Preparation method of nano circular truncated cone
Through the combination of secondary exposure technology and FEM model, the exposure parameters are optimized, and the complex shape limitation and uniformity problems of traditional single exposure technology in high-precision microstructure preparation are solved, and the precise preparation of high-deep and aspect ratio nanocircle stages is achieved, improving the improvement of The manufacturing accuracy and consistency of MEMS structures are achieved.
Patent Information
- Application Number
- CN202411357339.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-27
AI Technical Summary
Traditional single-shot exposure technology has complex shape limitations, uniformity problems and technical obstacles to the difficulty of realizing high-level structures when preparing high-precision microstructures, resulting in increased production costs and extended process cycles.
The secondary exposure technology combined with the FEM model is used to optimize the exposure energy and focal length matrix parameters to achieve accurate preparation of high-deep and aspect ratio nanocircle stages to ensure high accuracy and consistency of lithography.
It significantly improves the preparation accuracy, consistency and reliability of the nano-circle stage, improves the manufacturing accuracy of the MEMS structure, and meets the requirements of high-deep and aspect ratio.
Smart Images

Figure CN118963072A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of micro-electromechanical systems, and in particular relates to a method for preparing a nano frustum. Background Art
[0002] In the manufacturing process of MEMS (micro-electromechanical systems), the key to achieving high performance lies in precise control of microstructures. Although traditional single-shot exposure technology performs well in many application scenarios, it still has the following limitations when preparing high-precision microstructures:
[0003] 1. Complex shape limitations: For microstructures that require fine three-dimensional configurations, a single exposure often cannot achieve the required geometric accuracy. This usually requires multi-layer exposure and more complex lithography steps to build, which leads to increased production costs and longer process cycles. 2. Uniformity issues: When a large area of wafer is exposed at one time, the uneven distribution of light intensity may cause deviations in the size and morphology of microstructures between different regions on the same wafer, thereby affecting the consistency and stability of the product. 3. It is difficult to achieve high-aspect ratio structures: For certain specific MEMS devices, it is necessary to create fine structures with high aspect ratio features. However, as the depth of these structures increases, the difficulty of maintaining the sidewall inclination and overall consistency using a single exposure method also increases, which brings additional technical obstacles to actual operations.
[0004] Therefore, it is necessary to improve the existing photolithography technology to further improve the performance of MEMS devices. Summary of the invention
[0005] The present invention provides a method for preparing a nano frustum, which utilizes a secondary exposure technique to precisely control the size and morphology of a microstructure, thereby achieving precise preparation of a nano frustum with a high aspect ratio.
[0006] Other purposes and advantages of the present invention can be further understood from the technical features disclosed in the present invention.
[0007] To achieve one or part or all of the above purposes or other purposes, a method for preparing a nano frustum is provided by a technical solution of the present invention, characterized in that it comprises the following steps: Step 1: constructing a wafer bare chip FEM model, setting an exposure energy base value and an exposure focal length base value according to the required frustum size, establishing a wafer bare chip exposure energy value and exposure focal length matrix, using the parameters in the wafer bare chip exposure energy value and exposure focal length matrix to perform exposure and development to obtain a frustum structure, measuring the critical dimensions of the frustum structure and comparing them with the required critical dimensions of the frustum structure to obtain an optimal exposure energy value and an optimal exposure focal length; Step 2: performing an exposure at 40% of the optimal exposure energy value and an exposure focal length of 0um; And construct a double exposure FEM model, the double exposure energy base value is 70% of the optimal exposure energy value obtained in step 1, the double exposure basic focal length base value is the optimal exposure focal length obtained in step 1, establish a double exposure energy value and a double exposure focal length matrix, use the parameters in the double exposure energy value and the double exposure focal length matrix to perform double exposure and development on a wafer exposed once to obtain a truncated cone structure, measure the key dimensions of the truncated cone structure and compare them with the required key dimensions of the truncated cone, and obtain the optimal double exposure energy value and the optimal double exposure focal length; Step three: use the single exposure parameters and double exposure parameters obtained in step 2 to expose and develop on a wafer coated with photoresist to obtain the required nano-truncated cone structure. The beneficial effect of this technical solution is that the present invention combines the double exposure technology with the construction of the FEM model, uses the FEM model to simulate the parameters of the double exposure, and optimizes the parameters of the double exposure to ensure the high precision and consistency of the lithography. At the same time, the preparation accuracy, consistency and reliability of the nano-truncated cone can be significantly improved through the double exposure technology, and the manufacturing accuracy and high aspect ratio requirements of the MEMS structure can be improved.
[0008] In the step 1, the exposure focal length base value is set to 0um.
[0009] In step one, the exposure energy value of the wafer bare chip and the parameters in the exposure focal length matrix are exposed one by one on the wafer bare chip using the same mask; in step two, the secondary exposure energy value and the parameters in the secondary exposure focal length matrix are secondary exposed one by one on the wafer exposed once using the same mask.
[0010] If the measurement result of the parameters in the wafer bare die exposure energy value and exposure focal length matrix and the secondary exposure energy value and the secondary exposure focal length matrix that are closest to the required frustum critical dimension among the frustum critical dimensions after exposure and development are within ±10% of the required frustum critical dimension, then the parameter corresponding to the measurement result that is closest to the required frustum critical dimension is the optimal exposure parameter; otherwise, the exposure energy value and the exposure focal length matrix are reconstructed until the measurement result of the parameters in the matrix that are closest to the required frustum critical dimension among the frustum critical dimensions after exposure are within ±10% of the required frustum critical dimension.
[0011] The key dimension of measuring the truncated cone structure is the bottom diameter of the truncated cone structure.
[0012] In the step 2, the overlap accuracy of the second exposure pattern and the first exposure pattern is less than 0.2um.
[0013] In the step 2, the exposure equipment, temperature and humidity used in the second exposure are the same as those used in the first exposure.
[0014] The step three includes the following steps: S3.1 cleaning the back side of the wafer; S3.2 uniformly coating a BARC layer with a thickness of 30 nm and a photoresist located above the BARC layer on the wafer; S3.3 performing a first exposure according to the first exposure parameters obtained in step two; S3.4 performing a second exposure according to the second exposure parameters obtained in step two; S3.5 developing the exposed wafer surface to obtain a nano-cone structure; S3.6 removing impurities from the surface of the nano-cone structure to remove surface residues.
[0015] The developer is a 2.38% concentration tetramethylammonium hydroxide solution.
[0016] In step S3.6, a plasma cleaning machine is used to perform surface decontamination modification for 60 seconds.
[0017] Compared with the prior art, the beneficial effects of the present invention mainly include that the present invention combines the double exposure technology with the construction of the FEM model, uses the FEM model to simulate the parameters of the double exposure, and optimizes the parameters of the double exposure to ensure the high precision and consistency of the lithography. At the same time, the double exposure technology can significantly improve the preparation accuracy, consistency and reliability of the nano-truncated cone, and improve the manufacturing accuracy of the MEMS structure and the requirements of high aspect ratio. .
[0018] In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the specific embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 Schematic diagram of the preparation process of the nano frustum of the present invention.
[0021] Figure 2 This is a scanning electron microscope morphology image of the critical size of the nano-truncated cone prepared in Example 1.
[0022] Figure 3 This is a critical size measurement image of the nano-truncated cone prepared in Example 1 under a scanning electron microscope. DETAILED DESCRIPTION
[0023] The above and other technical contents, features and effects of the present invention will be clearly presented in the following detailed description of a preferred embodiment with reference to the drawings. The directional terms mentioned in the following embodiments, such as up, down, left, right, front or back, etc., are only referenced to the directions of the attached drawings. Therefore, the directional terms used are used to illustrate and not to limit the present invention.
[0024] Embodiment 1
[0025] Embodiment 1 provides a method for preparing a nano frustum, comprising the following steps:
[0026] Step 1: Construct a FEM (energy focal length matrix) model of a wafer bare die coated with photoresist.
[0027] The construction of the FEM model is a systematic process, including the following steps: demand analysis, determining the size and shape of the required microstructure. In the first embodiment of the truncated cone preparation method, the microstructure size and shape that need to be determined are mainly the bottom diameter and the height of the truncated cone;
[0028] Parameter selection, in Example 1, exposure energy and focal length are selected as the main parameters affecting the geometric characteristics of the truncated cone; experimental design, designing the selected parameters, changing the exposure value and the basic value of the focal length so that the parameters can cover the expected space; data collection, using statistical methods, conducting experiments according to the experimental parameters preset in the experimental design stage, and collecting the size and shape of the truncated cone under different experimental parameters; verification and optimization, adjusting the experimental parameters in the FEM model based on the comparison of the collected truncated cone size and shape under different experimental parameters with the required truncated cone size and shape, so as to optimize the FEM model.
[0029] According to the required size of the truncated cone, an exposure energy base value is set, which can be preset according to photolithography experience, and an exposure focal length base value is set, which is preset to 0um. The set exposure energy base value and exposure focal length base value are adjusted, and multiple values near the set base value are selected on the basis of the set base value, and a wafer bare die exposure energy value and exposure focal length matrix are established. The parameters in the wafer bare die exposure energy value and exposure focal length matrix are used for exposure and development to obtain a truncated cone structure, and the critical dimensions of the truncated cone structure are measured and compared with the required critical dimensions of the truncated cone structure, and the exposure energy value and exposure focal length closest to the required value are selected as the optimal exposure energy value and optimal exposure focal length;
[0030] Step 2: First, perform an exposure on the photoresist-coated wafer according to 40% of the optimal exposure energy value obtained in step 1 and an exposure focal length of 0 um to obtain a wafer after the exposure;
[0031] Reconstruct a secondary exposure FEM model, after the first exposure is completed, perform secondary exposure on the basis of the wafer after the first exposure, the secondary exposure FEM model established during the secondary exposure, the secondary exposure energy base value selected is 70% of the optimal exposure energy value obtained in step one, the secondary exposure base focal length base value is the optimal exposure focal length in step one, establish a secondary exposure energy value and a secondary exposure focal length matrix, the selection of the secondary exposure energy value and the secondary exposure focal length matrix is the same as in step one, use the secondary exposure energy value and the parameters in the secondary exposure focal length matrix to perform secondary exposure on the wafer after the first exposure, develop to obtain a truncated cone structure, measure the critical dimensions of the truncated cone structure and compare with the required critical dimensions of the truncated cone, and obtain the optimal secondary exposure energy value and the optimal secondary exposure focal length;
[0032] Step 3: Use the first exposure parameters and the second exposure parameters obtained in step 2 to expose and develop the wafer coated with photoresist to obtain the desired nano-truncated cone structure.
[0033] In order to ensure the implementation of the FEM model and to find the optimal lithography parameters, in step one, the same mask with the same pattern on the mask is used, and the exposure energy value of the wafer bare chip and the parameters in the exposure focal length matrix are exposed one by one on the wafer bare chip. Except for the exposure energy value and the exposure focal length parameters, other parameters during exposure are the same; in step two, the same mask is used, and the secondary exposure energy value and the parameters in the secondary exposure focal length matrix are secondary exposed one by one on the wafer exposed once to ensure the exposure identity. At the same time, the mask during the secondary exposure should be in the same position as the mask during the primary exposure.
[0034] In step one and step two, the method for obtaining the optimal exposure energy value and exposure focal length of the wafer bare chip and the optimal secondary exposure energy value and secondary exposure focal length is that if the measurement results of the parameters in the exposure energy value and exposure focal length matrix of the wafer bare chip and the secondary exposure energy value and the secondary exposure focal length matrix are closest to the required truncated cone structure key dimensions after exposure and development, and the difference range with the required truncated cone structure key dimensions is within ±10%, then the exposure parameters corresponding to the measurement results closest to the required truncated cone structure key dimensions are the optimal exposure parameters; otherwise, the exposure energy value and exposure focal length matrix are reconstructed until the measurement results of the parameters in the matrix are closest to the required truncated cone structure key dimensions after exposure and the difference range with the required truncated cone structure key dimensions is within ±10%.
[0035] In step 2, the overlap accuracy of the second exposure and the first exposure pattern is less than 0.2um. The second exposure uses the same exposure equipment, temperature, and humidity as the first exposure to reduce the impact of variables on the results.
[0036] See also Figure 1 Schematic diagram of the nanotruncated cone preparation process in FIG. 1 , step three includes the following steps:
[0037] S3.1 Clean the back side of the wafer; S3.2 Evenly coat a BARC layer with a thickness of 30 nm and a photoresist located above the BARC layer on the wafer; S3.3 Perform a first exposure according to the first exposure parameters obtained in step 2; S3.4 Perform a second exposure according to the second exposure parameters obtained in step 2; S3.5 Develop the wafer surface after exposure, using a 2.38% concentration of tetramethylammonium hydroxide solution as the developer to obtain a nano-truncated cone structure; S3.6 De-impurize the surface of the nano-truncated cone structure, using a plasma cleaner for 60 seconds to remove surface residues.
[0038] The following is a detailed description of the manufacturing of a truncated cone with a bottom diameter of 500 nm as an example. The truncated cone structure to be prepared is prepared on an 8-inch wafer coated with a photoresist thickness of 1.2 um, and the microstructure size designed on the mask is a circle of 500 nm.
[0039] The preparation process is as follows:
[0040] a) Establish a FEM model on a bare wafer. The exposure energy base value is set to 225mj based on exposure experience. Five energy groups of 175mj, 200mj, 225mj, 250mj, and 275mj are selected in sequence near 225mj. The exposure focal length base value is set to 0um. Seven focal length groups of 0um, -0.2um, -0.3um, -0.4um, -0.5um, -0.6um, and -0.7um are selected in sequence. Establish a FEM model on a bare wafer. Expose and develop the parameters in the above bare wafer FEM model one by one on a photolithography machine to obtain the corresponding truncated cone structure. The bottom diameter of the truncated cone is measured by CD-SEM (critical dimension scanning electron microscope). The measurement results are shown in Table 1 below.
[0041] Table 1 Wafer bare die FEM model parameters CD-SEM data after exposure
[0042]
[0043]
[0044] The NA in the above table indicates that the data cannot be measured due to the distortion of the image. After comparison, the energy of 250mj and the focal length of -0.2um are selected as the optimal exposure energy and optimal exposure focal length of the wafer bare die. Of course, other exposure energy values and exposure focal length values with the measurement result of 0.5um in Table 1 can also be selected.
[0045] b) The exposure energy value X=250mj obtained from step a, the exposure energy of one exposure is selected as 40% of the optimal exposure energy value in step a, that is, the exposure energy value of one exposure is 100mj, and the exposure focal length is selected as 0um. According to the selected exposure energy value and exposure focal length of one exposure, one exposure is performed on the wafer bare chip.
[0046] c) The energy base value of the second exposure is 70% of the optimal exposure energy value in step a, that is, the exposure energy base value of the second exposure is 175mj, and the focal length base value is the optimal exposure focal length -0.2um in step a. Referring to the base value, five energy values of 160mj, 170mj, 180mj, 90mj, and 200mj are selected, and six focal lengths of -0.6um, -0.4um, -0.3um, 0um, 0.2um, and 0.4um are selected to establish a second exposure FEM model, and each parameter in the second exposure FEM model is subjected to second exposure on the wafer bare die after the first exposure, wherein the overlap accuracy of the first exposure and the second exposure pattern should be less than 0.2um. After the second exposure, the corresponding truncated cone structure is obtained by development, and the bottom diameter of the truncated cone is measured by CD-SEM (critical dimension scanning electron microscope), and the measurement results are shown in Table 2.
[0047] Table 2. Parameters of the double-exposure FEM model. CD-SEM data after exposure.
[0048]
[0049] After comparison, after the second exposure, when the energy value is 190mj and the focal length is -0.6um, the obtained cone size is 0.52um. The bottom diameter of the cone is also the data closest to the target cone bottom diameter of 0.5um in the second exposure FEM model in Table 2. The difference between the measured result and the required cone bottom diameter is less than 10% of the target cone bottom diameter, which meets the design requirements. Therefore, the exposure energy of the second exposure is 190mj and the focal length is -0.6um.
[0050] d) Based on the first exposure parameters and the second exposure parameters obtained in step c and step d, the desired nano-truncated cones are prepared on an 8-inch wafer coated with a photoresist thickness of 1.2 um, specifically comprising the following steps:
[0051] d1 cleaning, cleaning the back side of the wafer;
[0052] d2 coating: evenly coating a 30nm BARC layer and a 1.2um photoresist on the wafer. The BARC layer is an anti-reflective layer used to reduce the reflection of the light source during photolithography and improve the photolithography effect.
[0053] d3 single exposure, set the exposure energy value to 100msec, focal length to 0um, and perform a single exposure;
[0054] D4 double exposure, set the exposure energy value to 190msec, focal length -0.6um, and perform double exposure;
[0055] d5 development, using 2.38% TMAH (tetramethylammonium hydroxide) solution for development;
[0056] D6 post-processing uses a plasma cleaner to perform a de-impurity modification process on the wafer surface after development to remove surface residues.
[0057] The process in step d is shown in Figure 1 Schematic diagram of the nanotruncated cone preparation process.
[0058] See also Figure 2 It can be found that when the exposure energy is 190mj and the exposure focal length is -0.6um, the sidewall angle and top flatness of the frustum can be optimized, so that the frustum structure meets the requirements of the MEMS structure for a high aspect ratio. Figure 3After the secondary exposure, the truncated cone structure was measured under CD-SEM (critical dimension scanning electron microscope) to confirm that the bottom size of the cone was 537nm, the height was 1.2um, and the aspect ratio of the nano-truncated cone was about 2.4. The size of the prepared truncated cone structure met the required truncated cone structure size, and the preparation process met the requirements.
[0059] The above is a detailed introduction to a method for preparing a nano-truncated cone provided by the present invention. In this article, a specific example is used to illustrate the structure and working principle of the present invention. The description of the above embodiment is only used to help understand the method and core idea of the present invention. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, several improvements and modifications can be made to the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a nano frustum, characterized in that: The steps include: Step 1: construct a wafer bare die FEM model, set the exposure energy base value and the exposure focal length base value according to the required frustum size, establish the wafer bare die exposure energy value and exposure focal length matrix, use the parameters in the wafer bare die exposure energy value and exposure focal length matrix to expose and develop to obtain a frustum structure, measure the key dimensions of the frustum structure and compare them with the required key dimensions of the frustum structure to obtain the optimal exposure energy value and the optimal exposure focal length; Step 2: Perform an exposure on the photoresist-coated wafer at 40% of the optimal exposure energy value obtained in step 1 and an exposure focal length of 0 um; A secondary exposure FEM model is constructed, wherein the secondary exposure energy base value is 70% of the optimal exposure energy value obtained in step 1, and the secondary exposure base focal length base value is the optimal exposure focal length obtained in step 1, and a secondary exposure energy value and a secondary exposure focal length matrix are established. Secondary exposure and development are performed on a wafer exposed once using the parameters in the secondary exposure energy value and the secondary exposure focal length matrix to obtain a truncated cone structure, and the critical dimensions of the truncated cone structure are measured and compared with the required critical dimensions of the truncated cone to obtain an optimal secondary exposure energy value and an optimal secondary exposure focal length; Step 3: Use the first exposure parameter and the second exposure parameter obtained in step 2 to expose and develop the wafer coated with photoresist to obtain the desired nano frustum structure.
2. A method for preparing a nano frustum according to claim 1, characterized in that: In the step 1, the exposure focal length base value is set to 0um.
3. The method for preparing a nano frustum according to claim 1, characterized in that: In the step 1, the exposure energy values of the wafer bare chips and the parameters in the exposure focal length matrix are exposed one by one on the wafer bare chips using the same photomask; In step 2, the same photomask is used to perform secondary exposure on the wafer that has been exposed once, with the secondary exposure energy value and the parameters in the secondary exposure focal length matrix one by one.
4. The method for preparing a nano frustum according to claim 1, characterized in that: The measurement result of the critical dimension of the truncated cone structure after exposure and development of the parameters in the exposure energy value and the exposure focal length matrix of the wafer bare die and the secondary exposure energy value and the secondary exposure focal length matrix is closest to the required critical dimension of the truncated cone, and the difference range with the required critical dimension of the truncated cone is within ±10%, then the parameter corresponding to the measurement result closest to the required critical dimension of the truncated cone is the optimal exposure parameter; Otherwise, the exposure energy value and exposure focal length matrix are reconstructed until the measurement result of the frustum critical dimension closest to the required frustum critical dimension among the parameters in the matrix after exposure is within a range of ±10% from the required frustum critical dimension.
5. The method for preparing a nano frustum according to claim 1, characterized in that: The key dimension of measuring the truncated cone structure is the bottom diameter of the truncated cone structure.
6. The method for preparing a nano frustum according to claim 1, characterized in that: In the step 2, the overlap accuracy of the second exposure pattern and the first exposure pattern is less than 0.2um.
7. The method for preparing a nano frustum according to claim 1, characterized in that: In the step 2, the exposure equipment, temperature and humidity used in the second exposure are the same as those used in the first exposure.
8. The method for preparing a nano frustum according to claim 1, characterized in that: The step three comprises the following steps: S3.1 Clean the back side of the wafer; S3.2 uniformly coating a BARC layer with a thickness of 30 nm and a photoresist located above the BARC layer on the wafer; S3.3 perform one exposure according to the one exposure parameters obtained in step 2; S3.4 Perform secondary exposure according to the secondary exposure parameters obtained in step 2; S3.5 developing the exposed wafer surface to obtain a nano frustum structure; S3.6 De-impurify and modify the surface of the nano-truncated cone structure to remove surface residues.
9. A method for preparing a nano frustum according to claim 8, characterized in that: The developer is a 2.38% concentration tetramethylammonium hydroxide solution.
10. The method for preparing a nano frustum according to claim 8, characterized in that: In step S3.6, a plasma cleaner is used to perform surface decontamination modification for 60 seconds.
Citation Information
Patent Citations
Method for improving photoresist profile
CN103645609A
Photoetching process method
CN110632829A
Method for setting photoetching exposure conditions
CN112213922A
Method for determining photoetching sequence of multiple patterning
CN113791526A
Method for manufacturing close-packed structural article, exposure mask used in the same, and microlens array
JP2005114865A