Process for preparing acidic metallized pellets from iron tailings for blast furnace ironmaking

The preparation of acidic metallized pellets through weak magnetic-strong magnetic separation and magnetization roasting technology solves the problems of difficult reuse of iron tailings resources and high impurities of blast furnaces, and achieves the effect of reducing resource reuse costs and blast furnace fuel consumption.

CN118957255APending Publication Date: 2024-11-15GANSU JIU STEEL GRP HONGXING IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411195803.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

It is difficult and costly to reuse iron tailings resources, high impurity content, low utilization coefficient, and large coke and fuel consumption in blast furnace process.

Method used

Acid metallized pellets are prepared by weak magnetic-strong magnetic inter-selection system and magnetization baking technology. Through magnetic separation, grinding, granulation, calcination consolidation and direct reduction rotary kiln treatment, it produces acidic properties with high strength and high metallization rate. Metalized pellets are used to replace blast furnace raw materials and reduce silica addition and coke consumption.

Benefits of technology

It reduces the reuse ratio and cost of iron tailings, reduces the impurity content of blast furnaces, improves the utilization coefficient of blast furnaces, and reduces fuel consumption and CO2 emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
Patent Text Reader

Abstract

The invention discloses a process for preparing acidic metallized pellets from iron tailings for blast furnace ironmaking. The process mainly comprises the steps of preselection, magnetizing roasting, magnetic separation, coal-free granulation, high-temperature solidification, rotary kiln reduction and blast furnace ironmaking. According to the method, iron in the iron tailings is subjected to resource recycling, part of SiO2 in the iron tailings can be recycled, the selection ratio of resource recycling of the iron tailings can be reduced, and the stacking amount of the iron tailings and the cost of resource recycling are further reduced. After the acidic metallized pellets are added into the blast furnace burden, the addition amount of blast furnace silica can be reduced, and the proportion of iron elements in the blast furnace burden is increased; blast furnace reduction load can be reduced, and blast furnace utilization coefficient can be improved; and furthermore, the blast furnace coke and coal injection quantity can be reduced, and the blast furnace molten iron cost, fuel consumption and CO2 emission are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy and relates to a process for preparing acidic metallized pellets from iron tailings for blast furnace ironmaking. Background Art

[0002] Iron tailings are tailings produced during the iron ore selection process, with the characteristics of large discharge and certain residual iron and SiO2. At present, all domestic iron tailings resource recycling processes are mainly aimed at the reuse of iron resources, with common problems of large selection ratio, high energy consumption and high cost, resulting in a large amount of iron tailings being stored and unable to be effectively used.

[0003] At the same time, blast furnaces use high-alkalinity, oxidizable iron materials such as oxidized pellets and sintered ore as their main raw materials, and in order to meet the acid-base balance requirements, a large amount of silica is often added to the blast furnace ironmaking, resulting in problems such as high impurity content in the iron-making blast furnace, low utilization coefficient, and high coke and fuel consumption. Summary of the invention

[0004] The purpose of the present invention is to provide a process for preparing acidic metallized pellets from iron tailings for blast furnace ironmaking, so as to solve the problems of great difficulty and high cost in utilizing iron tailings resources and high impurity content, low utilization coefficient, and large coke and fuel consumption in blast furnace processes.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is: A process for preparing acidic metallized pellets from iron tailings for blast furnace ironmaking comprises the following steps: (1) The iron tailings are transported to a weak magnetic-strong magnetic joint separation system with weak magnetic and strong magnetic field strengths of 0.08-0.16T and 1.0-1.5T respectively for magnetic separation. The slurry concentration of the magnetic separation system is 20-40%, and the flow rate of the medium ore washing water is 5-20Kg / min. Pre-selected ore and pre-selected tailings are produced; the pre-selected tailings are discharged to the tailings pond. The mass proportion of hematite and siderite in the iron tailings is ≥50% in the total iron, the mass proportion of SiO2 is ≥25%, and the mass proportion of total iron in the iron tailings is ≥10%.

[0006] (2) Drying the pre-selected ore produced in step (1) by using a drying device, the drying temperature is set at 120°C, and grinding or granulating equipment is used to prepare the dried pre-selected ore to the particle size range required by the magnetic roasting system; if suspended magnetic roasting is used, the particle size range is -0.074 mm, accounting for 50-60%, and if rotary kiln magnetic roasting is used, the particle size range is -30 mm.

[0007] (3) The pre-selected ore that meets the particle size requirements produced in step (2) is transported to a magnetized roasting system for magnetized roasting. The magnetized roasting system is a rotary kiln magnetized roasting system or a suspended magnetized roasting system. The rotary kiln magnetized roasting system has a kiln tail coal blend of 2-5%, a high temperature zone temperature of 700-900°C, and the ratio of magnetite and pseudohematite in the total iron in the magnetized roasted ore reaches more than 90%. The suspended magnetized roasting system uses a reducing gas with CO accounting for 20-50% and the rest being N2. The magnetized roasting temperature is 500-570°C, and the mass ratio of magnetite and pseudohematite in the total iron in the magnetized roasted ore reaches more than 90%.

[0008] (4) Grinding the magnetized roasted ore produced in step (3) to -0.074 mm, accounting for 60-80%, and then conveying it to a magnetic separator and filter press for magnetic separation and filtration. The magnetic field strength of the magnetic separator is 0.08-0.16T, the magnetic field slurry concentration is 20-40%, and the flow rate of the intermediate ore washing water is 5-20Kg / min, and the concentrate and magnetized roasted tailings are produced respectively; the magnetized roasted tailings are discharged to the tailings pond.

[0009] (5) The concentrate produced in step (4) is transported to a mixing device, and bentonite is added at a ratio of 2-5% of the dry weight of the concentrate, and mixed evenly.

[0010] (6) The mixed material produced in step (5) is granulated by a granulator with water, and the amount of water added is 6-9% of the total material amount, and wet balls with uniform particle size of 8-16 mm and strength ≥200N / ball are produced.

[0011] (7) The wet balls produced in step (6) are transported to a roasting and consolidation system. The high-temperature flue gas temperature of the roasting and consolidation system reaches 600-1100°C. The material stays in the roasting and consolidation system for 2-4 hours to complete drying, heating and consolidation. The pellet strength is ≥500N / ball.

[0012] (8) The pellets produced in step (7) are discharged from the roasting and consolidation system into the direct reduction rotary kiln, and at the same time, 10-30% of the mass of the pellets of coal 1 are added to the tail of the direct reduction rotary kiln, wherein the particle size of the coal 1 is 5-25 mm, the volatile matter is less than 20%, the ash content is less than 10%, and the calorific value is greater than 5000 cal / kg; after the pellets, coal 1 and their reaction products enter the high temperature zone, 10-20% of the mass of the pellets of coal 2 are thrown into the head of the direct reduction rotary kiln. The particle size of coal 2 is 5-25mm, the volatile matter is greater than 40%, the ash content is less than 10%, and the calorific value is greater than 5000cal / Kg; the temperature of the high-temperature section of the direct reduction rotary kiln reaches 1100-1200℃, and the length of the high-temperature section reaches 1 / 3-1 / 2 of the length of the whole kiln. The pellets are in the kiln for 2-3.5h to complete the heating and iron oxide reduction, and generate high-temperature metallized pellets with a metallization rate of ≥85% and a temperature of 700-900℃, which are then discharged into the cooling equipment together with the residual carbon.

[0013] (9) After the high-temperature metallized pellets and residual carbon and other materials produced in step (8) are cooled to less than 100° C., magnetic separation is performed by a magnetic drum with a magnetic field strength of 0.08-0.16 T, thereby producing acidic metallized pellets with a strength of ≥2200N / ball and non-magnetic materials mainly composed of residual carbon.

[0014] (10) The acidic metallized pellets produced in step (9) are uniformly added to the blast furnace pellets in a mass ratio of less than 10% for blast furnace smelting, and the non-magnetic material mainly composed of residual carbon is added to the tail of the direct reduction rotary kiln instead of part of coal 1.

[0015] Beneficial effects of the present invention: (1) Reduced iron tailings recycling ratio, tailings stockpile volume and resource recycling costs The present invention not only recycles the iron in the iron tailings, but also recycles part of SiO2 therein, thereby reducing the selection ratio of the iron tailings resource recycling and further reducing the iron tailings stockpile and resource recycling costs.

[0016] (2) Reduce the impurity content in blast furnaces, improve blast furnace utilization coefficient, and reduce blast furnace fuel consumption and molten iron costs After the acidic metallized pellets are added to the blast furnace charge, the amount of silica added to the blast furnace can be reduced and the proportion of iron in the blast furnace charge can be increased; the blast furnace reduction load can be reduced and the blast furnace utilization coefficient can be increased; further, the amount of blast furnace coke and coal injection can be reduced, and the blast furnace molten iron cost, fuel consumption and CO2 emissions can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of the process of the present invention. DETAILED DESCRIPTION Example

[0018] The iron tailings TFe is 20.85%, hematite and siderite account for 56% of the total iron, and SiO2 accounts for ≥39.71%.

[0019] The iron tailings are transported to a weak magnetic-strong magnetic joint separation system with magnetic field strengths of 0.12T and 1.4T respectively for magnetic separation. The slurry concentration of the magnetic separation system is 20-40%, and the flow rate of the intermediate ore washing water is 5-20Kg / min. The output is pre-selected ore with a yield of 68.42%, TFe 26.01%, and SiO2 36.20%, and pre-selected tailings with a yield of 31.58% and TFe 11.78%.

[0020] The pre-selected ore is dried in a rotary kiln with the drying temperature set at 120°C. Grinding equipment is used to grind the dried pre-selected ore to -0.074mm, accounting for 56.22%.

[0021] The pre-selected ore that meets the particle size requirements is transported to the magnetic roasting system for suspended magnetic roasting. The magnetic roasting system uses 40% CO in the reducing gas and the rest is N2. The magnetic roasting temperature is 500-570℃, and the output is 64.85% yield, 27.04% TFe, 38.34% SiO2 of the magnetic roasted ore. The mass ratio of magnetite and pseudohematite in the total iron in the magnetic roasted ore reaches 94.21%.

[0022] The magnetized roasted ore was ground to -0.074mm, accounting for 71.52%, and then transported to the magnetic separation and filter pressing equipment for magnetic separation and filtration. The magnetic field strength of the magnetic separator was 0.12T, the slurry concentration was 20-40%, and the flow rate of the intermediate ore washing water was 5-20Kg / min. The magnetized roasted ore concentrate with a yield of 30.49%, TFe 45.89%, and SiO221.48% and the magnetized roasted tailings with a yield of 34.36% and TFe 10.75% were produced respectively.

[0023] The concentrate is transported to the mixing equipment, and 2.5% of the dry weight of the concentrate is added with bentonite and mixed evenly.

[0024] The mixed material was granulated with water in a granulator, and the amount of water added was 7.22% of the total material amount, producing wet balls with uniform particle size of 8-16 mm and average strength of 466N / ball.

[0025] The wet balls are transported to the chain grate roasting and consolidation system. The high-temperature flue gas of the roasting and consolidation system is provided by the direct reduction rotary kiln. The temperature of the high-temperature flue gas reaches 750-800℃. The material stays in the chain grate rotary kiln for 3 hours to complete drying, heating and consolidation. The average strength of the produced pellets is 715N / ball.

[0026] The pellets are discharged from the roasting and consolidation system into the direct reduction rotary kiln. At the same time, 30% of coal 1 is added to the tail of the direct reduction rotary kiln. Coal 1 has a particle size of 5-25mm, a volatile matter of 13.5%, a fixed carbon of 72.71%, an ash content of 9.33%, and a calorific value of 6400cal / Kg. After the pellets, coal 1 and their reaction products enter the high-temperature zone, 20% of coal 2 is thrown into the head of the direct reduction rotary kiln. Coal 2 has a particle size of 5-25mm, a volatile matter of 42.60%, a fixed carbon of 51.17%, an ash content of 7.59%, and a calorific value of 5200cal / Kg. The temperature of the high-temperature section of the direct reduction rotary kiln is controlled at 1100-1200℃, and the length of the high-temperature section reaches 1 / 3 of the length of the whole kiln. The pellets are in the kiln for 3 hours to complete the heating and iron oxide reduction, and generate high-temperature metallized pellets with a metallization rate of 87.56% and a temperature of 750-820℃, which are then discharged into the cooling equipment together with the residual carbon.

[0027] After the cooling equipment cools the high-temperature metallized pellets and residual carbon and other materials to less than 80°C, magnetic separation is completed through a magnetic drum with a magnetic field strength of 0.12T, producing acidic metallized pellets with an average strength of 2600N / ball, a yield of 22.39%, and TFe 54.41%, and non-magnetic materials mainly composed of residual carbon.

[0028] The acidic metallized pellets were uniformly added to the blast furnace pellets at a mass ratio of 3% for blast furnace smelting, achieving the effects of reducing the molten iron coke ratio by 3.3kg / t, the coal ratio by 3.2kg / t, and the silica by 0.3%. The non-magnetic material mainly composed of residual carbon was added to the tail of the direct reduction rotary kiln to replace part of the coal.

Claims

1. A process for preparing acidic metallized pellets from iron tailings for blast furnace ironmaking, characterized in that The steps include: (1) The iron tailings are transported to the weak magnetic-strong magnetic joint selection system for magnetic separation to produce pre-selected ore and pre-selected tailings; the magnetic field strengths of the weak magnetic and strong magnetic in the weak magnetic-strong magnetic joint selection system are 0.08-0.16T and 1.0-1.5T respectively, the concentration of the magnetic separation slurry is 20-40%, and the flow rate of the middling washing water is 5-20Kg / min; (2) drying the pre-selected ore produced in step (1), and preparing the pre-selected ore to a particle size range required by the magnetization roasting system by using a grinding or granulating device; (3) transporting the pre-selected ore that meets the particle size requirements produced in step (2) to a magnetic roasting system for magnetic roasting to produce magnetic roasted ore; The magnetization roasting system is a rotary kiln magnetization roasting system or a suspension magnetization roasting system. The rotary kiln magnetization roasting system uses 2-5% coal at the kiln tail, and the temperature in the high temperature zone is 700-900°C. The suspension magnetization roasting system uses a reducing gas with CO accounting for 20-50% by volume, and the rest is N2, and the magnetization roasting temperature is 500-570°C. (4) Grinding the magnetized roasted ore produced in step (3) to -0.074 mm, accounting for 60-80%, and then transporting it to a magnetic separator and filter press equipment for magnetic separation and filter press to produce concentrate and magnetized roasted tailings respectively; (5) transporting the concentrate produced in step (4) to a mixing device, adding bentonite, and mixing evenly; (6) The mixed material produced in step (5) is granulated with water using a granulator to produce wet balls with a uniform particle size of 8-16 mm and a strength of ≥200 N / ball; (7) transporting the wet balls produced in step (6) to a roasting and consolidation system, completing drying, heating, and consolidation in the roasting and consolidation system to produce acidic balls with a ball strength of ≥500N / ball; (8) The acidic pellets produced in step (7) are discharged from the roasting and consolidation system into the direct reduction rotary kiln, and coal 1 is added to the tail of the direct reduction rotary kiln. After the pellets, coal 1 and their reaction products enter the high temperature zone, coal 2 is thrown into the head of the direct reduction rotary kiln. The pellets are heated and iron oxides are reduced in the direct reduction rotary kiln to generate high-temperature metallized pellets, which are then discharged into the cooling equipment together with the residual carbon; The particle size of coal 1 added at the end of the direct reduction rotary kiln is 5-25mm, and the addition ratio is 10-30% of the mass of the acidic pellets. The volatile matter of coal 1 is less than 20%, the ash content is less than 10%, and the calorific value is greater than 5000cal / Kg; the particle size of coal 2 thrown into the kiln head is 5-25mm, and the addition ratio is 10-20% of the mass of the acidic pellets. The volatile matter of coal 2 is greater than 40%, the ash content is less than 10%, and the calorific value is greater than 5000cal / Kg; The temperature of the high temperature section of the direct reduction rotary kiln reaches 1100-1200℃, the length of the high temperature section reaches 1 / 3-1 / 2 of the length of the whole kiln, and the pellets stay in the kiln for 2.5-3.5h; (9) After the high-temperature metallized pellets and carbon residue produced in step (8) are cooled by a cooling device, magnetic separation is performed by a magnetic separation device to produce acidic metallized pellets with a strength of ≥2200N / ball and non-magnetic materials mainly composed of carbon residue; (10) The acidic metallized pellets produced in step (9) are added to the blast furnace pellets for blast furnace smelting, and the non-magnetic material mainly composed of residual carbon is added to the tail of the direct reduction rotary kiln to replace part of the coal 1.

2. The process for preparing acidic metallized pellets from iron tailings for blast furnace ironmaking as claimed in claim 1, characterized in that: In step (1), the mass proportion of hematite and siderite in the iron tailings is ≥50% in the total iron, the mass proportion of SiO2 is ≥25%, and the mass proportion of total iron in the iron tailings is ≥10%.

3. The process for preparing acidic metallized pellets from iron tailings for blast furnace ironmaking as claimed in claim 1, characterized in that: In step (2), if suspended magnetization roasting is adopted, the particle size range is -0.074 mm, accounting for 50-60%; if rotary kiln magnetization roasting is adopted, the particle size range is -30 mm; in step (3), the magnetization roasting system is rotary kiln magnetization roasting or suspended magnetization roasting.

4. The process for preparing acidic metallized pellets from iron tailings for blast furnace ironmaking as claimed in claim 1, characterized in that: In step (4), the magnetic field strength of the magnetic separator is 0.08-0.16T, the magnetic field slurry concentration is 20-40%, and the flow rate of the medium ore washing water is 5-20Kg / min.

5. The process for preparing acidic metallized pellets from iron tailings for blast furnace ironmaking as claimed in claim 1, characterized in that: The proportion of bentonite in step (5) is 2-5% of the mass of the high silicon concentrate.

6. The process for preparing acidic metallized pellets from iron tailings for blast furnace ironmaking as claimed in claim 1, characterized in that: The amount of water added in step (6) is 6-9% of the total amount of bentonite and high silicon concentrate.

7. The process for preparing acidic metallized pellets from iron tailings for blast furnace ironmaking as claimed in claim 1, characterized in that: In step (7), the roasting and consolidation system is a chain grate rotary kiln or a vertical furnace. When a chain grate rotary kiln is used, the high-temperature flue gas is provided by the direct reduction rotary kiln in step (8); the temperature of the high-temperature flue gas reaches 600-1100° C., the material stays in the roasting and consolidation system for 2-4 hours, and the output pellet strength is ≥500N / ball.

8. The process for preparing acidic metallized pellets from iron tailings for blast furnace ironmaking as claimed in claim 1, characterized in that: The high-temperature metallized pellets generated in step (8) have a kiln exit temperature of 700-900°C and a metallization rate of ≥85%. The cooling device may be an external circulating water cooling device or a spray cooling device, which can reduce the temperature of the high-temperature mixed material to less than 100°C within 1 hour.

9. The process for preparing acidic metallized pellets from iron tailings for blast furnace ironmaking as claimed in claim 1, characterized in that: In step (9), the magnetic separation is carried out by a magnetic drum method, and the magnetic field strength is 0.08-0.16T.

10. The process for preparing acidic metallized pellets from iron tailings for blast furnace ironmaking according to claim 1, characterized in that: In step (10), the mass ratio of the acidic metallized pellets added to the blast furnace is controlled within 10%.