Catalyst-free oxidation method of oxidized wax

The oxidation wax is prepared by controlling the reaction conditions through the catalyst-free oxidation method, which solves the problem of dark color and complex treatment caused by the catalyst, and achieves lighter product colors and simplified process flow, which is suitable for the production of oxidation waxes with high acid value and high saponification value. .

CN118956451APending Publication Date: 2024-11-15ZHEJIANG HUANGXING CHEM CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411333649.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The use of catalysts in the existing oxidized wax production technology leads to darker product colors and subsequent catalyst separation and complex residue treatment, which limits the development of downstream products.

Method used

Using a catalyst-free oxidation method, the Fischer-Tropsch wax raw material and oxygen are sucked in through a vacuum system, the reaction temperature, pressurization pressure and oxygen concentration are controlled, the reaction pressure is adjusted using nitrogen, and the reaction pressure is heated and oxidized to prepare the oxidized wax.

Benefits of technology

The by-products are reduced, the product is lighter in color, and the problem of catalyst separation and residue treatment is avoided. The oxidized wax with high acid value and high saponification value is prepared by adjusting the reaction parameters, which simplifies the process duration.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of oxidized wax production, and particularly relates to a catalyst-free oxidation method of oxidized wax. In order to solve the problems that in the prior art, when a catalyst is used for catalytic oxidation, the color of a product is dark, and aftertreatment is difficult, the catalyst-free oxidation method of oxidized wax is provided and comprises the steps that a reactor is vacuumized, and then a Fischer-Tropsch wax raw material which is in a liquid state after being heated and oxygen are sucked into the reactor in a negative pressure suction mode through a vacuum pump; raising the temperature of the reactor, and maintaining the temperature to heat and oxidize the Fischer-Tropsch wax raw material; introducing nitrogen into the reactor, and adjusting the reaction pressure to enable the raw materials to continuously react under a pressurization condition; under the condition of maintaining the reaction pressure, oxygen is continuously supplemented in the reaction process, and after the reaction is finished, oxidation reaction materials are discharged from the bottom of the reactor. The invention provides a preparation method of oxidized wax without catalysis of a catalyst, by-products are fewer, the color of the product is lighter, and the problems of subsequent catalyst separation and residue treatment are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oxidized wax production, and in particular relates to a catalyst-free oxidation method of oxidized wax. Background Art

[0002] Oxidized wax has the characteristics of low viscosity, high softening point and high hardness, and has excellent dispersibility for fillers and pigments. It is produced by introducing polar groups such as -OH, -COOH, -CHO, -COC, and -COOR into the non-polar groups of the hydrocarbon group during the oxidation process of the raw wax. Therefore, the structure of the internal chain and the surface properties of the oxidized wax have changed, and its solubility, emulsification, lubrication and other properties have been greatly improved. It can be widely used in rubber processing aids, ink coatings, textile softeners, masterbatches, furniture polishes, cosmetics, wax processing aids and other fields.

[0003] In the prior art, Mn / Co catalysts are usually used to reduce the activation energy of the reaction and accelerate the slow stage of free radical chain initiation. However, the product obtained by this method is slightly darker in color, and the subsequent separation of the catalyst and the treatment of the residue are also relatively complicated, which has certain limitations in the development of downstream products.

[0004] For example, a Chinese invention patent discloses a high-acid-value and low-ester-value oxidized wax, its preparation process and the esterified wax obtained therefrom [application number: 202211128420.9]. The invention patent includes the following steps: the first step is to heat and melt the raw wax, add a certain amount of initiator, non-metallic catalyst and boric acid, mix them evenly, pass the mixed mixture and oxygen-containing gas into a microchannel reactor, and carry out a shallow oxidation reaction at a temperature below 150°C, with a retention time of 5-30 minutes; in the first step reaction, boric acid reacts with the alcohol obtained after oxidation of the raw wax to form a boric ester The intermediate is obtained; in the second step, the product after the first step reaction is heated and melted, a certain amount of initiator is added, and the mixture is evenly mixed, and the mixed material and oxygen-containing gas are introduced into a microchannel reactor to perform a deep oxidation reaction at a temperature of 160-180° C. The retention time is 0.5-25 min to obtain a high-acid-value and low-ester-value oxidized wax with an acid value greater than 60 mgKOH / g and an ester value less than 10 mgKOH / g; the retention time of the second step reaction is shorter than the retention time of the first step reaction, and the flow rate of the oxygen-containing gas in the second step reaction is greater than the flow rate of the oxygen-containing gas in the first step reaction.

[0005] This invention patent uses a non-metallic catalyst for catalytic oxidation, so the above-mentioned complex post-processing problem exists. Summary of the invention

[0006] The object of the present invention is to provide a catalyst-free oxidation method for oxidized wax with simple post-treatment in view of the above problems.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A catalyst-free oxidation method for oxidized wax comprises the following steps:

[0009] Step 1: evacuate the reactor using a vacuum system, and then suck the heated liquid Fischer-Tropsch wax raw material and oxygen into the reactor by negative pressure suction using a vacuum pump;

[0010] Step 2: The reactor is heated and maintained at this temperature to heat and oxidize the Fischer-Tropsch wax raw material;

[0011] Step 3: Introducing nitrogen into the reactor and adjusting the reaction pressure so that the raw materials continue to react under pressurized conditions;

[0012] Step 4: Under the condition of maintaining the above reaction pressure, continuously adding oxygen during the reaction process until the reaction is completed;

[0013] Step 5: Discharge the oxidation reaction material from the bottom of the reactor and cool it to room temperature to obtain oxidized wax.

[0014] In the above-mentioned catalyst-free oxidation method of oxidized wax, in step 1, the liquid level of the Fischer-Tropsch wax feedstock in the reactor is 50%.

[0015] In the above-mentioned catalyst-free oxidation method of oxidized wax, the reactor heating temperature in step 2 is 150-190°C.

[0016] In the above-mentioned catalyst-free oxidation method of oxidized wax, the reactor heating temperature in step 2 is 170°C.

[0017] In the above-mentioned catalyst-free oxidation method of oxidized wax, the heating oxidation time in step 2 is 10-30 minutes.

[0018] In the above-mentioned catalyst-free oxidation method of oxidized wax, the heating oxidation time in step 2 is 20 minutes.

[0019] In the above-mentioned catalyst-free oxidation method of oxidized wax, the pressurization pressure in step three is 0.5-1.5 MPa.

[0020] In the above-mentioned method for catalyst-free oxidation of oxidized wax, the pressurization pressure in step three is 1.0 MPa.

[0021] In the above-mentioned catalyst-free oxidation method of oxidized wax, the pressurized reaction time in step three is 1-2 hours.

[0022] In the above-mentioned catalyst-free oxidation method of oxidized wax, oxygen is added in step 4 so that the oxygen content in the reactor is 20-40%.

[0023] Compared with the prior art, the advantages of the present invention are:

[0024] 1. The present invention provides a method for preparing oxidized wax without the need for a catalyst. Compared with the method of using a catalyst to reduce the activation energy of the reaction for catalytic oxidation, the method has fewer by-products, a lighter product color, and does not cause the problem of subsequent catalyst separation and residue treatment.

[0025] 2. The present invention finds that the acid value and saponification value of the final oxidized wax can be affected by adjusting the reaction temperature, pressurization pressure, oxygen concentration and nitrogen addition time. By adjusting the above parameters, an oxidized wax with a high acid value and a high saponification value that is easy for further esterification reaction is finally obtained. At the same time, adjusting the nitrogen addition time also greatly shortens the entire oxidized wax preparation process. DETAILED DESCRIPTION

[0026] The present invention is further described in detail below in conjunction with specific implementation methods.

[0027] Example 1

[0028] This embodiment provides a catalyst-free oxidation method for oxidized wax, comprising the following steps:

[0029] Step 1: evacuate the reactor using a vacuum system, and then suck the heated liquid Fischer-Tropsch wax raw material and oxygen into the reactor by negative pressure suction using a vacuum pump, and the liquid level of the Fischer-Tropsch wax raw material in the reactor is 50%;

[0030] Step 2: The reactor is heated to 190° C. and maintained at this temperature to heat and oxidize the Fischer-Tropsch wax raw material for 30 minutes;

[0031] Step 3: Introduce nitrogen into the reactor and adjust the reaction pressure to 1.5 MPa, so that the raw materials continue to react under pressurized conditions for 2 hours;

[0032] Step 4: Under the condition of maintaining the above reaction pressure, oxygen is continuously added during the reaction process so that the oxygen content in the reactor is maintained at 40% until the reaction is completed;

[0033] Step 5: Discharge the oxidation reaction material from the bottom of the reactor and cool it to room temperature to obtain oxidized wax.

[0034] The Fischer-Tropsch wax raw material in this embodiment is refined Fischer-Tropsch wax FR80 produced by Zhejiang Huangxing Chemical Co., Ltd.

[0035] The acid value of the oxidized wax prepared in this example was measured to be 67 mgKOH / g, and the saponification value was 100 mgKOH / g.

[0036] Example 2

[0037] This embodiment provides a catalyst-free oxidation method for oxidized wax, comprising the following steps:

[0038] Step 1: evacuate the reactor using a vacuum system, and then suck the heated liquid Fischer-Tropsch wax raw material and oxygen into the reactor by negative pressure suction using a vacuum pump, and the liquid level of the Fischer-Tropsch wax raw material in the reactor is 50%;

[0039] Step 2: The reactor is heated to 150° C. and maintained at this temperature to heat and oxidize the Fischer-Tropsch wax raw material for 10 minutes;

[0040] Step 3: Introduce nitrogen into the reactor and adjust the reaction pressure to 0.5 MPa, so that the raw materials continue to react under pressurized conditions for 1 hour;

[0041] Step 4: Under the condition of maintaining the above reaction pressure, oxygen is continuously added during the reaction process so that the oxygen content in the reactor is maintained at 20% until the reaction is completed;

[0042] Step 5: Discharge the oxidation reaction material from the bottom of the reactor and cool it to room temperature to obtain oxidized wax.

[0043] The Fischer-Tropsch wax raw material in this embodiment is refined Fischer-Tropsch wax FR80 produced by Zhejiang Huangxing Chemical Co., Ltd.

[0044] The acid value of the oxidized wax prepared in this example was measured to be 71 mgKOH / g, and the saponification value was 102 mgKOH / g.

[0045] Example 3

[0046] This embodiment provides a catalyst-free oxidation method for oxidized wax, comprising the following steps:

[0047] Step 1: evacuate the reactor using a vacuum system, and then suck the heated liquid Fischer-Tropsch wax raw material and oxygen into the reactor by negative pressure suction using a vacuum pump, and the liquid level of the Fischer-Tropsch wax raw material in the reactor is 50%;

[0048] Step 2: The reactor is heated to 170° C. and maintained at this temperature to heat and oxidize the Fischer-Tropsch wax raw material for 20 minutes;

[0049] Step 3: Introduce nitrogen into the reactor and adjust the reaction pressure to 1.0 MPa, so that the raw materials continue to react under pressurized conditions for 1.5 hours;

[0050] Step 4: Under the condition of maintaining the above reaction pressure, oxygen is continuously added during the reaction process so that the oxygen content in the reactor is maintained at 30% until the reaction is completed;

[0051] Step 5: Discharge the oxidation reaction material from the bottom of the reactor and cool it to room temperature to obtain oxidized wax.

[0052] The Fischer-Tropsch wax raw material in this embodiment is refined Fischer-Tropsch wax FR80 produced by Zhejiang Huangxing Chemical Co., Ltd.

[0053] The acid value of the oxidized wax prepared in this example was measured to be 73 mgKOH / g, and the saponification value was 109 mgKOH / g.

[0054] Comparative Example 1

[0055] This comparative example provides a catalyst-free oxidation method for oxidized wax, comprising the following steps:

[0056] Step 1: evacuate the reactor using a vacuum system, and then suck the heated liquid Fischer-Tropsch wax raw material and oxygen into the reactor by negative pressure suction using a vacuum pump, and the liquid level of the Fischer-Tropsch wax raw material in the reactor is 50%;

[0057] Step 2: The reactor is heated to 170° C. and maintained at this temperature to heat and oxidize the Fischer-Tropsch wax raw material for 20 minutes;

[0058] Step 3: Introduce nitrogen into the reactor and adjust the reaction pressure to 1.0 MPa, so that the raw materials continue to react under pressurized conditions for 1.5 hours;

[0059] Step 4: Under the condition of maintaining the above reaction pressure, oxygen is continuously added during the reaction process so that the oxygen content in the reactor is maintained at 60% until the reaction is completed;

[0060] Step 5: Discharge the oxidation reaction material from the bottom of the reactor and cool it to room temperature to obtain oxidized wax.

[0061] The Fischer-Tropsch wax raw material in this comparative example is refined Fischer-Tropsch wax FR80 produced by Zhejiang Huangxing Chemical Co., Ltd.

[0062] The acid value of the oxidized wax prepared in this comparative example was measured to be 65 mgKOH / g, and the saponification value was 96 mgKOH / g.

[0063] Comparative Example 2

[0064] This comparative example provides a catalyst-free oxidation method for oxidized wax, comprising the following steps:

[0065] Step 1: evacuate the reactor using a vacuum system, and then suck the heated liquid Fischer-Tropsch wax raw material and oxygen into the reactor by negative pressure suction using a vacuum pump, and the liquid level of the Fischer-Tropsch wax raw material in the reactor is 50%;

[0066] Step 2: The reactor is heated to 170° C. and maintained at this temperature to heat and oxidize the Fischer-Tropsch wax raw material for 20 minutes;

[0067] Step 3: Introduce nitrogen into the reactor and adjust the reaction pressure to 1.0 MPa, so that the raw materials continue to react under pressurized conditions for 1.5 hours;

[0068] Step 4: Under the condition of maintaining the above reaction pressure, oxygen is continuously added during the reaction process so that the oxygen content in the reactor is maintained at 10% until the reaction is completed;

[0069] Step 5: Discharge the oxidation reaction material from the bottom of the reactor and cool it to room temperature to obtain oxidized wax.

[0070] The Fischer-Tropsch wax raw material in this comparative example is refined Fischer-Tropsch wax FR80 produced by Zhejiang Huangxing Chemical Co., Ltd.

[0071] The acid value of the oxidized wax prepared in this comparative example was measured to be 47 mgKOH / g, and the saponification value was 68 mgKOH / g.

[0072] Comparative Example 3

[0073] This comparative example provides a catalyst-free oxidation method for oxidized wax, comprising the following steps:

[0074] Step 1: evacuate the reactor using a vacuum system, and then suck the heated liquid Fischer-Tropsch wax raw material and oxygen into the reactor by negative pressure suction using a vacuum pump, and the liquid level of the Fischer-Tropsch wax raw material in the reactor is 50%;

[0075] Step 2: The reactor was heated to 170°C, nitrogen was introduced into the reactor, and the reaction pressure was adjusted to 1.0 MPa, so that the raw materials were reacted under pressure for 1.5 hours;

[0076] Step 3: Under the condition of maintaining the above reaction pressure, oxygen is continuously added during the reaction process so that the oxygen content in the reactor is maintained at 30% until the reaction is completed;

[0077] Step 4: Discharge the oxidation reaction material from the bottom of the reactor and cool it to room temperature to obtain oxidized wax.

[0078] The Fischer-Tropsch wax raw material in this comparative example is refined Fischer-Tropsch wax FR80 produced by Zhejiang Huangxing Chemical Co., Ltd.

[0079] The acid value of the oxidized wax prepared in this comparative example was measured to be 28 mgKOH / g, and the saponification value was 41 mgKOH / g.

[0080] Comparative Example 4

[0081] This comparative example provides a catalyst-free oxidation method for oxidized wax, comprising the following steps:

[0082] Step 1: evacuate the reactor using a vacuum system, and then suck the heated liquid Fischer-Tropsch wax raw material and oxygen into the reactor by negative pressure suction using a vacuum pump, and the liquid level of the Fischer-Tropsch wax raw material in the reactor is 50%;

[0083] Step 2: The reactor is heated to 170° C. and maintained at this temperature to heat and oxidize the Fischer-Tropsch wax raw material for 5 minutes;

[0084] Step 3: Introduce nitrogen into the reactor and adjust the reaction pressure to 1.0 MPa, so that the raw materials continue to react under pressurized conditions for 1.5 hours;

[0085] Step 4: Under the condition of maintaining the above reaction pressure, oxygen is continuously added during the reaction process so that the oxygen content in the reactor is maintained at 30% until the reaction is completed;

[0086] Step 5: Discharge the oxidation reaction material from the bottom of the reactor and cool it to room temperature to obtain oxidized wax.

[0087] The Fischer-Tropsch wax raw material in this comparative example is refined Fischer-Tropsch wax FR80 produced by Zhejiang Huangxing Chemical Co., Ltd.

[0088] The acid value of the oxidized wax prepared in this comparative example was measured to be 53 mgKOH / g, and the saponification value was 78 mgKOH / g.

[0089] Comparative Example 5

[0090] This comparative example provides a catalyst-free oxidation method for oxidized wax, comprising the following steps:

[0091] Step 1: evacuate the reactor using a vacuum system, and then suck the heated liquid Fischer-Tropsch wax raw material and oxygen into the reactor by negative pressure suction using a vacuum pump, and the liquid level of the Fischer-Tropsch wax raw material in the reactor is 50%;

[0092] Step 2: The reactor is heated to 170° C. and maintained at this temperature to heat and oxidize the Fischer-Tropsch wax raw material for 40 minutes;

[0093] Step 3: Introduce nitrogen into the reactor and adjust the reaction pressure to 1.0 MPa, so that the raw materials continue to react under pressurized conditions for 1.5 hours;

[0094] Step 4: Under the condition of maintaining the above reaction pressure, oxygen is continuously added during the reaction process so that the oxygen content in the reactor is maintained at 30% until the reaction is completed;

[0095] Step 5: Discharge the oxidation reaction material from the bottom of the reactor and cool it to room temperature to obtain oxidized wax.

[0096] The Fischer-Tropsch wax raw material in this comparative example is refined Fischer-Tropsch wax FR80 produced by Zhejiang Huangxing Chemical Co., Ltd.

[0097] The acid value of the oxidized wax prepared in this comparative example was measured to be 68 mgKOH / g, and the saponification value was 99 mgKOH / g.

[0098] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

Claims

1. A catalyst-free oxidation method for oxidized wax, characterized in that: The following steps are involved: Step 1: evacuate the reactor using a vacuum system, and then suck the heated liquid Fischer-Tropsch wax raw material and oxygen into the reactor by negative pressure suction using a vacuum pump; Step 2: The reactor is heated and maintained at this temperature to heat and oxidize the Fischer-Tropsch wax raw material; Step 3: Introducing nitrogen into the reactor and adjusting the reaction pressure so that the raw materials continue to react under pressurized conditions; Step 4: Under the condition of maintaining the above reaction pressure, continuously adding oxygen during the reaction process until the reaction is completed; Step 5: Discharge the oxidation reaction material from the bottom of the reactor and cool it to room temperature to obtain oxidized wax.

2. The catalyst-free oxidation method of an oxidized wax according to claim 1, characterized in that: In the step 1, the liquid level of the Fischer-Tropsch wax raw material in the reactor is 50%.

3. The catalyst-free oxidation method of an oxidized wax according to claim 1, characterized in that: In the step 2, the reactor is heated to a temperature of 150-190°C.

4. The catalyst-free oxidation method of oxidized wax according to claim 3, characterized in that: The reactor is heated to 170°C in step 2.

5. The catalyst-free oxidation method of oxidized wax according to claim 1, characterized in that: The heating oxidation time in the step 2 is 10-30 minutes.

6. The catalyst-free oxidation method of oxidized wax according to claim 5, characterized in that: The heating oxidation time in the step 2 is 20 minutes.

7. The catalyst-free oxidation method of oxidized wax according to claim 1, characterized in that: The pressurization pressure in the step three is 0.5-1.5 MPa.

8. The catalyst-free oxidation method of oxidized wax according to claim 7, characterized in that: The pressurization pressure in the step three is 1.0 MPa.

9. The catalyst-free oxidation method of oxidized wax according to claim 1, characterized in that: The pressure reaction time in step 3 is 1-2h.

10. The catalyst-free oxidation method of oxidized wax according to claim 1, characterized in that: In step 4, oxygen is added to make the oxygen content in the reactor 20-40%.

Citation Information

Patent Citations

  • Preparation method of continuous microchannel of oxidized wax

    CN113797867A

  • Production method for producing oxidized wax without catalytic oxidation

    CN114276836A

  • Improvements relating to the oxidation of residual petroleum waxes

    GB902621A