shocks during storage and use, resulting in low safety and stability, especially more dangerous after long-term storage.
Reduce the sensitivity of gunpowder by water-coated and fine-grained, and use fatty acid acid chloride modification treatment to form a hydrophobic layer, combined with polyazide glycidyl ether as a binder to improve the storage stability and safety of gunpowder and inhibit the self-heat of nitrogen oxides. Catalysis.
It improves the storage stability and safety of retired single-based gunpowder, reduces sensitivity to moisture and mechanical impact, extends the service life of the product, and enhances the safety of the processing process.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of gunpowder processing, and in particular relates to a method for processing national reserve retired single-base gunpowder. Background Art
[0002] State-owned retired single-base gunpowder refers to gunpowder used as a source of energy for firearms and cannons that has expired or been eliminated. The reuse of this type of gunpowder can not only reduce storage and handling costs, but also bring certain economic benefits. In recent years, some fireworks and firecracker manufacturers have used a large amount of state-owned retired single-base gunpowder to produce low-smoke fireworks. Since single-base gunpowder has a lower ignition temperature than black powder, the processing, storage, transportation and use of state-owned retired single-base gunpowder have higher safety requirements.
[0003] The main component of retired single-base gunpowder is nitrocellulose, which is relatively stable at room temperature. Since some retired single-base gunpowder has been stored for too long, the stabilizer has been basically consumed, the stability is poor, and the mechanical strength is also poor. Therefore, when the single-base gunpowder reaches its storage limit, there will be great uncertainty and danger. In particular, when the single-base gunpowder is subjected to severe impact or encounters sparks, it is very easy to produce violent combustion, causing great danger and pollution. Therefore, it is particularly important to improve safety during the processing and recycling of retired single-base gunpowder. Summary of the invention
[0004] The purpose of the present invention is to provide a method for processing retired single-base gunpowder in the national reserve, so as to provide a method for resource utilization of retired fireworks and improve the safety of the processing process.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for processing retired single-base gunpowder in national reserves, comprising the following steps:
[0007] The first step is to grind the retired single-base gunpowder with water and finely grind it to obtain a wet powder; the wet powder is centrifugally dehydrated, sieved, and dried at 40°C to a moisture content of ≤5% to obtain a dry material;
[0008] Step 2: Add the dry material into chloroform, then add fatty acid chloride in an ice-water bath, raise the temperature to 40°C after the addition, stir and react for 4-6 hours, wash with water, and vacuum dry at 40°C to constant weight to obtain the modified material;
[0009] The third step is to mix the modified material, stabilizer and adhesive, add solvent, knead and plasticize to obtain a sample.
[0010] Furthermore, the fatty acid chloride is one of lauroyl chloride, palmitoyl chloride and oleoyl chloride.
[0011] Furthermore, the usage ratio of the dry material and fatty acid chloride is 1-1.5 g: 0.001 mol.
[0012] Furthermore, the retired single-base gunpowder is preliminarily removed manually or by equipment to remove metals and impurities.
[0013] Furthermore, the water-compounding comprises the following steps:
[0014] After the retired single-base gunpowder is soaked in water (to reduce the sensitivity of the gunpowder to static sparks or slight mechanical effects), it is initially crushed to less than 40 mesh.
[0015] Furthermore, the mesh number of the sieving is 60-80 meshes.
[0016] Further, the kneading temperature is 20-30°C.
[0017] Further, the mass ratio of the modified material to the solvent is 1:1;
[0018] The mass ratio of the modified material, the stabilizer and the adhesive is 77-80:1.1-1.2:7.
[0019] Furthermore, the solvent is a mixture of ethanol and ether in a volume ratio of 1:1.2-1.3.
[0020] Furthermore, the stabilizer is one of diphenylamine, N-phenylaniline and nitrodiphenylamine.
[0021] Furthermore, the adhesive is polyazide glycidyl ether or a mixture of polyazide glycidyl ether and branched modified polyazide glycidyl ether in a mass ratio of 10:3.2-3.5.
[0022] Furthermore, the branched modified polyazide glycidyl ether is prepared by the following steps:
[0023] The hyperbranched glycidyl ether and dichloromethane are mixed, and then boron trifluoride ether is added, stirred and dispersed, cooled to 0°C, and epichlorohydrin is added. After the addition, stirring and reacting for 24 hours are continued. After the reaction is completed, sodium carbonate is added to terminate the reaction, and after washing and drying, an intermediate product is obtained. The intermediate product is added to N,N-dimethylformamide, sodium azide is added at 60°C, the temperature is raised to 95°C, and the reaction is stirred for 24 hours. After the reaction is completed, the temperature is cooled to room temperature, mixed with water, precipitated, and dried to obtain branched modified polyazido glycidyl ether. The hyperbranched glycidyl ether is synthesized by anionic polymerization.
[0024] Furthermore, the mass ratio of the hyperbranched glycidyl ether, boron trifluoride ethyl ether, epichlorohydrin and sodium azide is 10:0.6:30:18-20; the mass ratio of the hyperbranched glycidyl ether and dichloromethane is 1g:5mL; and the mass ratio of the intermediate product and N,N-dimethylformamide is 1g:5mL.
[0025] Beneficial effects of the present invention:
[0026] The present invention provides a method for processing state-owned retired single-base gunpowder. The main energy component of the single-base gunpowder is nitrocellulose, which will produce nitrogen oxides with autocatalytic effect during storage, and will continue to slowly release heat to produce heat accumulation, affecting the safety of production and storage. The present invention reduces the sensitivity of the gunpowder to electrostatic sparks or slight mechanical effects through wet pulverization (pulverization with water), and uses fatty acid chloride to modify the recycled material obtained by pulverization. The fatty acid chloride can react with the hydroxyl group on the surface of the recycled gunpowder to form a hydrophobic layer (long-chain alkyl), thereby improving the insensitivity of the recycled gunpowder and reducing the sensitivity of the prepared product to moisture, thereby further improving the storage stability.
[0027] In the processing method of the present invention, polyazide glycidyl ether can be used as a binder for the raw material, and a mixture of polyazide glycidyl ether and branched modified polyazide glycidyl ether can also be used as a binder. The branched polymer has good solubility and low viscosity to improve the dispersibility of the raw material. The branched structure in the branched modified polyazide glycidyl ether has a large cavity inside, which can also absorb and recover nitrogen oxides released by decomposition in the prepared gunpowder, thereby inhibiting the autocatalytic effect of nitrogen oxides on the decomposition of the sample, further improving the safety of the processing process of resource utilization of retired fireworks and the safety of the prepared products. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] A method for processing retired single-base gunpowder in national reserves, comprising the following steps:
[0031] The first step is to grind the retired single-base gunpowder with water and finely grind it to obtain a wet powder; the grinding with water is to soak the retired single-base gunpowder in water and then grind it to less than 40 mesh; the wet powder is centrifugally dehydrated and sieved, and the mesh number of the sieve is 60 mesh; then it is dried at 40°C to a moisture content of ≤5% to obtain a dry material;
[0032] Step 2: Add the dry material into chloroform, then add lauroyl chloride in an ice-water bath, raise the temperature to 40°C after the addition, stir and react for 4 hours, wash with water, and vacuum dry at 40°C to constant weight to obtain a modified material; the ratio of the dry material to lauroyl chloride is 1g:0.001mol;
[0033] Step 3: The modified material, diphenylamine and polyazide glycidyl ether are mixed, and a solvent is added, and the sample is kneaded and plasticized to obtain the sample at a kneading temperature of 20°C. The mass ratio of the modified material and the solvent is 1:1; the solvent is a mixture of ethanol and ether in a volume ratio of 1:1.2; the mass ratio of the modified material, diphenylamine and polyazide glycidyl ether is 77:1.1:7.
[0034] Example 2
[0035] A method for processing retired single-base gunpowder in national reserves, comprising the following steps:
[0036] The first step is to grind the retired single-base gunpowder with water and finely grind it to obtain a wet powder; the grinding with water is to soak the retired single-base gunpowder in water (to reduce the sensitivity of the gunpowder to static sparks or slight mechanical effects), and then grind it to less than 40 mesh; the wet powder is centrifugally dehydrated and sieved, and the mesh size of the sieve is 60 mesh; then it is dried at 40°C to a moisture content of ≤5% to obtain a dry material;
[0037] Step 2: Add the dry material into chloroform, then add palmitoyl chloride in an ice-water bath, raise the temperature to 40°C, stir and react for 4 hours, wash with water, and vacuum dry at 40°C to constant weight to obtain the modified material;
[0038] Step 3: The modified material, diphenylamine and polyazide glycidyl ether are mixed, and a solvent is added to knead and plasticize to obtain a sample, and the kneading temperature is 20-30°C. The dosage ratio of the dry material and palmitoyl chloride is 1.2g:0.001mol. The mass ratio of the modified material and the solvent is 1:1; the solvent is a mixture of ethanol and ether in a volume ratio of 1:1.2; the mass ratio of the modified material, diphenylamine and polyazide glycidyl ether is 77:1.1:7.
[0039] Example 3
[0040] A method for processing retired single-base gunpowder in national reserves, comprising the following steps:
[0041] The first step is to grind the retired single-base gunpowder with water and finely grind it to obtain a wet powder; the grinding with water is to soak the retired single-base gunpowder in water and then grind it to less than 40 mesh; the wet powder is centrifugally dehydrated and sieved, and the mesh number of the sieve is 60 mesh; then it is dried at 40°C to a moisture content of ≤5% to obtain a dry material;
[0042] Step 2: Add the dry material into chloroform, then add oleoyl chloride in an ice-water bath, raise the temperature to 40°C after the addition, stir and react for 4 hours, wash with water after the reaction is completed, and vacuum dry at 40°C to constant weight to obtain the modified material;
[0043] Step 3: The modified material, diphenylamine and polyazide glycidyl ether are mixed, and a solvent is added to knead and plasticize to obtain a sample, and the kneading temperature is 20-30°C. The amount ratio of the dry material and oleyl chloride is 1.5g:0.001mol. The mass ratio of the modified material and the solvent is 1:1; the solvent is a mixture of ethanol and ether in a volume ratio of 1:1.2; the mass ratio of the modified material, diphenylamine and polyazide glycidyl ether is 77:1.1:7.
[0044] Example 4
[0045] A method for processing retired single-base gunpowder in national reserves, comprising the following steps:
[0046] The first step is to grind the retired single-base gunpowder with water and grind it into fine powder to obtain a wet powder; the grinding with water is to soak the retired single-base gunpowder in water and then grind it to less than 40 mesh; the wet powder is centrifugally dehydrated and sieved, and the mesh number of the sieve is 70 mesh; and then dried at 40°C to a moisture content of ≤5% to obtain a dry material;
[0047] Step 2: Add the dry material into chloroform, then add lauroyl chloride in an ice-water bath, raise the temperature to 40°C after the addition, stir and react for 5 hours, wash with water, and vacuum dry at 40°C to constant weight to obtain a modified material;
[0048] Step 3: The modified material, diphenylamine and adhesive are mixed, and the solvent is added to knead and plasticize to obtain a sample, and the kneading temperature is 20-30°C. The dosage ratio of the dry material and lauroyl chloride is 1g:0.001mol. The mass ratio of the modified material and the solvent is 1:1; the solvent is a mixture of ethanol and ether in a volume ratio of 1:1.2; the mass ratio of the modified material, diphenylamine and polyazide glycidyl ether is 80:1.1:7.
[0049] Example 5
[0050] A method for processing retired single-base gunpowder in national reserves, comprising the following steps:
[0051] The first step is to grind the retired single-base gunpowder with water and finely grind it to obtain a wet powder; the grinding with water is to soak the retired single-base gunpowder in water and then grind it to less than 40 mesh; the wet powder is centrifugally dehydrated and sieved, and the mesh number of the sieve is 80 mesh; and then dried at 40°C to a moisture content of ≤5% to obtain a dry material;
[0052] Step 2: Add the dry material into chloroform, then add lauroyl chloride in an ice-water bath, raise the temperature to 40°C after the addition, stir and react for 6 hours, wash with water after the reaction is completed, and vacuum dry at 40°C to constant weight to obtain a modified material;
[0053] Step 3: The modified material, diphenylamine and adhesive are mixed, and the solvent is added to knead and plasticize to obtain a sample, and the kneading temperature is 20-30°C. The dosage ratio of the dry material and lauroyl chloride is 1g:0.001mol. The mass ratio of the modified material and the solvent is 1:1; the solvent is a mixture of ethanol and ether in a volume ratio of 1:1.3; the mass ratio of the modified material, diphenylamine and polyazide glycidyl ether is 80:1.2:7.
[0054] Example 6
[0055] Compared with Example 1, the adhesive in this example is a mixture of polyazide glycidyl ether and branched modified polyazide glycidyl ether in a mass ratio of 3:1. The branched modified polyazide glycidyl ether is prepared by the following steps:
[0056] The hyperbranched glycidyl ether and dichloromethane are mixed, and then boron trifluoride ether is added, stirred and dispersed, and then cooled to 0°C, and epichlorohydrin is added. After the addition, stirring and reacting for 24 hours are continued. After the reaction is completed, sodium carbonate is added to terminate the reaction. After washing and drying, an intermediate product is obtained. The intermediate product is added to N, N-dimethylformamide, and sodium azide is added at 60°C, and the temperature is raised to 95°C and stirred for 24 hours. After the reaction is completed, the temperature is cooled to room temperature and mixed with water, precipitated, and dried to obtain branched modified polyazido glycidyl ether. The hyperbranched glycidyl ether is synthesized by anionic polymerization. The mass ratio of the hyperbranched glycidyl ether, boron trifluoride ether, epichlorohydrin and sodium azide is 10:0.6:30:19; the mass ratio of the hyperbranched glycidyl ether and dichloromethane is 1g:5mL; the mass ratio of the intermediate product and N, N-dimethylformamide is 1g:5mL.
[0057] Comparative Example 1
[0058] Compared with Example 1, this comparative example does not perform modification treatment, that is, does not perform the second step treatment.
[0059] The samples prepared in Examples 1 to 6 and Comparative Example 1 were tested, and the chemical stability (Viennese stability and 120°C methyl violet stability) of the samples was tested according to the GJB770B gunpowder test method; the stability at different temperatures was tested, and the test results are shown in Table 1 below:
[0060] Table 1
[0061] project 106.5℃Vieri / h 120℃ Methyl violet / min Example 1 7h 232 Example 2 7h 231 Example 3 7h 235 Example 4 7h 231 Example 5 7h 233 Example 6 7h 245 Comparative Example 1 7h 182
[0062] It can be seen from Table 1 that the results of the two tests are similar, and the stability of the modified samples to be tested in the present invention is better than that of Comparative Example 1; the stability of the modified samples to be tested is good.
[0063] The samples prepared in Examples 1 to 6 and Comparative Example 1 were tested, and the fracture conditions of the samples after impact were recorded. The test temperature was -40°C, and the weight of a single test sample was approximately 64-65g. The drop hammer impact crushing rate under a 5kg drop hammer and a 70cm drop hammer impact was measured. The crushing impact speed was approximately 80-90m / s, and the integrity was recorded.
[0064] The results are shown in Table 2 below:
[0065] Table 2
[0066] project Drop hammer impact crushing rate / % Crushing impact integrity / % Example 1 20 23.6 Example 2 19 24.0 Example 3 21 23.9 Example 4 20 23.4 Example 5 21 23.7 Example 6 17 25.5 Comparative Example 1 29 15.1
[0067] Long alkyl chains are introduced into the modified recycled material, which improves the bonding effect between the recycled material and the adhesive. In addition, the introduction of the hyperbranched structure makes the cross-linking network in the sample to be tested more complex. From the test results, it can be seen that the samples prepared by the present invention have stable low-temperature mechanical properties and have good processing properties and mechanical properties compared with the samples that have not been modified.
[0068] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0069] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for processing retired single-base gunpowder in national reserve, characterized in that: The steps include: The first step is to grind the retired single-base gunpowder with water and finely grind it to obtain a wet powder; the wet powder is centrifugally dehydrated, sieved, and dried at 40°C to a moisture content of ≤5% to obtain a dry material; Step 2: Add the dry material into chloroform, then add fatty acid chloride in an ice-water bath, raise the temperature to 40°C after the addition, stir and react for 4-6 hours, wash with water and vacuum dry after the reaction to obtain the modified material; The third step is to mix the modified material, stabilizer and adhesive, add solvent, and knead and plasticize.
2. A method for processing retired single-base gunpowder from national reserves according to claim 1, characterized in that: The fatty acid chloride is one of lauroyl chloride, palmitoyl chloride and oleoyl chloride.
3. The method for processing retired single-base gunpowder in national reserve according to claim 1, characterized in that: The usage ratio of the dry material and fatty acid chloride is 1-1.5 g: 0.001 mol.
4. A method for processing retired single-base gunpowder from national reserves according to claim 1, characterized in that: The retired single-base gunpowder is preliminarily manually or by equipment to remove metal and impurities; The step of water-compounding is to soak the retired single-base propellant in water and then initially crush it to less than 40 meshes; The mesh number of the sieving is 60-80 meshes.
5. The method for processing retired single-base gunpowder in national reserve according to claim 1, characterized in that: The kneading temperature is 20-30°C.
6. A method for processing retired single-base gunpowder from national reserves according to claim 1, characterized in that: The mass ratio of the modified material to the solvent is 1:1; The mass ratio of the modified material, the stabilizer and the adhesive is 77-80:1.1-1.2:
7.
7. The method for processing retired single-base gunpowder in national reserve according to claim 1, characterized in that: The solvent is a mixture of ethanol and ether in a volume ratio of 1:1.2-1.
3.
8. The method for processing retired single-base gunpowder in national reserve according to claim 1, characterized in that: The stabilizer is one of diphenylamine, N-phenylaniline and nitrodiphenylamine.
9. The method for processing retired single-base gunpowder in national reserve according to claim 1, characterized in that: The adhesive is polyazide glycidyl ether or a mixture of polyazide glycidyl ether and branched modified polyazide glycidyl ether in a mass ratio of 10:3.2-3.
5.
10. A method for processing retired single-base gunpowder from national reserves according to claim 9, characterized in that: The branched modified polyazide glycidyl ether is prepared by the following steps: The hyperbranched glycidyl ether and dichloromethane are mixed, and then boron trifluoride etherate is added, stirred and dispersed, and then the temperature is lowered to 0°C, and epichlorohydrin is added. After the addition, stirring and reacting for 24 hours are continued. After the reaction is completed, sodium carbonate is added to terminate the reaction. After washing and drying, an intermediate product is obtained. The intermediate product is added to N,N-dimethylformamide, and sodium azide is added at 60°C, and the temperature is raised to 95°C and stirred for 24 hours. After the reaction is completed, the temperature is lowered to room temperature, mixed with water, precipitated, and dried to obtain branched modified polyazido glycidyl ether; the mass ratio of the hyperbranched glycidyl ether, boron trifluoride ether, epichlorohydrin and sodium azide is 10:0.6:30:18-20.
Citation Information
Patent Citations
Production method of nitrocellulose for indoor fireworks
CN109251116A
Industrial powdery insensitive explosive and preparation method thereof
CN117567222A
Mixed cellulose nitrates with phthalate groups as polymer basis for glues, paints, coatings, solid rocket fuels, and method of preparation thereof
RU2170235C2
Nano-enhanced explosive material
US10766832B1
Methods for modifying nitrocellulose having lyophobic properties
US9856328B1