Polyethylene micropolyethylene membrane, method of making said
By using sequential biaxial stretching and heat treatment processes in the polyethylene microporous membrane, the heat resistance and breathability at high temperatures are improved, and the thermal resistance of the polyethylene microporous membrane in the prior art is solved. The thermal resistance of the polyethylene microporous membrane at high temperatures is insufficient in the prior art. The problem has achieved improvements in the thermal safety and power characteristics of the battery.
Patent Information
- Application Number
- CN202410569935.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-15
AI Technical Summary
The existing polyethylene microporous membranes lack heat resistance at high temperatures, making it difficult to meet the needs of high breathability and high porosity at the same time, resulting in a fire risk for batteries in high temperature environments.
Using a polyethylene microporous membrane with a thickness of 3-30μm, the puncture strength and thermal stability are improved through sequential biaxial tensile technology and heat treatment technology, ensuring that the lateral shrinkage rate at 121℃ is less than 5%, and passing the PS index ( The permeability × porosity ÷ lateral shrinkage rate) reaches more than 110.
The significant heat resistance of the polyethylene microporous membrane at high temperature is achieved, ensuring the thermal safety and power characteristics of the battery, while improving the mechanical strength and safety of the battery.
Smart Images

Figure BDA0004830537310000141 
Figure BDA0004830537310000151
Abstract
Description
Technical Field
[0001] The present invention relates to a polyethylene microporous membrane, a method for preparing the microporous membrane, and a diaphragm comprising the microporous membrane. According to one embodiment, the present invention relates to a polyethylene microporous membrane having significantly high air permeability and porosity and improved heat resistance, a method for preparing the microporous membrane, and a diaphragm comprising the microporous membrane. Background Art
[0002] Polyethylene microporous membranes are used in various fields such as separation filters, secondary battery diaphragms, fuel cell diaphragms, and supercapacitor diaphragms. Among them, polyethylene microporous membranes are widely used as secondary battery diaphragms due to their excellent electrical insulation and ion permeability.
[0003] In recent years, secondary batteries are being made high-capacity and large-scale for use in electric vehicles, energy storage systems (ESS), etc., so ensuring the safety of the battery has become a more important factor. For example, when the battery is exposed to a high temperature environment or is working, the diaphragm shrinks, so an internal short circuit may be caused, and a fire may occur due to the internal short circuit. Therefore, it is necessary to develop a polyethylene microporous membrane with excellent heat resistance that can cope with the increase in battery temperature. In addition to heat resistance, high mechanical strength is also required to improve the safety of the battery during manufacturing and use, and high transmittance and high porosity are required to increase capacity and power.
[0004] In particular, in view of the recent trend of high capacity and large size of batteries, it is very necessary to develop a separator with higher levels of heat resistance and transmittance. However, high transmittance has an inverse relationship with excellent heat resistance and / or strength, so existing separators that achieve high transmittance have the disadvantage of reduced thermal safety despite having excellent capacity and power characteristics.
[0005] As a solution to the above problems, Korean Patent Publication No. 10-2012-0032539 discloses a polyolefin microporous membrane having a large pore size, excellent electrical properties, excellent strength, and low heat shrinkage. However, the microporous membrane as described above has a heat shrinkage rate of less than 20% in the width direction at 130°C, a porosity of 40-50%, and an air permeability of only 100-200 seconds / 100ml, and therefore does not meet the physical properties required for batteries with higher capacity and higher power.
[0006] Therefore, it is necessary to develop a polyethylene microporous membrane having significantly high permeability and porosity and significantly improved heat resistance at high temperatures. Summary of the invention
[0007] Technical issues to be solved
[0008] In order to solve the above problems, an object of the present invention is to provide a polyethylene microporous membrane having significantly high air permeability and porosity while having significantly improved heat resistance at high temperatures, a method for preparing the microporous membrane, and a separator including the microporous membrane.
[0009] The diaphragm of the present invention can be widely used in electric vehicles, battery charging stations, other green technology fields such as solar power generation and wind power generation using batteries. In addition, the diaphragm of the present invention can be used in eco-friendly electric vehicles and hybrid vehicles to prevent climate change by suppressing air pollution and greenhouse gas emissions.
[0010] Technical Solution
[0011] As a method for achieving the above technical problem, the present invention provides a polyethylene microporous membrane, wherein the thickness of the polyethylene microporous membrane is 3-30 μm, the puncture strength is above 0.15 N / μm, the lateral shrinkage measured after being placed at 121° C. for 1 hour is below 5%, and the PS index represented by the following formula 1 is above 110.
[0012] [Formula 1]
[0013] PS index = [air permeability × porosity] ÷ [transverse shrinkage at 121°C]
[0014] In the above formula 1, the unit of air permeability is "×10 -5 The unit of the porosity is "%", and the unit of the transverse shrinkage at 121°C is "%".
[0015] In one embodiment, the air permeability of the polyethylene microporous membrane can be 10.0×10 -5 Darcy above.
[0016] In one embodiment, the porosity of the polyethylene microporous membrane may be 55-70%, specifically 60-70%.
[0017] In one embodiment, the PS index of the polyethylene microporous membrane may be greater than 220, specifically greater than 400.
[0018] In one embodiment, the polyethylene microporous membrane may include a polyethylene microporous membrane having a weight average molecular weight of 1×10 5 g / mol to 10×10 5 g / mol of polyethylene.
[0019] In one embodiment, the polyethylene microporous membrane may be prepared by a wet process including a sequential biaxial stretching process.
[0020] In addition, as another method for achieving the above-mentioned technical problem, the present invention provides a method for preparing a polyethylene microporous membrane, the method comprising the following steps: (a) melt-kneading a mixture containing a polyethylene resin and a diluent by an extruder to prepare a melt; (b) extruding the melt to form a sheet; (c) stretching the sheet longitudinally by more than 4 times; (d) extracting the diluent from the longitudinally stretched sheet and drying it; (e) stretching the dried sheet transversely by more than 4 times to form a film; and (f) heat-treating the transversely stretched film.
[0021] In one embodiment, the step (f) may include a thermal relaxation process to fix the longitudinal length and shrink the transverse width, and the thermal relaxation process may relax the width in the transverse direction to 80-95% of the width before the thermal relaxation process.
[0022] Another embodiment of the present invention provides a separator, which includes the polyethylene microporous film.
[0023] Another embodiment of the present invention provides an electrochemical device including the separator.
[0024] As an embodiment, the electrochemical device may be a secondary battery including the separator between a positive electrode and a negative electrode.
[0025] In addition, as another method for achieving the above technical problem, the present invention provides a separator including the polyethylene microporous membrane as described above.
[0026] Beneficial Effects
[0027] The polyethylene microporous membrane according to the present invention can have high air permeability and porosity while ensuring significantly improved heat resistance at high temperatures.
[0028] Furthermore, the polyethylene microporous membrane according to the present invention may have a puncture strength of 0.15 N / μm or more, a transverse shrinkage rate measured after being left at 121° C. for 1 hour of 5% or less, and may have significantly high air permeability and porosity.
[0029] Therefore, the present invention can provide a battery having improved power characteristics and thermal safety at high temperatures by including the polyethylene microporous film as described above. DETAILED DESCRIPTION
[0030] The embodiments described in this specification can be modified into various forms, and the technology according to one embodiment is not limited to the embodiments described below. In addition, the implementation form of one embodiment is provided to more completely explain the present invention to those skilled in the art.
[0031] Furthermore, unless otherwise specifically stated herein, singular forms used in the specification and the claims may also include plural forms.
[0032] In addition, the numerical range used in this specification includes the lower limit value and the upper limit value and all values in the range, the increments logically derived from the form and width of the defined range, all values defined therein, and all possible combinations of the upper and lower limits of the numerical range defined in different forms. In this specification, unless otherwise specifically defined, values outside the numerical range that may be generated due to experimental errors or rounding of values are also included in the defined numerical range.
[0033] Furthermore, throughout the specification, unless otherwise specifically stated to the contrary, the description “comprising” or “including” a certain constituent element means that other constituent elements may also be included, rather than excluding other constituent elements.
[0034] The present invention provides a polyethylene microporous membrane, wherein the polyethylene microporous membrane has a thickness of 3-30 μm, a puncture strength of 0.15 N / μm or more, a transverse shrinkage of less than 5% measured after being placed at 121° C. for 1 hour, and a PS index represented by the following formula 1 of more than 110.
[0035] [Formula 1]
[0036] PS index = [air permeability (×10 -5 Darcy) × porosity (%) ÷ [transverse shrinkage at 121°C (%)]
[0037] In recent years, with the high capacity and large size of secondary batteries, it is necessary to meet better power characteristics and thermal safety. For this reason, the separators for secondary batteries need to have higher levels of heat resistance and transmittance at the same time. However, due to the incompatibility between high transmittance and heat resistance, the separators developed in the past have limitations in achieving heat resistance and transmittance above a certain level at the same time.
[0038] As a result of repeated research by the inventors, it has been confirmed that a polyethylene microporous membrane can be prepared, wherein the transverse shrinkage rate of the polyethylene microporous membrane measured after being placed at 121°C for 1 hour satisfies less than 5% and the PS index according to formula 1 satisfies more than 110, thereby having significantly high air permeability and porosity while having significantly improved heat resistance at high temperatures.
[0039] In a secondary battery according to one embodiment, by including a polyethylene microporous membrane that satisfies the physical properties as described above, excellent power characteristics and thermal safety can be ensured. In particular, the present invention can provide a battery having excellent high-temperature thermal safety in which smoke or fire of the battery does not occur in a high-temperature hot-box evaluation at 125°C. The manufacturing and evaluation methods of the battery for the above evaluation are as follows. The positive electrode using NCM 622 (Ni: Co: Mn = 6: 2: 2) as the active material and the negative electrode using graphite carbon as the active material are wound together with the microporous membrane of the present invention and placed in an aluminum soft pack to make a battery. Next, an electrolyte in which 1M of lithium hexafluorophosphate (LiPF6) is dissolved in a solution containing ethylene carbonate, ethyl methyl carbonate and diethyl carbonate in a volume ratio of 3: 5: 2 is injected into the interior of the battery and sealed to manufacture a battery with a capacity of 2Ah. Next, the battery was aged and degassed, fully charged to 4.2V, placed in an oven, heated at 5°C / min, and left at 125°C for 30 minutes to confirm whether the battery smoked or caught fire. That is, the polyethylene microporous membrane of the present invention satisfies the above-mentioned physical properties at the same time, and is therefore suitable for use in high-power / high-capacity batteries.
[0040] The above physical properties of the polyethylene microporous membrane of the present invention can be achieved by performing a step of extracting a diluent before the transverse stretching step or performing a transverse heat treatment step under specific conditions during the preparation of the polyethylene microporous membrane, but it is not necessarily limited thereto.
[0041] The PS index according to Formula 1 increases with the increase of air permeability and porosity and the decrease of transverse heat shrinkage, and the PS index may be 110 or more, specifically 220 or more, more specifically 400 or more, and further specifically 500 or more. The larger the PS index, the better, and there is no particular limit on its upper limit, but for example, it may be 2000 or 1500. In a specific embodiment, the PS index may be 110 to 2000, 220 to 2000, 400 to 1500, or 500 to 1500, but is not limited thereto. When the PS index within the above range is met, it has high air permeability and porosity while having excellent heat resistance, and is therefore suitable for application in high power / high capacity batteries.
[0042] In one embodiment, the polyethylene microporous membrane may have a PS index within the above range and a transverse shrinkage rate measured at 121° C. for 1 hour may be 5% or less, 3% or less, or 2.5% or less, and the lower limit thereof is not particularly limited, but may be, for example, 0.1%, 0.5% or 1%. In a specific embodiment, the shrinkage rate may be 0.1-5%, 0.5-5%, 1-3% or 1-2.5%, but is not limited thereto.
[0043] In one embodiment, the thickness of the polyethylene microporous membrane can be 3-30 μm, specifically 5-20 μm, and more specifically 5-15 μm. The microporous membrane of the present invention can also simultaneously achieve excellent levels of puncture strength, air permeability, and thermal shrinkage at the thickness in the above range. Therefore, it has excellent resistance to external stress generated during the manufacture of the battery, temperature rise and dendrites that occur during the charge and discharge of the battery, and the internal resistance of the battery is low, so the charge and discharge performance of the battery can be improved.
[0044] In one embodiment, the polyethylene microporous membrane may also have a puncture strength of 0.15N / μm or more at a thickness in the above range. Specifically, the puncture strength may be 0.17N / μm or more, 0.26N / μm or more, and the upper limit thereof is not particularly limited, but for example, may be 1.0N / μm or less. In a specific embodiment, the puncture strength may be 0.15-1.0N / μm or 0.17-1.0N / μm or 0.26-1.0N / μm, but is not limited thereto. By satisfying the puncture strength in the above range, it has excellent resistance to external stresses generated during the manufacture of the battery and dendrites generated during the charging and discharging of the battery, thereby ensuring the safety of the battery. In addition, the thin film of the separator for secondary batteries can be achieved, so it is suitable for application in high-capacity / high-power batteries.
[0045] In one embodiment, the polyethylene microporous membrane may have a -5 Darcy or higher air permeability, specifically, the air permeability may be 15.0×10 -5 Darcy or more, more specifically 20.0×10 -5 Darcy or more, and more specifically, 25.0×10 -5 Darcy or more. There is no particular restriction on the upper limit of the air permeability, but for example, it can be 50.0×10 -5 Darcy or less, 40.0×10 -5 Darcy or less or 35.0×10 -5 In a specific embodiment, the air permeability can be 10.0×10 -5 Darcy to 50.0×10-5 Darcy, 15.0×10 -5 Darcy to 50.0×10 -5 Darcy, 20.0×10 -5 Darcy to 40.0×10 -5 Darcy or 25.0×10 -5 Darcy to 35.0×10 -5 By satisfying the air permeability within the above range, the battery can have excellent ion conductivity, and thus the power characteristics of the battery can be significantly improved due to the low internal resistance of the battery.
[0046] In one embodiment, the porosity of the polyethylene microporous membrane may be 55-70%, specifically 60-70%. When the porosity is within the above range, the power characteristics of the battery can be significantly improved due to the low internal resistance of the battery.
[0047] In one embodiment, the polyethylene microporous membrane may include a polyethylene microporous membrane having a weight average molecular weight of 1×10 5 g / mol to 10×10 5 g / mol polyethylene, specifically, may include a polyethylene having a weight average molecular weight of 3×10 5 g / mol to 8×10 5 g / mol of polyethylene, but is not necessarily limited thereto.
[0048] In one embodiment, the polyethylene microporous membrane can be prepared by a wet process including a sequential biaxial stretching process, and by using a specific process sequence or changing the conditions of a specific heat treatment process, a polyethylene microporous membrane that simultaneously satisfies the physical properties described above can be provided.
[0049] In one embodiment, the polyethylene microporous membrane can be prepared by a method of stretching in one direction, extracting the diluent, and stretching in another direction, a method of heat-treating a sequentially biaxially stretched membrane under specific conditions, or a combination thereof.
[0050] Specifically, the polyethylene microporous membrane can be prepared by extracting a diluent after longitudinal stretching and before transverse stretching during the preparation of the polyethylene microporous membrane, but is not necessarily limited thereto as long as a microporous membrane having the physical properties described above can be prepared.
[0051] Hereinafter, the method for producing a polyethylene microporous membrane of the present invention will be described.
[0052] According to one embodiment, a method for preparing a polyethylene microporous membrane may include the following steps: (a) melt-kneading a mixture containing a polyethylene resin and a diluent by an extruder to prepare a melt; (b) extruding the melt to form a sheet; (c) stretching the sheet more than 4 times in the longitudinal direction; (d) extracting the diluent from the longitudinally stretched sheet and drying it; (e) stretching the dried sheet more than 4 times in the transverse direction to form a film; and (f) heat-treating the film.
[0053] In the present invention, unlike the existing method of performing a diluent extraction process after the longitudinal and transverse stretching processes, transverse stretching is performed after the diluent is extracted from the sheet that has completed the longitudinal stretching, so that the pores can be expanded to a greater extent by stretching, thereby preparing a polyethylene microporous membrane with significantly high porosity and air permeability, and can have high heat resistance.
[0054] Hereinafter, each preparation step will be described.
[0055] First, step (a) is a step of preparing a melt by melt-kneading a mixture containing a polyethylene resin and a diluent through an extruder. In order to form pores, the mixture may contain a polyethylene resin and a diluent in a weight ratio of 10 to 60:90 to 40, specifically, a polyethylene resin and a diluent in a weight ratio of 20 to 40:80 to 60, but is not particularly limited as long as the purpose of the present invention can be achieved. When the weight ratio within the above range is met, the melt has sufficient fluidity, so that it is easy to be formed into a uniform sheet in the subsequent steps, and sufficient orientation is achieved during the stretching process, so that mechanical strength is easily ensured, so that problems such as rupture during the stretching process can be prevented.
[0056] In terms of strength, extrusion kneading properties, stretchability, heat resistance of the final microporous film, etc., the polyethylene resin may be a high-density polyethylene or include a high-density polyethylene.
[0057] In one embodiment, the weight average molecular weight of the polyethylene resin may be 1×10 5 g / mol to 10×10 5 g / mol, specifically 3×10 5 g / mol to 8×10 5 g / mol, but is not necessarily limited thereto.
[0058] In one embodiment, the melting temperature of the polyethylene resin may be above 130° C., specifically 130-140° C., but is not necessarily limited thereto. The melting temperature of the polyethylene resin may be measured by differential scanning calorimetry (DSC).
[0059] In one embodiment, the diluent may be any organic compound that forms a single phase with the polyethylene resin at the extrusion temperature without limitation. For example, the diluent may be selected from aliphatic hydrocarbons or cyclic hydrocarbons such as nonane, decane, decalin, paraffin oil, paraffin wax, phthalic acid esters such as dibutyl phthalate and dioctyl phthalate, C10-C20 fatty acids such as palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, and C10-C20 fatty alcohols such as cetyl alcohol, stearyl alcohol, and oleyl alcohol, or a combination of two or more thereof. As a specific example of the diluent, paraffin oil having a kinetic viscosity of 20-200 cSt at 40° C. can be cited, but the present invention is not limited thereto.
[0060] Furthermore, the mixture may further contain any one or more conventional additives for improving specific functions, such as an oxidation stabilizer, a UV stabilizer, and an antistatic agent, within a range that the properties of the microporous membrane are not significantly reduced.
[0061] Step (b) is a step of extruding the melt to form a sheet, which can be performed without limitation by methods known to those skilled in the art. As an example, the melt can be extruded through a T-die and cooled to a temperature of 10-80°C and formed into a sheet by casting or calendaring.
[0062] The longitudinal stretching ratio in step (c) can be specifically more than 4 times, 4 times to 15 times, and more specifically 6 times to 10 times. By making the longitudinal stretching ratio satisfy the above range, a polyethylene microporous membrane having the desired physical properties of the present invention can be prepared.
[0063] The stretching in step (c) can be carried out by a roller method or a tenter method, and can be carried out at a temperature ranging from 60°C lower than the melting temperature of polyethylene to the melting temperature range of polyethylene. When the stretching is carried out at a temperature in the above range, the fluidity of the polyethylene resin for effective stretching can be ensured. In detail, uniform stretching is carried out throughout the sheet, and no rupture caused by stretching occurs, so that the stretching can be carried out stably, and therefore a high-quality microporous membrane having uniform air permeability, puncture strength, porosity and other physical properties can be prepared throughout the film. As an example, the stretching can be carried out at 80-140°C or 90-125°C, but is not limited thereto.
[0064] Step (d) is a step of extracting the diluent from the longitudinally stretched sheet and drying it, which is performed by extracting the diluent inside the film with an organic solvent and drying the organic solvent in the film in which the diluent is replaced with the organic solvent. The organic solvent can be used without particular limitation as long as it can extract the diluent. Specifically, in terms of high extraction efficiency and rapid drying, the organic solvent can use methyl ethyl ketone, dichloromethane, hexane, etc.
[0065] Step (d) is preferably performed at a high temperature to increase the solubility of the diluent and the organic solvent, but may be performed at a temperature below 40° C. in view of safety caused by boiling of the organic solvent.
[0066] Step (e) is a step of stretching the dried sheet material in the transverse direction by more than 4 times to form a film, and the stretching ratio, stretching method and stretching temperature of the transverse stretching can be the same as those of the longitudinal stretching, so the specific description is omitted. As an example, the stretching can be carried out at 80-140° C. or 90-125° C., but is not limited thereto.
[0067] Step (f) is a step of subjecting the transversely stretched film to heat treatment, which can be performed using a roll method or a tenter method, and as an example, can be performed at a temperature of 120-140°C.
[0068] In one embodiment, step (f) may include a heat relaxation process to fix the longitudinal length of the transversely stretched film and relax (contract) the transverse width. By including the above heat relaxation process, a polyethylene microporous film having the desired physical properties of the present invention can be prepared.
[0069] Specifically, the polyethylene microporous membrane according to one embodiment is prepared by including the above-mentioned thermal relaxation process, and thus has the characteristics of increased porosity (or air permeability) and significantly improved heat resistance. In particular, a battery applying the above-mentioned microporous membrane can have a low initial resistance and can achieve excellent thermal safety in a hot box evaluation.
[0070] The thermal relaxation process may relax the substrate to 80-100% of the lateral width before the thermal relaxation process.
[0071] The thermal relaxation process may relax the steel sheet to 80-95% or 90-95% of the lateral width before the thermal relaxation process, so as to more effectively achieve the desired physical properties of the present invention.
[0072] In one embodiment, step (f) may include a heat stretching process for fixing the longitudinal length of the transversely stretched film and stretching the transverse width, a heat setting process for fixing the longitudinal and transverse lengths / widths and applying heat, and the above-mentioned heat relaxation process. In a non-limiting manner, the film may be stretched to 120-160% or 120-140% of the transverse width before the heat stretching process in the heat stretching process.
[0073] When the film stretched in the order of the longitudinal stretching step, the extraction step, and the transverse stretching step is heat-treated under the above conditions, a polyethylene microporous film having significantly high air permeability and porosity and significantly improved heat resistance at high temperatures can be prepared, unlike the previous view that it is difficult to simultaneously achieve heat resistance and transmittance above a certain level due to the incompatible relationship between high transmittance and heat resistance. The microporous film having such physical properties is suitable for application in high power / high capacity batteries.
[0074] The present invention provides a diaphragm including the polyethylene microporous membrane as described above. The diaphragm can be used for all known energy storage devices without any particular limitation. However, as a non-limiting example, a diaphragm for a lithium secondary battery can be cited.
[0075] Hereinafter, the embodiments and experimental examples will be specifically illustrated and described. However, the following embodiments and experimental examples are only illustrative of a part, and the technology described in this specification is not limited thereto.
[0076] [Measurement methods of physical properties]
[0077] 1. Weight average molecular weight (g / mol)
[0078] The weight average molecular weight (Mw) was measured by using a high temperature gel permeation chromatograph (GPC) with a model name of PL220 from Agilent Technologies, Inc. PLgel Guard and PLgel Olexis were used as GPC columns, 1,2,4-trichlorobenzene (TCB) was used as a solvent, polystyrene was used as a standard sample, and the analysis was performed at 140°C.
[0079] 2. Thickness of microporous membrane (μm)
[0080] The thickness of the microporous membrane was measured using a contact thickness gauge with a thickness accuracy of 0.1 μm. The measurement was performed using a TESA μ-Hite Electronic Height Gauge manufactured by TESA Corporation and a measuring pressure of 0.63 N.
[0081] 3. Puncture strength (N / μm)
[0082] The puncture strength was measured by installing a pin tip with a diameter of 1.0 mm and a radius of curvature of 0.5 mm in a Universal Test Machine (UTM) 3345 from INSTRON and pressing the microporous membrane at a speed of 120 mm / min. At this time, the puncture strength was calculated by dividing the load (N) at the time of rupture of the microporous membrane by the thickness (μm) of the microporous membrane.
[0083] 4. Air permeability (Darcy)
[0084] The air permeability is measured by using a pore size analyzer (Porometer; CFP-1500-AEL of PMI). Generally, the air permeability is expressed as a Gurley number, but the Gurley number does not correct the effect of thickness, so it is difficult to know the relative permeability according to the pore structure. In order to solve this problem, the air permeability of the present invention is measured by using the Darcy permeability constant calculated by the following mathematical formula 1. Nitrogen is used as the gas, and the average value of the Darcy permeability constant measured in the region of 100-200 psi is calculated.
[0085] [Mathematical formula 1]
[0086] Darcy transmittance constant (C) = (8F·T·V) / (πD 2 (P 2 -1))
[0087] F = flow rate (cc / min)
[0088] T = thickness of sample (mm)
[0089] V = viscosity of the gas (N2 is 0.185 cP)
[0090] D = diameter of sample (mm)
[0091] P = Pressure (psi)
[0092] 5. Porosity (%)
[0093] The porosity of the microporous membrane was calculated using the following Mathematical Formula 2. Specifically, a sample with a width of Acm, a length of Bcm, and a thickness of Tcm was prepared and the mass was measured, and the porosity was calculated by the ratio of the mass of the same volume of resin to the mass of the microporous membrane.
[0094] [Mathematical formula 2]
[0095] Porosity (%) = 100 × {1-M / (A × B × T × ρ)}
[0096] In the above formula 2, M is the mass of the microporous membrane (g), and ρ is the density of the polyethylene resin forming the microporous membrane (g / cm 3 ).
[0097] 6. Transverse shrinkage (%)
[0098] A 15 cm×15 cm microporous film with longitudinal and transverse directions marked with a length of 10 cm was placed in an oven (DKN612 manufactured by Yamato) at a temperature stabilized at 121° C. for 1 hour, and then the length change was measured and the transverse shrinkage was calculated using the following formula 3.
[0099] [Mathematical formula 3]
[0100] Transverse shrinkage (%) = {(transverse length before heating - transverse length after heating) / transverse length before heating} × 100
[0101] 7.PS Index (Performance & Safety Index)
[0102] The PS index of the microporous membrane is an index for simultaneously evaluating power performance and safety, and is obtained by calculation using the following Formula 1.
[0103] [Formula 1]
[0104] PS index = [air permeability (×10 -5 Darcy) × porosity (%) ÷ [transverse shrinkage at 121°C (%)]
[0105] 8. Initial resistance test
[0106] The initial resistance test was performed by using a battery assembled using a polyethylene microporous membrane as a separator. Specifically, the positive electrode using NCM 622 (Ni: Co: Mn = 6: 2: 2) as the active material and the negative electrode using graphite carbon as the active material were wound together with the prepared microporous membrane and placed in an aluminum soft pack, and then injected with an electrolyte containing 1M lithium hexafluorophosphate (LiPF6) dissolved in a solution containing ethylene carbonate, ethyl methyl carbonate and diethyl carbonate in a volume ratio of 3: 5: 2 and sealed, thereby assembling a battery with a capacity of 2Ah. After aging and degassing the assembled battery, it was fully charged to 4.2V and the initial resistance (mΩ) was measured.
[0107] When the initial resistance is 30 mΩ or less, it is confirmed that 50% or more of the capacity is maintained in a discharge test at a 3C rate (C-rate), so the initial resistance value becomes an evaluation index for power characteristics.
[0108] 9. Hot box evaluation
[0109] The hot box evaluation is carried out by using a battery assembled using a polyethylene microporous membrane as a separator. Specifically, the positive electrode using NCM 622 (Ni: Co: Mn = 6: 2: 2) as the active material and the negative electrode using graphite carbon as the active material are wound together with the prepared microporous membrane and placed in an aluminum soft pack, and then injected into a solution containing ethylene carbonate, ethyl methyl carbonate and diethyl carbonate in a volume ratio of 3: 5: 2. 1M of lithium hexafluorophosphate (LiPF6) is dissolved in the electrolyte and sealed to assemble a battery with a capacity of 2Ah. After aging and degassing, the assembled battery is fully charged to 4.2V, placed in an oven, heated at 5°C / min, and placed for 30 minutes after reaching 125°C to measure the changes in the battery.
[0110] If the battery emits smoke or catches fire after being placed at 125°C for 30 minutes, it is judged as a failure. If the battery voltage / current does not change and no smoke or fire occurs, it is judged as a pass.
[0111] <Example 1>
[0112] Using a twin-screw extruder, a weight-average molecular weight of 5.0×10 5 g / mol and a high-density polyethylene resin with a melting temperature of 135°C (0.95 g / cm 3 ) and a paraffin oil having a dynamic viscosity of 80 cSt at 40° C. were melt-kneaded to prepare a melt. The melting temperature was measured using a differential scanning calorimeter (DSC) Discovery DSC250 provided by TA Instruments, and was measured under the conditions of a sample weight of 5 mg and a scanning speed of 10° C. / min.
[0113] The melt was continuously extruded through a T-die, and a sheet having a width of 300 mm and an average thickness of 1100 μm was prepared using a casting roll set at 30°C.
[0114] The sheet was longitudinally stretched by a roller method at a stretching temperature of 95° C. so that the sheet was stretched 7 times, and paraffin oil was extracted from the longitudinally stretched sheet at 25° C. using methylene chloride, and the sheet from which the paraffin oil had been extracted was dried at 60° C. The dried sheet was transversely stretched by a tenter method at a stretching temperature of 122° C. so that the sheet was stretched 8 times.
[0115] The film having been stretched in the transverse direction was heat-treated in the transverse direction at 130° C. using a tenter-type heat-setting device while fixing the length in the longitudinal direction, thereby preparing a microporous film having a thickness of 11.5 μm. Specifically, the heat treatment in the transverse direction was performed by heat-setting for 10 seconds after heat-stretching to 135% in the transverse direction and heat-relaxing (shrinking) to 93% of the width before the heat-relaxation process.
[0116] The physical properties of the finally prepared microporous membrane and the performance of the battery using the microporous membrane are shown in Table 1 below.
[0117] <Example 2>
[0118] A polyethylene microporous membrane was prepared by the same method as in Example 1 except that the heat treatment was performed with the longitudinal and transverse directions fixed, and the results are shown in Table 1.
[0119] <Comparative Example 1>
[0120] The polyethylene microporous membrane was prepared by the same method as in Example 1, except that a polyethylene microporous membrane having a weight average molecular weight of 3.0×10 5 g / mol of a high-density polyethylene resin, and after sequentially stretching to 8 times in the longitudinal and transverse directions, an extraction step was performed, and a heat treatment was performed at 130.5°C. The results are shown in Table 1.
[0121] <Comparative Example 2>
[0122] A polyethylene microporous membrane was prepared by the same method as in Example 1, except that an extraction step was performed after sequentially stretching to 8 times in the longitudinal and transverse directions, and after heat treatment at 132°C and heat stretching to 155% in the transverse direction, heat setting for 10 seconds and heat relaxing (shrinking) to 97% of the width before the heat relaxation process, and the results are shown in Table 1.
[0123] [Table 1]
[0124]
[0125]
[0126] Referring to Table 1, the transverse shrinkage of the microporous membranes of Examples 1 and 2 measured after being placed at 121°C for 1 hour is less than 5%, and the PS index satisfies 110 or more. As a result, the initial resistance of the battery using the microporous membrane is less than 30 mΩ and passes the hot box evaluation, thereby achieving excellent power characteristics and thermal safety at the same time.
[0127] In particular, in Example 1, heat treatment was performed in the transverse direction while the longitudinal length was fixed. Therefore, it can be seen that compared with Example 2 in which heat treatment was performed while the longitudinal and transverse directions were fixed, it has better air permeability, porosity and thermal shrinkage. Therefore, the PS index of Example 1 is about 5 times the PS index of Example 2.
[0128] In the microporous membrane of Comparative Example 1, the diluent extraction step is performed after the longitudinal and transverse stretching steps as in the prior art. As a result, the transverse shrinkage measured after being placed at 121°C for 1 hour is less than 5%, but the PS index is less than 110. Therefore, although the battery using this microporous membrane has excellent thermal safety, it has the disadvantage of greatly reduced power characteristics.
[0129] In the microporous membrane of Comparative Example 2, a diluent extraction step is performed after the longitudinal and transverse stretching steps as in the prior art. As a result, the transverse shrinkage measured after being placed at 121°C for 1 hour exceeds 5%, and the PS index is less than 110. Therefore, the battery using this microporous membrane has the disadvantages of poor thermal safety and power characteristics.
[0130] As described above, in this specification, the present invention is described through specific content and limited embodiments, but this is only provided to help a more comprehensive understanding of the present invention. The present invention is not limited to the above embodiments, and those skilled in the art can make various modifications and variations from these descriptions.
Claims
1. A polyethylene microporous membrane having a thickness of 3-30 μm, a puncture strength of 0.15 N / μm or more, a transverse shrinkage of 5% or less measured after being placed at 121° C. for 1 hour, and a PS index of 110 or more represented by the following formula 1, [Formula 1] PS index = [air permeability × porosity] ÷ [transverse shrinkage at 121°C] In the formula 1, the unit of air permeability is ×10 -5 The unit of Darcy porosity is %, and the unit of transverse shrinkage at 121°C is %.
2. The polyethylene microporous membrane according to claim 1, wherein The air permeability of the polyethylene microporous membrane is 10.0×10 -5 Darcy above.
3. The polyethylene microporous membrane according to claim 1, wherein The porosity of the polyethylene microporous membrane is 55-70%.
4. The polyethylene microporous membrane according to claim 1, wherein The porosity of the polyethylene microporous membrane is 60-70%.
5. The polyethylene microporous membrane according to claim 1, wherein The PS index is 220 or more.
6. The polyethylene microporous membrane according to claim 1, wherein The PS index is 400 or more.
7. The polyethylene microporous membrane according to claim 1, wherein The polyethylene microporous membrane comprises a weight average molecular weight of 1×10 5 g / mol to 10×10 5 g / mol of polyethylene.
8. The polyethylene microporous membrane according to claim 1, wherein The polyethylene microporous membrane is prepared by a wet method including a sequential biaxial stretching process.
9. A method for preparing a polyethylene microporous membrane, comprising the following steps: (a) melt-kneading a mixture containing a polyethylene resin and a diluent by an extruder to prepare a melt; (b) extruding the melt to form a sheet; (c) stretching the sheet longitudinally by more than 4 times; (d) extracting the diluent from the longitudinally stretched sheet and drying it; (e) stretching the dried sheet in the transverse direction by more than 4 times to form a film; as well as (f) subjecting the transversely stretched film to heat treatment.
10. The method for preparing a polyethylene microporous membrane according to claim 9, wherein: The step (f) comprises a heat relaxation process for fixing the longitudinal length and shrinking the transverse width, wherein the transverse width is relaxed to 80-95% of the width before the heat relaxation process.
11. A separator comprising the polyethylene microporous membrane according to any one of claims 1 to 8. 12 . An electrochemical device comprising the separator according to claim 11 .
13. The electrochemical device according to claim 12, wherein: The electrochemical device is a secondary battery including the separator between a positive electrode and a negative electrode.
Citation Information
Patent Citations
Polyolefin microporous membrane
KR1020120032539A