Method for efficiently recovering lead and zinc in zinc leaching residues
By adopting a two-stage treatment method of side blowing and top blowing and blowing in the wet zinc slag treatment, the melt pool is formed by combining a cylindrical cylinder and an alternating spray gun, which solves the serious pollution and low treatment efficiency in the prior art. The problem of this is to achieve efficient recycling and continuous production of lead and zinc in zinc leaching slag.
Patent Information
- Application Number
- CN202411031399.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
During the existing wet zinc slag treatment process, there are problems such as serious pollution, long treatment process, low side blower treatment efficiency, slow volatility rate of smoke furnace, and inability to achieve continuous production.
Using the two-stage treatment method of side blowing and top blowing and blowing, in a cylindrical cylinder treatment furnace, the melt pool is formed by alternating oxygen-rich air and pulverized coal side blowing guns, and the top rich The oxygen air spray gun is suspended to achieve continuous recovery of lead and zinc in the zinc leaching slag.
The melting and volatilization process of zinc leaching slag has been greatly shortened, the recycling efficiency of zinc has been improved, the equipment has been reduced, the combustion efficiency has been improved, and continuous production has been achieved.
Smart Images

Figure CN118957280A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of hydrometallurgy, and in particular relates to a method for efficiently recovering lead and zinc from zinc leaching slag. Background Art
[0002] The treatment of wet zinc smelting slag usually includes rotary kiln volatilization method and hot acid leaching method. The pollution is relatively serious during the rotary kiln treatment process, and the slag treatment process is too long. The waste slag from the hot acid leaching method contains sulfuric acid and heavy metal ions, which are prone to secondary pollution. At present, the treatment process of using side-blown furnace for smelting desulfurization and fuming furnace for blowing is relatively simple, but the side-blown furnace cannot significantly increase the width of the furnace body due to the insufficient penetration depth of the side-blowing injection. There is a central area with weak flow between the two lances, which makes it impossible to increase the treatment efficiency of side-blown smelting. At the same time, the combustion efficiency is not high in the form of adding granular coal on the top. In addition, the two furnaces work intermittently, not only the volatilization rate of the fuming furnace is not fast enough, but also continuous production cannot be achieved. Summary of the invention
[0003] The object of the present invention is to provide a method for significantly shortening the melting and volatilization process of zinc leaching slag to efficiently recover lead and zinc in the zinc slag.
[0004] The method for efficiently recovering lead and zinc from zinc leaching slag provided by the present invention adopts a two-stage treatment of side-blowing smelting + top-blowing blowing to simultaneously and continuously recover lead and zinc from the slag in one treatment furnace.
[0005] When the above method is implemented, the furnace body of the treatment furnace is a cylindrical body, and two side-blowing lances for oxygen-enriched air and pulverized coal are alternately and evenly distributed on the same circumferential surface at the bottom of the cylindrical body, and a top-blowing lance for spraying oxygen-enriched air is inserted in the center of the top of the cylindrical body.
[0006] When the above method is implemented, the following steps are included:
[0007] (1) Two side-blowing lances work simultaneously to melt the slag to obtain a molten pool of a specified height, with lead liquid at the bottom and high-zinc molten slag at the top;
[0008] (2) Open the top blowing spray gun to perform top suspended spraying;
[0009] (3) The crude lead flows out through the lead liquid outlet at the bottom of the furnace, and the zinc at the top of the molten pool is blown into smoke and enters the smoke dust recovery.
[0010] When the above method is implemented, the hearth area of the cylindrical furnace body is 3.79-8m 2 between.
[0011] When the above method is implemented, the feature is that the height of the molten pool is 1700-2300 mm.
[0012] When the above method is implemented, the number of both side-blowing lances is two. The diameter of the side-blowing lance used for blowing oxygen-enriched air is 44 mm, and the diameter of the side-blowing lance used for blowing pulverized coal is 33 mm. The blowing speed of the two side-blowing lances is 150-250 m / s.
[0013] When the above method is implemented, the effective stirring distance of the two side-blowing spray guns is 600-800 mm.
[0014] When the above method is implemented, the distance between the lower end of the top-blowing lance and the liquid surface of the molten pool is 100-300 mm, and the blowing speed of the top-blowing lance is 160-200 m / s.
[0015] When the above method is implemented, the number of side-blowing lances and the blowing speed of the top-blowing lance are determined according to the calculated values of the speed and component concentration at each spatial point inside the furnace body at each moment, as follows:
[0016] 1) Mass conservation equation
[0017]
[0018] (1) In the formula, α i , i and Respectively represent the volume fraction, density and velocity of the i-th phase; in the Euler-Euler model, each phase is considered to be a continuous medium occupying a certain volume, satisfying the conservation of mass and momentum, and the phases can penetrate each other; in each calculation grid, the sum of the volume fractions of each phase is 1:
[0019]
[0020] (2)In the formula, the subscript i represents different phases;
[0021] 2) Momentum conservation equation
[0022]
[0023] (3) In the formula, p is the pressure, is the strain tensor of the ith phase, is the drag force between the gas and liquid phases, is the virtual mass force corresponding to the ith phase; the subscript p represents the gas phase, and q represents the liquid phase;
[0024] is defined as follows:
[0025]
[0026] (4) In the formula, μ i and λ i are the shear viscosity and bulk viscosity of the ith phase, is the unit stress tensor; the virtual mass force corresponding to the gas is:
[0027]
[0028] (5) In the formula, C vm is the virtual mass force coefficient, which is taken as 0.5; according to Newton's third law, the virtual mass force corresponding to the liquid and the virtual mass force corresponding to the gas are a pair of interaction forces, so the virtual mass force corresponding to the liquid is:
[0029]
[0030] Finally, the velocity and component concentration values of each spatial point inside the furnace at each moment are obtained.
[0031] The present invention continuously recovers lead and zinc in the zinc leaching slag in the same treatment furnace. The furnace body of the treatment furnace adopts a cylindrical barrel, which can greatly reduce the floor space of the equipment and shorten the volatilization process of the zinc element. The temperature is raised by the combination of oxygen-enriched air and pulverized coal side-blowing spray guns alternately and evenly distributed on the same circumferential surface of the bottom of the cylindrical barrel, so that a molten pool of a specified height can be quickly formed, and then the top slag layer of the molten pool is suspended and sprayed by the oxygen-enriched air top-blowing spray gun above the liquid surface of the molten pool, so that the liquid surface of the molten pool is broken into a large number of small droplets, so that the zinc slag is fully reacted with oxygen for reduction, and the fuming efficiency of zinc is greatly improved. Therefore, the present invention can efficiently recover lead and zinc in zinc slag. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a schematic structural diagram of a preferred embodiment of the present invention.
[0033] Figure 2 This is a comparison diagram of the stirring effect of the side-blowing spray gun on the molten pool in this preferred embodiment.
[0034] Figure 3 This is a comparison chart for determining the number of side-blowing spray guns in this preferred embodiment.
[0035] Figure 4 This is a comparison chart for determining the top blowing lance speed in this preferred embodiment. DETAILED DESCRIPTION
[0036] The method for efficiently recovering lead and zinc from zinc leaching slag disclosed in the present invention has the general idea of: adopting a two-stage treatment of side-blowing smelting + top-blowing blowing to simultaneously and continuously recover lead and zinc from the slag in one treatment furnace.
[0037] In the preferred embodiment guided by this idea, the furnace body adopts a cylindrical body, and two side-blowing lances of oxygen-enriched air and pulverized coal are alternately and evenly distributed on the same circumferential surface at the bottom of the cylindrical body, and a top-blowing lance for spraying oxygen-enriched air is inserted in the center of the top of the cylindrical body. Figure 1shown.
[0038] The molten pool is stirred by the oxygen-enriched air side-blowing lance, and the pulverized coal side-blowing lance is used to supplement the molten pool with fuel. After a stable molten pool height is obtained, the oxygen-enriched air top-blowing lance performs top suspended blowing to increase the stirring function of the central area.
[0039] The specific steps are as follows:
[0040] (1) The oxygen-enriched air side-blowing lance and the pulverized coal side-blowing lance work simultaneously to melt the slag to obtain a molten pool, the bottom of the molten pool is lead liquid, and the top is high-zinc molten slag;
[0041] (2) Open the oxygen-enriched air top-blowing spray gun for top suspension spraying;
[0042] (3) The crude lead flows out through the lead liquid outlet at the bottom of the furnace, and the zinc at the top of the molten pool is fumed and enters the smoke recovery.
[0043] Since the furnace bed area of the sealing area of the side-blowing furnace cannot be expanded infinitely, the furnace width of the side-blowing furnace is generally 2.2m. In the present invention, the furnace body is a cylindrical barrel, and the radiation distance of the top-blowing jet can reach 1m. Therefore, in the present invention, the furnace body diameter ranges from 2.2-3.2m, and the furnace bed area is 3.79-8m 2 .
[0044] Other parameters are as follows:
[0045] The molten pool height is 1700-2300 mm, and is 2000 mm in this embodiment.
[0046] The diameters of the oxygen-enriched air side-blowing lance and the pulverized coal side-blowing lance are selected from the commonly used specifications of 44 mm and 33 mm in the field, but the specific selection needs to be determined by simulation calculation. The spraying speed of the two side-blowing lances is 150-250 m / s, and 200 m / s is specifically selected in this embodiment.
[0047] The effective stirring distance of the two side-blowing spray guns is 600-800 mm, and 800 mm is taken in this embodiment.
[0048] The diameter of the oxygen-enriched air top-blowing lance is 78 mm, which is a common specification for top-blowing furnaces. The distance between the lower end and the molten pool liquid surface is 100-300 mm, and 100 mm is selected in this embodiment. The effective stirring radius of the top-blowing lance is about 1 m.
[0049] The furnace bed capacity is 35 tons / m 2 .d or so.
[0050] Other parameters that need to be determined through simulation calculations include: the number of two side-blowing spray guns and the top-blowing spray speed.
[0051] The specific steps of simulation calculation are as follows:
[0052] 1) Mass conservation equation
[0053]
[0054] (1) In the formula, α i , i and Respectively represent the volume fraction, density and velocity of the i-th phase; in the Euler-Euler model, each phase is considered to be a continuous medium occupying a certain volume, satisfying the conservation of mass and momentum, and the phases can penetrate each other; in each calculation grid, the sum of the volume fractions of each phase is 1:
[0055]
[0056] (2)In the formula, the subscript i represents different phases;
[0057] 2) Momentum conservation equation
[0058]
[0059] (3) In the formula, p is the pressure, is the strain tensor of the ith phase, is the drag force between the gas and liquid phases, is the virtual mass force corresponding to the ith phase; the subscript p represents the gas phase, and q represents the liquid phase;
[0060] is defined as follows:
[0061]
[0062] (4) In the formula, μ i and λ i are the shear viscosity and bulk viscosity of the ith phase, is the unit stress tensor; the virtual mass force corresponding to the gas is:
[0063]
[0064] (5) In the formula, C vm is the virtual mass force coefficient, which is 0.5. According to Newton's third law, the virtual mass force corresponding to the liquid and the virtual mass force corresponding to the gas are a pair of interaction forces, so the virtual mass force corresponding to the liquid is:
[0065]
[0066] Finally, the velocity and component concentration values of each spatial point inside the furnace at each moment are obtained.
[0067] There are two types of spray gun diameters commonly used in this field: 44mm and 33mm. The two specifications of spray guns were tested at the same spray speed (200m / s). The results are shown in Figure 2 The isosurface diagram of gas distribution in the molten pool is shown. Figure 2 It can be seen that the bubbles produced by the 44mm diameter spray gun blowing oxygen-enriched air are larger and have a stronger driving force for stirring the molten pool liquid surface.
[0068] Figure 3 The isosurface diagrams of the blowing gas of 2, 4 and 6 side-blowing spray guns with a diameter of 44 mm (blowing speed 200 m / s) are shown respectively.
[0069] from Figure 3 It can be seen that the stirring of the molten pool by 2 spray guns is too small, and the stirring of the molten pool by 6 spray guns is too intense, resulting in serious melt splashing. Therefore, it is necessary to combine two diameter spray guns to reduce splashing while maintaining good dynamic conditions of the molten pool. The stirring of the molten pool by 4 spray guns is basically appropriate, but after simulation calculation, the combination of two 44mm and two 33mm side-blowing spray guns has the best effect, which can obtain efficient molten pool dynamic conditions and complete the smelting process within 100 minutes. The efficiency of melting zinc leaching slag is 20% higher than that of general side-blowing. At the same time, the scouring effect on the upper furnace wall of the furnace body is small, the furnace body has a longer life, and there will be no melt splashing accidents.
[0070] After simulation calculation, the top blowing speed can obtain better blowing power conditions at 160m / s-200m / s, such as Figure 4 As shown, the molten pool liquid surface is broken up into a large number of tiny droplets, which is conducive to the full reaction of the molten zinc slag with oxygen, so that volatilization can be completed in 90 minutes, which is 25% higher than the blowing rate of the traditional fuming furnace.
[0071] After the above parameters are determined, for a cylindrical shell with a size (diameter × height) of 3000mm × 4500mm and a furnace area of 2.5m 2 、Heat bed area 5.4m 2 The treatment furnace (in the tuyere area) can process high lead zinc slag (lead content above 30%) for 100 min, blowing time for 90 min, oxygen-to-material ratio for 400, and oxygen volume for 5.4*35 / 24=3150m 3 / h; the annual processing capacity can reach 56,700 tons (35*330*5.4). If the existing side-blowing furnace + fuming furnace treatment process is adopted, the smelting time for one treatment is 150 minutes and the blowing time is 120 minutes.
[0072] It is obvious that the two-stage treatment process in a treatment furnace disclosed in the present invention can continuously recover lead and zinc in the zinc in-and-out slag, and can greatly improve the recovery efficiency compared with the intermittent production process of the side-blowing furnace + fuming furnace in the prior art.
Claims
1. A method for efficiently recovering lead and zinc from zinc leaching residue, characterized in that: The method adopts a two-stage treatment of side-blowing smelting + top-blowing blowing to continuously recover lead and zinc from the slag simultaneously in one treatment furnace.
2. The method for efficiently recovering lead and zinc from zinc leaching residue according to claim 1, characterized in that: The furnace body of the treatment furnace is a cylindrical body, and two side-blowing lances of oxygen-enriched air and pulverized coal are alternately and evenly distributed on the same circumferential surface at the bottom of the cylindrical body, and a top-blowing lance for spraying oxygen-enriched air is inserted in the center of the top of the cylindrical body.
3. The method for efficiently recovering lead and zinc from zinc leaching residue as claimed in claim 2, characterized in that The following steps are involved: (1) Two side-blowing lances work simultaneously to melt the slag to obtain a molten pool of a specified height, with lead liquid at the bottom and high-zinc molten slag at the top; (2) Open the top blowing spray gun to perform top suspended spraying; (3) The crude lead flows out through the lead liquid outlet at the bottom of the furnace, and the zinc at the top of the molten pool is blown into smoke and enters the smoke dust recovery.
4. The method for efficiently recovering lead and zinc from zinc leaching residue according to claim 2, characterized in that: The hearth area of the cylindrical furnace body is 3.79-8m 2 between.
5. The method for efficiently recovering lead and zinc from zinc leaching residue according to claim 4, characterized in that: The characteristics are: The molten pool height is 1700-2300 mm.
6. The method for efficiently recovering lead and zinc from zinc leaching residue according to claim 5, characterized in that: There are two side-blowing lances for both types. The diameter of the side-blowing lance used for spraying oxygen-enriched air is 44 mm, and the diameter of the side-blowing lance used for spraying pulverized coal is 33 mm. The spraying speeds of the two side-blowing lances are 150-250 m / s.
7. The method for efficiently recovering lead and zinc from zinc leaching residue according to claim 6, characterized in that: The effective stirring distance of the two side-blowing spray guns is 600-800mm.
8. The method for efficiently recovering lead and zinc from zinc leaching residue according to claim 7, characterized in that: The distance between the lower end of the top-blowing lance and the liquid surface of the molten pool is 100-300 mm, and the blowing speed of the top-blowing lance is 160-200 m / s.
9. The method for efficiently recovering lead and zinc from zinc leaching residue as claimed in claim 8, characterized in that The number of side-blowing lances and the blowing speed of the top-blowing lance are determined according to the calculated values of the speed and component concentration at each spatial point inside the furnace at each moment, as follows: 1) Mass conservation equation (1) In the formula, α i , i and Respectively represent the volume fraction, density and velocity of the i-th phase; in the Euler-Euler model, each phase is considered to be a continuous medium occupying a certain volume, satisfying the conservation of mass and momentum, and the phases can penetrate each other; in each calculation grid, the sum of the volume fractions of each phase is 1: (2)In the formula, the subscript i represents different phases; 2) Momentum conservation equation (3) In the formula, p is the pressure, is the strain tensor of the ith phase, is the drag force between the gas and liquid phases, is the virtual mass force corresponding to the ith one; The subscript p represents the gas phase, and q represents the liquid phase; is defined as follows: (4) In the formula, μ i and λ i are the shear viscosity and bulk viscosity of the ith phase, is the unit stress tensor; The virtual mass force corresponding to the gas is: (5) In the formula, C vm is the virtual mass force coefficient, which is taken as 0.5; according to Newton's third law, the virtual mass force corresponding to the liquid and the virtual mass force corresponding to the gas are a pair of interaction forces, so the virtual mass force corresponding to the liquid is: Finally, the velocity and component concentration values of each spatial point inside the furnace at each moment are obtained.