Method for producing sintered ore by using high-proportion iron ore concentrate
By adding high silicon flux to the sintering ingredients and combining granulation and sintering processes, the problems of fine particle size of iron concentrate and insufficient SiO2 content are solved, the strength and quality of sintering ore are improved, and the sintering process of low ferrosilicon concentrate is realized high proportion of applications and resource utilization.
Patent Information
- Application Number
- CN202411015186.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When using iron concentrate for sintering, poor breathability, low production efficiency, and insufficient SiO2 content of low ferrosilicon concentrate, limits its application ratio in the sintering process.
Add high silicon flux to the sintering ingredients to increase the SiO2 content in the sintered ore to more than 4.9%. Through granulation and sintering processes and combined with air extraction treatment, the sintered ore strength meets the blast furnace smelting requirements.
It has achieved a high proportion of low ferrosilicon concentrate in the sintering process, improved the strength and quality of sintering ore, and broadened the utilization range of iron ore resources for sintering.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sintered ore production, and in particular relates to a method for producing sintered ore by utilizing high-proportion iron concentrate. Background Art
[0002] Sintered ore is the main raw material for blast furnace ironmaking in my country. As my country's steel production capacity continues to maintain a high production trend, a large amount of iron ore resources are needed to provide pigment guarantee. On the one hand, due to the relatively small number of high-grade rich ores in my country, most iron ores need to go through mineral processing to obtain high-grade iron concentrate for sintering and pelletizing. On the other hand, a large amount of hematite and semi-limonite in imported mineral resources have good sintering properties. Therefore, every year my country needs to import a large amount of iron ore from overseas for sintering. Most of the iron concentrate produced by my country through mineral processing is used in the pelletizing process.
[0003] The main problem with using iron concentrate in sintering is that the iron concentrate has a relatively fine particle size, which leads to poor permeability of the sintering material layer and reduced sintering production efficiency. At the same time, since the SiO2 content of iron concentrate is generally low after the beneficiation process, and the liquid phase consolidation of the sintering process requires a certain SiO2 content in the sintered ore to ensure the strength of the sintered ore, this greatly limits the proportion of low-silicon iron concentrate used in the sintering process. Summary of the invention
[0004] The purpose of the present invention is to provide a method for producing sintered ore using high-proportion iron ore concentrate, by adding high-silicon flux during the sintering batching process, ensuring that the SiO2 content of the sintered ore reaches more than 4.9%, thereby ensuring the amount of liquid phase in the sintered ore, and ultimately achieving the purpose of the sintered ore strength meeting the requirements of blast furnace smelting, thereby realizing the high-proportion application of low-silicon iron concentrate in the sintering process.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] The invention discloses a method for producing sintered ore by utilizing high-proportion iron ore concentrate. The method comprises the following steps of mixing raw materials in percentage by mass: 2%-5% of high silicon flux, 20%-40% of low silicon iron ore concentrate A, 0%-20% of low silicon iron ore concentrate B, 15%-35% of iron ore powder C, 4.0%-8.0% of limestone, 1.0%-3.5% of quicklime, 2.0%-7.0% of coke powder, and 20%-40% of returned ore; adding water to the raw materials, mixing them, and then granulating them to obtain a mixture; and sintering the mixture to obtain sintered ore.
[0007] Furthermore, the low silicon iron concentrate A, low silicon iron concentrate B, and iron ore powder C are iron materials, the mass percentage of the low silicon iron concentrate A to the iron material is 20-60%, the mass percentage of the low silicon iron concentrate B to the iron material is 0-30%, and the mass percentage of the iron ore powder C to the iron material is 40-50%.
[0008] Furthermore, the high silicon flux comprises the following components in percentage by mass: CaO 4.00-10.00%, SiO2 30.00-38.00%, MgO 30.00-38.00%, Al2O3 2.00-6.00%, S 0.035-0.20%.
[0009] Furthermore, the low silicon iron concentrate A comprises the following components in percentage by mass: TFe 60.50-68.50%, FeO 25.00-31.50%, CaO 1.00-2.50%, SiO2 0.85-2.15%, MgO 0.65-1.35%, F 0.08-0.45%, P 0.025-0.095%, S 0.50-1.05%.
[0010] Furthermore, the low silicon iron concentrate B comprises the following components in percentage by mass: TFe 61.50-67.50%, FeO 26.00-31.50%, CaO 1.00-2.20%, SiO21.15-2.15%, MgO 1.00-1.80%, F 0.02-0.15%, P 0.025-0.075%, S1.50-3.05%.
[0011] Furthermore, the iron ore powder C includes the following components in percentage by mass: TFe 55.20-62.50%, FeO 0.20-0.80%, CaO 0.10-0.80%, SiO2 3.50-6.30%, MgO 0.05-0.35%, F 0-0.1%, P 0-0.15%, S 0.01-0.08%.
[0012] Furthermore, the basicity of the sintered ore is 1.95-2.05, and the mass percentage of MgO in the sintered ore is 2.1%-2.4%;
[0013] The granulation time is 2-5min;
[0014] The mass percentage of water in the mixture is 7%-9%;
[0015] The ignition time of sintering is 1-3min, and the ignition negative pressure is 3000-6000Pa;
[0016] The sintering process is accompanied by ventilation treatment, and the negative pressure of the ventilation is 9000-12000Pa.
[0017] Compared with the prior art, the beneficial technical effects of the present invention are:
[0018] The present invention ensures the SiO2 content of the sintered ore by adding a high-silicon flux, thereby improving the strength of the sintered ore, solving the problem of using low-silicon iron concentrate in the sintering process, ensuring the quality indicators of the sintered ore while achieving a high proportion of application of the low-silicon iron concentrate in the sintering process, and broadening the iron ore resources for sintering. DETAILED DESCRIPTION
[0019] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0020] The specific process of the method for preparing sintered ore by using steel rolling iron oxide scale of the present invention is as follows:
[0021] Step S1: Prepare the raw materials according to the following mass percentage:
[0022] High silicon flux 2%-5%, low silicon iron concentrate A 20%-40%, low silicon iron concentrate B iron ore powder B 0%-20%, iron ore powder C 15%-35%, limestone 4.0%-8.0%, quicklime 1.0%-3.5%, coke powder 2.0%-7.0%, return ore 20%-40%;
[0023] Low silicon iron concentrate A, low silicon iron concentrate B and iron ore powder C are iron materials, wherein the mass percentage of the low silicon iron concentrate A to the iron material is 20-60%, the mass percentage of the low silicon iron concentrate B to the iron material is 0-30%, and the mass percentage of the iron ore powder C to the iron material is 40-50%.
[0024] The high silicon flux comprises the following components in percentage by mass: CaO 4.00-10.00%, SiO2 30.00-38.00%, MgO 30.00-38.00%, Al2O3 2.00-6.00%, and S 0.035-0.20%.
[0025] Furthermore, the low silicon iron concentrate A comprises the following components in percentage by mass: TFe 60.50-68.50%, FeO2 5.00-31.50%, CaO 1.00-2.50%, SiO2 0.85-2.15%, MgO 0.65-1.35%, F 0.08-0.45%, P 0.025-0.095%, S 0.50-1.05%.
[0026] The low silicon iron concentrate B includes the following components in percentage by mass: TFe 61.50-67.50%, FeO2 6.00-31.50%, CaO 1.00-2.20%, SiO2 1.15-2.15%, MgO 1.00-1.80%, F 0.02-0.15%, P 0.025-0.075%, S 1.50-3.05%.
[0027] The iron ore powder C includes the following components in percentage by mass: TFe 55.20-62.50%, FeO 0.20-0.80%, CaO 0.10-0.80%, SiO2 3.50-6.30%, MgO 0.05-0.35%, F 0-0.1%, P 0-0.15%, S 0.01-0.08%.
[0028] Step S2: adding water to the raw materials, mixing, and granulating to obtain a mixed material.
[0029] Specifically, water is first added to the raw materials in step S1 to mix them once, and after mixing, the obtained mixture is granulated, and the granulation time is 2-5 minutes. The granulation process can be carried out in a granulator. Of course, the present application is not limited to this, and it can also be carried out in other suitable equipment.
[0030] Step S3: sintering the mixture to obtain sintered ore.
[0031] The mass percentage of water in the mixture is 7%-9%. The ignition time of sintering is 1-3 minutes, and the ignition negative pressure is 8000-12000 Pa. The sintering process is accompanied by exhaust treatment, and the exhaust negative pressure is 9000-15000 Pa.
[0032] The sintering process can be carried out on a sintering machine, but the present application is not limited thereto, and other suitable equipment can also be used. The sintering process can be carried out in the following manner:
[0033] The mixed material is evenly distributed on the sintering machine trolley through the distributor to form a certain thickness of the material layer, and then ignited by the igniter of the sintering machine head. The ignition fuel is coke oven gas, and the ignition time is 1-3 minutes. At the same time, the bottom of the sintering machine begins to exhaust air, forming a certain negative pressure under the grate. The ignition negative pressure is 8000-12000Pa. After ignition, the air is extracted from top to bottom through the sintering material layer. The sintering flue gas is discharged into the atmosphere after the desulfurization process. The sintering exhaust negative pressure is 9000-15000Pa. After ignition, the burning zone on the surface of the material layer gradually moves to the lower material layer as the upper fuel is burned. When the burning zone reaches the grate, the sintering process ends and sintered ore is obtained.
[0034] The basicity of the sintered ore of the present invention is 1.95-2.05, and the mass percentage of MgO in the sintered ore is 2.1%-2.4%.
[0035] The method of the present invention is further described below with reference to specific embodiments.
[0036] The specific ingredients of the raw materials used in the following examples are shown in Table 1.
[0037] Table 1 Chemical composition of raw materials used (wt%)
[0038]
[0039] Example 1
[0040] The raw materials and proportions are prepared according to Table 2. The raw materials are mixed in the primary mixer, and then granulated in the secondary mixer. The granulation time is 3 minutes, and the mass percentage of water in the mixture is controlled to be 7.5%. The granulated mixture is evenly distributed on the sintering machine trolley through the distributor, and the material layer thickness is 700mm. It is ignited by the igniter of the sintering machine head. The ignition fuel is coke oven gas. The ignition time is 1.5 minutes. At the same time, the bottom of the sintering machine begins to evacuate, and a certain negative pressure is formed under the grate. The ignition negative pressure is 11000Pa. After ignition, the air is evacuated from top to bottom through the sintering material layer. The sintering flue gas is discharged into the atmosphere after the desulfurization process. The sintering exhaust negative pressure is 13000Pa. After ignition, the burning zone on the surface of the material layer gradually moves to the lower material layer as the upper fuel is burned. When the burning zone reaches the grate, the sintering process ends and sintered ore is obtained.
[0041] The chemical composition and process parameters of the sintered ore are shown in Table 3.
[0042] Example 2
[0043] The raw materials and proportions are prepared according to Table 2. The raw materials are mixed in the primary mixer, and then granulated in the secondary mixer. The granulation time is 4.0 minutes, and the mass percentage of water in the mixture is controlled to be 7.8%. The granulated mixture is evenly distributed on the sintering machine trolley through the distributor, and the material layer thickness is 700mm. It is ignited by the igniter of the sintering machine head. The ignition fuel is coke oven gas. The ignition time is 2.0 minutes. At the same time, the bottom of the sintering machine begins to evacuate, and a certain negative pressure is formed under the grate. The ignition negative pressure is 11000Pa. After ignition, the air is evacuated from top to bottom through the sintering material layer. The sintering flue gas is discharged into the atmosphere after the desulfurization process. The sintering exhaust negative pressure is 13000Pa. After ignition, the burning zone on the surface of the material layer gradually moves to the lower material layer as the upper fuel is burned. When the burning zone reaches the grate, the sintering process ends and sintered ore is obtained.
[0044] Example 3
[0045] The raw materials and proportions are prepared according to Table 3. The raw materials are mixed in the primary mixer, and then granulated in the secondary mixer. The granulation time is 4.5 minutes, and the mass percentage of water in the mixture is controlled to be 7.9%. The granulated mixture is evenly distributed on the sintering machine trolley through the distributor. The material layer thickness is 700mm. It is ignited by the igniter of the sintering machine head. The ignition fuel is coke oven gas. The ignition time is 2.0 minutes. At the same time, the bottom of the sintering machine begins to exhaust air, forming a certain negative pressure under the grate. The ignition negative pressure is 11000Pa. After ignition, the air is evacuated from top to bottom through the sintering material layer. The sintering flue gas is discharged into the atmosphere after the desulfurization process. The sintering exhaust negative pressure is 13000Pa. After ignition, the burning zone on the surface of the material layer gradually moves to the lower material layer as the upper fuel is burned. When the burning zone reaches the grate, the sintering process ends and sintered ore is obtained.
[0046] The chemical composition and process parameters of the sintered ore are shown in Table 3.
[0047] Table 2 Raw material ratio (wt%) of the embodiment
[0048]
[0049]
[0050] Table 3 Chemical composition and process parameters of the sintered ore of the embodiment
[0051]
[0052] It can be seen from Table 3 that the addition of high-proportion low-silicon iron ore concentrate with high-silicon flux can ensure that the SiO2 content of the sintered ore reaches a certain level, thereby ensuring that the sintered ore drum strength can meet the blast furnace smelting requirements, realizing the high-proportion application of low-silicon iron ore concentrate in the sintering process.
[0053] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for producing sintered ore using high-proportion iron concentrate, characterized in that: The raw materials are prepared according to the following mass percentages: high silicon flux 2%-5%, low silicon iron concentrate A 20%-40%, low silicon iron concentrate B iron ore powder B 0%-20%, iron ore powder C 15%-35%, limestone 4.0%-8.0%, quicklime 1.0%-3.5%, coke powder 2.0%-7.0%, and returned ore 20%-40%; the raw materials are mixed with water and granulated to obtain a mixture; the mixture is sintered to obtain a sintered ore.
2. The method for producing sintered ore using high-proportion iron concentrate according to claim 1, characterized in that: The low silicon iron concentrate A, low silicon iron concentrate B and iron ore powder C are iron materials, wherein the mass percentage of the low silicon iron concentrate A to the iron material is 20-60%, the mass percentage of the low silicon iron concentrate B to the iron material is 0-30%, and the mass percentage of the iron ore powder C to the iron material is 40-50%.
3. The method for producing sintered ore using high-proportion iron concentrate according to claim 1, characterized in that: The high silicon flux comprises the following components in percentage by mass: CaO 4.00-10.00%, SiO2 30.00-38.00%, MgO 30.00-38.00%, Al2O3 2.00-6.00%, and S 0.035-0.20%.
4. The method for producing sintered ore using high-proportion iron concentrate according to claim 1, characterized in that: The low silicon iron concentrate A comprises the following components in percentage by mass: TFe 60.50-68.50%, FeO2 5.00-31.50%, CaO 1.00-2.50%, SiO2 0.85-2.15%, MgO 0.65-1.35%, F 0.08-0.45%, P 0.025-0.095%, S 0.50-1.05%.
5. The method for producing sintered ore using high-proportion iron concentrate according to claim 1, characterized in that: The low silicon iron concentrate B comprises the following components in percentage by mass: TFe 61.50-67.50%, FeO2 6.00-31.50%, CaO 1.00-2.20%, SiO2 1.15-2.15%, MgO 1.00-1.80%, F 0.02-0.15%, P 0.025-0.075%, S 1.50-3.05%.
6. The method for producing sintered ore using high-proportion iron concentrate according to claim 1, characterized in that: The iron ore powder C comprises the following components in percentage by mass: TFe 55.20-62.50%, FeO 0.20-0.80%, CaO 0.10-0.80%, SiO2 3.50-6.30%, MgO 0.05-0.35%, F 0-0.1%, P 0-0.15%, S 0.01-0.08%.
7. The method for producing sintered ore using high-proportion iron concentrate according to claim 1, characterized in that: The basicity of the sintered ore is 1.95-2.05, and the mass percentage of MgO in the sintered ore is 2.1%-2.4%; The granulation time is 2-5min; The mass percentage of water in the mixture is 7%-9%; The ignition time of sintering is 1-3min, and the ignition negative pressure is 3000-6000Pa; The sintering process is accompanied by ventilation treatment, and the negative pressure of the ventilation is 9000-12000Pa.
Citation Information
Patent Citations
Method used for preparing sintered ore from high sulfur iron concentrate
CN104531981A
Method for preparing sinter ore by using high-silicon fine ore
CN104651602A
Sintered ore with improved yield and quality by controlling particle size of high-silicon flux and preparation method thereof
CN112195337A
Sintered ore capable of improving yield and quality by controlling particle size of high-silicon flux and method thereof
CN113817919A
Method for preparing sintered ore from high-grade, vanadium rich, chromium-bearing vanadium–titanium magnetite concentrate mixture
WO2019001180A1