Aero-engine sealing ring with coating in specific area and preparation method of aero-engine sealing ring

Through cold press forming and supersonic flame spraying technology, the CoMoCrSi coating is sprayed in specific areas of aircraft engine seal rings, which solves the problem of weak points of thin-walled metal seal rings in high-temperature environments, improves sealing performance and service life, and achieves the realization of the sealing performance and service life. High temperature stability and low leakage effects.

CN118959099APending Publication Date: 2024-11-15SHANGHAI INST OF CERAMIC CHEM & TECH CHINESE ACAD OF SCI
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411019032.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Thin-walled metal sealing rings are difficult to meet the strict working conditions of aircraft engines in high temperature, heat alternation and vibration environments. Traditional welding processes lead to weak points, affecting sealing performance and service life.

Method used

The cold press forming process is used to have no welding, combined with vacuum heat treatment and supersonic flame spraying technology, spraying CoMoCrSi coating in specific areas, forming a "C" arc structure aircraft engine sealing ring, improving high-temperature wear resistance and service life.

Benefits of technology

It has achieved stable operation at high temperature of 1000℃. After 1000h neutral salt spray corrosion and 50 thermal shocks, the coating is intact, no cracks or peeling, and the air leakage under pressure difference of 0.6MPa is not greater than 5×10-3m3/ s.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118959099A_ABST
    Figure CN118959099A_ABST
Patent Text Reader

Abstract

The invention relates to an aero-engine sealing ring with a coating in a specific area and a preparation method of the aero-engine sealing ring. The section of the aero-engine sealing ring with the coating in the specific area is in a C shape, the aero-engine sealing ring is integrally of an arc structure, a groove is formed in the middle of the arc structure, and the opening direction of the groove points to the outer side of the overall arc structure of the sealing ring. The specific area with the coating is an arc-shaped sealing face composed of the arc end face of the aero-engine sealing ring and the structures on the two sides of the groove, the arc-shaped sealing face with the large diameter is the large end, and the arc-shaped sealing face with the small diameter is the small end. Preferably, the diameter of the large end ranges from 125 mm to 250 mm, and the diameter of the small end ranges from 120 mm to 245 mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thin-wall metal sealing ring preparation, and in particular relates to an aero-engine sealing ring with a coating in a specific area and a preparation method thereof. Background Art

[0002] Thin-walled metal sealing rings are an important industrial basic part, mainly used for sealing in the compressor, turbine, combustion chamber and external pipelines of aircraft engines. Thin-walled metal sealing rings have the advantages of light weight, good self-tightening ability and excellent sealing performance. With the development of modern aircraft engine industrial technology, in order to achieve higher operating efficiency, the internal working environment of the engine has become more stringent. The sealing device has extremely important research significance for the operating efficiency, service life and working environment of aircraft engines.

[0003] Thin-walled metal sealing rings generally need to withstand high temperature, thermal alternation, vibration and other harsh working conditions for a long time during service. Traditional single-material metal sealing rings often cannot meet these requirements. Using thermal spraying technology to deposit a layer of coating with strong bonding, good wear resistance and thermal shock resistance on the surface of a specific area of ​​the sealing ring can effectively enhance the performance and service life of the sealing structure. However, the parts of thin-walled metal sealing rings often have small wall thickness, high precision requirements, and great processing difficulty. Conventional processing includes welding process, and there is heat input during welding, so the welding parts are often weak points, which greatly affects the high-temperature wear resistance and service life of the sealing ring. Summary of the invention

[0004] In view of the above technical problems, the purpose of the present invention is to provide an aircraft engine sealing ring with a coating in a specific area and a preparation method thereof. The blank forming process of the thin-walled metal sealing ring provided by the present invention does not include a welding process, and the coating can effectively improve the high temperature wear resistance and service life of the sealing ring.

[0005] In a first aspect, the present invention provides an aircraft engine sealing ring with a coating in a specific area, wherein the cross section of the aircraft engine sealing ring with a coating in a specific area is "C"-shaped, and the whole is an arc structure, a groove is formed in the middle of the arc structure, and the opening direction of the groove points to the outside of the overall arc structure of the sealing ring; The specific area with coating is the arc-shaped sealing surface composed of the arc end surface of the aircraft engine sealing ring and the structures on both sides of the groove, the arc-shaped sealing surface with a larger diameter is the large end, and the arc-shaped sealing surface with a smaller diameter is the small end; Preferably, the diameter of the large end is 125-250 mm, and the diameter of the small end is 120-245 mm.

[0006] Preferably, the base material of the sealing ring is made of Waspaloy, GH738 or GH3128, with a thickness of 0.2 to 0.3 mm; The coating is a CoMoCrSi coating; preferably, the element composition of the CoMoCrSi coating includes: in mass percentage, Mo: 27.5-33.6wt.%, Cr: 16.9-18.5wt.%, Si: 3.1-4.9wt.%, Co: balance; the thickness of the coating is 40-160μm; The area of ​​the specific region to which the coating is attached accounts for 40-70% of the total area of ​​the aircraft engine sealing ring with the coating in the specific region.

[0007] Preferably, the air leakage of the aircraft engine sealing ring with coating in the specific area is not more than 5×10 -3 m 3 / s.

[0008] In a second aspect, the present invention provides a method for preparing the above-mentioned aircraft engine sealing ring with a coating in a specific area, the preparation method comprising the following steps: (1) forming the substrate by cold pressing to obtain an aircraft engine sealing ring blank with a specific area to be sprayed; (2) subjecting the specific area of ​​the aircraft engine sealing ring blank to be sprayed to solid solution, primary aging, and secondary aging treatment under vacuum conditions to obtain the specific area of ​​the aircraft engine sealing ring blank to be sprayed after heat treatment; (3) using a multi-piece combined inner and outer support mold to perform surface roughening pretreatment on the specific area of ​​the aircraft engine sealing ring blank to be sprayed after the heat treatment, so as to obtain the aircraft engine sealing ring blank to be sprayed after the pretreatment of the specific area; (4) Spraying a CoMoCrSi coating on the specific area of ​​the aircraft engine sealing ring blank to be sprayed in the specific area after the pretreatment by using supersonic flame spraying technology to obtain an aircraft engine sealing ring with a coating in the specific area.

[0009] Preferably, in step (1), the process flow of the cold press forming includes stretching the main body, shaping the main body, cutting off waste materials, forming at both ends, and shaping at both ends; preferably, the temperature of the cold press forming does not exceed 50°C.

[0010] Preferably, in step (2), the vacuum degree of the vacuum heat treatment condition is 10 -2 ~10 -1 Pa.

[0011] Preferably, in step (2), the solution temperature is 1000-1100°C, and the solution time is 5 min-4 h; The primary aging temperature is 835-855°C, and the primary aging time is 4-24h; The secondary aging temperature is 750-770° C., and the secondary aging time is 15-17 hours.

[0012] Preferably, in step (3), the multi-piece combined inner and outer supporting mold includes a base, an outer ring combined fixing plate, an inner ring positioning boss, a center limiting groove, a lateral positioning hole component, an anti-slip stopper, and a fastener located on the base for fixing the sealing ring blank; Preferably, when a multi-piece combined inner and outer supporting mold is used, a flexible copper wire matching the curvature is embedded inside the large end of the inner concave surface of the sealing ring blank, and an elastic polyurethane ring matching the curvature is mounted inside the small end of the sealing ring blank to fix the sealing ring and protect the non-sandblasting area. The axial and radial tensions are adjusted by fasteners. The roughening treatment is performed by sandblasting with white corundum sand; preferably, the particle size of the white corundum sand is in the range of 250 to 600 μm, and the sandblasting pressure is in the range of 1.0 to 3.5 bar.

[0013] Preferably, in step (4), the fuel gas used in the supersonic flame spraying technology is hydrogen and oxygen, the fuel gas flow rate is 860-901 SLPM, the flow rate ratio of oxygen to hydrogen is 0.20-0.50, preferably 0.30-0.35; the powder feeding disk speed is 15-25%, and the number of spraying passes is 5-20; The HVOF spray gun is clamped by an industrial robot and cuts forward, spraying at a variable angle from the outside to the inside. The spraying direction of the flame jet deviates from the center of the blank by a certain distance, and at the cutting point, the speed component of the flame jet spraying along the blank rotation direction is equal to the blank rotation linear speed; Preferably, the angle between the flame jet and the horizontal direction is 45°, the linear speed of the blank rotation is 105,000-135,000 mm / min, the jet speed is 200-500 m / s, and the jet beam spot diameter is 8-12 mm. The angle of the jet center direction deviating from the center is 0.5-2.0°, and the spatial distance between the flame jet entry point and the blank rotation center is 4.0-6.5 mm.

[0014] Preferably, in step (4), a shadow shielding method is used to control the spraying area of ​​the CoMoCrSi coating; Preferably, the shadow shielding method uses the shadow shielding principle to adjust the flame flow angle of the HVOF spray gun, the protruding height of the inner ring positioning boss, and the gap between the inner ring positioning boss and the sealing ring blank to control the boundary of the inner spraying area. At the same time, a circular ring made of 304 stainless steel or high-temperature alloy strip with a thickness equivalent to that of the sealing ring blank is embedded in the groove of the sealing ring blank to form an elastic fit with the outer edge of the spraying area to control the edge of the outer spraying area.

[0015] Beneficial Effects The application temperature of the aircraft engine sealing ring with coating in the specific area obtained by the preparation method provided by the present invention can reach 1000°C; after 1000h of neutral salt spray corrosion at room temperature, there is no rust on the surface of the coating; after 50 times of thermal shock (900°C to room temperature, 500°C to room temperature), the coating is intact without cracks, peeling and the like; the air leakage under the pressure difference of 0.6MPa and room temperature is not more than 5×10 -3 m 3 / s. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 A schematic diagram of an aircraft engine sealing ring structure with a coating on a specific area and a coated area according to an example of the present invention; Figure 2 This is a physical picture of a partial area of ​​the aerospace engine sealing ring blank to be sprayed in a specific area prepared in Example 1; Figure 3 A physical picture of a specific area of ​​the aeroengine sealing ring belt coating prepared in Example 1; Figure 4 This is a physical picture of the coating area of ​​the aircraft engine sealing ring with coating in a specific area prepared in Example 1 after being subjected to neutral salt spray corrosion for 1000 hours; Figure 5 This is a photo of the coated test piece prepared in Example 2 after 50 thermal shocks (500°C to room temperature); Figure 6 This is a real picture of the coated test piece prepared in Example 4 after 50 thermal shocks (900°C to room temperature); Figure 7 This is a physical picture of the sealing ring prepared in Comparative Example 2; Figure 8 This is a physical picture of the sealing ring prepared in Comparative Example 3. DETAILED DESCRIPTION

[0017] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.

[0018] First, the present invention provides an aircraft engine sealing ring with a coating in a specific area. Figure 1 As shown, the cross-section of the aircraft engine sealing ring with coating in the specific area is "C"-shaped, and the overall structure is an arc structure. A groove is formed in the middle of the arc structure, and the opening direction of the groove points to the outside of the overall arc structure of the sealing ring; wherein, the specific area with coating is an arc-shaped sealing surface composed of the arc end face of the aircraft engine sealing ring and the structures on both sides of the groove, the arc-shaped sealing surface with a larger diameter is the large end, and the arc-shaped sealing surface with a smaller diameter is the small end.

[0019] In some embodiments, the diameter of the large end is 125-250 mm, and the diameter of the small end is 120-245 mm.

[0020] In some embodiments, the brand of the base material of the sealing ring may be Waspaloy, GH738 or GH3128.

[0021] In some embodiments, the thickness of the base material of the sealing ring may be 0.2-0.3 mm. If the base material thickness is too large, it will affect the molding; if the base material thickness is too small, the sealing ring blank after molding is easy to deform.

[0022] In some embodiments, the coating may be a CoMoCrSi coating; preferably, the element composition of the CoMoCrSi coating may include: in mass percentage, Mo: 27.5-33.6wt.%, Cr: 16.9-18.5wt.%, Si: 3.1-4.9wt.%, Co: balance. Among them, the Mo element can increase the diffusion activation energy and reduce the diffusion in the alloy, thereby enhancing the interatomic bonding force, improving the hardness and high temperature strength of the alloy, and Mo can also promote the formation of Laves phase in the coating. If the Mo content is too low, it will affect the formation of the Laves phase; if the Mo content is too high, it will affect the mechanical properties of the coating and easily cause the creep performance to decrease. In addition, too low a content of Cr element will greatly weaken the oxidation resistance and corrosion resistance of the alloy coating, while too high a content of Cr element will strongly promote the precipitation of TCP (Topologically Close-Packed) phase, thereby damaging the mechanical properties of the material. At the same time, the addition of Si can increase the strength and hardness of the alloy, but if the content is not appropriate, it will affect the mechanical properties of the coating.

[0023] In some embodiments, the coating may have a thickness of 40 to 160 μm. If the coating thickness is too large, the coating may peel off during thermal shock; if the coating thickness is too small, the coating may not evenly cover the substrate, affecting the wear resistance.

[0024] In some embodiments, the specific area where the coating is attached can account for 40-70% of the total area of ​​the aircraft engine sealing ring with the coating in the specific area. When the coating exceeds the coverage area, the elastic expansion and contraction of the sealing ring will be directly reduced, and the metal elastic seal cannot be achieved; if the coating coverage area is insufficient, the coating reinforcement effect will be reduced, affecting the wear resistance and service life of the sealing ring.

[0025] In some embodiments, the air leakage of the aircraft engine sealing ring with coating in the specific area is not more than 5×10 -3 m 3 / s.

[0026] The following is an exemplary description of the method for preparing the aircraft engine sealing ring with a coating in a specific region provided by the present invention, wherein the preparation method may include the following steps.

[0027] (1) Strip forming: The substrate is formed by cold pressing to obtain an aircraft engine sealing ring blank with a specific area to be sprayed.

[0028] In some embodiments, the process flow of the cold press forming may include stretching the main body, shaping the main body, cutting off waste materials, forming at both ends, and shaping at both ends; preferably, the temperature of the cold press forming does not exceed 50°C.

[0029] The cold press forming process adopted by the present invention has no welding process in the whole process. There is heat input during welding, and the welding position is often a weak point. If there is misalignment during welding, it is very easy to introduce additional stress into the sealing ring, thereby greatly affecting the high temperature wear resistance and service life of the sealing ring. Cold press forming can make the obtained sealing ring blank have no weak points, thereby improving the reliability of the sealing ring, but generally cold press forming has high requirements on molds and technology, the process is difficult, and improper operation can easily cause the strip to crack.

[0030] (2) Vacuum heat treatment of the sealing ring blank. The specific area of ​​the aircraft engine sealing ring blank to be sprayed in step (1) is subjected to solid solution, primary aging, and secondary aging treatment under vacuum conditions to obtain the specific area of ​​the aircraft engine sealing ring blank to be sprayed after heat treatment.

[0031] In some embodiments, the vacuum degree of the vacuum condition can be maintained at 10 -2 ~10 -1 Pa. Otherwise, if heat treated in air, oxide scale will form on the surface of the blank, affecting the mechanical properties of the blank.

[0032] Solution treatment can be used to homogenize the alloy composition of the blank, reduce or eliminate the component segregation formed during the condensation process, and dissolve all or most of the precipitated phases in the alloy, preparing for the subsequent failure precipitation of uniform, fine and dispersed strengthening phases. In some embodiments, the solution temperature can be 1000-1100°C, and the solution time can be 5min-4h. Too high a solution temperature will cause the alloy grains to be too coarse, and too low a temperature will not be conducive to component homogenization; too long a solution time will easily cause the sealing ring blank to deform, and too short a time will not be conducive to component homogenization.

[0033] The primary aging treatment can make the blank alloy precipitate the strengthening phase uniformly, thereby improving the strength of the alloy. In some embodiments, the temperature of the primary aging treatment can be 835-855°C, and the time of the primary aging treatment can be 4-24 hours.

[0034] The secondary aging treatment can play a role in re-precipitating the phase and comprehensively coordinating the size and distribution of the strengthening phase, thereby improving the performance of the high-temperature alloy. In some embodiments, the temperature of the secondary aging treatment can be 750-770°C, and the time of the secondary aging treatment can be 15-17 hours.

[0035] (3) Pretreatment of the sealing ring blank before spraying: A multi-piece combined inner and outer support mold is used to perform surface roughening pretreatment on the specific area of ​​the aircraft engine sealing ring blank to be sprayed after the heat treatment in step (2), thereby obtaining the aircraft engine sealing ring blank to be sprayed after the pretreatment of the specific area.

[0036] In some embodiments, the multi-piece combined inner and outer support mold includes a base, an outer ring combined fixing plate, an inner ring positioning boss, a center limiting groove, a lateral positioning hole component, and an anti-slip block and fasteners located on the base for fixing the sealing ring blank.

[0037] Preferably, when a multi-piece combined inner and outer supporting mold is used, a flexible copper wire matching its curvature can be embedded inside the large end of the inner concave surface of the sealing ring blank, and an elastic polyurethane ring matching its curvature can be mounted inside the small end of the sealing ring blank to fix the sealing ring and protect the non-sandblasting area. The axial and radial tensions are adjusted by the fasteners.

[0038] In some embodiments, the roughening treatment may be performed by sandblasting with white corundum sand; preferably, the particle size of the white corundum sand may range from 250 to 600 μm, and the sandblasting pressure may range from 1.0 to 3.5 bar. Too large a particle size or too high a sandblasting pressure may easily cause deformation of the sealing ring blank, while too small a particle size or too low a sandblasting pressure may easily lead to poor roughening effect.

[0039] The aircraft engine sealing ring to be sprayed in the specific area provided by the present invention is a thin-walled metal part (the base material thickness is about 0.2 to 0.3 mm), which is very easy to curl and deform during the sandblasting process, causing the workpiece size to be out of tolerance and scrapped. Therefore, the present invention adopts a multi-piece combined internal and external support mold in view of the structural characteristics of the thin-walled sealing ring, and embeds a flexible copper wire matching the curvature on the inner side of the large end of the inner concave surface of the blank, and sets an elastic polyurethane ring matching the curvature on the inner side of the small end to fix the sealing ring and protect the non-sandblasting area. The axial and radial tensions are adjusted by fasteners. At the same time, when manually sandblasting in the present invention, the operator needs to evenly sweep along the circumferential direction and pay attention to the color changes of the sandblasted surface to avoid plastic deformation due to excessive local stress caused by uneven sandblasting.

[0040] (4) Thermally spraying a CoMoCrSi coating on the specific area of ​​the sealing ring. The specific area of ​​the aircraft engine sealing ring blank to be sprayed with a CoMoCrSi coating is sprayed with a supersonic oxygen fuel (HVOF) coating after pretreatment in step (3) to obtain an aircraft engine sealing ring with a coating on the specific area.

[0041] In some embodiments, the fuel gas used in the supersonic flame spraying technology is hydrogen and oxygen, the fuel gas flow rate can be 860-901 SLPM, the flow ratio of oxygen to hydrogen can be 0.20-0.50, preferably 0.30-0.35; the powder feeding disk speed can be 15-25%, and the number of spraying times can be 5-20.

[0042] It should be noted that the preparation process of the CoMoCrSi coating directly affects the physical phase and structure of the coating, and thus affects the coating performance. The fuel gas used in the present invention does not contain C element, which can avoid the introduction of carbon residues in the coating. The jet velocity is relatively large, and a denser coating can be obtained. By regulating the gas flow rate, the CoMoCrSi powder can be fully melted during the preparation process, so that the various elements of the powder can react appropriately during spraying and deposition.

[0043] In some embodiments, the HVOF spray gun can be clamped by an industrial robot and cut in forward (the flame flow cuts in from the outside of the blank), and the flame jet can be sprayed at a variable angle from the outside to the inside. The direction of the flame jet spraying deviates from the center of the blank by a certain distance, and the speed component of the flame jet spraying along the direction of rotation of the blank at the cutting point is equal to the linear speed of the blank rotation; preferably, the angle between the flame jet and the horizontal direction is 45°, the linear speed of the blank rotation is 105,000 to 135,000 mm / min (for example, 120,000 mm / min), and the jet speed can be adjusted by 2 00~500m / s, the effective diameter of the jet beam is calculated as 8~12mm, the angle of the jet center direction deviating from the center can be 0.5~2.0°, and the spatial distance between the flame jet entry point and the blank rotation center can be 4.0~6.5mm; more preferably, calculated based on the jet speed of 300m / s, the effective diameter of the jet beam is 10mm, and the diameter of the large end of the blank arc is 200mm, the angle of the jet center direction deviating from the center is 0.5°, and the spatial distance between the flame jet entry point and the blank rotation center is 5.1mm.

[0044] The H2 / O2 high-speed flame jet temperature of the HVOF spraying process used in the present invention can reach 2600°C, and the workpiece needs to be sprayed multiple times, which can easily cause thermal deformation of the thin-walled metal sealing ring blank. The industrial robot clamps the HVOF spray gun and cuts in forward, spraying at a variable angle from the outside to the inside, so that the velocity component of the flame jet spraying along the rotation direction of the workpiece and the linear velocity of the spraying surface are 105,000-135,000 mm / min, reducing the thermal shock caused by the high-speed flame and alleviating the thermal deformation of the thin-walled metal sealing ring blank during HVOF spraying. The application temperature of the aircraft engine sealing ring with a coating in a specific area prepared by the present invention can reach 1000°C.

[0045] In some embodiments, a shadow shielding method can be used to control the spraying area of ​​the CoMoCrSi coating; preferably, the shadow shielding method uses the shadow shielding principle to adjust the flame flow angle of the HVOF spray gun, the protruding height of the inner ring positioning boss, and the gap between the inner ring positioning boss and the sealing ring blank to control the inner spraying area boundary, and at the same time, a circular ring made of 304 stainless steel or high-temperature alloy strip with a thickness equivalent to that of the sealing ring blank is embedded in the groove of the sealing ring blank to form an elastic fit with the outer edge of the spraying area to control the edge of the outer spraying area.

[0046] Some areas of the thin-walled metal sealing ring are coated, while other areas are not. When the coating exceeds the coverage area, the elastic expansion and contraction of the sealing ring will be directly reduced, which is also the key to achieving metal elastic sealing; insufficient coating coverage will lead to insufficient reinforcement of the coating, affecting the wear resistance and service life of the sealing ring. The present invention controls the coating spraying area through the shadow shielding method, and the coating thickness in the coverage area is uniform, which overcomes the problem of adhesion between the coating area boundary and the supporting mold. The coating boundary is smooth and clear, reducing the risk of coating peeling induced by jagged notches at the coating boundary, thereby improving the reliability of the coating.

[0047] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention all belong to the scope of protection of the present invention. The specific process parameters of the following examples are also only examples within a suitable range, that is, those skilled in the art can make selections within a suitable range through the description of this article, and are not limited to the specific values ​​​​exemplified below. If not specifically stated, the technical means used in the embodiments are conventional means well known to those skilled in the art.

[0048] Example 1

[0049] The method for preparing the aircraft engine sealing ring with a coating in a specific area provided in this embodiment comprises the following steps: (1) Strip forming: The substrate is formed by cold pressing to obtain an aircraft engine sealing ring blank with a specific area to be sprayed; the substrate thickness is 0.25 mm, and the substrate brand is GH738. The forming process includes stretching the main body, shaping the main body, cutting off the waste, forming at both ends, and shaping at both ends, and the temperature does not exceed 50°C. (2) Vacuum heat treatment of the sealing ring blank: The specific area of ​​the aircraft engine sealing ring blank to be sprayed in step (1) is subjected to solid solution, primary aging, and secondary aging treatment under vacuum conditions to obtain the specific area of ​​the aircraft engine sealing ring blank to be sprayed after heat treatment; the vacuum degree is maintained at 10 -2 ~10 -1 Pa, solution temperature is 1080℃, solution time is 4h, primary aging temperature is 845℃, primary aging time is 24h, secondary aging temperature is 760℃, secondary aging time is 16h. (3) Pretreatment of the sealing ring blank before spraying: using a multi-piece combined inner and outer support mold to perform surface roughening pretreatment on the specific area of ​​the aircraft engine sealing ring blank to be sprayed after the heat treatment in step (2), so as to obtain the aircraft engine sealing ring blank to be sprayed after the pretreatment; the roughening treatment is performed by sandblasting with white corundum sand, the particle size range of the white corundum sand is 250 to 600 μm, and the sandblasting pressure is 1.0 to 3.5 bar; during the sandblasting process, using a multi-piece combined inner and outer support mold, and embedding a flexible copper wire matching the curvature on the inner side of the large end of the inner concave surface of the blank, and installing an elastic polyurethane ring matching the curvature on the inner side of the small end to fix the sealing ring and protect the non-sandblasting area, and the axial and radial tensions are adjusted by fasteners; when manually sandblasting, the circumferential direction is evenly scanned, and the color change of the sandblasted surface is observed to avoid plastic deformation caused by excessive local stress due to uneven sandblasting. (4) thermally spraying a CoMoCrSi coating on a specific area of ​​the sealing ring: a CoMoCrSi coating is sprayed on a specific area of ​​the aircraft engine sealing ring blank to be sprayed after pretreatment in step (3) by using a high velocity oxygen fuel (HVOF) spraying technique to obtain an aircraft engine sealing ring with a coating on the specific area; The element composition of the alloy coating powder raw material includes: in terms of mass percentage, Mo: 33.0wt%, Cr: 17.4wt%, Si: 4.1wt%, Co: balance; the thickness of the CoMoCrSi coating is 100μm; The flame flow angle of the HVOF spray gun, the height of the inner ring positioning protrusion, and the gap between the inner ring positioning protrusion and the blank are adjusted through the shadow shielding principle to control the boundary of the inner spraying area. A circular ring made of 304 stainless steel strip with the same thickness as the blank is embedded in the groove of the sealing ring blank to form an elastic fit with the outer edge of the spraying area to control the edge of the outer spraying area. The HVOF spray gun is clamped by a robot, so that the flame flow cuts in from the outside of the blank and sprays at a variable angle from the outside to the inside. The spray direction of the flame jet does not pass through the center of the blank, but deviates by a certain distance. At the entry point, the velocity component of the flame jet along the rotation direction of the blank is equivalent to the rotation speed of the blank (the angle between the flame jet and the horizontal direction is 45°, the linear speed of the blank rotation is 120,000mm / min, the jet speed is 300m / s, and the jet beam spot diameter is 10mm. When the diameter of the large end of the blank arc is 200mm, the corresponding angle of the jet center direction deviates from the center by 0.5°, and the spatial distance between the flame jet entry point and the blank rotation center is 5.1mm); the fuel gas used is hydrogen and oxygen, and the fuel gas flow rate is 897SLPM, wherein the flow ratio of oxygen to hydrogen is 0.3, the rotation speed of the powder feeding plate is 20%, and the number of spraying coverage is 10 times.

[0050] Figure 2 This is a physical picture of a part of the specific area of ​​the aircraft engine sealing ring blank to be sprayed prepared in Example 1. As can be seen from the figure, the specific area of ​​the aircraft engine sealing ring blank to be sprayed prepared by cold pressing in Example 1 has no welding parts.

[0051] Figure 3 This is a physical picture of a specific area of ​​the aircraft engine sealing ring belt coating prepared in Example 1. It can be seen from the figure that the coating is tightly combined with the substrate, the coating spraying area is controllable, and the coating area boundary is smooth and clear without gaps.

[0052] The sealing ring with coating in the specific area prepared in Example 1 was tested for leakage. The air leakage under the pressure difference of 0.6 MPa and room temperature was 5×10 -3 m 3 / s.

[0053] The aircraft engine sealing ring with coating in specific area prepared in Example 1 was placed in a salt spray test box, and a continuous spray test was carried out for 1000 hours under the conditions of (50±5) g / L NaCl, temperature (35±2)°C, and pH 6.5-7.2 according to the test method of GB / T10125-2012. Figure 4 This is a real picture of the coating area of ​​the aircraft engine sealing ring with coating in specific area prepared in Example 1 after being corroded by neutral salt spray for 1000 hours. It can be seen from the figure that there is no rust spot on the surface of the coating area.

[0054] Example 2

[0055] The preparation method of the coated test piece provided in this embodiment refers to that in embodiment 1, the main difference is that the present invention directly uses the GH738 strip test piece for processing, and the number of spraying coverage is 13 times, and the thickness of the CoMoCrSi coating is 130 μm.

[0056] Figure 5 This is a photo of the coated test piece prepared in Example 2 after 50 thermal shocks (500°C to room temperature). It can be seen from the photo that after the thermal shock, the coating is intact without cracks or peeling.

[0057] Example 3

[0058] The method for preparing the aircraft engine sealing ring with a coating in a specific area provided in this embodiment refers to that in Embodiment 1, the main difference is that the strip material grade is Waspaloy.

[0059] The leakage test of the aircraft engine sealing ring with coating in the specific area prepared in Example 3 was carried out. The air leakage under the pressure difference of 0.6 MPa and room temperature was 6×10 -4 m 3 / s.

[0060] Example 4

[0061] The preparation method of the coated test piece provided in this embodiment refers to that of Embodiment 2, with the main difference being that the substrate is a GH3128 wafer.

[0062] Figure 6 This is a photo of the coated test piece prepared in Example 4 after 50 thermal shocks (900°C to room temperature). It can be seen from the figure that after the thermal shock, the coating is intact without cracks or peeling.

[0063] Comparative Example 1

[0064] The preparation method of the sealing ring provided in this comparative example refers to Example 1, with the main difference being that in step (3), a multi-piece combined inner and outer support mold is used during the sandblasting process, and the flexible copper wire is not embedded inside the large end of the inner concave surface of the C-shaped ring, and the elastic polyurethane ring is not embedded inside the small end.

[0065] Upon testing, it was found that the sealing ring prepared in this comparative example was deformed.

[0066] Comparative Example 2

[0067] The preparation method of the sealing ring provided in this comparative example refers to Example 1, with the main difference being that in step (4), the outer ring clamp is rigidly supported during the spraying process and fits tightly with the outer edge of the blank, and a circular ring made of 304 stainless steel or high-temperature alloy strip with a thickness equivalent to that of the sealing ring blank is not used to embed the groove of the sealing ring blank into the outer edge of the spraying area to form an elastic fit with the outer edge of the spraying area to control the edge of the outer spraying area.

[0068] Figure 7 This is a real picture of the sealing ring prepared in Comparative Example 2. As can be seen from the figure, there is a gap at the edge of the coating area of ​​the sealing ring.

[0069] Comparative Example 3

[0070] The preparation method of the sealing ring provided in this comparative example refers to Example 3, with the main difference being that in step (4), during the spraying process, the jet cuts in in the forward direction, the jet centerline passes through the rotation centerline of the blank, and a rigid clamp is used to fit the joint of the inner spraying area as the "wall root".

[0071] The "wall root effect" formed between the inner spray surface and the fixture causes coating accumulation, and the coating accumulation is irregularly peeled off when the fixture is removed. Figure 8 This is a physical picture of the sealing ring prepared in Comparative Example 3. As can be seen from the figure, there is a gap at the boundary of the coating area of ​​the sealing ring.

[0072] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.

Claims

1. An aircraft engine sealing ring with a coating in a specific area, characterized in that: The cross section of the aircraft engine sealing ring with coating in the specific area is "C" shaped, and the whole is an arc structure, a groove is formed in the middle of the arc structure, and the opening direction of the groove points to the outside of the overall arc structure of the sealing ring; The specific area with coating is the arc-shaped sealing surface composed of the arc end surface of the aircraft engine sealing ring and the structures on both sides of the groove, the arc-shaped sealing surface with a larger diameter is the large end, and the arc-shaped sealing surface with a smaller diameter is the small end; Preferably, the diameter of the large end is 125-250 mm, and the diameter of the small end is 120-245 mm.

2. The aircraft engine sealing ring with coating in specific area according to claim 1, characterized in that: The base material of the sealing ring is made of Waspaloy, GH738 or GH3128, with a thickness of 0.2 to 0.3 mm; The coating is a CoMoCrSi coating; preferably, the element composition of the CoMoCrSi coating includes: in mass percentage, Mo: 27.5-33.6wt.%, Cr: 16.9-18.5wt.%, Si: 3.1-4.9wt.%, Co: balance; the thickness of the coating is 40-160μm; The area of ​​the specific region to which the coating is attached accounts for 40-70% of the total area of ​​the aircraft engine sealing ring with the coating in the specific region.

3. The aircraft engine sealing ring with coating in specific area according to claim 1 or 2, characterized in that: The air leakage of the aircraft engine sealing ring with coating in the specific area is not more than 5×10 -3 m 3 / s.

4. A method for preparing an aircraft engine sealing ring with a coating in a specific area according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) forming the substrate by cold pressing to obtain an aircraft engine sealing ring blank with a specific area to be sprayed; (2) subjecting the specific area of ​​the aircraft engine sealing ring blank to be sprayed to solid solution, primary aging, and secondary aging treatment under vacuum conditions to obtain the specific area of ​​the aircraft engine sealing ring blank to be sprayed after heat treatment; (3) using a multi-piece combined inner and outer support mold to perform surface roughening pretreatment on the specific area of ​​the aircraft engine sealing ring blank to be sprayed after the heat treatment, so as to obtain the aircraft engine sealing ring blank to be sprayed after the pretreatment of the specific area; (4) Spraying a CoMoCrSi coating on the specific area of ​​the aircraft engine sealing ring blank to be sprayed in the specific area after the pretreatment by using supersonic flame spraying technology to obtain an aircraft engine sealing ring with a coating in the specific area.

5. The preparation method according to claim 4, characterized in that: In step (1), the process flow of the cold press forming includes stretching the main body, shaping the main body, cutting off the waste, forming at both ends and shaping at both ends; preferably, the temperature of the cold press forming does not exceed 50°C.

6. The preparation method according to claim 4 or 5, characterized in that: In step (2), the vacuum degree of the vacuum heat treatment condition is 10 -2 ~10 -1 Pa.

7. The preparation method according to any one of claims 4 to 6, characterized in that: In step (2), the solution temperature is 1000-1100° C., and the solution time is 5 min-4 h; The primary aging temperature is 835-855°C, and the primary aging time is 4-24h; The secondary aging temperature is 750-770° C., and the secondary aging time is 15-17 hours.

8. The preparation method according to any one of claims 4 to 7, characterized in that: In step (3), the multi-piece combined inner and outer supporting mold includes a base, an outer ring combined fixing plate, an inner ring positioning boss, a center limiting groove, a lateral positioning hole component, an anti-slip block, and a fastener located on the base for fixing the sealing ring blank; Preferably, when a multi-piece combined inner and outer supporting mold is used, a flexible copper wire matching the curvature is embedded inside the large end of the inner concave surface of the sealing ring blank, and an elastic polyurethane ring matching the curvature is mounted inside the small end of the sealing ring blank to fix the sealing ring and protect the non-sandblasting area. The axial and radial tensions are adjusted by fasteners. The roughening treatment is performed by sandblasting with white corundum sand; preferably, the particle size of the white corundum sand is in the range of 250 to 600 μm, and the sandblasting pressure is in the range of 1.0 to 3.5 bar.

9. The preparation method according to any one of claims 4 to 8, characterized in that: In step (4), the fuel gas used in the supersonic flame spraying technology is hydrogen and oxygen, the fuel gas flow rate is 860-901 SLPM, the flow rate ratio of oxygen to hydrogen is 0.20-0.50, preferably 0.30-0.35; the speed of the powder feeding plate is 15-25%, and the number of spraying passes is 5-20; The HVOF spray gun is clamped by an industrial robot and cuts forward, spraying at a variable angle from the outside to the inside. The spraying direction of the flame jet deviates from the center of the blank by a certain distance, and at the cutting point, the speed component of the flame jet spraying along the blank rotation direction is equal to the blank rotation linear speed; Preferably, the angle between the flame jet and the horizontal direction is 45°, the linear speed of the blank rotation is 105,000-135,000 mm / min, the jet speed is 200-500 m / s, and the jet beam spot diameter is 8-12 mm. The angle of the jet center direction deviating from the center is 0.5-2.0°, and the spatial distance between the flame jet entry point and the blank rotation center is 4.0-6.5 mm.

10. The preparation method according to any one of claims 4 to 9, characterized in that: In step (4), a shadow shielding method is used to control the spraying area of ​​the CoMoCrSi coating; Preferably, the shadow shielding method uses the shadow shielding principle to adjust the flame flow angle of the HVOF spray gun, the protruding height of the inner ring positioning boss, and the gap between the inner ring positioning boss and the sealing ring blank to control the boundary of the inner spraying area. At the same time, a circular ring made of 304 stainless steel or high-temperature alloy strip with a thickness equivalent to that of the sealing ring blank is embedded in the groove of the sealing ring blank to form an elastic fit with the outer edge of the spraying area to control the edge of the outer spraying area.

Citation Information

Cited By

  • Thin-wall special-shaped metal sealing ring surface toughening CoMoCrSi coating

    CN121575358A

  • A surface toughened CoMoCrSi coating for thin-walled profiled metal seals

    CN121575358B