Functional dual-network chitosan hydrogel as well as preparation method and application thereof

By constructing a dual-network structure through crosslinking of acrylated chitosan with N,N-bis(acryloyl)cysteine ​​and complexation with copper ions, the problems of insufficient antibacterial and mechanical properties of chitosan hydrogels are solved, realizing the application of highly efficient antibacterial materials.

CN118955804AActive Publication Date: 2024-11-15ANHUI POLYTECHNIC UNIV

Patent Information

Application Number
CN202411023537.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

Existing chitosan hydrogel materials have shortcomings in terms of antibacterial and mechanical properties. In particular, Ti3C2Mxene hybrid hydrogels are expensive and lack antibacterial properties, making it difficult to achieve a dual network structure and synergistic antibacterial effect.

Method used

A single-network hydrogel was formed by crosslinking acryloylchitosan with N,N-bis(acryloyl)cysteine, and a double-network structure was constructed by complexing copper ions with carboxyl groups to enhance the mechanical properties and antibacterial ability of the hydrogel.

Benefits of technology

Significant improvements in mechanical properties and synergistic antibacterial effects have been achieved. The dual-network chitosan hydrogel exhibits excellent antibacterial properties and broad application potential in antibacterial materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955804A_ABST
    Figure CN118955804A_ABST
Patent Text Reader

Abstract

The invention provides functional dual-network chitosan hydrogel, a preparation method and application, acrylic acid and N, N-bis (acryloyl) cystamine serving as a cross-linking agent are utilized to simply polymerize and cross-link acryloylated chitosan, single-network hydrogel is prepared, and the mechanical property of a product is optimized. And copper ions are introduced to perform complexing on carboxyl groups in the network to complete double network construction of the hydrogel, so that the mechanical property of the hydrogel is further enhanced. And the use of the copper ions embodies role value in the two aspects of structural optimization, antibacterial application effect and the like of the hydrogel. Compared with the prior art, the double-network hydrogel disclosed by the invention is simple and green in preparation process, adjustable and excellent mechanical properties are provided by different forms of double-network structures, and the hydrogel is endowed with an antibacterial function by positive charges of rich amino groups carried by chitosan; the metal ions involved in the construction of the second network further improve the antibacterial ability of the material, that is, the hydrogel has dual antibacterial efficacy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional hydrogels, and in particular relates to a functional double-network chitosan hydrogel, a preparation method and an application thereof. Background Art

[0002] Chitosan is the only alkaline polysaccharide in nature. It is a natural polymer material that is non-toxic, odorless, and has good biocompatibility and biodegradability. The chitosan molecular chain carries abundant active functional groups such as amino and hydroxyl groups, which is conducive to application-oriented functional modification or modification, and can prepare functional materials for a variety of application scenarios. Therefore, hydrogels with chitosan frameworks are widely used in wound dressings, tissue engineering, sustained release of drugs or growth factors, biosensors or actuators, heavy metal ion adsorption and other fields due to their advantages such as injectability, adhesion, degradability, biocompatibility, antibacterial activity, coagulation, antioxidant and positive charge.

[0003] Metal-loaded hydrogels are antibacterial materials that have emerged in recent years. The main preparation methods include loading metal particles or ions into the hydrogel by encapsulation, in situ generation, and electrostatic complexation. Based on the structure carrying antibacterial factors, large surface area contact of metal elements, or stimulated release, the hydrogel can achieve efficient antibacterial effects.

[0004] In addition, the design of polymer network structure can give hydrogels a variety of functional characteristics, such as redox, magnetic, optical and thermal responsiveness; in addition to achieving intrinsic antibacterial properties, metal elements can also use their derivative structures to implement more efficient antibacterial applications of photothermal or electrothermal conversion. Commonly used metal elements are: gold (Au), silver (Ag), copper (Cu), iron (Fe), etc. Metal elements loaded on hydrogels can not only improve the antibacterial properties, but also maintain antibacterial activity for a long time, greatly reducing the emergence of bacterial resistance.

[0005] The patent with publication number CN 117116667A published on November 24, 2023 discloses a chitosan / polyacrylamide / MXene hybrid hydrogel electrolyte and its preparation method and application: a certain amount of single-layer Ti is added to the acetic acid solution of chitosan 3 C 2 After the Mxene aqueous dispersion and acrylamide monomer are stirred evenly, zinc salt, crosslinking agent and initiator are dissolved in turn to obtain a mixed solution, which is reacted at a predetermined temperature for a predetermined time to obtain a hybrid hydrogel electrolyte. The prepared hybrid hydrogel electrolyte has high conductivity, excellent mechanical tensile properties and self-healing properties. However, its use of Ti 3 C 2 Mxene is expensive and has no antibacterial properties. Summary of the invention

[0006] The purpose of the present invention is to provide a functional double network chitosan hydrogel and a preparation method thereof, wherein a single network hydrogel is prepared by simply polymerizing and cross-linking acryloyl chitosan using acrylic acid and N,N-bis(acryloyl)cystamine as a cross-linking agent, and the mechanical properties of the product can be optimized by structural regulation. The double network construction of the hydrogel is completed by introducing copper ions to carry out complexation of the carboxyl groups in the network, thereby further strengthening its mechanical properties. The use of copper ions has a role value in both structural optimization of the hydrogel and antibacterial application effects. The preparation method is simple, the raw materials are readily available, and the cost is low.

[0007] Another object of the present invention is to provide an application of a functional double-network chitosan hydrogel for use as an antibacterial material.

[0008] The specific technical solutions of the present invention are as follows:

[0009] A method for preparing a functional double-network chitosan hydrogel comprises the following steps:

[0010] 1) preparing acryloyl chitosan;

[0011] 2) preparing single network chitosan hydrogel;

[0012] 3) Preparation of double network chitosan hydrogel;

[0013] In step 1), chitosan is modified by acryloyl chloride;

[0014] In step 1), specifically, acryloyl chloride solution and sodium hydroxide solution are simultaneously added dropwise to the water-soluble chitosan aqueous solution under ice bath conditions, after the addition is completed, the mixture is stirred under ice bath conditions and then at room temperature, and then the pH is adjusted to be neutral, and the mixture is separated and purified to obtain acryloyl chitosan.

[0015] In step 1), the concentration of the water-soluble chitosan aqueous solution is 0.05-0.1 g / mL; preferably 0.08 g / mL; the water-soluble chitosan is dissolved in deionized water to prepare a water-soluble chitosan aqueous solution;

[0016] In step 1), the acryloyl chloride solution is obtained by dissolving acryloyl chloride in dichloromethane; the volume ratio of acryloyl chloride dissolved in dichloromethane is 0.3-0.8:1, preferably 0.5:1;

[0017] In step 1), the sodium hydroxide solution refers to an aqueous sodium hydroxide solution, and the mass concentration of the sodium hydroxide solution is 25-30%, preferably 27%;

[0018] In step 1), the ratio of water-soluble chitosan in the water-soluble chitosan aqueous solution to acryloyl chloride in the acryloyl chloride solution is 3-5:1 g / mL, preferably 4:1 g / mL;

[0019] In step 1), the ratio of water-soluble chitosan to sodium hydroxide solution in the water-soluble chitosan aqueous solution is 1.5-3:1 g / mL, preferably 2:1 g / mL;

[0020] In step 1), the dropping time is controlled within 10 minutes; the two solutions are added dropwise simultaneously);

[0021] In step 1), after the dropwise addition is completed, the stirring time in the ice bath is 2.5-3.5 hours, preferably 3 hours;

[0022] In step 1), the stirring time at room temperature is 15-18 h, preferably 16 h at 25 °C;

[0023] In step 2), N,N-bis(acryloyl)cystamine and acrylic acid are polymerized and cross-linked to form a single network chitosan hydrogel;

[0024] Step 2) is specifically as follows: dissolving acryloyl chitosan in water, adding N,N-bis(acryloyl)cystamine and acrylic acid, stirring and mixing, adding potassium persulfate solution, bubbling nitrogen, placing the mixed solution in a mold for heating, and cooling to obtain a single network chitosan hydrogel.

[0025] In step 2), the ratio of acryloyl chitosan to water is 0.05-0.1 g / mL, preferably 0.0625 g / mL;

[0026] In step 2), the mass ratio of acryloyl chitosan to N,N-bis(acryloyl)cystamine is 8-12:1; preferably 10:1;

[0027] In step 2), the ratio of acryloyl chitosan to acrylic acid is 0.1-0.3 g / mL;

[0028] In step 2), the mass ratio of acryloyl chitosan to potassium persulfate in the potassium persulfate solution is 2-3:1;

[0029] The potassium persulfate solution is a potassium persulfate aqueous solution, and the dosage ratio of potassium persulfate to solvent water is 0.1 g / mL;

[0030] In step 2), nitrogen was bubbled in for 30 min;

[0031] In step 2), the mold used is a polytetrafluoroethylene mold;

[0032] In step 2), heating refers to heating to 55-65°C for 3.5-4.5 hours, preferably 60°C for 4 hours;

[0033] In step 2), cooling refers to cooling to room temperature and keeping for 1.5-2.5 hours, preferably cooling to room temperature and keeping for 2.0 hours.

[0034] In step 3), a double network chitosan hydrogel is prepared using metal cations; the metal cations are copper ions;

[0035] Step 3) is specifically as follows: freeze-dry the single network chitosan hydrogel, immerse it in a copper ion aqueous solution, and take it out to obtain the hydrogel.

[0036] In step 3), the freeze drying refers to freeze drying at (-40°C)-(-50°C) for 24 hours;

[0037] In step 3), the mass concentration of the copper ion aqueous solution is 9-11%, preferably 10%;

[0038] In step 3), the copper ion aqueous solution is selected from a copper chloride aqueous solution, a copper sulfate aqueous solution or a copper nitrate aqueous solution.

[0039] In step 3), the soaking refers to immersing the single network chitosan hydrogel in the copper ion solution at room temperature for 10-14 hours; preferably, soaking for 10 hours;

[0040] The present invention provides a functional double-network chitosan hydrogel, which is prepared by adopting the above method.

[0041] The invention provides an application of a functional double-network chitosan hydrogel for use as an antibacterial material.

[0042] The inventors found that chitosan carrying a positive charge, based on structural modification to obtain a material containing a network, further utilizes the active groups (such as carboxyl groups) introduced in the network to achieve complexation with metal cations to strengthen the mechanical strength of the material in the form of a double network; at the same time, the chitosan and the metal ions on the network structure enable the prepared hydrogel material to obtain a synergistic dual antibacterial ability. The metal cation model selected in the present invention is copper ion. In the present invention, chitosan itself has an antibacterial effect, and the introduction of metal cations can achieve its dual-modal antibacterial function while completing the construction of the hydrogel double network.

[0043] Compared with the prior art, the chitosan hydrogel with a double network provided by the present invention has abundant positively charged amino groups on the chitosan backbone chain that can act on the negative charge on the surface of microorganisms and exhibit good antibacterial activity. The positively charged copper ions introduced by constructing the double network further enhance the antibacterial function of the hydrogel, making it have great potential as an antibacterial functional material. In the preparation, acrylic acid and N, N-bis (acryloyl) cystamine as a crosslinking agent are used to simply polymerize and crosslink acryloyl chitosan to prepare a single network hydrogel, and the mechanical properties of the product can be optimized by structural regulation. The double network construction of the hydrogel is completed by introducing copper ions to implement complexation of the carboxyl groups in the network, the crosslinking density is increased, and its mechanical properties are further enhanced. Chitosan itself is antibacterial, and the introduction of copper ions with antibacterial properties also synergistically enhances the antibacterial properties. The use of copper ions reflects the role value in both structural optimization of hydrogels and antibacterial application effects. The materials used in the present invention all have corresponding functionality. If one is missing, it is difficult to obtain a double network structure, which will also lead to a reduction in the antibacterial effect. In addition, the change of acrylic acid dosage affects the mechanical properties of hydrogel. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 is the H NMR spectrum of acryloyl modified chitosan;

[0045] Figure 2 The infrared spectra of chitosan, acryloyl chitosan, single network chitosan hydrogel and double network chitosan hydrogel;

[0046] Figure 3 The stress-strain curves of single-network chitosan hydrogel and double-network chitosan hydrogel (3 ml acrylic acid dosage);

[0047] Figure 4 Comparison of frequency sweep rheological properties of functional single-network and double-network chitosan hydrogels (3 ml acrylic acid dosage);

[0048] Figure 5 Comparison of the swelling behaviors of single-network chitosan hydrogel and double-network chitosan hydrogel (3 ml acrylic acid dosage);

[0049] Figure 6 The results of the study on the antibacterial properties of single-network and double-network chitosan hydrogels; (a) The left side is the control group with Staphylococcus aureus, and the right side is the single-network hydrogel (left) and double-network hydrogel (right); (b) The left side is the control group with Escherichia coli, and the right side is the single-network hydrogel (left) and double-network hydrogel (right); (c) Comparison of the inhibition zone values ​​of chitosan hydrogels. DETAILED DESCRIPTION

[0050] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0051] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0052] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0053] Example 1

[0054] A method for preparing a functional double-network chitosan hydrogel comprises the following steps:

[0055] 1) Preparation of acryloyl chitosan

[0056] 4 grams of water-soluble chitosan were dissolved in 50 ml of deionized water, 1 ml of acryloyl chloride was dissolved in 2 ml of dichloromethane and placed in a dropping funnel, and 2 ml of 27% (mass fraction) of sodium hydroxide aqueous solution was placed in another dropping funnel. Under ice-water bath stirring, the solutions in the two funnels were dripped into the chitosan aqueous solution at the same time, and the mixture was completed within 10 minutes. After stirring in an ice bath for 3 hours, stirring was continued at room temperature for 16 hours. Subsequently, the pH value of the mixed solution was adjusted to neutral with 1 mol / L sodium hydroxide solution, and the mixture was washed three times with cold ethanol precipitation to remove impurities such as sodium acrylate and salt. After the solid was dried overnight in vacuum at room temperature, the nuclear magnetic resonance hydrogen spectrum confirmed that the result was acryloyl chitosan. Figure 1 H NMR spectrum of acryloyl chitosan, 1 H NMR (D 2 O,δ,ppm):4.36(H a ) and 3.96-3.18(H b ,H c ,H d ,H e ,H f ), belonging to hydrogen at different positions of the chitosan skeleton structure; 6.19 (H g ) and 5.75(H h ) is the proton peak on the double bond of grafted acrylamide.

[0057] 2) Preparation of single network chitosan hydrogel

[0058] Take 0.5 g of acryloyl chitosan and dissolve it in 8 ml of deionized water, add 0.05 g of N, N-bis (acryloyl) cystamine and 2 ml, 3 ml, 4 ml or 5 ml of acrylic acid in turn, and stir at room temperature until the solution is clear. Add 2 ml of aqueous solution dissolved with 0.2 g of potassium persulfate to the above mixture, mix at room temperature, and after bubbling nitrogen for 30 minutes, the homogenized mixture is transferred and sealed in a polytetrafluoroethylene mold. The mold is heated to 60 ° C for 4 hours, cooled to room temperature and kept for 2 hours, and the resulting dark yellow transparent gel is a single network chitosan hydrogel. Figure 2 The infrared spectra of acryloyl chitosan and single network chitosan hydrogel are shown. The hydrogel has a wavelength of 1738 cm -1 A new peak is added at the , which can be attributed to the C=O stretching vibration on the carboxyl group, indicating that acrylic acid cross-links chitosan through polymerization to form a network structure. In the figure, CS is water-soluble chitosan, AC-CS is acryloyl chitosan, SN-CS-Gel is a single network chitosan hydrogel, and DN--CS-Gel is a double network chitosan hydrogel.

[0059] The amount of acrylic acid used in the experiment can be adjusted within the range of 2 ml, 3 ml, 4 ml and 5 ml. The tensile test shows that the tensile stress of the prepared single network hydrogel is 10.71 KPa, 48.53 KPa, 58.09 KPa and 79.19 KPa, and the corresponding strain is 37.71%, 40.73%, 47.37% and 74.82%, respectively. This shows that the increase of polyacrylic acid components in the hydrogel network is beneficial to improving the mechanical properties of the material.

[0060] 3) Preparation of double network chitosan hydrogel

[0061] The single-network chitosan hydrogel prepared with 3 ml of acrylic acid in step 2) was selected, freeze-dried, and then immersed in a 10 wt% (mass fraction) copper chloride aqueous solution (20 mL) for 12 hours. Subsequently, the hydrogel was taken out and rinsed to remove the ions adsorbed on the surface, thus obtaining a green double-network chitosan hydrogel. Its infrared spectrum is as follows Figure 2 As shown in Figure 2, compared with the single network hydrogel, the double network hydrogel material has a -1 A new signal peak is generated, which belongs to the near-infrared characteristic absorption of metal copper ions. At the same time, the symmetrical stretching vibration peak of the carboxyl group increases from 1385 cm -1 Move to 1403cm -1The tensile test based on GB / T 16491-2008 shows that the stress of the double network hydrogel increased sharply from 48.53KPa of its corresponding single network hydrogel to 199.81KPa, an increase of more than 4 times; while the elongation at break increased from 40.73% of its corresponding single network hydrogel to 121.66%, an increase of nearly 3 times (such as Figure 3 As shown). The results show that the second network constructed by the metal ion complex carboxyl group dramatically improves the mechanical properties of the hydrogel from a structural perspective and expands the application space of the material. On the other hand, the rheological properties test of the hydrogel (the test method follows the industry standard JY / T0590-2020) further proves that the double network structure improves the mechanical strength of the material. Figure 4 As shown, under the same feed rate, the storage modulus of the single-network hydrogel is as high as 10385Pa, while the storage modulus of the double-network hydrogel is as high as 45573Pa.

[0062] In terms of swelling performance, the prepared hydrogel (single network hydrogel or double network hydrogel) was immersed in 100 ml of deionized water for 48 h to allow the hydrogel to reach swelling equilibrium. The hydrogel before immersion was weighed and the mass was recorded as W. i During the soaking process, the hydrogel was weighed at certain time intervals. Before weighing, the water on the surface of the hydrogel was absorbed with absorbent paper. The obtained mass was recorded as W s The swelling rate is given by the formula: The result is as follows: Figure 5 As shown in the figure, the hydrogel was basically saturated after immersion for 24 hours. The swelling rates of the single network hydrogel and the double network hydrogel reached 191.8% and 208.1% respectively, indicating that the entry and cross-linking of copper ions had little effect on the water absorption capacity of the hydrogel network.

[0063] Example 2

[0064] An application of a functional double-network chitosan hydrogel for antibacterial materials, and the specific application method is as follows:

[0065] Prepare 300 ml of Luria-Bertani (LB) medium and incubate at 37°C for 12 h before use. Sterilize the materials involved in the experiment at 120°C for 1 h. Take 50 ml of LB solution to prepare bacterial suspensions of Escherichia coli and Staphylococcus aureus (both at a concentration of 1×10 8CFU / mL). Add 200 ml of LB solution to agar to prepare a solid culture medium. The single-network chitosan hydrogel and double-network chitosan hydrogel samples and other supplies used in the experiment were sterilized under ultraviolet light in a clean bench for 1 hour. Take 100 microliters of each bacterial suspension on the surface of the LB solid culture medium, spread it evenly with a glass ball, and stick the sterilized single-network chitosan hydrogel and double-network chitosan hydrogel samples to be tested on the solid culture medium plate. Put 2 pieces of single-network and double-network hydrogel samples in each culture dish, and perform 3 parallel tests for each group of samples. Lightly press the sample to fully contact the solid culture medium. Keep the whole process sterile. At the same time, keep a group of blank samples of Escherichia coli and Staphylococcus aureus. Then turn the plate upside down and place it in a constant temperature incubator at 37°C for 12 hours, and calculate the area of ​​the inhibition zone. The results are as follows Figure 6 As shown, against Escherichia coli, the antibacterial rate of the double network hydrogel was 61.98% higher than that of the single network hydrogel; and against Staphylococcus aureus, the antibacterial rate of the double network hydrogel was 53.29% higher than that of the single network hydrogel, indicating that the antibacterial efficacy of the double network hydrogel constructed with the participation of metal ions has been greatly improved due to the synergistic effect of the two factors.

[0066] The present invention prepares a single network chitosan hydrogel by simple free radical polymerization of a mixed aqueous solution of acryloyl modified chitosan, N, N-bis (acryloyl) cystamine and acrylic acid; wherein, cystamine with two double bonds at the ends is used as a cross-linking agent, and is copolymerized with acrylic acid to cross-link chitosan to form a network, and the carboxyl groups on the short chain of polyacrylic acid can synergistically enhance the mechanical properties of the hydrogel with the abundant amino groups on the chitosan chain in the form of multiple electrostatic interactions. In addition, metal ions are dispersed into the hydrogel by diffusion and assisted by the complexation promotion of carboxyl groups in the hydrogel, and a second network is constructed based on the complexation of metal ions with a large number of carboxyl groups in the single network hydrogel, so as to prepare a double network hydrogel with better mechanical properties. The preparation process of the double network hydrogel of the present invention is simple and green, and different forms of double network structures provide adjustable and excellent mechanical properties, and the positive charge of the rich amino groups carried by chitosan gives the hydrogel an antibacterial function, and the metal ions involved in the construction of the second network further enhance the antibacterial ability of the material, that is, the hydrogel has a dual antibacterial effect. The double-network chitosan hydrogel provided by the present invention is a functional material with optimized mechanical properties and structure, and has great application potential in antibacterial and tissue repair.

[0067] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a functional double-network chitosan hydrogel, characterized in that: The preparation method comprises the following steps: 1) Modifying chitosan with acryloyl chloride to prepare acryloyl chitosan; 2) cross-linking acryloyl chitosan by polymerization of N,N-bis(acryloyl)cystamine and acrylic acid to prepare a single network chitosan hydrogel; 3) Preparation of double network chitosan hydrogel using metal cations.

2. The preparation method according to claim 1, characterized in that: In step 1), specifically, acryloyl chloride solution and sodium hydroxide solution are simultaneously added dropwise to the water-soluble chitosan aqueous solution under ice bath conditions, after the addition is completed, the mixture is stirred under ice bath conditions and then at room temperature, and then the pH is adjusted to be neutral, and the mixture is separated and purified to obtain acryloyl chitosan.

3. The preparation method according to claim 2, characterized in that: In step 1), the amount ratio of water-soluble chitosan in the water-soluble chitosan aqueous solution to acryloyl chloride in the acryloyl chloride solution is 3-5:1 g / mL; the amount ratio of water-soluble chitosan in the water-soluble chitosan aqueous solution to sodium hydroxide solution is 1.5-3:1 g / mL.

4. The preparation method according to claim 1, characterized in that: Step 2) is specifically as follows: dissolving acryloyl chitosan in water, adding N,N-bis(acryloyl)cystamine and acrylic acid, stirring and mixing, adding potassium persulfate solution, bubbling nitrogen, placing the mixed solution in a mold for heating, and cooling to obtain a single network chitosan hydrogel.

5. The preparation method according to claim 4, characterized in that: In step 2), the ratio of acryloyl chitosan to water is 0.05-0.1 g / mL; the mass ratio of acryloyl chitosan to N,N-bis(acryloyl)cystamine is 8-12:1; the ratio of acryloyl chitosan to acrylic acid is 0.1-0.3 g / mL; the mass ratio of acryloyl chitosan to potassium persulfate in potassium persulfate solution is 2-3:

1.

6. The preparation method according to claim 4 or 5, characterized in that: In step 2), heating refers to heating to 55-65° C. for 3.5-4.5 h; cooling refers to cooling to room temperature for 1.5-2.5 h.

7. The preparation method according to claim 1, characterized in that: In step 3), the metal cation is a copper ion.

8. The preparation method according to claim 1 or 7, characterized in that: Step 3) is specifically as follows: freeze-dry the single network chitosan hydrogel, immerse it in a copper ion aqueous solution, and take it out to obtain the hydrogel.

9. A functional double-network chitosan hydrogel prepared by the preparation method according to any one of claims 1 to 8.

10. An application of the functional double network chitosan hydrogel according to claim 9, characterized in that: The functional double-network chitosan hydrogel is used as an antibacterial material.

Citation Information

Patent Citations

  • Method for preparing high-strength chitosan-based hydrogel

    CN106947020A

  • High-strength, anti-freezing and conductive chitosan / acrylamide dual-network hydrogel and preparation method thereof

    CN109134762A

  • Chitosan / poly(N-hydroxyethyl acrylamide) high-toughness antifouling double-network hydrogel and a preparation method thereof

    CN109971105A

  • Dual-network organogel as well as preparation method and application thereof

    CN113943425A

  • Chitosan / polyacrylamide / MXene hybrid hydrogel electrolyte as well as preparation method and application thereof

    CN117116667A

Cited By

  • Preparation method of in-situ curing hydrogel, hydrogel and application thereof

    CN119499431A