Quadripolymer scale inhibitor for inhibiting formation of calcium carbonate scale in high-temperature geothermal fluid and preparation method of quadripolymer scale inhibitor

Through the quaternary copolymer scale inhibitor, it can effectively inhibit the formation of calcium carbonate scale in geothermal wellbore at high temperatures, and solve the problems of low scale resistance and unfriendly environmental protection at high temperatures, and it has high efficiency and low cost. and environmentally friendly characteristics.

CN118955781APending Publication Date: 2024-11-15TIANJIN UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411206082.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The scale inhibitors in existing geothermal wellbores have low scale resistance under high temperature conditions, and phosphorus-containing scale inhibitors are not friendly to the environment, and there is a problem of low cost performance.

Method used

Using quaternary copolymer scale inhibitor prepared by free radical polymerization of four monomers: itaconic acid, acrylic acid, hydroxyethyl methacrylate and sodium allyl sulfonate, the mass ratio and polymerization conditions of the monomer are adjusted to form high efficiency. The quaternary copolymer scale inhibitor can reach a scale inhibition rate of more than 95% at a high temperature of 120°C, and does not contain phosphorus and has good biodegradability.

Benefits of technology

It has achieved efficient inhibition of the formation of calcium carbonate scale at high temperatures, and is used efficiently in low amounts, suitable for industrial applications, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a quadripolymer scale inhibitor for inhibiting formation of calcium carbonate scale in a high-temperature geothermal fluid and a preparation method of the quadripolymer scale inhibitor. The quadripolymer scale inhibitor is obtained by free radical polymerization of four monomers including itaconic acid, acrylic acid, ethyl methacrylate and sodium allysulfonate, the mass ratio of the itaconic acid to the acrylic acid to the ethyl methacrylate to the sodium allysulfonate is (1-2): (6-7): (1): (1). The copolymer scale inhibitor can reach a scale inhibition rate of more than 95% at a high temperature of 120 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a scale inhibitor in a geothermal wellbore, and in particular to a high-efficiency scale inhibitor capable of inhibiting the formation of calcium carbonate scale attached to the wall of a geothermal wellbore during the utilization of high-temperature geothermal fluid. Background Art

[0002] There are scaling and corrosion problems in geothermal energy mining and utilization facilities and pipes, especially high-temperature geothermal wells, which are high-cost and low-efficiency due to scaling. There are several effective methods to control scaling in geothermal fluids: 1. Adding scale inhibitors to geothermal fluids can prevent the deposition of insoluble salts; 2. Applying physical fields to mechanically remove scale in geothermal wells; 3. Adding scale-inhibiting coatings to the walls of geothermal wells to prevent scale accumulation; 4. Pre-descaling treatment before using geothermal water. Scale inhibitors have a series of advantages such as low quantity, high efficiency and convenient use.

[0003] Research on scale inhibitors for inhibiting the scaling of high-temperature geothermal fluids has been carried out at home and abroad. According to Ma Yongli, Yan Jiajia, Liu Mengyuan, et al. Research on compound scale inhibitors for inhibiting the scaling of calcium carbonate in high-temperature geothermal fluids. New Energy Progress, 2023, 11(1): 8-13, it is disclosed that four common green scale inhibitors: hydrolyzed polymaleic anhydride (HPMA), polyaspartic acid (PASP), polyepoxysuccinic acid (PESA), and polyacrylic acid (PAA) were selected for compounding experiments to study their scale inhibition performance in geothermal water. The results showed that at 80°C, the scale inhibition rate of HPMA, PASP, and PAA at the optimal volume ratio (HPMA: PASP: PAA = 1:1:4) can reach 97%. However, when the temperature is higher than 100°C, the scale inhibition rate of the compound scale inhibitor is less than 90%.

[0004] Lin Hongbo, Yu Huagui, Lei Hongwu. Experimental study on anti-scaling and antiscalant optimization of geothermal system. Shandong Chemical Industry, 2022, 51(10): 54-57. The authors disclosed that five chemical antiscalants were tested for their antiscaling effects under the temperature and pressure conditions of geothermal wells, and the residual antiscalant concentration of the solution after the reaction was measured by spectrophotometer. It was found that GS antiscalant had a better antiscaling effect on the test well, and at 3×10 -5 When the scale inhibition rate can reach 94.43%. However, GS scale inhibitors contain phosphorus, and excessive phosphorus promotes the rapid growth of algae and phytoplankton. This is not good for the ecosystem and can kill fish because it reduces the concentration of dissolved oxygen in the water. Therefore, phosphorus-containing scale inhibitors have been largely replaced and are now almost no longer used in industrial production.

[0005] Qiao S, Chen Y, Li J, et al. A novel and efficient CaCO3 scale inhibitor in high-temperature and high-salinity geothermal systems: A deprotonated quadripolymer. Molecular Surface Science, 2023, 9(10): 1-14 disclosed that a novel modified carboxymethylated cyclodextrin tetrapolymer (CAAS) scale inhibitor was synthesized by free radical polymerization using carboxymethylated β-cyclodextrin, acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and styrene sulfonate (SSS) as raw materials. Under geothermal experimental conditions, static experiments showed that the scale inhibition rate of 50 mg / L scale inhibitor was 90%, which was 13.5% higher than that of commercial scale inhibitors. The scale inhibition effect of the scale inhibitor was poor at low concentrations.

[0006] Yu Rong, Lu Peining, Yan Cheng, Ma Zhixiang, He Leigang, Zhao Dan, Liu Yuanbo. Scale inhibition and biodegradability of AA / MA / HEMA terpolymer. Journal of Environmental Engineering, 2016, 10(10): 5549-5554. A new biodegradable terpolymer scale inhibitor MA / AA / HEMA was synthesized by aqueous free radical polymerization. The results showed that the scale inhibitor had a scale inhibition rate of 91.35% when the dosage was 3 mg / L, the water temperature was 80°C, and the calcium ion concentration was 480 mg / L. Its substrate removal rate BOD5 / COD was 55.2%, and its degradation rate was 75%. It is an environmentally friendly scale inhibitor. This new scale inhibitor focuses on environmental friendliness on the basis of improving scale inhibition performance. However, this scale inhibitor has almost no scale inhibition performance at high temperatures. The high temperature resistance of scale inhibitors is a direction that needs to be strengthened in the current and future research.

[0007] At present, the research on geothermal water scale inhibitors is still in the development stage at home and abroad. Most of the research is to study the existing scale inhibitors or compound them to study their scale inhibition performance. Some scholars have improved the scale inhibition of scale inhibitors in geothermal water environments by grafting and modifying the existing scale inhibitors. The application of existing commercial scale inhibitors in high-temperature geothermal water is immature, and there are problems such as phosphorus elements that are not friendly to the environment, low scale inhibition rate at high temperatures, and low cost performance. Summary of the invention

[0008] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a tetrapolymer scale inhibitor and a preparation method thereof which can efficiently remove scale and is resistant to high temperatures in the process of utilizing geothermal water and inhibit the formation of calcium carbonate scale in high-temperature geothermal fluids.

[0009] The present invention discloses a tetrapolymer scale inhibitor for inhibiting the formation of calcium carbonate scale in high-temperature geothermal fluid. The tetrapolymer scale inhibitor is obtained by free radical polymerization of four monomers, namely itaconic acid, acrylic acid, ethyl methacrylate and sodium allyl sulfonate. The mass ratio of the four monomers, namely itaconic acid, acrylic acid, ethyl methacrylate and sodium allyl sulfonate, is (1-2):(6-7):(1):(1).

[0010] The method for preparing a tetrapolymer scale inhibitor for inhibiting the formation of calcium carbonate scale in high-temperature geothermal fluids of the present invention comprises the following steps:

[0011] The first step is to turn on the constant temperature magnetic stirrer and heat it to 90°C for preheating;

[0012] The second step is to put a mixture of itaconic acid, acrylic acid, hydroxyethyl methacrylate and sodium allyl sulfonate into a four-necked flask, and then add deionized water to completely dissolve the solid to form a mixed solution; the mass ratio of itaconic acid, acrylic acid, hydroxyethyl methacrylate, sodium allyl sulfonate and deionized water is (1-2):(6-7):(1):(1):(10);

[0013] The third step is to adjust the pH value of the mixed solution in the four-necked flask to 4-5 with a sodium hydroxide solution, and then add tert-butanol in a mass ratio of 12% to the total mass of the four monomers, and pour ammonium persulfate with a mass percentage concentration of 13.13% into the separatory funnel of the four-necked flask with the piston closed, the mass ratio of ammonium persulfate to the total mass of the four monomers is 4:10, and the mass fraction of the tert-butanol is 99%;

[0014] The fourth step is to place the four-necked flask in a 90°C constant temperature magnetic stirrer, connect a reflux condenser to the four-necked flask, slowly open the piston of the separatory funnel, control the ammonium persulfate to drip into the four-necked flask at a rate of 1 to 4 drops / second until it is finished, and continue to heat at a constant temperature for 3 hours;

[0015] Step 5: After the reaction is completed, the four-necked flask is taken out from the constant temperature magnetic stirrer and cooled to 22-25 degrees to obtain a yellow transparent solution;

[0016] In the sixth step, a 30% by mass potassium hydroxide solution is added to the yellow transparent solution to adjust the pH value of the yellow transparent solution to 5.0; the precipitate is then washed with anhydrous methanol, and the washed precipitate is filtered and dried with a vacuum filter pump with a vacuum degree of 0.1 MPa to obtain a purified IA / AA / HEMA / SAS copolymer.

[0017] The advantages of the present invention compared with existing antiscalants are:

[0018] 1. The copolymer scale inhibitor can achieve a scale inhibition rate of more than 95% at a high temperature of 120°C.

[0019] 2. Copolymer scale inhibitors are low-dosage and high-efficiency. Only a small amount of scale inhibitor is needed to solve the wellbore scale problem and improve the circulation efficiency of geothermal water in the wellbore.

[0020] 3. The monomers of synthetic scale inhibitors do not contain phosphorus, and itaconic acid and hydroxyethyl methacrylate are highly biodegradable, making them environmentally friendly scale inhibitors.

[0021] 4. The four monomers are cheap and readily available, and are copolymerized into a scale inhibitor for the first time, which is cost-effective and suitable for industrial application.

[0022] 5. Compared with existing scale inhibitors, the four new monomers selected by the present invention for preparing copolymers have unique advantages and are important raw materials for synthesizing high-performance scale inhibitors. For example, itaconic acid (IA) is a dicarboxylic acid monomer, which is widely used in the preparation of copolymers because of its high carboxylic acid content and good water solubility. Acrylic acid (AA) has significant water solubility and dispersibility, and its carboxylic acid group has the ability to chelate and disperse substances. In addition, this type of copolymer can also interfere with the crystallization process of calcium scale and induce lattice distortion, thereby achieving the purpose of effective scale inhibition. The polymerization of hydroxyethyl methacrylate (HEMA) will introduce active hydroxyl groups, which have an inhibitory effect on the formation of salt scale. These hydroxyl groups form hydrogen bonds with CaCO3, resulting in lattice distortion. In addition, HEMA also has significant biodegradability and will not pollute the environment. Sodium allyl sulfonate (SAS) contains sulfonic acid groups, has strong chemical activity, can effectively disperse metal oxides, and because of its strong acidity, it is easily ionized in water. The copolymer scale inhibitor prepared using these four monomers (IA / AA / HEMA / SAS) shows great potential. DETAILED DESCRIPTION

[0023] The present invention will be further described in detail below in conjunction with the embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the protection scope of the present invention.

[0024] The invention discloses a tetrapolymer scale inhibitor for inhibiting the formation of calcium carbonate scale in high-temperature geothermal fluid. The tetrapolymer scale inhibitor is obtained by free radical polymerization of four monomers, namely itaconic acid (IA), acrylic acid (AA), ethyl methacrylate (HEMA) and sodium allyl sulfonate (SAS). The mass ratio of the four monomers, namely itaconic acid (IA), acrylic acid (AA), ethyl methacrylate (HEMA) and sodium allyl sulfonate (SAS), is (1-2):(6-7):(1):(1). The tetrapolymer scale inhibitor has a scale inhibition rate of more than 95% in 120°C geothermal water.

[0025] A method for preparing a tetrapolymer scale inhibitor for inhibiting the formation of calcium carbonate scale in high-temperature geothermal fluids of the present invention comprises the following steps:

[0026] The first step is to turn on the constant temperature magnetic stirrer and heat it to 90°C for preheating;

[0027] In the second step, a mixture of itaconic acid (IA), acrylic acid (AA), hydroxyethyl methacrylate (HEMA) and sodium allyl sulfonate (SAS) is placed in a four-necked flask, and deionized water is then added to completely dissolve the solids to form a mixed solution; the mass ratio of itaconic acid (IA), acrylic acid (AA), hydroxyethyl methacrylate (HEMA), sodium allyl sulfonate (SAS) and deionized water is (1-2):(6-7):(1):(1):(10);

[0028] The third step is to adjust the pH value of the mixed solution in the four-necked flask to 4-5 with a sodium hydroxide solution, and then add tert-butanol in a mass ratio of 12% to the total mass of the four monomers, and pour ammonium persulfate with a mass percentage concentration of 13.13% into the separatory funnel of the four-necked flask with the piston closed, the mass ratio of ammonium persulfate to the total mass of the four monomers is 4:10, and the mass fraction of the tert-butanol is 99%;

[0029] The fourth step is to place the four-necked flask in a 90°C constant temperature magnetic stirrer, connect a reflux condenser to the four-necked flask, slowly open the piston of the separatory funnel, control the ammonium persulfate to drip into the four-necked flask at a rate of 1 to 4 drops / second until it is finished, and continue to heat at a constant temperature for 3 hours;

[0030] Step 5: After the reaction is completed, the four-necked flask is taken out from the constant temperature magnetic stirrer and cooled to 22-25 degrees to obtain a yellow transparent solution;

[0031] In the sixth step, a 30% by mass potassium hydroxide solution is added to the yellow transparent solution to adjust the pH value of the yellow transparent solution to 5.0; the precipitate is then washed with anhydrous methanol, and the washed precipitate is filtered and dried with a vacuum filter pump with a vacuum degree of 0.1 MPa to obtain a purified IA / AA / HEMA / SAS copolymer.

[0032] The scale inhibitor of the present invention has a scale inhibition mechanism in which functional groups such as carboxyl hydroxyl groups in the copolymer scale inhibitor can effectively chelate calcium ions, so that calcium ions cannot combine with carbonate ions to form calcium carbonate microcrystals, thereby preventing the formation of calcium carbonate precipitation. At the same time, the long chains of the copolymer macromolecules can effectively adsorb and disperse the formed calcium carbonate microcrystals, so that the microcrystals cannot collide and aggregate to form large calcium carbonate grains.

[0033] The effect of the present invention is verified below in conjunction with specific tests:

[0034] The specific chemical components in geothermal water are shown in Table 1. Table 2 shows the main components of the simulated geothermal fluid obtained from the geothermal fluid detection report in the geothermal well in Table 1. The scale inhibition rate of the copolymer scale inhibitor was determined by referring to GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents-calcium carbonate precipitation method" for static scale inhibition experiments in simulated geothermal water configured in Table 2. (Li Shuai, Simple prediction of scale location of geothermal wellbore fluid and scale inhibitor research, Tianjin University, 2022.)

[0035] Table 1 Geothermal fluid detection report

[0036]

[0037] Table 2 Main components of geothermal fluid simulated in Boye area

[0038]

[0039] Example 1

[0040] (1) A novel tetrapolymer scale inhibitor IA-AA-HEMA-SAS with a mass ratio of 1:7:1:1 of four monomers of itaconic acid (IA), acrylic acid (AA), ethyl methacrylate (HEMA) and sodium allyl sulfonate (SAS) was prepared; the preparation process is as follows:

[0041] The first step is to turn on the constant temperature magnetic stirrer and heat it to 90°C for preheating;

[0042] The second step is to put a mixture of itaconic acid (IA), acrylic acid (AA), hydroxyethyl methacrylate (HEMA) and sodium allyl sulfonate (SAS) into a four-necked flask, and then add deionized water to completely dissolve the solid to form a mixed solution; the mass ratio of itaconic acid (IA), acrylic acid (AA), hydroxyethyl methacrylate (HEMA), sodium allyl sulfonate (SAS) and deionized water is 1:7:1:1:10;

[0043] The third step is to adjust the pH value of the mixed solution in the four-necked flask to 4 with a sodium hydroxide solution, and then add tert-butanol in a mass ratio of 12% to the total mass of the four monomers, and pour ammonium persulfate with a mass percentage concentration of 13.13% into the separatory funnel of the four-necked flask with the piston closed, the mass ratio of ammonium persulfate to the total mass of the four monomers is 4:10, and the mass fraction of the tert-butanol is 99%;

[0044] Step 4: Place the four-necked flask in a 90°C constant temperature magnetic stirrer, connect a reflux condenser to the four-necked flask, slowly open the piston of the separatory funnel, control the ammonium persulfate to drip into the four-necked flask at a rate of 1 drop / second until it is finished, and continue to heat at a constant temperature for 3 hours;

[0045] Step 5: After the reaction is completed, the four-necked flask is taken out from the constant temperature magnetic stirrer and cooled to 22 degrees to obtain a yellow transparent solution;

[0046] In the sixth step, a 30% by mass potassium hydroxide solution is added to the yellow transparent solution to adjust the pH value of the yellow transparent solution to 5.0; the precipitate is then washed with anhydrous methanol, and the washed precipitate is filtered and dried with a vacuum filter pump with a vacuum degree of 0.1 MPa to obtain a purified IA / AA / HEMA / SAS copolymer.

[0047] (2) A static scale inhibition experiment was carried out in accordance with GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - Calcium carbonate deposition method" to determine the scale inhibition rate of the new tetrapolymer scale inhibitor IA-AA-HEMA-SAS prepared in (1) at a concentration of 10 mg / L. The measurement temperature was 80°C, and the static scale inhibition rate of the new IA-AA-HEMA-SAS scale inhibitor for CaCO3 was found to be 90.4%.

[0048] Example 2

[0049] (1) A novel tetrapolymer scale inhibitor IA-AA-HEMA-SAS was prepared with the mass ratio of four monomers, namely itaconic acid (IA), acrylic acid (AA), ethyl methacrylate (HEMA) and sodium allyl sulfonate (SAS) being 1.5:6.5:1:1.

[0050] The preparation process is the same as that of embodiment 1, except that in the second step, the mass ratio of itaconic acid (IA), acrylic acid (AA), hydroxyethyl methacrylate (HEMA), sodium allyl sulfonate (SAS), and ionized water is adjusted to 1.5:6.5:1:1:10;

[0051] In the third step, the pH value of the mixed solution is adjusted to 5; in the fifth step, the cooling temperature is adjusted to 25 degrees;

[0052] (2) A static scale inhibition experiment was carried out in accordance with GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - Calcium carbonate deposition method" to determine the scale inhibition rate of the new tetrapolymer scale inhibitor IA-AA-HEMA-SAS prepared in (1) at a concentration of 10 mg / L. The measurement temperature was 80°C, and the static scale inhibition rate of the new IA-AA-HEMA-SAS scale inhibitor for CaCO3 was found to be 80.8%.

[0053] Example 3

[0054] (1) A new tetrapolymer scale inhibitor IA-AA-HEMA-SAS was prepared with a mass ratio of 2:6:1:1 of four monomers: itaconic acid (IA), acrylic acid (AA), ethyl methacrylate (HEMA) and sodium allyl sulfonate (SAS).

[0055] The preparation process is the same as that of embodiment 1, except that in the second step, the mass ratio of itaconic acid (IA), acrylic acid (AA), hydroxyethyl methacrylate (HEMA), sodium allyl sulfonate (SAS), and ionized water is adjusted to 2:6:1:1:10;

[0056] The pH value of the mixed solution in the third step is adjusted to 4.5; in the fifth step, the cooling temperature is adjusted to 23 degrees;

[0057] (2) A static scale inhibition experiment was carried out in accordance with GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - Calcium carbonate deposition method" to determine the scale inhibition rate of the new tetrapolymer scale inhibitor IA-AA-HEMA-SAS prepared in (1) at a concentration of 10 mg / L. The measurement temperature was 80°C, and the static scale inhibition rate of the new IA-AA-HEMA-SAS scale inhibitor for CaCO3 was found to be 78.76%.

[0058] Example 4

[0059] (1) A novel tetrapolymer antiscalant IA-AA-HEMA-SAS with a mass ratio of 1:7:1:1 of four monomers, namely itaconic acid (IA), acrylic acid (AA), ethyl methacrylate (HEMA) and sodium allyl sulfonate (SAS) was prepared. The preparation process was the same as that of Example 1.

[0060] (2) A static scale inhibition experiment was carried out in accordance with GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - Calcium carbonate deposition method" to determine the scale inhibition rate of the new tetrapolymer scale inhibitor IA-AA-HEMA-SAS prepared in (1) at a concentration of 10 mg / L. The difference from Example 1 is that the measurement temperature is set to 100°C. The static scale inhibition rate of the new IA-AA-HEMA-SAS scale inhibitor for CaCO3 was measured to be 94.08%.

[0061] Example 5

[0062] (1) A novel tetrapolymer scale inhibitor IA-AA-HEMA-SAS with a mass ratio of 1:7:1:1 of four monomers of itaconic acid (IA), acrylic acid (AA), ethyl methacrylate (HEMA) and sodium allyl sulfonate (SAS) was prepared. The preparation process was the same as that of Example 1;

[0063] (2) A static scale inhibition experiment was carried out in accordance with GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method" to determine the scale inhibition rate of the new tetrapolymer scale inhibitor IA-AA-HEMA-SAS prepared in (1) at a concentration of 10 mg / L. The difference from Example 1 was that the measurement temperature was set at 120°C. The static scale inhibition rate of the new IA-AA-HEMA-SAS scale inhibitor for CaCO3 was measured to be 95.3%.

[0064] Example 6

[0065] (1) A novel tetrapolymer antiscalant IA-AA-HEMA-SAS with a mass ratio of 1:7:1:1 of four monomers, namely itaconic acid (IA), acrylic acid (AA), ethyl methacrylate (HEMA) and sodium allyl sulfonate (SAS) was prepared. The preparation process was the same as that of Example 1.

[0066] (2) A static scale inhibition experiment was carried out in accordance with GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method" to determine the scale inhibition rate of the new tetrapolymer scale inhibitor IA-AA-HEMA-SAS prepared in (1) at a concentration of 10 mg / L. The difference from Example 1 is that the measurement temperature is set to 140°C. The static scale inhibition rate of the new IA-AA-HEMA-SAS scale inhibitor for CaCO3 was measured to be 88.56%.

[0067] Example 7

[0068] (1) A novel tetrapolymer antiscalant IA-AA-HEMA-SAS with a mass ratio of 1:7:1:1 of four monomers, namely itaconic acid (IA), acrylic acid (AA), ethyl methacrylate (HEMA) and sodium allyl sulfonate (SAS) was prepared. The preparation process was the same as that of Example 1.

[0069] (2) A static scale inhibition experiment was carried out in accordance with GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method" to determine the scale inhibition rate of the new tetrapolymer scale inhibitor IA-AA-HEMA-SAS prepared in (1) at a concentration of 10 mg / L. The difference from Example 1 is that the measurement temperature is set to 160°C. The static scale inhibition rate of the new IA-AA-HEMA-SAS scale inhibitor for CaCO3 was measured to be 86.32%.

[0070] Example 8

[0071] (1) A novel tetrapolymer antiscalant IA-AA-HEMA-SAS with a mass ratio of 1:7:1:1 of four monomers, namely itaconic acid (IA), acrylic acid (AA), ethyl methacrylate (HEMA) and sodium allyl sulfonate (SAS) was prepared. The preparation process was the same as that of Example 1.

[0072] (2) A static scale inhibition experiment was carried out in accordance with GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - Calcium carbonate deposition method" to determine the scale inhibition rate of the new tetrapolymer scale inhibitor IA-AA-HEMA-SAS prepared in (1) with a concentration of 8 mg / L. The measurement temperature was set to 100°C, and the static scale inhibition rate of the new IA-AA-HEMA-SAS scale inhibitor for CaCO3 was measured to be 83.05%.

[0073] Example 9

[0074] (1) A novel tetrapolymer antiscalant IA-AA-HEMA-SAS with a mass ratio of 1:7:1:1 of four monomers, namely itaconic acid (IA), acrylic acid (AA), ethyl methacrylate (HEMA) and sodium allyl sulfonate (SAS) was prepared. The preparation process was the same as that of Example 1.

[0075] (2) A static scale inhibition experiment was carried out in accordance with GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - Calcium carbonate deposition method" to determine the scale inhibition rate of the new tetrapolymer scale inhibitor IA-AA-HEMA-SAS with a concentration of 9 mg / L prepared in (1). The measurement temperature was set to 100°C, and the static scale inhibition rate of the new IA-AA-HEMA-SAS scale inhibitor for CaCO3 was measured to be 87.95%.

[0076] Example 10

[0077] (1) A novel tetrapolymer antiscalant IA-AA-HEMA-SAS with a mass ratio of 1:7:1:1 of four monomers, namely itaconic acid (IA), acrylic acid (AA), ethyl methacrylate (HEMA) and sodium allyl sulfonate (SAS) was prepared. The preparation process was the same as that of Example 1.

[0078] (2) A static scale inhibition experiment was carried out in accordance with GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - calcium carbonate deposition method" to determine the scale inhibition rate of the new tetrapolymer scale inhibitor IA-AA-HEMA-SAS prepared in (1) with a concentration of 11 mg / L. The measurement temperature was set to 100°C, and the static scale inhibition rate of the new IA-AA-HEMA-SAS scale inhibitor for CaCO3 was measured to be 92.04%.

[0079] Embodiment 11

[0080] (1) A novel tetrapolymer antiscalant IA-AA-HEMA-SAS with a mass ratio of 1:7:1:1 of four monomers, namely itaconic acid (IA), acrylic acid (AA), ethyl methacrylate (HEMA) and sodium allyl sulfonate (SAS) was prepared. The preparation process was the same as that of Example 1.

[0081] (2) A static scale inhibition experiment was carried out in accordance with GB / T 16632-2019 "Determination of scale inhibition performance of water treatment agents - Calcium carbonate deposition method" to determine the scale inhibition rate of the new tetrapolymer scale inhibitor IA-AA-HEMA-SAS prepared in (1) with a concentration of 12 mg / L. The measurement temperature was set to 100°C, and the static scale inhibition rate of the new IA-AA-HEMA-SAS scale inhibitor for CaCO3 was measured to be 89.99%.

[0082] Comparative Example 1

[0083] (1) Using 10 mg / L of polyacrylic acid (PAA) scale inhibitor equal to the copolymer scale inhibitor in Example (5), under the same conditions, the static scale inhibition rate of acrylic acid against CaCO3 was measured to be 80.6%.

[0084] Comparative Example 2

[0085] (1) Using 10 mg / L of polyepoxysuccinic acid (PESA) scale inhibitor, which is equal to the copolymer scale inhibitor in Example (5), under the same conditions, the static scale inhibition rate of acrylic acid against CaCO3 was measured to be 69.98%.

[0086] Comparative Example 3

[0087] (1) Using 10 mg / L of polyaspartic acid (PASP) scale inhibitor, which is equal to the copolymer scale inhibitor in Example (5), under the same conditions, the static scale inhibition rate of acrylic acid against CaCO3 was measured to be 60.59%.

[0088] Comparative Example 4

[0089] (1) Using 10 mg / L of polyacrylic acid (PAA) scale inhibitor equal to the copolymer scale inhibitor in Example (4), under the same conditions, the static scale inhibition rate of acrylic acid against CaCO3 was 78.76%.

[0090] Comparative Example 5

[0091] (1) Using 10 mg / L of polyepoxysuccinic acid (PESA) scale inhibitor, which is equal to the copolymer scale inhibitor in Example (4), under the same conditions, the static scale inhibition rate of acrylic acid against CaCO3 was measured to be 72.64%.

[0092] Comparative Example 6

[0093] (2) Using 10 mg / L of polyaspartic acid (PASP) scale inhibitor, which is equal to the copolymer scale inhibitor in Example (4), under the same conditions, the static scale inhibition rate of acrylic acid against CaCO3 was measured to be 69.98%.

Claims

1. A tetrapolymer scale inhibitor for inhibiting the formation of calcium carbonate scale in high-temperature geothermal fluids, characterized in that: The tetrapolymer scale inhibitor is obtained by free radical polymerization of four monomers, namely itaconic acid, acrylic acid, ethyl methacrylate and sodium allyl sulfonate, wherein the mass ratio of the four monomers, namely itaconic acid, acrylic acid, ethyl methacrylate and sodium allyl sulfonate, is (1-2):(6-7):(1):(1).

2. The method for preparing the tetrapolymer scale inhibitor for inhibiting the formation of calcium carbonate scale in high-temperature geothermal fluid according to claim 1, characterized in that The following steps are involved: The first step is to turn on the constant temperature magnetic stirrer and heat it to 90°C for preheating; The second step is to put a mixture of itaconic acid, acrylic acid, hydroxyethyl methacrylate and sodium allyl sulfonate into a four-necked flask, and then add deionized water to completely dissolve the solid to form a mixed solution; the mass ratio of itaconic acid, acrylic acid, hydroxyethyl methacrylate, sodium allyl sulfonate and deionized water is (1-2):(6-7):(1):(1):(10); The third step is to adjust the pH value of the mixed solution in the four-necked flask to 4-5 with a sodium hydroxide solution, and then add tert-butanol in a mass ratio of 12% to the total mass of the four monomers, and pour ammonium persulfate with a mass percentage concentration of 13.13% into the separatory funnel of the four-necked flask with the piston closed, the mass ratio of ammonium persulfate to the total mass of the four monomers is 4:10, and the mass fraction of the tert-butanol is 99%; The fourth step is to place the four-necked flask in a 90°C constant temperature magnetic stirrer, connect a reflux condenser to the four-necked flask, slowly open the piston of the separatory funnel, control the ammonium persulfate to drip into the four-necked flask at a rate of 1 to 4 drops / second until it is finished, and continue to heat at a constant temperature for 3 hours; Step 5: After the reaction is completed, the four-necked flask is taken out from the constant temperature magnetic stirrer and cooled to 22-25 degrees to obtain a yellow transparent solution; In the sixth step, a 30% by mass potassium hydroxide solution is added to the yellow transparent solution to adjust the pH value of the yellow transparent solution to 5.0; the precipitate is then washed with anhydrous methanol, and the washed precipitate is filtered and dried with a vacuum filter pump with a vacuum degree of 0.1 MPa to obtain a purified IA / AA / HEMA / SAS copolymer.

Citation Information

Cited By

  • Cationic polymer scale inhibitor as well as preparation method and application thereof

    CN120795244A

  • High-temperature-resistant quaternary copolymer water treatment scale inhibitor and preparation method thereof

    CN123083018A