Preparation method of bio-based environment-friendly PU insole

By introducing double bond modifiers and isocyanate-based modified jute fibers into the bio-based PU midsole, the problem of insufficient compatibility and mechanical properties of the bio-based PU midsole is solved, and higher mechanical strength, elasticity and bio-based Degradability expands its application areas and improves sustainability.

CN118955852AInactive Publication Date: 2024-11-15ENPING MEIXIANGDA NEW MATERIALS CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411240612.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing bio-based PU midsole has shortcomings in compatibility, mechanical properties, toughness and durability, which limits its expansion in composite materials applications, and its wear resistance and tear resistance are not as good as traditional petroleum-based PUs.

Method used

Polycaprolactone and allyl glycidyl ether are used for transesterification reaction, double bond modifier is introduced, combined with eugenol and modified jute fibers, and the interface strength and elasticity of the fibers are improved through laccase catalysis and peroxide system. Hexamethylene diisocyanate is also used for surface treatment to form isocyanate-based modified jute fibers, which enhances the mechanical properties and compatibility of the material.

Benefits of technology

It improves the mechanical strength, elasticity and biodegradability of bio-based environmentally friendly PU midsole, enhances the compatibility and durability of materials, expands its application potential in the field of environmentally friendly materials, and reduces its dependence on petroleum-based raw materials. Improves sustainability and environmental protection.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of PU materials, in particular to a preparation method of a bio-based environment-friendly PU insole. The preparation method comprises the following steps: uniformly mixing polyester polyol, bio-based polyol, a chain extender, a catalyst, a foaming agent and a foam stabilizer to obtain a component A; uniformly mixing polyether polyol, hexamethylene diisocyanate, isocyanate modified jute fibers and phosphoric acid to obtain a component B; uniformly mixing the component A and the component B, injecting the mixture into an insole mold, and demolding to obtain the bio-based environment-friendly PU insole. The bio-based environment-friendly PU insole prepared by the invention has excellent mechanical properties, good elasticity and wear resistance, the environment-friendly characteristic is further enhanced due to the relatively high bio-based content, and meanwhile, comfortable wearing experience is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of PU materials, and in particular to a method for preparing a bio-based environmentally friendly PU midsole. Background Art

[0002] In recent years, as people's awareness of environmental protection and sustainable development has increased, bio-based polyurethane (PU) materials have gradually received attention. As a new type of material, bio-based environmentally friendly PU midsoles are widely used in the footwear industry due to their good flexibility, wear resistance and light weight. This type of material is usually synthesized from biological raw materials (such as vegetable oils, natural fibers, etc.), is biodegradable, and meets environmental protection requirements.

[0003] However, most of the existing bio-based PU midsoles are polyester or polyether materials. Polyester materials have high physical strength and low cost, but general fluidity, high molding density, and easy hydrolysis and biodegradation of products; polyether materials have a soft feel, good air permeability, and hydrolysis resistance, but high cost and poor physical properties. Due to the differences in molecular structure and chemical properties between the two types, their compatibility is poor, which may lead to phase separation, affect the mechanical properties, toughness and durability of the material, and limit the application field of composite materials. In addition, although bio-based PU midsoles have advantages in environmental protection, their wear resistance, tear resistance and elasticity may still be inferior to traditional petroleum-based PU.

[0004] Therefore, we propose a method for preparing a bio-based environmentally friendly PU midsole. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a bio-based environmentally friendly PU midsole to solve the problems raised in the prior art.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a bio-based environmentally friendly PU midsole comprises the following steps:

[0008] Step S1: mixing polyester polyol, bio-based polyol, chain extender, catalyst, foaming agent and foam leveling agent, stirring evenly at 50-70° C., and cooling to room temperature to obtain component A;

[0009] Step S2: uniformly mixing polyether polyol, hexamethylene diisocyanate, isocyanate-modified jute fiber and phosphoric acid, prepolymerizing at 70-80° C. for 2-3 hours, and cooling to room temperature to obtain component B;

[0010] Step S3: Mix component A and component B evenly, inject into the midsole mold, and demould after 2-4 minutes to obtain a bio-based environmentally friendly PU midsole.

[0011] Furthermore, the component A comprises the following components by weight: 30-50 parts of polyester polyol, 40-60 parts of bio-based polyol, 5-10 parts of chain extender, 3-7 parts of catalyst, 1-3 parts of foaming agent, and 0.5-2.5 parts of foam leveling agent.

[0012] Furthermore, the bio-based polyol is a cashew nut shell oil bio-based modified polyol.

[0013] Furthermore, the chain extender is a mixture of one or more of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol and diethylene glycol.

[0014] Furthermore, the catalyst is a mixture of one or more of triethylenediamine, diethanolamine, triethanolamine and dibutyltin dilaurate.

[0015] Furthermore, the foaming agent is pure water.

[0016] Furthermore, the foam leveling agent is dimethyl silicone oil.

[0017] Furthermore, the B component includes the following components by weight: 30-40 parts of polyether polyol, 60-70 parts of hexamethylene diisocyanate, 30-40 parts of isocyanate-modified jute fiber, and 0.002-0.010 parts of phosphoric acid.

[0018] Furthermore, the preparation method of the isocyanate-modified jute fiber is as follows:

[0019] Step (1): placing jute fiber in a mixed solution of benzene-ethanol, extracting for 12-14 hours, and drying to obtain pretreated jute fiber;

[0020] Step (2): eugenol and ethanol are mixed evenly, and the pH is adjusted to 3.8-4.2 using an acetic acid-sodium acetate buffer solution, and the pretreated jute fiber and laccase are added and mixed evenly, and the mixture is reacted at 50-60° C. for 3-5 hours, filtered, washed, and dried, and then extracted with acetone for 12-14 hours to obtain jute fiber containing double bonds;

[0021] Step (3): uniformly mixing the double bond-containing jute fiber and the modifier, adjusting the pH to 3.8-4.2 using an acetic acid-sodium acetate buffer solution, adding laccase and tert-butyl hydroperoxide, reacting at 50-60° C. for 22-24 hours, filtering, washing, and drying to obtain modified jute fiber;

[0022] Step (4): uniformly mix hexamethylene diisocyanate and acetone, add modified jute fiber, react at 60-70° C. for 4-6 hours, and obtain isocyanate-modified jute fiber after washing, filtering and drying.

[0023] Furthermore, in the step (1), the volume ratio of benzene-ethanol is 2:1, and the solid-liquid ratio of the mixed solution of jute fiber and benzene-ethanol is 1: (20-40) g / mL.

[0024] Furthermore, in the step (2), the solid-liquid ratio of the pretreated jute fiber and ethanol is 1:(10-12) g / mL, the concentration of eugenol is 5-8 mmol / L, and the concentration of laccase is 1.6-2.0 U / mL.

[0025] Furthermore, in the step (3), the mass ratio of the double-bond jute fiber, the modifier and tert-butyl hydroperoxide is 1:(2-4):(0.1-0.3), and the laccase concentration is 2.0-2.5 U / mL.

[0026] Furthermore, the preparation method of the modifier is as follows:

[0027] Heat polycaprolactone to 100-110°C, evacuate for 1-2 hours, and then add tetrahydrofuran, allyl glycidyl ether and toluene under argon protection and mix evenly. After 3 cycles of "freeze-evacuate-fill with argon", add phosphazene base t-BuP 4 , react at 50-60°C for 46-48h, add dilute hydrochloric acid to terminate the reaction, and obtain the modifier after dissolution, sedimentation and drying.

[0028] In the above technical scheme, polycaprolactone (PCL) and allyl glycidyl ether (AGE) are used as reactants, and phosphazene base t-BuP 4 At the same time, it catalyzes the transesterification reaction of PCL and the ring-opening reaction of AGE, introduces double bonds into the side chains of the polymer, and obtains a modifier containing double bonds, which contains both ether bonds and ester bonds, and can improve the compatibility of polyether polyols and polyester polyols.

[0029] Furthermore, the mass ratio of polycaprolactone, tetrahydrofuran, allyl glycidyl ether and toluene is 1:(0.5-1.0):(1-2):(0.5-1.0), and the phosphazene base t-BuP 4 The dosage is 1-3% of the total mass of polycaprolactone and allyl glycidyl ether.

[0030] Furthermore, in the step (4), the mass ratio of hexamethylene diisocyanate, acetone and modified jute fiber is 1:(40-50):(0.1-0.2).

[0031] Furthermore, the mass ratio of component A to component B is 1:(1.2-1.6).

[0032] Furthermore, the preheating temperature of the midsole mold is 45-60°C.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. A method for preparing a bio-based environmentally friendly PU midsole of the present invention, wherein polycaprolactone has good mechanical strength and elasticity, good compatibility with polymer materials, and excellent biodegradability and biocompatibility. By using polycaprolactone (PCL) and allyl glycidyl ether (AGE) as reactants, using phosphazene base t-BuP4 to simultaneously catalyze the transesterification reaction of PCL and the ring-opening reaction of AGE, a double bond is introduced into the side chain of the polymer to obtain a double bond-containing modifier, which contains both ether bonds and ester bonds, thereby improving the compatibility of polyether polyols and polyester polyols;

[0035] Taking advantage of the fact that eugenol monomers have both phenolic hydroxyl groups and vinyl groups, the lignin on the surface of jute fibers is bridged by laccase to form a transition monomer eugenol, which makes the fiber surface rich in C=C free radical active reaction sites, thereby obtaining jute fibers with hydroxyl groups and containing double bonds. Then, under the laccase / peroxide catalysis system, the C=C double bonds on eugenol are induced to react with the modifier, and the modifier is grafted onto the jute fibers, which can improve the interfacial strength and elasticity of the jute fibers and improve their compatibility with the polymer matrix. Finally, the modified jute fibers are surface treated with hexamethylene diisocyanate, so that the isocyanate groups react with the hydroxyl groups on the surface of the modified jute fibers, thereby obtaining isocyanate-modified jute fibers, which can participate in the polymerization process of polyurethane, thereby not only enhancing the mechanical properties and interfacial bonding strength of the fibers, but also improving the durability and stability of the materials, further expanding their application potential in the field of bio-based environmentally friendly materials.

[0036] 2. The preparation method of a bio-based environmentally friendly PU midsole of the present invention adopts bio-based polyols, which significantly reduces the dependence on petroleum-based raw materials and improves the sustainability and environmental protection of the material; at the same time, the use of isocyanate-modified jute fiber enhances the strength and toughness of the material, while giving the midsole good air permeability; therefore, the bio-based environmentally friendly PU midsole prepared by the present invention has excellent mechanical properties, good elasticity and wear resistance, and the higher bio-based content makes it more environmentally friendly and in line with the concept of sustainable development. DETAILED DESCRIPTION

[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] In this embodiment, polyester polyol: brand CMA-1044, sourced from Jining Liduo Chemical Co., Ltd.; bio-based polyol: cashew nut shell oil bio-based modified polyol, model FX-9014, sourced from Shandong Mobai Chemical Co., Ltd.; dimethyl silicone oil: model PMX-200; polyether polyol: model LEP-330N, sourced from Shandong Hongquan Chemical Technology Co., Ltd.; jute fiber: 1-2 mm long, product number HMS012, sourced from Poyang County Changjiang Textile Co., Ltd.; polycaprolactone: BASF D809 of Germany.

[0039] In the following examples and comparative examples, 1 part is equal to 10 g.

[0040] Embodiment 1: A method for preparing a bio-based environmentally friendly PU midsole, comprising the following processes:

[0041] Step S1: 30 parts of polyester polyol, 40 parts of bio-based polyol, 5 parts of 1,3-propylene glycol, 3 parts of triethylene diamine, 1 part of pure water and 1 part of dimethyl silicone oil are mixed, stirred evenly at 50° C., and cooled to room temperature to obtain component A;

[0042] Step S2: 30 parts of polyether polyol, 60 parts of hexamethylene diisocyanate, 30 parts of isocyanate-modified jute fiber and 0.002 parts of phosphoric acid are uniformly mixed, prepolymerized at 70° C. for 2 hours, and cooled to room temperature to obtain component B;

[0043] Step S3: Component A and component B are mixed evenly in a mass ratio of 1:1.2, injected into a midsole mold at 45° C., and demoulded after 4 minutes to obtain a bio-based environmentally friendly PU midsole;

[0044] The preparation method of isocyanate-modified jute fiber is as follows:

[0045] Step (1): placing 3 parts of jute fiber in 20 mL of a mixed solution of benzene-ethanol, extracting for 12 hours, and drying to obtain pretreated jute fiber;

[0046] Step (2): 5 mmol / L eugenol and 30 parts of ethanol are mixed evenly, and the pH is adjusted to 3.8 using an acetic acid-sodium acetate buffer solution, and 3 parts of pretreated jute fiber and 1.6 U / mL laccase are added and mixed evenly, reacted at 50° C. for 3 hours, filtered, washed, and dried, and extracted with acetone for 12 hours to obtain jute fiber containing double bonds;

[0047] Step (3): 3 parts of jute fiber containing double bonds and 6 parts of a modifier are uniformly mixed, pH is adjusted to 3.8 using an acetic acid-sodium acetate buffer solution, 2.0 U / mL laccase and 0.3 parts of tert-butyl hydroperoxide are added, reacted at 50° C. for 22 hours, filtered, washed, and dried to obtain modified jute fiber;

[0048] Step (4): 30 parts of hexamethylene diisocyanate and 1200 parts of acetone are mixed evenly, 3 parts of modified jute fiber are added, and the mixture is reacted at 60° C. for 4 hours. After washing, filtering and drying, isocyanate-modified jute fiber is obtained;

[0049] The preparation method of the modifier is as follows:

[0050] Heat 6 parts of polycaprolactone to 100°C, evacuate for 1 hour, then add 3 parts of tetrahydrofuran, 6 parts of allyl glycidyl ether and 3 parts of toluene under argon protection and mix well. After 3 cycles of "freeze-evacuate-fill with argon", add 0.12 parts of phosphazene base t-BuP 4 , react at 50°C for 46 hours, add dilute hydrochloric acid to terminate the reaction, and obtain the modifier after dissolution, sedimentation and drying.

[0051] Embodiment 2: A method for preparing a bio-based environmentally friendly PU midsole, comprising the following process:

[0052] Step S1: 40 parts of polyester polyol, 50 parts of bio-based polyol, 8 parts of 1,3-propylene glycol, 5 parts of triethylene diamine, 2 parts of pure water and 2 parts of dimethyl silicone oil are mixed, stirred evenly at 60° C., and cooled to room temperature to obtain component A;

[0053] Step S2: 35 parts of polyether polyol, 65 parts of hexamethylene diisocyanate, 35 parts of isocyanate-modified jute fiber and 0.005 parts of phosphoric acid are uniformly mixed, prepolymerized at 75° C. for 2.5 hours, and cooled to room temperature to obtain component B;

[0054] Step S3: Component A and component B are mixed evenly at a mass ratio of 1:1.5, injected into a midsole mold at 50° C., and demoulded after 3 minutes to obtain a bio-based environmentally friendly PU midsole;

[0055] The preparation method of isocyanate-modified jute fiber is as follows:

[0056] Step (1): placing 6 parts of jute fiber in a mixed solution of 180 parts of benzene-ethanol, extracting for 13 hours, and drying to obtain pretreated jute fiber;

[0057] Step (2): 7 mmol / L eugenol and 66 parts of ethanol are mixed evenly, and the pH is adjusted to 4 using an acetic acid-sodium acetate buffer solution, and 6 parts of pretreated jute fiber and 1.8 U / mL laccase are added and mixed evenly, reacted at 55° C. for 4 hours, filtered, washed, and dried, and extracted with acetone for 13 hours to obtain jute fiber containing double bonds;

[0058] Step (3): 6 parts of double-bond jute fiber and 18 parts of a modifier are uniformly mixed, pH is adjusted to 4 using an acetic acid-sodium acetate buffer solution, 2.2 U / mL laccase and 0.12 parts of tert-butyl hydroperoxide are added, reacted at 55° C. for 23 hours, filtered, washed, and dried to obtain modified jute fiber;

[0059] Step (4): 35 parts of hexamethylene diisocyanate and 1600 parts of acetone are mixed evenly, 6 parts of modified jute fiber are added, and the mixture is reacted at 65° C. for 5 hours. After washing, filtering and drying, isocyanate-modified jute fiber is obtained;

[0060] The preparation method of the modifier is as follows:

[0061] 18 parts of polycaprolactone were heated to 105°C and vacuumed for 1.5 hours. Then, under the protection of argon, 15 parts of tetrahydrofuran, 27 parts of allyl glycidyl ether and 15 parts of toluene were added and mixed evenly. After three cycles of "freezing-vacuuming-argon filling", 0.9 parts of phosphazene base t-BuP 4 , react at 55°C for 47 hours, add dilute hydrochloric acid to terminate the reaction, and obtain the modifier after dissolution, sedimentation and drying.

[0062] Embodiment 3: A method for preparing a bio-based environmentally friendly PU midsole, comprising the following process:

[0063] Step S1: 50 parts of polyester polyol, 60 parts of bio-based polyol, 10 parts of 1,3-propylene glycol, 7 parts of triethylene diamine, 3 parts of pure water and 3 parts of dimethyl silicone oil are mixed, stirred evenly at 70° C., and cooled to room temperature to obtain component A;

[0064] Step S2: 40 parts of polyether polyol, 70 parts of hexamethylene diisocyanate, 40 parts of isocyanate-modified jute fiber and 0.010 parts of phosphoric acid are uniformly mixed, prepolymerized at 80° C. for 3 hours, and cooled to room temperature to obtain component B;

[0065] Step S3: Component A and component B are mixed evenly at a mass ratio of 1:1.5, injected into a midsole mold at 60° C., and demoulded after 2 minutes to obtain a bio-based environmentally friendly PU midsole;

[0066] The preparation method of isocyanate-modified jute fiber is as follows:

[0067] Step (1): 8 parts of jute fiber are placed in a mixed solution of 320 parts of benzene-ethanol, extracted for 14 hours, and dried to obtain pretreated jute fiber;

[0068] Step (2): 8 mmol / L eugenol and 96 parts of ethanol are mixed evenly, and the pH is adjusted to 4.2 using an acetic acid-sodium acetate buffer solution, 8 parts of pretreated jute fiber and 2.0 U / mL laccase are added and mixed evenly, reacted at 60° C. for 5 h, filtered, washed, and dried, and extracted with acetone for 14 h to obtain jute fiber containing double bonds;

[0069] Step (3): 8 parts of double-bond jute fiber and 32 parts of a modifier are uniformly mixed, pH is adjusted to 4.2 using an acetic acid-sodium acetate buffer solution, 2.5 U / mL laccase and 0.24 parts of tert-butyl hydroperoxide are added, reacted at 60° C. for 24 hours, filtered, washed, and dried to obtain modified jute fiber;

[0070] Step (4): 40 parts of hexamethylene diisocyanate and 2000 parts of acetone are mixed evenly, 8 parts of modified jute fiber are added, and the mixture is reacted at 70° C. for 6 hours, and after washing, filtering and drying, isocyanate-modified jute fiber is obtained;

[0071] The preparation method of the modifier is as follows:

[0072] 32 parts of polycaprolactone were heated to 110°C and vacuumed for 2 hours. Then, under the protection of argon, 32 parts of tetrahydrofuran, 64 parts of allyl glycidyl ether and 32 parts of toluene were added and mixed evenly. After three cycles of "freezing-vacuuming-argon filling", 2.88 parts of phosphazene base t-BuP were added. 4 , react at 60°C for 48 hours, add dilute hydrochloric acid to terminate the reaction, and obtain the modifier after dissolution, sedimentation and drying.

[0073] Comparative Example 1: A method for preparing a bio-based environmentally friendly PU midsole, comprising the following processes:

[0074] Compared with Example 2, in Comparative Example 1, the isocyanate-modified jute fiber in step S2 is replaced with hexamethylene diisocyanate of the same mass, and the other steps are the same as those in Example 2.

[0075] Comparative Example 2: A method for preparing a bio-based environmentally friendly PU midsole, comprising the following processes:

[0076] Compared with Example 2, Comparative Example 2 does not include step (2), and the double bond-containing jute fiber in step (3) is replaced by pretreated jute fiber of the same mass, and the other steps are the same as those in Example 2.

[0077] Comparative Example 3: A method for preparing a bio-based environmentally friendly PU midsole, comprising the following processes:

[0078] The preparation method of isocyanate-modified jute fiber is as follows:

[0079] Step (1): placing 6 parts of jute fiber in a mixed solution of 180 parts of benzene-ethanol, extracting for 13 hours, and drying to obtain pretreated jute fiber;

[0080] Step (2): 7 mmol / L eugenol and 66 parts of ethanol are mixed evenly, and the pH is adjusted to 4 using an acetic acid-sodium acetate buffer solution, and 6 parts of pretreated jute fiber and 1.8 U / mL laccase are added and mixed evenly, reacted at 55° C. for 4 hours, filtered, washed, and dried, and extracted with acetone for 13 hours to obtain jute fiber containing double bonds;

[0081] Step (3): 35 parts of hexamethylene diisocyanate and 1600 parts of acetone are mixed evenly, 6 parts of double bond-containing jute fiber are added, and the mixture is reacted at 65° C. for 5 hours. After washing, filtering and drying, isocyanate-modified jute fiber is obtained;

[0082] Compared with Example 2, Comparative Example 3 does not include the preparation method of the modifier, and the other steps are the same as those of Example 2.

[0083] Comparative Example 4: A method for preparing a bio-based environmentally friendly PU midsole, comprising the following processes:

[0084] The preparation method of isocyanate-modified jute fiber is as follows:

[0085] Step (1): placing 6 parts of jute fiber in a mixed solution of 180 parts of benzene-ethanol, extracting for 13 hours, and drying to obtain pretreated jute fiber;

[0086] Step (2): 7 mmol / L eugenol and 66 parts of ethanol are mixed evenly, and the pH is adjusted to 4 using an acetic acid-sodium acetate buffer solution, and 6 parts of pretreated jute fiber and 1.8 U / mL laccase are added and mixed evenly, reacted at 55° C. for 4 hours, filtered, washed, and dried, and extracted with acetone for 13 hours to obtain jute fiber containing double bonds;

[0087] Step (3): 6 parts of double-bond jute fiber and 18 parts of a modifier are uniformly mixed, pH is adjusted to 4 using an acetic acid-sodium acetate buffer solution, 2.2 U / mL laccase and 0.12 parts of tert-butyl hydroperoxide are added, reacted at 55° C. for 23 hours, filtered, washed, and dried to obtain modified jute fiber;

[0088] Step (4): 35 parts of hexamethylene diisocyanate and 1600 parts of acetone are mixed evenly, 6 parts of modified jute fiber are added, and the mixture is reacted at 65° C. for 5 hours, and after washing, filtering and drying, isocyanate-modified jute fiber is obtained;

[0089] Compared with Example 2, in step (3) of Comparative Example 4, the mass ratio of the double bond-containing jute fiber to the modifier is 1:1, and the other steps are the same as those of Example 2.

[0090] Experiment: Take the bio-based environmentally friendly PU midsoles obtained in Examples 1-3 and Comparative Examples 1-4, prepare samples, test their properties respectively and record the test results:

[0091] According to ISO 527-1:2012 and 527-2:2012 [24,25], a Zwick / Roell Z020 universal testing machine was used for static tensile testing. The test crosshead speed of the dumbbell-shaped sample (type 5A) was 100 mm / min. The measurement was carried out at room temperature and the average value was taken. The impact resilience was measured according to GB / T 1681-2009. The sample size was a 13 mm thick and 29 mm diameter disc. The sample was placed horizontally on the rebound tester. The height from the bottom of the steel ball to the surface of the sample was adjusted to 460 mm. The steel ball with a diameter of 12.5 mm was released, and three rebound readings were recorded and the average value was taken. Biobased testing was performed by BETA Laboratory, which is accredited by ISO 17025:2017. C-14 analysis was performed according to ASTM D6866 standard method B to determine the percentage of biobased content in the sample. This standard uses an accelerator mass spectrometer (AMS) for determination.

[0092] Test Results

[0093] Impact resilience / % Tensile strength / MPa Bio-based content / % Example 1 67 7.9 35 Example 2 70 8.2 38 Example 3 68 8.0 36 Comparative Example 1 52 6.5 20 Comparative Example 2 58 7.3 29 Comparative Example 3 55 7.1 26 Comparative Example 4 64 7.6 33

[0094] According to the data in the above table, we can clearly draw the following conclusions:

[0095] 1. Compared with Examples 1-3, the impact resilience, tensile strength and bio-based content of the product obtained in Comparative Example 1 are all reduced, indicating that the isocyanate-modified jute fiber prepared by the present invention has better mechanical properties and biocompatibility, thereby effectively improving the performance of the PU midsole.

[0096] 2. Compared with Examples 1-3, the impact resilience, tensile strength and biobased content of the products obtained in Comparative Examples 2 and 3 are all reduced, which indicates that the present invention uses laccase to catalyze the bridging of lignin on the surface of jute fiber with eugenol to introduce double bonds, which is beneficial to the subsequent reaction; at the same time, the mechanical properties and interfacial compatibility of the jute fiber are further improved by reacting the modifier with the jute fiber containing double bonds, thereby improving the comprehensive performance of the PU midsole.

[0097] 3. Compared with Examples 1-3, the impact resilience, tensile strength and bio-based content of the product obtained in Comparative Example 4 are all reduced. It can be seen that when the amount of modifier added is reduced, the performance of the material will be reduced accordingly.

[0098] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

Claims

1. A method for preparing a bio-based environmentally friendly PU midsole, characterized by: The steps include: Step S1: mixing polyester polyol, bio-based polyol, chain extender, catalyst, foaming agent and foam leveling agent, stirring evenly at 50-70° C., and cooling to room temperature to obtain component A; Step S2: uniformly mixing polyether polyol, hexamethylene diisocyanate, isocyanate-modified jute fiber and phosphoric acid, prepolymerizing at 70-80° C. for 2-3 hours, and cooling to room temperature to obtain component B; Step S3: Mix component A and component B evenly, inject them into the midsole mold, and demould after 2-4 minutes to obtain a bio-based environmentally friendly PU midsole.

2. The method for preparing a bio-based environmentally friendly PU midsole according to claim 1, characterized in that: The component A comprises the following components by weight: 30-50 parts of polyester polyol, 40-60 parts of bio-based polyol, 5-10 parts of chain extender, 3-7 parts of catalyst, 1-3 parts of foaming agent, and 0.5-2.5 parts of foam leveling agent.

3. The method for preparing a bio-based environmentally friendly PU midsole according to claim 2, characterized in that: The chain extender is a mixture of one or more of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol and diethylene glycol.

4. The method for preparing a bio-based environmentally friendly PU midsole according to claim 2, characterized in that: The catalyst is one or more mixtures of triethylenediamine, diethanolamine, triethanolamine and dibutyltin dilaurate.

5. The method for preparing a bio-based environmentally friendly PU midsole according to claim 2, characterized in that: The foaming agent is pure water.

6. The method for preparing a bio-based environmentally friendly PU midsole according to claim 1, characterized in that: The B component comprises the following components by weight: 30-40 parts of polyether polyol, 60-70 parts of hexamethylene diisocyanate, 30-40 parts of isocyanate-modified jute fiber, and 0.002-0.010 parts of phosphoric acid.

7. The method for preparing a bio-based environmentally friendly PU midsole according to claim 6, characterized in that: The preparation method of the isocyanate-modified jute fiber is as follows: Step (1): placing jute fiber in a mixed solution of benzene-ethanol, extracting for 12-14 hours, and drying to obtain pretreated jute fiber; Step (2): eugenol and ethanol are mixed evenly, and the pH is adjusted to 3.8-4.2 using an acetic acid-sodium acetate buffer solution, and the pretreated jute fiber and laccase are added and mixed evenly, and the mixture is reacted at 50-60° C. for 3-5 hours, filtered, washed, and dried, and then extracted with acetone for 12-14 hours to obtain jute fiber containing double bonds; Step (3): uniformly mixing the double bond-containing jute fiber and the modifier, adjusting the pH to 3.8-4.2 using an acetic acid-sodium acetate buffer solution, adding laccase and tert-butyl hydroperoxide, reacting at 50-60° C. for 22-24 hours, filtering, washing, and drying to obtain modified jute fiber; Step (4): uniformly mix hexamethylene diisocyanate and acetone, add modified jute fiber, react at 60-70° C. for 4-6 hours, and obtain isocyanate-modified jute fiber after washing, filtering and drying.

8. The method for preparing a bio-based environmentally friendly PU midsole according to claim 7, characterized in that: The preparation method of the modifier is as follows: Heat polycaprolactone to 100-110°C, evacuate for 1-2 hours, add tetrahydrofuran, allyl glycidyl ether and toluene under argon protection and mix evenly, repeat "freeze-evacuate-fill with argon" for 3 cycles, add phosphazene base t-BuP4, react at 50-60°C for 46-48 hours, add dilute hydrochloric acid to terminate the reaction, and obtain the modifier after dissolution, sedimentation and drying.

9. The method for preparing a bio-based environmentally friendly PU midsole according to claim 1, characterized in that: The mass ratio of the component A to the component B is 1:(1.2-1.6).

10. A bio-based environmentally friendly PU midsole prepared according to the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Water-based UV (ultraviolet) primer for floor and preparation method of water-based UV primer

    CN120310404A

  • Water-based uv primer for floor and preparation method thereof

    CN120310404B

  • Rapidly-formed high-wear-resistance transparent polyurethane sole material and preparation method thereof

    CN120904418A