Antibacterial metal phenolic acid composite material and preparation method thereof

By forming zinc-luolin complex under weak alkaline conditions, as a metal phenolic acid composite, the resistance and toxicity of existing antibacterial agents are solved, effective inhibition of pathogenic bacteria is achieved, and Biocompatible and broad-spectrum antibacterial effects, suitable for anticorrosion and medical supplies.

CN118955452APending Publication Date: 2024-11-15SHAANXI UNIV OF SCI & TECH

Patent Information

Application Number
CN202411051320.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing antibacterial agents have problems such as drug resistance, small quantity, limited effect, poor heat resistance, low bactericidal rate and toxicity, and the toxicity of inorganic antibacterial agents affects the antibacterial effect.

Method used

The zinc-luolin complex formed by reaction of zinc acetate and luolin under weak alkaline conditions is used as a metal phenolic acid composite material to generate nanosphere particles through coordination reaction to prepare antibacterial agents.

Benefits of technology

The composite material significantly improves the inhibitory effect on pathogenic bacteria at low concentrations, especially on Escherichia coli, Yersinia enterocolitis, etc., and the preparation process is simple and can be expanded to produce. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004975012920000051
    Figure BDA0004975012920000051
  • Figure BDA0004975012920000061
    Figure BDA0004975012920000061
  • Figure BDA0004975012920000071
    Figure BDA0004975012920000071
Patent Text Reader

Abstract

The invention discloses an antibacterial metal phenolic acid composite material and a preparation method thereof, zinc acetate and luteolin are added according to a chemical reaction molar ratio, the zinc acetate and the luteolin can react under a weakly alkaline condition through continuous heating and stirring, and a zinc-luteolin compound obtained through the reaction has an excellent broad-spectrum antibacterial effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of antibacterial properties and relates to a metal phenolic acid composite material with antibacterial properties and a preparation method thereof. Background Art

[0002] Antimicrobial agents are generally divided into pharmaceutical antimicrobial agents, organic antimicrobial agents, natural antimicrobial agents, and inorganic antimicrobial agents. Pharmaceutical antimicrobial agents are mainly antibiotics, including antibacterial antibiotics, antifungal antibiotics, antitumor antibiotics, antiviral antibiotics and other microbial drugs, which are widely used and highly effective, but there are problems such as drug resistance. Natural antimicrobial agents mainly come from natural plant extracts, such as chitin, mustard, castor oil, wasabi, etc. They are easy to use, but there are problems such as small quantity, limited effect, poor heat resistance, low sterilization rate, and they cannot be used for a wide spectrum and long-term effect. The main varieties of organic antimicrobial agents are vanillin and ethyl vanillin compounds, which are often used in polyethylene food packaging films. There are also acylanilides, imidazoles, thiazoles, isothiazolone derivatives, quaternary ammonium salts, bisquads, phenols, etc. Although organic antimicrobial agents have high antibacterial efficiency and fast speed, they have poor heat resistance, are easily hydrolyzed, and have a short shelf life. Inorganic antimicrobial agents are generally made by fixing metals such as silver, copper, zinc (or their ions) on carriers such as zirconium phosphate, glass, zeolite, ceramics, activated carbon, etc. through physical adsorption or ion exchange. Inorganic antimicrobial agents have certain toxicity issues, which often affect their antimicrobial effects.

[0003] The survival and reproduction of microorganisms depend on the absorption of transition metal elements, such as iron, manganese, copper, and zinc, because they can stabilize the folding conformation of metalloproteins and participate in important biochemical reactions. Studies have shown that such metalloproteins account for one-third of the total microbial proteins. Among them, zinc-binding proteins are involved in many important biochemical reactions, including DNA replication, transcription, translation, cell division, glycolysis, pH regulation, etc. In addition, there are zinc ion binding proteins on the cell membranes of microorganisms. Zinc is closely related to a large number of metabolic and toxic pathways of microorganisms, and is particularly important in the process of microbial infection. By inhibiting the zinc ion transport system to affect the homeostasis of zinc ions, it will have an inhibitory effect on microbial contamination and infection. Currently, it is commonly used in the form of nano zinc oxide. Luteolin is a class of flavonoid compounds with a molecular formula of C 15 H 10 O 6 , which exists in many plants. Luteolin has a variety of pharmacological activities, such as anti-inflammatory, anti-allergic, uric acid-lowering, anti-tumor, antibacterial, and antiviral. Luteolin combined with other flavonoids can enhance the inhibitory effect on methicillin-resistant Staphylococcus.

[0004] In addition, Chinese patent CN107936630A provides an antibacterial coating for the surface of medical devices, and its coating preparation process includes a process of stirring and heating luteolin and micro-nano powder (including zinc oxide powder) added to the glaze. However, due to the limited stirring and heating time, it is only for the purpose of achieving blending between the raw materials so as to better play the respective roles of different components. Summary of the invention

[0005] The purpose of the present invention is to provide an antibacterial metal phenolic acid composite material and a preparation method thereof.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] In a first aspect, a metal phenolic acid composite material is provided, wherein the composite material comprises a zinc-luteolin composite, wherein the zinc-luteolin composite adopts a zinc ion:luteolin coordination ratio of 1 to 3:1.

[0008] Preferably, the zinc-luteolin complex is in the form of nano-spherical particles.

[0009] Preferably, the composite material is prepared by complexing zinc ions and luteolin through a coordination reaction.

[0010] The preparation method of the metal phenolic acid composite material comprises the following steps:

[0011] Under weak alkaline conditions, zinc acetate and luteolin are reacted in a solvent by continuous heating and stirring (in the reaction, zinc acetate dissociates to form acetate and zinc ions, and the zinc ions formed after the dissociation of zinc acetate bind to the luteolin after the hydrogen ions are removed through coordination bonds, thereby forming a zinc-luteolin complex), and the chemical reaction molar ratio of zinc acetate to luteolin is 1 to 3:1; after the reaction is completed, the solids in the reaction system are separated and purified to obtain the metal phenolic acid composite material (i.e., the zinc-luteolin composite material).

[0012] Preferably, the zinc acetate and luteolin are of analytical grade.

[0013] Preferably, the weakly alkaline condition is obtained by using an alkaline reagent and adjusting the pH to 7.8-8.0 (the weakly alkaline environment can better dissociate zinc acetate in the reaction, and luteolin can be better dissolved in the solvent in the weakly alkaline environment).

[0014] Preferably, the solvent for the reaction is water.

[0015] Preferably, the initial concentration of zinc acetate in the solvent is 2000-6000 μM.

[0016] Preferably, the reaction temperature is 55-65° C. (more conducive to the forward reaction), the reaction time is 4-5 h, and the stirring speed during the reaction is 450-600 r / min.

[0017] Preferably, the separation specifically comprises the following steps: centrifuging the system after the reaction at 8000-10000g, then discarding the upper liquid, and retaining the precipitate (mainly containing nano-spherical zinc-luteolin complex).

[0018] Preferably, the purification specifically comprises the following steps: washing the precipitate containing the zinc-luteolin complex alternately with anhydrous ethanol and ultrapure water (to wash away the incompletely reacted substances therein to increase the purity of the product), and after washing, vacuum drying at 45-60°C.

[0019] In a second aspect, an antibacterial agent is provided, comprising the above-mentioned metal phenolic acid composite material.

[0020] Preferably, the antibacterial spectrum of the antibacterial agent includes pathogenic bacteria such as Escherichia coli, Yersinia (such as Yersinia enterocolitica), and Salmonella.

[0021] In a third aspect, the invention provides application of the metal phenolic acid composite material in the preparation of an antibacterial agent.

[0022] Preferably, the antibacterial agent further comprises a carrier and / or other compatible drugs.

[0023] Preferably, the carrier includes one or more of ceramics, zeolites and the like.

[0024] Preferably, the compatible drugs include one or more of acylanilides, imidazoles, thiazoles, isothiazolone derivatives, quaternary ammonium salts, bisguanidines, and antibiotics.

[0025] The beneficial effects of the present invention are embodied in:

[0026] The metal phenolic acid composite material of the present invention is mainly composed of a zinc-luteolin complex with a certain coordination ratio. It is confirmed by relevant co-culture coating plate and spot plate antibacterial experiments that it has an inhibitory effect on pathogenic bacteria at low concentrations, and its antibacterial performance on Escherichia coli, Yersinia enterocolitica, etc. is significantly improved, and it can be used as an antibacterial agent.

[0027] The present invention can efficiently prepare a metal phenolic acid composite material with significant antibacterial effect by controlling the chemical reaction molar ratio of zinc acetate and luteolin during the reaction of the two raw materials and separating and purifying the solids in the system after the reaction. The reaction conditions are easy to obtain (such as heating and stirring in water), which is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the appearance of the zinc-luteolin complex suspension obtained after the reaction.

[0029] Figure 2a Scanning electron microscope images of the materials: from left to right: luteolin, zinc acetate, and zinc-luteolin composite material.

[0030] Figure 2b This is the EDS spectrum of the zinc-luteolin composite material: from left to right are C, O, Zn and the element distribution map (this distribution map is different from the element distribution map of the raw material zinc acetate).

[0031] Figure 3 This is a plate diagram of the inhibition experiment of luteolin, zinc acetate, zinc-luteolin composite material, and mixed solution of zinc acetate and luteolin on Escherichia coli CICC 25013 and Yersinia enterocolitica CICC 21669 (CK is the blank group; the mixed solution in the fourth column was coated with a sterile coating rod, and the rest were coated with sterile glass beads).

[0032] Figure 4 The dot plate diagram of the inhibition experiment of different zinc-luteolin composite materials on Salmonella Enteritidis CICC 21513 (CK is the blank group; numbers 1 to 11 are gradient numbers): (A) zinc-luteolin composite material prepared with zinc acetate and luteolin as raw materials; (B) zinc-luteolin composite material prepared with zinc sulfate and luteolin as raw materials. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. The embodiments are only used to explain the present invention, but not to limit the scope of protection of the present invention.

[0034] (I) Preparation and antibacterial activity of zinc-luteolin composite materials

[0035] 1.1 Preparation experiment

[0036] Experimental process: In a weakly alkaline reaction environment, ultrapure water is used as the reaction solvent, and the measured zinc acetate and luteolin are added according to the chemical reaction molar ratio (the molar ratios of multiple substances are determined according to the possible chemical reaction formula, and experiments are carried out separately), and the reaction system is continuously heated and stirred until the reaction is completed. The zinc-luteolin complex formed in the reaction system is separated and purified, and the purified complex is observed by electron microscopy. In the experiment, it was found that the selection of reaction conditions (in addition to the reaction solvent, it also includes the pH of the reaction environment, the chemical reaction molar ratio, the reaction temperature, the reaction time, etc.) has an important influence on the morphological structure (including particle size, etc.) of the obtained zinc-luteolin complex, especially on the antibacterial properties of the complex. In addition, for the convenience of the experiment, the reaction raw materials used in the experiment, such as zinc acetate and luteolin, are all analytically pure.

[0037] Preparation example of zinc-luteolin composite material: the reaction solvent used is ultrapure water, the reaction environment pH = 8.0, the chemical reaction molar ratio is 2: 1 (zinc acetate: luteolin), and the reaction temperature is 55 ° C, and the reaction time is 4h; the reaction is carried out in a reaction bottle (or serum bottle) with a certain volume capacity, and after adding the reaction raw materials zinc acetate (4000 μM) and luteolin to the reaction solvent, the reaction environment pH is first adjusted using 1mol / L NaOH solution, and the reaction system in the reaction bottle is heated to the reaction temperature after the pH is adjusted until the reaction is completed, and the reaction is continuously stirred at a speed of 500r / min during the reaction. After the reaction is completed, the heating and stirring are stopped, and the reaction system (in the form of a suspension) at this time is centrifuged at 8000g (room temperature) for 10min to preliminarily separate the solid after the reaction, and the solid is washed alternately with anhydrous ethanol and ultrapure water 4 times, and centrifuged at 8000g (room temperature) for 10min after each washing, and finally dried in a 45°C vacuum drying oven to obtain a solid powder.

[0038] Experimental results: Figure 1 The suspension shown in the figure is the reaction system after the zinc-luteolin composite is synthesized under the reaction conditions of the above example; the solid powder obtained after further separation and purification is subjected to electron microscopy sample preparation, and the morphology of the zinc-luteolin composite material can be observed through the scanning electron microscope image, such as Figure 2a As shown in the figure, after zinc acetate and luteolin reacted under certain conditions, a composite material with a stacked nanoparticle structure was finally prepared (which is different from the scanning electron microscope images of the two single-component raw materials, luteolin and zinc acetate). The large number of spherical nanoparticles in the structure are the synthesized zinc-luteolin complex; EDS energy dispersive spectrometer detection, as shown Figure 2b As shown, the elemental composition of the zinc-luteolin composite material is C, O, and Zn, and they occupy a certain proportion. It can be seen that the obtained product is a zinc-containing composite (the presence of Zn in the composite material represents a successful synthesis), which verifies that the zinc-luteolin composite material is formed by the complex of luteolin and zinc ions.

[0039] 1.2 Antibacterial experiment

[0040] Experimental principle: Escherichia coli and Yersinia enterocolitica were used to compare the growth of bacterial suspensions treated with zinc acetate, luteolin, a mixture of zinc acetate and luteolin, and a zinc-luteolin composite material after coating, to obtain the antibacterial effect of the zinc-luteolin composite material (specifically the synthetic zinc-luteolin complex).

[0041] Experimental procedure: Single colonies of Escherichia coli CICC 25013 and Yersinia enterocolitica CICC 21669 were selected and placed in LB and TSB liquid culture medium, and cultured in a shaking incubator at 37°C for 12 to 1 hour to activate the first generation of bacteria. Then, 100 μL of the first generation of bacteria were taken and inoculated into sterile shaking bottles containing 30 mL of LB and TSB liquid culture medium and cultured for about 4 hours. The concentration of the bacterial solution was determined to be 1×10 8 After the CFU / mL, 1mL of bacterial solution was taken into a centrifuge tube, centrifuged at 8000g (room temperature) for 5min to remove the culture medium, and the bacterial precipitate was washed twice with sterilized saline, and finally resuspended with 1mL of zinc-luteolin composite material solution as the experimental group; according to the same operation steps, luteolin solution, zinc acetate solution, zinc acetate and luteolin mixed solution and 1mL of saline were used to prepare the resuspended bacterial solution of control group-1, control group-2, control group-3 and blank group. After co-culture for 4h (37℃ shaker), 50μL of the two bacterial solutions of each group were taken and coated on LB and TSB solid culture media respectively, and cultured at 37℃ for 10 hours to observe the growth of the colonies.

[0042] The preparation of the above solutions is described as follows (the concentrations of the solutions are shown in Table 1): luteolin and zinc acetate are prepared separately or mixed with physiological saline to form luteolin suspension, zinc acetate solution, and mixed suspension of luteolin and zinc acetate; the zinc-luteolin composite material solution is obtained by resuspending the powder in physiological saline.

[0043] Table 1. Bacterial inhibition test of zinc-luteolin composite materials

[0044]

[0045] Note: All the drug solutions were prepared with physiological saline as solvent. The “luteolin”, “zinc acetate”, and “zinc-luteolin composite material” in Table 1

[0046] is the drug component of the corresponding group of drug solutions, “-” indicates that the drug concentration is 0, and the “zinc-luteolin composite material” specifically adopts the composite material prepared in Example 1.1.

[0047] Experimental results: From Figure 3 It can be seen that for Escherichia coli and Yersinia enterocolitica, only the experimental group treated with zinc-luteolin composite material did not grow colonies, which was significantly different from the blank group, while the control group treated with luteolin and zinc acetate alone was similar to the blank group, with colonies growing. It can be seen that zinc-luteolin composite material has good antibacterial properties and is significantly better than luteolin and zinc acetate. Figure 3 It can also be seen that the control group treated with the mixture of zinc acetate and luteolin still had colonies growing.

[0048] Based on the results of the above experiments, it can be concluded that the composite material with a nanosphere structure (i.e., zinc-luteolin composite material) prepared by controlling the reaction conditions obtained the potential multi-target synergistic effect of zinc acetate and luteolin in antibacterial performance; and to a certain extent, it shows that the synthesis of zinc-luteolin complex is conducive to the improvement of antibacterial performance.

[0049] (II) Comparison of antibacterial activity with other zinc-luteolin composite materials

[0050] 2.1 Preparation of other zinc-luteolin composites

[0051] Referring to the preparation example of the composite material in (I), under the same weakly alkaline reaction environment, ultrapure water was used as the reaction solvent, and other zinc-containing metal salts (specifically zinc sulfate) and luteolin (zinc sulfate: luteolin is 3:2) were added according to the chemical reaction molar ratio, and then heated and stirred for a certain time (reaction temperature was 55°C, reaction time was 4h). After the reaction, the obtained zinc-luteolin complex suspension was further separated and purified (i.e., after centrifugation, it was washed alternately with anhydrous ethanol and ultrapure water for 4 times, and finally dried in a 45°C vacuum drying oven to form a solid powder) to obtain a zinc-luteolin composite material with a spherical structure (similar to the synthesis mechanism of the zinc-luteolin complex in 1.1, the difference is that zinc sulfate is not easy to dissociate to form zinc ions, so the coordination effect with dehydrogenated luteolin is not as good as zinc acetate).

[0052] 2.2 Antibacterial experiment

[0053] Experimental principle: The growth of colonies after spotting the bacterial solution obtained by mixed co-culture was used to compare the antibacterial properties of the composite materials made of zinc sulfate, zinc acetate and luteolin, and the comparative results of the antibacterial effects of different zinc-luteolin composite materials were obtained.

[0054] Experimental procedure: A single colony of Enteritidis Salmonella (strain number CICC 21513) was selected and placed in LB liquid culture medium. The culture was shaken at 37°C for 12-14 hours to activate the first generation of bacteria. Then, 100 μL of the first generation of bacteria was inoculated into a sterile shake flask containing 30 mL of LB liquid culture medium and cultured for another 4 hours. The concentration of the bacterial solution was determined to be 1×10 8After the CFU / mL was measured, 1 mL of bacterial solution was taken into different centrifuge tubes according to the set drug gradient, centrifuged at 8000g (room temperature) for 5 minutes to remove the culture medium, and the bacterial precipitate was washed twice with sterilized saline, and finally resuspended with 1 mL of zinc-luteolin composite drug solution made from zinc sulfate and luteolin in the corresponding gradient; the resuspended bacterial solution was prepared according to the same operation steps and 1 mL of zinc-luteolin composite drug solution made from zinc acetate and luteolin with the same gradient as the control; and the blank group resuspended bacterial solution was prepared with 1 mL of saline. After co-culture for 4 hours (37°C shaker), 3 μL of the bacterial solution treated with different zinc-luteolin composite materials in the two groups was taken according to each gradient and plated on LB solid culture medium, and the blank group bacterial solution was plated at the same time, and cultured at 37°C for 10 hours to observe the growth of the colonies.

[0055] The preparation of the above solutions is described as follows (the concentrations of the solutions are shown in Table 2): The two zinc-luteolin composite solutions are obtained by resuspending the powder in physiological saline.

[0056] Table 2. Chemical gradients of two composite material point plates

[0057]

[0058]

[0059] Note: The drug solutions were prepared with normal saline as solvent; "Zinc-luteolin complex prepared with zinc acetate and luteolin as raw materials

[0060] The “composite material” specifically adopts the composite material prepared in Example 1.1.

[0061] Experimental results: From Figure 4 It can be seen that for the inhibition of Enteritidis Salmonella, the minimum inhibitory concentration of the zinc-luteolin composite material prepared by zinc sulfate and luteolin is about 250 μM, and the minimum inhibitory concentration of the zinc-luteolin composite material prepared by zinc acetate and luteolin is about 31.25 μM. From this comparison, it can be seen that the zinc-luteolin composite material prepared by zinc acetate and luteolin has significantly improved inhibition of Enteritidis Salmonella, thereby having a better antibacterial effect.

[0062] In summary, the present invention proposes a composite material based on metal phenolic acid substances with a certain coordination ratio. Taking the zinc-luteolin composite material prepared from zinc acetate and luteolin as an example, compared with traditional single metal salts or metal antibacterial agents, it not only has the advantage of good biocompatibility due to the presence of natural plant-derived substances, but also has excellent broad-spectrum antibacterial effects, and can be used in related antiseptic and medical supplies (such as instruments). At the same time, the present invention proposes a composite material preparation method that uses metal zinc salts to react with phenolic acid substances under weak alkaline conditions in ultrapure water to synthesize a composite material (such as synthesizing a zinc-luteolin composite from zinc acetate and luteolin), which has the advantages of simple preparation process, high repeatability, and high yield, and is easy to scale up production.

Claims

1. A metal phenolic acid composite material, Features: The composite material comprises a zinc-luteolin composite, wherein the zinc ion:luteolin coordination ratio adopted by the zinc-luteolin composite is 1-3:

1.

2. A metal phenolic acid composite material according to claim 1, Features: The zinc-luteolin complex is a nano-spherical particle.

3. The metal phenolic acid composite material according to claim 1, Features: The composite material is prepared by complexing zinc ions and luteolin through coordination reaction.

4. A method for preparing a metal phenolic acid composite material, Features: The following steps are involved: Zinc acetate and luteolin are reacted in a solvent, and zinc ions formed by the dissociation of zinc acetate in the reaction are combined with luteolin after dehydrogenation through coordination bonds, and the molar ratio of zinc acetate to luteolin is 1 to 3:1; after the reaction is completed, the solid matter in the reaction system is separated and purified to obtain a metal phenolic acid composite material.

5. A method for preparing a metal phenolic acid composite material according to claim 4, Features: The reaction is carried out under weakly alkaline conditions of pH 7.8-8.

0.

6. A method for preparing a metal phenolic acid composite material according to claim 4, Features: The solvent is water.

7. A method for preparing a metal phenolic acid composite material according to claim 4, Features: The initial concentration of the zinc acetate in the solvent is 2000-6000 μM.

8. A method for preparing a metal phenolic acid composite material according to claim 4, Features: The reaction temperature is 55-65° C., the reaction time is 4-5 hours, and the stirring speed during the reaction is 450-600 r / min.

9. An antimicrobial agent, Features: The invention comprises the metal phenolic acid composite material as claimed in any one of claims 1 to 3.

10. Use of the metal phenolic acid composite material according to any one of claims 1 to 3 in the preparation of an antibacterial agent.

Citation Information

Patent Citations

  • Special surface antibacterial coating of medical device and preparation process of special surface antibacterial coating

    CN107936630A

  • Luteolin-Zn complex capable of promoting consumption of cell glucose as well as preparation and application

    CN106632427A

  • Method of preparing high-purity luteolin by zinc salt

    CN108864021A

  • Flavonoid metal complex for inhibiting pathogenic bacteria of citrus canker

    CN112442051A

  • Metal-luteolin nano polymer material Lut-Sm as well as preparation method and application thereof

    CN117903451A

Cited By

  • Polyvinyl alcohol / luteolin-zinc composite fresh-keeping solution and application

    CN121605999A