A composite diaphragm material and its preparation method and application
By using composite materials of polysulfone and polyvinylidene fluoride additives in lithium-ion battery separators, the problem of insufficient thermal stability and wettability of lithium-ion battery separators is solved, and the mechanical strength and lithium-ion transmission capacity of the battery are improved. Ensure long-term stability and safety of the battery.
Patent Information
- Application Number
- CN202210698114.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-20
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-06-20
AI Technical Summary
The existing lithium-ion battery composite separators have shortcomings in thermal stability, wetting and lithium ion transmission capabilities, resulting in battery instability and safety problems.
Polysulfone and polyvinylidene fluoride additives are mixed with solvents, and composite membranes are prepared by soaking and vacuum drying to improve the mechanical strength, thermal stability and wettability of the membranes and ensure uniform transmission of lithium ions.
The high mechanical strength, good thermal stability and wettability of the composite separator are achieved, the stable circulation performance of lithium-ion batteries is extended, the cost and volume of the battery is reduced, and the safety of the battery is improved.
Smart Images

Figure CN115172991B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a composite diaphragm material and a preparation method and application thereof, belonging to the technical field of preparation of lithium ion battery diaphragm microporous membrane materials. Background Art
[0002] With the rapid development of electronic devices, the demand for high-capacity, high-safety, and low-cost lithium metal batteries is becoming increasingly urgent. Among them, lithium-ion battery separators play an extremely critical and important role. The separator is located between the positive and negative electrodes of the battery, acts as an insulator, and provides a path for ion conduction by storing electrolyte. Therefore, factors such as the material, pore structure, porosity, tensile strength, thermal stability, wettability, and thickness of the separator have a significant impact on the performance of the battery. In particular, the thickness of the separator, a thin separator can accommodate the volume expansion during the battery charge and discharge process, and from a cost perspective, a thin separator will reduce costs to a certain extent. Therefore, thin and strong separators have the potential to be widely used in the next generation of high-capacity, high-safety, and low-cost lithium batteries.
[0003] In addition to thickness, the thermal stability of the diaphragm is also one of the determining factors controlling battery safety. During the battery cycle, as heat accumulates, the temperature rises, and the high temperature can cause the diaphragm to shrink or even melt, causing serious safety accidents. In recent years, in order to improve the thermal stability of composite diaphragms, heat-resistant ceramic materials such as Al2O3, SiO2, and TiO2 have been introduced into the diaphragm. The incorporation of these ceramic particles improves the thermal stability of the composite diaphragm to a certain extent, but it greatly increases the cost and volume ratio of the battery, not to mention the incompatibility between the ceramic material and the electrolyte, which causes a significant decrease in the battery's discharge specific capacity. Good wettability can increase the liquid absorption rate of the diaphragm and reduce Li + Impedance during transmission, polyethylene and polypropylene are used as mainstream commercial diaphragms due to their chemical stability, however, poor hydrophobicity and thermal stability are stumbling blocks to their further large-scale application, and are also one of the factors that make batteries unstable and unsafe. There are two main aspects to improve the performance of diaphragms: one is to modify traditional polyolefins, and to design composite diaphragms by coating or grafting organic / inorganic materials on the surface of polyolefins. The other is to find new materials, but currently diaphragms based on new materials still cannot simultaneously meet all the expected properties of an ideal diaphragm. Therefore, it is very necessary to provide a new composite diaphragm material and a preparation method thereof that have both high mechanical strength and wettability. Summary of the invention
[0004] In order to solve the deficiencies of existing polyethylene-based lithium metal battery composite diaphragms in terms of thermal stability, wettability, lithium ion transmission ability and stability, the present invention provides a composite diaphragm material and a preparation method and application thereof.
[0005] The technical solution of the present invention:
[0006] One of the purposes of the present invention is to provide a method for preparing a composite diaphragm material, the method comprising the following steps:
[0007] S1, mixing a polysulfone additive, a polyvinylidene fluoride additive and a solvent, heating and stirring until completely dissolved, and cooling to room temperature to obtain an additive solution;
[0008] S2, soaking the membrane substrate in the additive solution, and taking out the film after it is fully wetted;
[0009] S3, spread the film flat on a glass plate, scrape off excess slurry on the surface with a scraper, and vacuum dry for 8-12 hours to obtain a composite diaphragm.
[0010] It is further defined that the polysulfone additive is one or a mixture of two or more of polysulfone, polyethersulfone and polyphenylsulfone in any proportion.
[0011] It is further defined that the polyvinylidene fluoride additive is one or a mixture of two or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, and polyvinylidene fluoride-chlorotrifluoroethylene in any proportion.
[0012] It is further defined that the solvent is one or a mixture of two or more of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide in any proportion.
[0013] It is further defined that the sum of the masses of the polysulfone additive and the polyvinylidene fluoride additive is 10% of the total mass of the additive solution.
[0014] It is further defined that the mass of the polysulfone additive is 3% to 7% of the total mass of the additive solution.
[0015] It is further defined that the mass of the polyvinylidene fluoride additive is 3% to 7% of the total mass of the additive solution.
[0016] It is further defined that the heating temperature in S1 is 50°C to 80°C.
[0017] It is further defined that the stirring time in S1 is 30-60 min.
[0018] The second object of the present invention is to provide a composite diaphragm material, which is prepared by the above method. The composite diaphragm material is intended to fully improve the thermal stability, wettability and uniform lithium ion transmission ability of the diaphragm and the long-term stable charge and discharge performance of the battery.
[0019] The third object of the present invention is to provide an application of the above-mentioned composite diaphragm material, wherein the composite diaphragm material is used as a primary battery or secondary battery diaphragm material.
[0020] The present invention immerses PE in a mixed slurry of PSU (polysulfone) and PVDF (polyvinylidene fluoride). PSU and PVDF fill the uneven pore size of PE, making PESV have higher porosity and more uniform pore distribution. A PESV ultra-stable composite diaphragm with a thickness of 16μm is reasonably designed. The PSU with good rigidity and thermal stability and the PVDF with affinity for electrolyte make the PESV composite diaphragm have both high mechanical strength and wettability, and can be stably cycled for a long time in the battery. Compared with the prior art, this patent also has the following beneficial effects:
[0021] (1) The present invention uses a rigid polysulfone material PSU with a large number of benzene rings as one of the membrane additives. The additive soaks the PE membrane so that the mechanical strength of the prepared composite membrane is greatly improved to 125MPa; and the polysulfone material PSU has good thermal stability, and can also greatly improve the thermal stability of the composite membrane. In addition, the polysulfone PSU has a strong binding energy with lithium ions, which enables the composite membrane to evenly transmit lithium ions, so that the assembled lithium ion battery can be stably cycled for a long time without the formation of obvious lithium dendrites. Among them, the lithium ion battery is a lithium iron phosphate or lithium cobalt oxide positive electrode to lithium negative electrode half-cell.
[0022] (2) The present invention uses polyvinylidene fluoride (PVDF) with excellent electrolyte wettability as another diaphragm additive, so that the wettability of the prepared composite diaphragm is significantly improved, and the impedance of the assembled lithium ion battery is reduced. The lithium ion battery is a lithium iron phosphate or lithium cobalt oxide positive electrode with a lithium negative electrode half-cell.
[0023] (3) The composite membrane provided by the present invention is simple to prepare and easy to implement, and also has the advantages of high production efficiency and low manufacturing cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a stress-strain comparison diagram of the composite diaphragm PESV prepared in Example 4 and commercial polyethylene PE;
[0025] Figure 2 This is a comparison chart of the liquid absorption rate of the composite diaphragm PESV prepared in Example 4 and the commercial polyethylene PE;
[0026] Figure 3 Schematic diagram of the electrolyte contact angle of the composite diaphragm PESV prepared in Example 4;
[0027] Figure 4 Schematic diagram of the electrolyte contact angle of commercial polyethylene PE;
[0028] Figure 5 LSV diagram of stainless steel (SS)||Li battery assembled with PESV and PE as separators respectively;
[0029] Figure 6 The stable cycle performance diagram of Li / Li symmetric battery assembled with PESV and PE as separators respectively;
[0030] Figure 7 The long cycle performance diagram of LFP / Li half-cell assembled with PESV and PE as separators respectively;
[0031] Figure 8 This is a comparison chart of the thermal stability of the composite diaphragm PESV prepared in Example 4 and commercial polyethylene PE. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0033] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.
[0034] The following examples relate to the manufacturers and models of medicines:
[0035] The chemical formula of polysulfone PSU is [C6H4-4-C(CH3)2C6H4-4-OC6H4-4-SO2C6H4-4-O] n , the structural formula is: Model P303212, Mn is 35000~80000; chemical formula of polyvinylidene fluoride PVDF is (C2H2F2) n , the structural formula is: Model 5130, Mn is 300,000 to 1.1 million.
[0036] Comparative Example 1:
[0037] Commercial polyethylene PE was selected as a comparative sample, and the thickness of the diaphragm was measured with a spiral micrometer, which was 16 μm. The commercial polyethylene PE film was punched into circular sheets with a punching machine for use in battery equipment.
[0038] Embodiment 2:
[0039] The specific process of preparing the composite diaphragm material in this embodiment is carried out according to the following steps:
[0040] (1) mixing polysulfone PSU, polyvinylidene fluoride PVDF and solvent NMP in a mass ratio of 3:7:90;
[0041] (2) stirring the mixed solution in an oil bath at 80° C. for 30 min until the polysulfone PSU and polyvinylidene fluoride PVDF are completely dissolved, and then cooling to room temperature to obtain an additive solution;
[0042] (3) spreading the additive solution obtained in step (2) onto a culture dish, soaking the commercial polyethylene PE in the additive solution, and taking it out after it is fully soaked at room temperature;
[0043] (4) The film was spread flat on a glass plate, and the excess slurry on the surface was scraped off with a scraper. The film was vacuum dried for 12 h to obtain a composite diaphragm.
[0044] (5) The thickness of the composite diaphragm obtained in step (4) was measured by a spiral micrometer, and the thickness was 16 μm. The composite diaphragm was punched into circular sheets for use in battery equipment using a punching machine.
[0045] Embodiment 3:
[0046] The difference between this embodiment and embodiment 2 is that in step (1), the mass ratio of polysulfone PSU, polyvinylidene fluoride PVDF and solvent NMP is 4:6:90, and the rest of the operation process and parameter settings are the same as those in embodiment 2.
[0047] The specific operation process is as follows:
[0048] (1) mixing polysulfone PSU, polyvinylidene fluoride PVDF and solvent NMP in a mass ratio of 4:6:90;
[0049] (2) stirring the mixed solution in an oil bath at 80° C. for 30 min until the polysulfone PSU and polyvinylidene fluoride PVDF are completely dissolved, and then cooling to room temperature to obtain an additive solution;
[0050] (3) spreading the additive solution obtained in step (2) onto a culture dish, soaking the commercial polyethylene PE in the additive solution, and taking it out after it is fully soaked at room temperature;
[0051] (4) The film was spread flat on a glass plate, and the excess slurry on the surface was scraped off with a scraper. The film was vacuum dried for 12 h to obtain a composite diaphragm.
[0052] (5) The thickness of the composite diaphragm obtained in step (4) was measured by a micrometer and found to be 16 μm. The composite diaphragm was punched into circular sheets by a punching machine for use in battery equipment.
[0053] Embodiment 4:
[0054] The difference between this embodiment and embodiment 2 is that in step (1), the mass ratio of polysulfone PSU, polyvinylidene fluoride PVDF and solvent NMP is 5:5:90, and the rest of the operation process and parameter settings are the same as those in embodiment 2.
[0055] The specific operation process is as follows:
[0056] (1) Mixing polysulfone PSU, polyvinylidene fluoride PVDF and solvent NMP in a mass ratio of 5:5:90;
[0057] (2) stirring the mixed solution in an oil bath at 80° C. for 30 min until the polysulfone PSU and polyvinylidene fluoride PVDF are completely dissolved, and then cooling to room temperature to obtain an additive solution;
[0058] (3) spreading the additive solution obtained in step (2) onto a culture dish, soaking the commercial polyethylene PE in the additive solution, and taking it out after it is fully soaked at room temperature;
[0059] (4) The film was spread flat on a glass plate, and the excess slurry on the surface was scraped off with a scraper. The film was vacuum dried for 12 h to obtain a composite membrane, which was recorded as PESV.
[0060] (5) The thickness of the composite diaphragm obtained in step (4) was measured by a micrometer and found to be 16 μm. The composite diaphragm was punched into circular sheets by a punching machine for use in battery equipment.
[0061] Embodiment 5:
[0062] The difference between this embodiment and embodiment 2 is that in step (1), the mass ratio of polysulfone PSU, polyvinylidene fluoride PVDF and solvent NMP is 6:4:90, and the rest of the operation process and parameter settings are the same as those in embodiment 2.
[0063] The specific operation process is as follows:
[0064] (1) Mixing polysulfone PSU, polyvinylidene fluoride PVDF and solvent NMP in a mass ratio of 6:4:90;
[0065] (2) stirring the mixed solution in an oil bath at 80° C. for 30 min until the polysulfone PSU and polyvinylidene fluoride PVDF are completely dissolved, and then cooling to room temperature to obtain an additive solution;
[0066] (3) spreading the additive solution obtained in step (2) onto a culture dish, soaking the commercial polyethylene PE in the additive solution, and taking it out after it is fully soaked at room temperature;
[0067] (4) The film was spread flat on a glass plate, and the excess slurry on the surface was scraped off with a scraper. The film was vacuum dried for 12 h to obtain a composite diaphragm.
[0068] (5) The thickness of the composite diaphragm obtained in step (4) was measured by a micrometer and found to be 16 μm. The composite diaphragm was punched into circular sheets by a punching machine for use in battery equipment.
[0069] Embodiment 6:
[0070] The difference between this embodiment and embodiment 2 is that in step (1), the mass ratio of polysulfone PSU, polyvinylidene fluoride PVDF and solvent NMP is 7:3:90, and the rest of the operation process and parameter settings are the same as those in embodiment 2.
[0071] The specific operation process is as follows:
[0072] (1) mixing polysulfone PSU, polyvinylidene fluoride PVDF and solvent NMP in a mass ratio of 7:3:90;
[0073] (2) stirring the mixed solution in an oil bath at 80° C. for 30 min until the polysulfone PSU and polyvinylidene fluoride PVDF are completely dissolved, and then cooling to room temperature to obtain an additive solution;
[0074] (3) spreading the additive solution obtained in step (2) onto a culture dish, soaking the commercial polyethylene PE in the additive solution, and taking it out after it is fully soaked at room temperature;
[0075] (4) The film was spread flat on a glass plate, and the excess slurry on the surface was scraped off with a scraper. The film was vacuum dried for 12 h to obtain a composite diaphragm.
[0076] (5) The thickness of the composite diaphragm obtained in step (4) was measured by a micrometer and found to be 16 μm. The composite diaphragm was punched into circular sheets by a punching machine for use in battery equipment.
[0077] Effect example 1:
[0078] The mechanical properties and porosity of the composite diaphragms prepared in Examples 2 to 6 and the commercial polyethylene PE of Comparative Example 1 were characterized, and the results are shown in Table 1 below:
[0079] Table 1
[0080] Serial number Elongation at break (%) Mechanical strength (MPa) Porosity (%) Comparative Example 1 102.5 78 42 Example 2 145.4 85 51 Example 3 138.9 94 58 Example 4 130.8 104 65 Example 5 118.6 112 60 Example 6 109.3 125 52
[0081] It can be seen from Table 1 above that the porosity and mechanical properties of the composite membranes prepared in Examples 2 to 6 are higher than those of commercial polyethylene PE, and as the mass ratio of polysulfone PSU increases, the mechanical properties are greatly and steadily improved; and as the mass ratio of polyvinylidene fluoride PVDF decreases, the toughness will also decrease accordingly; but the porosity of the composite membrane will show a trend of first increasing and then decreasing. Considering the mechanical strength, toughness and porosity of the composite membrane, it is found that the performance of the composite membrane prepared when the mass ratio of the two additives is 5% (Example 4) is the most outstanding. While improving the mechanical strength, the toughness of the membrane is not sacrificed, and at the same time, the membrane has a very high porosity, reaching 65%.
[0082] Effect example 2:
[0083] The stress-strain, liquid absorption rate, electrolyte contact angle and thermal stability of the composite diaphragm PESV prepared in Example 4 and the commercial polyethylene PE in Comparative Example 1 were characterized, and the results are as follows:
[0084] (1) Figure 1 The stress-strain comparison diagram of the composite diaphragm PESV prepared in Example 4 and the commercial polyethylene PE is shown in FIG. Figure 1 It can be seen that the mechanical strength of PE can reach 78MPa, while the mechanical strength of the PESV composite diaphragm is as high as 104MPa. The elongation at break of PE is 102%, while the elongation at break of the PESV composite diaphragm is as high as 130% due to the addition of flexible PVDF. It can be seen that the composite diaphragm PESV prepared in Example 4 improves the mechanical strength without sacrificing the toughness of the composite diaphragm, and takes both strength and toughness into account. This is because the rigidity of PSU and the toughness of PVDF make the PESV composite diaphragm have higher mechanical strength and toughness on the basis of the PE diaphragm.
[0085] (2) The composite diaphragm PESV and commercial polyethylene PE were immersed in the electrolyte and the diaphragm mass was measured every 5 minutes. The results are as follows: Figure 2 As shown by Figure 2 It can be seen that the electrolyte absorption rate of the PSEV composite membrane is stable at 60%, while that of PE is stable at 52.5%. It can be seen that the composite membrane PESV prepared in Example 4 has good wettability.
[0086] (3) Figure 3 and Figure 4 Schematic diagrams of contact angles of the composite diaphragm PESV prepared in Example 4 and the commercial polyethylene PE electrolyte in Comparative Example 1. It can be seen from the figure that the contact angle of PE is as high as 48° due to the hydrophobicity of its surface, while the contact angle of the composite diaphragm PESV is only 20°. This is because the good interaction between PSU and the electrolyte and the electrolytic affinity of PVDF make the PESV composite diaphragm show certain electrolytic affinity performance.
[0087] (4) Figure 8 This is a comparison chart of the thermal stability of the composite diaphragm PESV prepared in Example 4 and commercial polyethylene PE. Infrared thermal imaging (FLIR) is used to intuitively feel and compare the morphology of PESV and PE diaphragms at different temperatures. Figure 8 It can be seen that the PESV composite diaphragm can still maintain most of its morphology intact at 150°C, while the commercial mainstream PE diaphragm undergoes obvious deformation at 60°C.
[0088] Effect example 3:
[0089] (1) The diaphragm should maintain at least 4.5V (vs Li + / Li) electrochemical stability, because during battery application, the voltage often reaches this value or even higher. Therefore, the composite separator PESV prepared in Example 4 and the commercial polyethylene PE of Comparative Example 1 were used to assemble stainless steel (SS)||Li batteries, and their electrochemical oxidation windows were tested and compared. The results are as follows Figure 5 As shown, the battery using the PESV composite separator is 4.5V (vs Li + / Li), while the battery using PE separator has a voltage rise at 4.0V (vsLi + The results show that the addition of PSU and PVDF improves the electrochemical stability of the PESV composite membrane, mainly because the bond energy of S=O in PSU is 522 kJ·mol -1 The bond energy of CF in PVDF is 413 kJ·mol higher than that of CH in PE. -1 , so the decomposition of PESV is more difficult than PE itself.
[0090] (2) In order to further study the ability of the composite separator to inhibit lithium dendrites, the -2 At a current density of , the PE and PESV separators were assembled into a symmetric Li||Li battery. The test results are shown in Figure 6 As shown, the battery assembled with the PESV composite separator cycled stably for nearly 1000 h without significant change in current, while the battery assembled with PE suffered a catastrophic short circuit after only 400 h.
[0091] (3) The cycling performance of LFP / Li half-cells assembled with PESV and PE as separators is shown in Figure 2. Figure 7 As shown, the LFP / Li assembled with PESV composite separator has a high conductivity at 1C (1.28 mA cm -2 ) After 1000 cycles, it can still reach 89mAh·g -1 The discharge capacity of the LFP / Li battery assembled with PE diaphragm is only 41mAh·g after 1000 cycles. -1 .
[0092] Although the present invention has been disclosed as above in the preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for preparing a composite diaphragm material, It is characterized in that The following steps are involved: S1, mixing a polysulfone additive, a polyvinylidene fluoride additive and a solvent, heating and stirring until completely dissolved, and cooling to room temperature to obtain an additive solution; The sum of the mass of the polysulfone additive and the polyvinylidene fluoride additive is 10% of the total mass of the additive solution; S2, soaking the membrane substrate in the additive solution, and taking out the film after it is fully wetted; S3, spread the film flat on a glass plate, scrape off excess slurry on the surface with a scraper, and vacuum dry for 8-12 hours to obtain a composite diaphragm.
2. The preparation method according to claim 1, It is characterized in that The polysulfone additive is one or a mixture of two or more of polysulfone, polyethersulfone and polyphenylsulfone in any proportion.
3. The preparation method according to claim 1, It is characterized in that The polyvinylidene fluoride additive is one or a mixture of two or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, and polyvinylidene fluoride-chlorotrifluoroethylene in any proportion.
4. The preparation method according to claim 1, It is characterized in that The solvent is one or a mixture of two or more of N-methylpyrrolidone, N,N-dimethylformamide and N,N-dimethylacetamide in any proportion.
5. The preparation method according to claim 1, It is characterized in that The mass of the polysulfone additive or the polyvinylidene fluoride additive is 3% to 7% of the total mass of the additive solution.
6. The preparation method according to claim 1, It is characterized in that The heating temperature in S1 is 50°C to 80°C.
7. The preparation method according to claim 1, It is characterized in that The stirring time in S1 is 30-60 min.
8. A composite diaphragm material prepared by the method according to claim 1.
9. A composite diaphragm material prepared by the method according to claim 1, used as a primary or secondary battery diaphragm material.