Low-sulfur vanadium-aluminum intermediate alloy and preparation method thereof
By using magnesium oxide powder, nanocarbon powder and sodium fluoride powder to generate magnesium vapor to remove sulfur impurities during the furnace thermal aluminum smelting process of vanadium aluminum intermediate alloy, the problem of high sulfur impurities in titanium alloy is solved and the ductility of the material is improved and toughness, and reduce production costs, achieving low-cost industrialized preparation.
Patent Information
- Application Number
- CN202411028779.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The existing high sulfur impurities exist in the preparation process of existing vanadium aluminum intermediate alloys, which leads to the titanium alloy being prone to cracking and deforming during processing, and reduces ductility and toughness. The existing sulfur removal method has high cost or poor effect, which cannot meet the high-end titanium. The requirements of alloys for low impurity sulfur content.
Magnesium oxide powder, nanocarbon powder and sodium fluoride powder are used as base materials to generate magnesium vapor and sulfur in the thermal smelting process outside the furnace. The sulfur impurities in the vanadium-aluminum intermediate alloy are removed through the slag of magnesium vapor. The combination is carried out. The catalytic action of sodium fluoride improves reaction activity and efficiency.
The preparation of low-sulfur vanadium aluminum intermediate alloy is realized, which significantly reduces the impurity sulfur content, improves the ductility and toughness of high-end titanium alloys, and reduces production costs, making it suitable for low-cost industrial preparation.
Smart Images

Figure BDA0004969337220000041 
Figure BDA0004969337220000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of master alloy metal materials, and in particular to a low-sulfur vanadium-aluminum master alloy and a preparation method thereof. Background Art
[0002] Vanadium aluminum master alloy is mainly used in the preparation of titanium alloy. It can play the role of solid solution strengthening β phase, significantly reduce the phase transition point, increase hardenability, thereby enhancing the heat treatment strengthening effect, and has good organizational stability at high temperature. Therefore, the amount of master alloy used in titanium alloy accounts for more than 80%. At present, the main methods of preparing vanadium aluminum master alloy are aluminum thermal reduction outside the furnace (also known as "one-step method") or aluminum thermal reduction outside the furnace plus vacuum induction melting method (also known as "two-step method"), and the raw materials used mainly include vanadium pentoxide and aluminum. The preparation process of vanadium pentoxide (V2O5) mainly includes six steps: raw material treatment, sodium roasting, leaching, vanadium precipitation, melting, and wastewater treatment. The chemical reactions related to the vanadium precipitation and melting process are shown in formula (1) and formula (2), respectively:
[0003] 6NaVO3+(NH4)2SO4+2H2SO4=(NH4)2V6O 16 +3Na2SO4+2H2O(1)
[0004] (NH4)2V6O 16 =3V2O5+H2O+2NH3↑(2)
[0005] Due to the inevitable presence of sulfuric acid residue in the ammonium salt vanadium precipitation process, the sulfur content in vanadium pentoxide is generally as high as 0.07%-0.15%, which will cause the produced vanadium aluminum master alloy to have a high content of impurity S. When further produced into titanium alloy, the sulfur element will be concentrated in the grain boundary in the form of sulfide during the processing to form a brittle phase, causing the titanium alloy to be easy to crack or deform, and reducing the ductility and toughness of the titanium alloy. At present, the impurity sulfur content of vanadium aluminum master alloy prepared by the aluminum thermal reduction method outside the furnace or the aluminum thermal reduction method outside the furnace plus vacuum induction melting method is usually 0.02%-0.05%, which cannot meet the stringent requirements of high-end titanium alloys for impurity sulfur content ≤0.002%.
[0006] If magnesium metal blocks are used directly for desulfurization, on the one hand, since the raw materials used in vanadium-aluminum master alloys mainly include vanadium pentoxide and aluminum, the presence of magnesium metal blocks will replace part of the aluminum and directly react with vanadium pentoxide to produce magnesium thermal reduction. The magnesium metal blocks only play the role of reducing and replacing vanadium in vanadium pentoxide, and cannot play the role of desulfurization; on the other hand, the density of magnesium metal blocks is very small, only about 1.74g / cm 3 , compared with vanadium aluminum master alloy about 4.05-5.06g / cm 3Due to the large density of magnesium, the magnesium metal block can easily and quickly float to the surface of the vanadium-aluminum intermediate alloy that needs to be desulfurized, and cannot effectively remove sulfur. Also due to the large difference in density and melting point between the alloy and magnesium, the steel and other industries usually use magnesium-containing cored wires or magnesium gas for desulfurization. For example, CN114438285A discloses a magnesium-containing cored wire for desulfurization of molten steel. However, for the vanadium-aluminum intermediate alloy produced by self-propagating reaction, a large amount of high-melting-point aluminum oxide slag will be generated during the reaction process. These slags play an important role in isolating the vanadium-aluminum intermediate alloy from the air and preventing oxidation and nitridation. The weight of the slag is equivalent to the weight of the generated vanadium-aluminum intermediate alloy, and the melting point of the vanadium-aluminum intermediate alloy (melting point is about 1600-1750℃) is much lower than aluminum oxide (melting point is about 2050℃), so it is impossible to add magnesium to the vanadium-aluminum master alloy in the form of cored wire to achieve the purpose of desulfurization of the vanadium-aluminum master alloy; CN117512267A discloses a method for desulfurizing molten steel using magnesium gas. The temperature of the molten steel is usually lower than 1650℃. Since the self-propagating reaction time for producing the vanadium-aluminum master alloy is usually only about 1 minute, and the instantaneous temperature during the reaction exceeds 2500℃, it is impossible to achieve desulfurization using magnesium gas in the self-propagating reaction process. Summary of the invention
[0007] The object of the present invention is to provide a low-sulfur vanadium aluminum master alloy and a preparation method thereof. The prepared low-sulfur vanadium aluminum master alloy can well meet the requirements of high ductility and high toughness of high-end titanium alloys. In addition, the preparation method has low cost and will not cause a significant increase in the production cost of the vanadium aluminum master alloy, which is convenient for low-cost industrial preparation.
[0008] To achieve the above technical purpose, the present invention provides a low-sulfur vanadium-aluminum master alloy, comprising the following components: 55-87wt% V, 0.0005-0.0015wt% S, and the balance being Al and unavoidable impurities.
[0009] Preferably, the following components are included: 57-85wt% V, 0.0005-0.001wt% S, and the balance is Al and inevitable impurities.
[0010] The present invention also provides a method for preparing a low-sulfur vanadium aluminum master alloy, comprising the following steps: mixing magnesium oxide powder, nano-carbon powder and sodium fluoride powder and placing them as a base material at the bottom of a corundum crucible, and then charging raw materials of vanadium pentoxide powder and aluminum beans into a furnace for aluminothermic smelting outside the furnace to obtain a low-sulfur vanadium aluminum master alloy.
[0011] Preferably, in parts by mass, the magnesium oxide powder is 2.5-6.25 parts, the nano carbon powder is 0.75-1.9 parts, the sodium fluoride powder is 0.16-0.41 parts, the vanadium pentoxide powder is 10000-16000 parts, and the aluminum beans are 9000-9350 parts.
[0012] Preferably, the magnesium oxide powder is 3-5 parts, the nano carbon powder is 1-1.5 parts, the sodium fluoride powder is 0.2-0.35 parts, the vanadium pentoxide powder is 10500-15500 parts, and the aluminum beans are 9100-9250 parts.
[0013] Preferably, the purity of the magnesium oxide powder is above 95%, the purity of the nano carbon powder is above 99.9%, the purity of the sodium fluoride powder is above 98%, the purity of the vanadium pentoxide powder is above 98%, and the purity of the aluminum beans is above 99.7%.
[0014] Preferably, the particle size of the magnesium oxide powder is ≤0.05 mm, the particle size of the nano carbon powder is ≤30 nm, the particle size of the sodium fluoride powder is ≤0.05 mm, the particle size of the vanadium pentoxide is ≤1 mm, and the particle size of the aluminum beans is 8-10 mm.
[0015] Preferably, the aluminothermic smelting outside the furnace comprises the following steps: drying and mixing the weighed magnesium oxide powder, nano-carbon powder and sodium fluoride powder, and placing them evenly on the bottom of a corundum crucible as a base material, and then drying and mixing the weighed vanadium pentoxide powder and aluminum beans, loading them into a furnace, and carrying out alloy smelting by an aluminothermic smelting method outside the furnace to obtain a low-sulfur vanadium aluminum intermediate alloy.
[0016] Preferably, the drying temperature is 90-110° C. and the drying time is 8-12 hours.
[0017] More preferably, the drying temperature is 95-105° C. and the drying time is 10-12 h.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The present invention uses magnesium oxide powder and nano-carbon powder as the base material because magnesium oxide powder and nano-carbon powder will react at high temperature (≥1850°C) under standard atmospheric pressure to generate magnesium vapor. Magnesium and sulfur have strong binding energy. Magnesium vapor can combine with sulfur to form magnesium sulfide during the floating process of the vanadium-aluminum master alloy melt. Low-density magnesium sulfide will float to the upper part of the vanadium-aluminum master alloy in the form of slag, ultimately achieving effective removal of sulfur as an impurity in the vanadium-aluminum master alloy.
[0020] 2. The present invention adds a small amount of sodium fluoride powder to the magnesium oxide powder and nano-carbon powder base material. On the one hand, since the radius of fluorine ions in sodium fluoride is close to that of oxygen ions in magnesium oxide, they can partially replace oxygen ions on the surface of magnesium oxide, causing lattice distortion on the surface of magnesium oxide, increasing the reaction energy of the surface of magnesium oxide, improving its activity, and catalyzing the reaction of magnesium oxide powder and nano-carbon powder; on the other hand, the Gibbs free energy of sodium fluoride is close to that of magnesium oxide, which can ensure that under a lower energy state, the surface activity of sodium fluoride on magnesium oxide is improved, thereby promoting the reaction of magnesium oxide powder and nano-carbon powder.
[0021] 3. The present invention uses magnesium oxide powder with a purity of more than 95%, nano carbon powder with a purity of more than 99.9%, sodium fluoride powder with a purity of more than 98%, vanadium pentoxide powder with a purity of more than 98%, and aluminum beans with a purity of more than 99.7% as raw materials, so that the aluminum hot smelting outside the furnace is carried out smoothly, and it is conducive to the preparation of low-sulfur vanadium aluminum intermediate alloy with low impurity content and good composition uniformity.
[0022] 4. The present invention controls the particle size of magnesium oxide powder to be ≤0.05 mm, the particle size of nano-carbon powder to be ≤30 nm, the particle size of sodium fluoride powder to be ≤0.05 mm, and the particle size of vanadium pentoxide to be ≤1 mm, which is conducive to full contact of the materials. On the one hand, it can promote the reaction of magnesium oxide powder and nano-carbon powder to generate magnesium vapor; on the other hand, it can ensure a high actual yield of vanadium-aluminum master alloy smelting by aluminothermic smelting method outside the furnace.
[0023] 5. The particle size of the aluminum beans in the present invention is controlled to be 8-10 mm, because too small a particle size will cause splashing during aluminum hot smelting outside the furnace; too large a particle size will cause greater component segregation in the vanadium-aluminum intermediate alloy.
[0024] 6. The present invention performs drying treatment on magnesium oxide powder, nano-carbon powder and sodium fluoride powder before using them as base materials, which can effectively remove moisture therein, prevent the moisture from vaporizing at high temperature, isolate the contact between magnesium oxide powder, nano-carbon powder and sodium fluoride, and affect the reaction to generate magnesium vapor.
[0025] 7. The present invention performs drying treatment on vanadium pentoxide powder and aluminum beans before use, which can effectively remove moisture therein and prevent serious splashing during the aluminum hot smelting process outside the furnace.
[0026] 8. The low-sulfur vanadium-aluminum master alloy provided by the present invention has a lower impurity sulfur content, which is beneficial to improving the ductility and toughness of high-end titanium alloys.
[0027] 9. The preparation method provided by the present invention requires low production cost and is convenient for low-cost industrial preparation. DETAILED DESCRIPTION
[0028] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0029] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0030] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0031] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.
[0032] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0033] Raw materials used in the present invention:
[0034] The main components of magnesium oxide powder are: MgO ≥ 95%, CaO ≤ 1%, SiO2 ≤ 0.15%, Al2O3 ≤ 0.1%, Fe ≤ 0.05%.
[0035] The main components of nano carbon powder are: C ≥ 99.9%, S ≤ 0.005%, O ≤ 0.03%, N ≤ 0.01%, Si ≤ 0.02%, and Fe ≤ 0.01%.
[0036] The main components of sodium fluoride powder are: NaF ≥ 98%, SiO2 ≤ 0.5%, Fe ≤ 0.3%.
[0037] The main components of vanadium pentoxide powder are: V2O5≥98%, Fe≤0.1%, Si≤0.1%, C≤0.01%, S≤0.2%.
[0038] The main components of aluminum beans are: Al≥99.7%, Fe≤0.12%, Si≤0.05%, C≤0.015%, S≤0.01%.
[0039] Examples 1-12
[0040] Preparation method of low sulfur vanadium aluminum master alloy:
[0041] (1) Weigh magnesium oxide powder, nano carbon powder and sodium fluoride powder, dry them at 90-110° C. for 8-12 hours, and mix them evenly;
[0042] (2) placing the mixed material evenly at the bottom of a corundum crucible at room temperature;
[0043] (3) Weigh vanadium pentoxide powder and aluminum beans, dry them at 90-110° C. for 8-12 hours, and mix them evenly;
[0044] (4) The mixed material is placed in a corundum crucible at room temperature, and the alloy is smelted by an aluminum heat smelting method outside the furnace to obtain a low-sulfur vanadium aluminum intermediate alloy.
[0045] The low-sulfur vanadium-aluminum master alloys of Examples 1-12 were prepared according to the parameters in Table 1.
[0046] Table 1 Preparation parameters of low sulfur vanadium aluminum master alloys in Examples 1-12 of the present invention
[0047]
[0048]
[0049] The chemical composition analysis of the low-sulfur vanadium aluminum master alloys prepared in Examples 1-12 was performed, and the results are shown in Table 2.
[0050] Table 2 Chemical composition of low sulfur vanadium aluminum master alloys in Examples 1-12 of the present invention wt%
[0051] Alloy composition V Fe Si C S O N Al Example 1 57 0.18 0.12 0.004 0.001 0.016 0.021 margin Example 2 87 0.26 0.16 0.006 0.0015 0.122 0.024 margin Example 3 60 0.20 0.13 0.004 0.0005 0.024 0.020 margin Example 4 85 0.24 0.15 0.005 0.0007 0.131 0.025 margin Example 5 73 0.22 0.13 0.005 0.0006 0.032 0.019 margin Example 6 55 0.17 0.11 0.003 0.0011 0.015 0.020 margin Example 7 57 0.18 0.11 0.003 0.0012 0.017 0.018 margin Example 8 87 0.27 0.15 0.007 0.0014 0.126 0.024 margin Example 9 57 0.17 0.12 0.004 0.001 0.018 0.020 margin Example 10 60 0.19 0.13 0.004 0.0006 0.022 0.021 margin Embodiment 11 84 0.25 0.15 0.007 0.0007 0.124 0.025 margin Example 12 85 0.25 0.16 0.006 0.0007 0.130 0.024 margin
[0052] It can be seen from Table 2 that the low-sulfur vanadium aluminum master alloy prepared by the present invention has stable composition and low impurity sulfur content.
[0053] Comparative Example 1
[0054] The same as Example 1, except that magnesium oxide powder and nano-carbon powder are not added in the alloy smelting by the aluminothermic smelting method outside the furnace.
[0055] The results show that: due to the absence of magnesium vapor generated by the reaction of magnesium oxide powder and nano-carbon powder for desulfurization, the impurity S content in the obtained vanadium-aluminum master alloy is significantly increased compared with Example 1.
[0056] Comparative Example 2
[0057] The same as Example 1, except that no sodium fluoride powder is added during alloy smelting by the aluminothermic smelting method outside the furnace.
[0058] The results showed that due to the lack of sodium fluoride powder as a catalyst for the reaction between magnesium oxide powder and nano-carbon powder, the reaction between magnesium oxide powder and nano-carbon powder was slow, and some materials floated to the surface of the vanadium-aluminum intermediate alloy before reacting, affecting the desulfurization effect.
[0059] Comparative Example 3
[0060] The same as Example 1, except that magnesium fluoride powder is added to replace sodium fluoride during alloy smelting by the aluminothermic smelting method outside the furnace.
[0061] The results showed that due to the large difference in Gibbs free energy between magnesium fluoride and magnesium oxide, a higher energy state is required to achieve the catalytic effect of the reaction between magnesium oxide powder and nano-carbon powder, which affects the effective generation of magnesium vapor and the desulfurization effect.
[0062] Comparative Example 4
[0063] The same as Example 1, except that the magnesium oxide powder, nano carbon powder and sodium fluoride powder are used as base materials without being dried.
[0064] The results showed that due to the presence of moisture in the base material, the magnesium oxide powder and nano-carbon powder did not react fully, and the sodium fluoride powder as a catalyst could not effectively catalyze the reaction, which ultimately led to a significant increase in the residual impurity sulfur content in the prepared vanadium-aluminum intermediate alloy.
[0065] Comparative Example 5
[0066] Same as Example 1, except that the vanadium pentoxide powder and aluminum beans are not dried.
[0067] The results showed that due to the presence of moisture in the raw materials, severe splashing occurred during the aluminum hot smelting process outside the furnace, which ultimately resulted in a significant reduction in the yield of the prepared vanadium-aluminum master alloy, from 99% to 92%.
[0068] Comparative Example 6
[0069] Same as Example 1, except that the corundum crucible is replaced by a graphite crucible.
[0070] The results showed that the C impurity content in the vanadium-aluminum intermediate alloy obtained was significantly increased through detection.
[0071] The chemical composition analysis of the vanadium-aluminum master alloys prepared in Comparative Examples 1-6 was performed, and the results are shown in Table 3.
[0072] Table 3 Chemical composition of vanadium aluminum master alloys of comparative examples 1-6 wt%
[0073] Alloy composition V Fe Si C S O N Al Comparative Example 1 57 0.18 0.12 0.004 0.022 0.018 0.020 margin Comparative Example 2 57 0.19 0.12 0.003 0.015 0.017 0.019 margin Comparative Example 3 57 0.18 0.12 0.004 0.018 0.018 0.020 margin Comparative Example 4 57 0.18 0.12 0.004 0.020 0.018 0.021 margin Comparative Example 5 57 0.19 0.12 0.004 0.001 0.016 0.020 margin Comparative Example 6 57 0.18 0.12 0.052 0.001 0.016 0.020 margin
[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a low-sulfur vanadium-aluminum master alloy, It is characterized in that After mixing magnesium oxide powder, nano-carbon powder and sodium fluoride powder, they are placed at the bottom of a corundum crucible as a base material, and then raw materials such as vanadium pentoxide powder and aluminum beans are charged into a furnace for aluminothermic smelting outside the furnace to obtain a low-sulfur vanadium aluminum intermediate alloy.
2. The preparation method according to claim 1, It is characterized in that By mass, the magnesium oxide powder is 2.5-6.25 parts, the nano carbon powder is 0.75-1.9 parts, the sodium fluoride powder is 0.16-0.41 parts, the vanadium pentoxide powder is 10000-16000 parts, and the aluminum beans are 9000-9350 parts.
3. The preparation method according to claim 1, It is characterized in that The purity of the magnesium oxide powder is above 95%, the purity of the nano carbon powder is above 99.9%, the purity of the sodium fluoride powder is above 98%, the purity of the vanadium pentoxide powder is above 98%, and the purity of the aluminum beans is above 99.7%.
4. The preparation method according to claim 1, It is characterized in that The particle size of the magnesium oxide powder is ≤0.05mm, the particle size of the nano carbon powder is ≤30nm, the particle size of the sodium fluoride powder is ≤0.05mm, the particle size of the vanadium pentoxide is ≤1mm, and the particle size of the aluminum beans is 8-10mm.
5. The preparation method according to claim 1, It is characterized in that The magnesium oxide powder, nano carbon powder, sodium fluoride powder, vanadium pentoxide powder and aluminum beans need to be dried before use, the drying temperature is 90-110° C., and the drying time is 8-12 hours.
6. A low-sulfur vanadium-aluminum master alloy prepared by the preparation method according to any one of claims 1 to 5, It is characterized in that The invention comprises the following components: 55-87 wt % V, 0.0005-0.0015 wt % S, and the balance is Al and inevitable impurities.
7. The low-sulfur vanadium-aluminum master alloy according to claim 6, It is characterized in that The invention comprises the following components: 57-85wt% V, 0.0005-0.001wt% S, and the balance is Al and inevitable impurities.