Method for predicting service life of nickel-based surface coating of descaling roller

By establishing a finite element model and using the NormalStress criterion for fatigue life prediction, the problem of low accuracy in predicting the life of nickel-based surface coatings on descaling rollers was solved, achieving high-precision life prediction results.

CN118965877APending Publication Date: 2024-11-15UNIV OF SCI & TECH LIAONING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411007860.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing technology, the life prediction accuracy of the nickel-based surface coating of the descaling roller is not high, and its service life cannot be accurately predicted.

Method used

By establishing a finite element model for life prediction, and combining the stress-life curves of 42CrMO and WC45 materials, the rolling contact fatigue damage of the descaling roller is simulated using the finite element analysis method. The fatigue life is predicted using the NormalStress criterion, and the model accuracy is corrected according to the actual working conditions to calculate the predicted life of the coating.

Benefits of technology

The accuracy of predicting the lifespan of the nickel-based surface coating on the descaling roller reached over 90%, improving the accuracy and reliability of the prediction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118965877A_ABST
    Figure CN118965877A_ABST
Patent Text Reader

Abstract

The invention discloses a descaling roller nickel-based surface coating service life prediction method, which comprises the following steps: obtaining a material stress-service life curve of a base material 42CrMO and a surface coating WC45 of a descaling roller, establishing a service life prediction finite element model, and calculating the service life of the descaling roller according to the shape, size and relative friction relation of the descaling roller and a plate blank in an original working condition. The method comprises the following steps: respectively establishing a 42CrMO rolling contact fatigue damage geometric model and a WC45 rolling contact fatigue damage geometric model, constructing a 42CrMO rolling contact fatigue damage constitutive model and a WC45 rolling contact fatigue damage constitutive model, and carrying out finite element analysis and model precision correction and optimization: observing according to the actual working condition of the descaling roller without the coating to obtain the actual service life of the descaling roller; and the calculated service life of the base material 42CrMO is obtained according to the analysis, the actual service life and the calculated service life of the base material 42CrMO are compared, an error is calculated, a service life curve is obtained, and the predicted service life is calculated. The method has the advantages of being high in prediction precision, convenient to use and wide in application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of life prediction of descaling roller coating materials, and in particular to a life prediction method for a nickel-based surface coating of a descaling roller of descaling equipment. Background Art

[0002] The fatigue failure process is usually divided into three stages: fatigue crack initiation, fatigue crack extension and final fracture. When mechanical parts are subjected to repeated stress or strain cycles, even if the stress level is lower than the static strength limit of the material, damage will gradually accumulate, eventually leading to the formation and extension of cracks. Common forms of fatigue failure include bearing spalling, gear tooth surface wear, welded structure cracks, spring fracture, etc. The study of mechanical fatigue failure began in the 19th century, and there have been extensive theoretical and experimental research results so far. Classical theories such as Paris's law and SN curve (stress-life curve) provide the basis for fatigue life prediction. Modern research not only focuses on the fatigue behavior of traditional metal materials, but also extends to the fatigue properties of composite materials, ceramic materials and polymer materials. At the same time, advanced fatigue testing equipment and numerical simulation techniques, such as finite element analysis (FEA) and fracture mechanics models, also provide powerful tools for in-depth understanding of fatigue failure mechanisms and the formulation of preventive measures.

[0003] Document CN106295005B discloses a multi-factor prediction method for contact fatigue life of spray coating, and specifically discloses "determining the factors that affect the contact fatigue life of the spray coating when the spray coating is subjected to rolling and sliding, and setting the value range of each factor; combining the values ​​of each factor according to the combination method of n factors and 2 levels to obtain multiple combinations, where n is the number of factors; conducting contact fatigue tests according to the values ​​of each factor in each combination to obtain the contact fatigue life corresponding to the combination; establishing a multivariate regression model between the contact fatigue life and each factor according to the values ​​of each factor in each combination and the contact fatigue life corresponding to each combination; predicting the contact fatigue life of the spray coating to be predicted according to the multivariate regression model." In this prior art, the multivariate regression model is used to predict the contact fatigue life of the spray coating, eliminating the limitation of the single factor method in the application of life prediction. However, its prediction accuracy is still insufficient.

[0004] Especially for descaling equipment, the current service life of the nickel-based descaling roller (42CrMO) in actual use is about 6 months. In order to increase the service life, a coating needs to be coated on the nickel-based surface. In order to obtain the service life of the descaling roller with the coating, a prediction method needs to be used for prediction. However, the currently known prediction methods all have the problem of low accuracy. Summary of the invention

[0005] In view of this, the present invention proposes a life prediction method for a nickel-based surface coating of a descaling roller with high prediction accuracy.

[0006] The object of the present invention is achieved through the following technical scheme: A method for predicting the life of a nickel-based surface coating of a descaling roller, characterized in that it comprises the following steps:

[0007] Step 1, obtaining material stress-life curves of the base material 42CrMO and the surface coating WC45 of the descaling roller;

[0008] Step 2: Establish a life prediction finite element model:

[0009] Step 2.1, according to the shape and size of the descaling roller and the plate and the relative friction relationship in the original working condition, the 42CrMO rolling contact fatigue damage geometric model and the WC45 rolling contact fatigue damage geometric model are established respectively;

[0010] Step 2.2, on the basis of the 42CrMO rolling contact fatigue damage geometric model and the WC45 rolling contact fatigue damage geometric model, assign material properties and perform meshing to form a 42CrMO rolling contact fatigue damage constitutive model and a WC45 rolling contact fatigue damage constitutive model, and perform finite element simulation calculation on the 42CrMO rolling contact fatigue damage constitutive model and the WC45 rolling contact fatigue damage constitutive model, select a fatigue life prediction method and convert the stress-life curves of the substrate 42CrMO and the surface coating WC45 in step 1 into data and import them into a finite element analysis system, and obtain the calculated life of the rolling contact fatigue damage of the substrate 42CrMO and the surface coating WC45 through finite element simulation calculation and analysis;

[0011] Step 3: Model accuracy correction and optimization:

[0012] The actual life of the descaling roller is obtained by observing the actual working condition of the descaling roller without coating, and the calculated life of the substrate 42CrMO is obtained according to the analysis in step 2.2, and the actual life and calculated life of the substrate 42CrMO are compared and the error is calculated;

[0013] Step 4: Obtain the service life curve and calculate the actual service life:

[0014] According to the calculation error obtained in step 3, combined with the calculated life of coating WC45 obtained in step 2.2, the predicted life of the descaling roller after coating the surface coating WC45 is calculated.

[0015] Among them, the 42CrMO rolling contact fatigue damage geometric model and the WC45 rolling contact fatigue damage geometric model established in step 2.1 are respectively symmetrical models with the plane of the diameter of the midpoint of the axis of the descaling roller as the left-right symmetrical model, and the left half or the right half of the 42CrMO rolling contact fatigue damage geometric model and the WC45 rolling contact fatigue damage geometric model are respectively taken to perform step 2.2. Rigid patches are set on the left and right end surfaces of the descaling roller in the half of the 42CrMO rolling contact fatigue damage geometric model and the WC45 rolling contact fatigue damage geometric model, and the size of the rigid patches is In step 2.2, the NormalStress criterion is selected as the fatigue life prediction method.

[0016] Further, in step 2.1, in step 2.1, the diameter of the descaling roller in the 42CrMO rolling contact fatigue damage geometric model and the diameter of the descaling roller in the WC45 rolling contact fatigue damage geometric model are both However, in the WC45 rolling contact fatigue damage geometric model, the outermost 7 mm of the scale roller is the surface coating.

[0017] Beneficial effect: The life prediction method of the nickel-based surface coating of the descaling roller provided by the present invention is based on the life curve of the material and uses the same fatigue life algorithm to carry out service life prediction for the substrate 42CrMO and the surface coating WC45 respectively, and calculates the predicted life of the surface coating of the descaling roller containing the coating according to the actual life of the descaling roller in the original working condition and the accuracy value of the calculated life, and the prediction accuracy can reach more than 90%. Compared with the existing technology, this method has the advantages of high prediction accuracy, easy use and wide application. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The accompanying drawings of the present invention are as follows.

[0019] Figure 1 (a) is the SN curve of material 42CrMo;

[0020] Figure 1(b) is the SN curve of material WC;

[0021] Figure 2 It is the geometric model of rolling contact fatigue damage of 42CrMo;

[0022] Figure 3 It is the geometric model of rolling contact fatigue damage of WC45;

[0023] Figure 4 This is the finite element analysis diagram of 42CrMo rolling contact fatigue life;

[0024] Figure 5 This is the finite element analysis diagram of WC45 rolling contact fatigue life. DETAILED DESCRIPTION

[0025] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be construed as limiting the present application. On the contrary, the embodiments of the present application include all changes, modifications and equivalents that fall within the spirit and connotation of the appended claims.

[0026] Example 1: As shown in Figures 1-5, this example is a method for predicting the service life of a descaling roller in a descaling device after the surface is coated with WC45. In the existing original working conditions, the surface of the descaling roller is uncoated, and its base material is 42CrMo.

[0027] The specific prediction steps are as follows:

[0028] Step 1: Obtain the stress-life curves of the nickel base (42CrMO) and surface coating (WC) of the descaling roller of the descaling equipment.

[0029] Since the life curves of the nickel base (42CrMO) and surface coating (WC) of the descaling roller have been disclosed in the prior art, such as "Feng Hao. Study on oblique incidence deposition process and microstructure characteristics of WC particle reinforced composite coating sprayed by supersonic flame [D]. Dalian University of Technology, 2016" and "Yu Yonghua, Jie Meiqiang, Li Baoyue, et al. Stress prediction of marine diesel engine crankshaft based on digital twin [J]. Chinese Ship Research, 2023, 18(05): 50-56.". Therefore, the data disclosed in the prior art will be directly used in this embodiment, specifically referring to Figure 1, Figure 1 (a) is the stress-life curve of material 42CrMO, and Figure 1 (b) is the stress-life curve of material WC.

[0030] Step 2: Establish a life prediction finite element model;

[0031] Step 2.1. Establish the geometric model of the mechanical parts: Since the model of the friction between the descaling roller and the slab is symmetrical with respect to the symmetry plane of the slab length, in order to appropriately reduce the amount of calculation and speed up the simulation process, the geometric model is simplified into a symmetrical model (cut along the XOY plane), and half of it is taken for simulation calculation. According to the simulation needs, it is determined to establish a total of two geometric models, namely the "42CrMo 'rolling contact fatigue damage' geometric model" and the "WC45 'rolling contact fatigue damage' geometric model". According to the shape and size of the descaling roller and the slab in the original working condition, as well as the relative friction relationship between the two, the following is established: Figure 3 The geometric model of 42CrMo "rolling contact fatigue damage", such as Figure 4 WC45 "rolling contact fatigue damage" geometry model.

[0032] (1) Slab model: In rolling contact fatigue, there is no relative sliding between the descaling roller and the slab. The descaling roller rotates one circle, and the length of the slab transported is 1256.63704mm. Combined with the field survey data, the maximum slab size is taken, and the size of the slab in the model is set to 1256.63704×1000×200 (mm). Figure 2 , 3 .

[0033] (2) Descaling roller model: The original working condition (i.e., the descaling roller is not coated) and the descaling roller with coated WC45 has the same dimensions as the original working condition (i.e., the descaling roller is not coated). The diameter is 400mm. However, on the descaling roller with coating, the hard surface layer is 3mm thick, the transition layer is 4mm thick, and the total thickness of the coating is 7mm. Figure 2 , 3 .

[0034] (3) Relative position: During the simulation, the descaling roller rotates around the Z axis for one circle, and the slab moves 1256.63704 mm to the left along the X axis. Therefore, the friction between the descaling roller and the left edge of the slab is set as the starting point of the simulation analysis. In the geometric model, the symmetrical section of the descaling roller is flush with the symmetrical section of the slab; the descaling roller is at the bottom and is tangent to the slab line contact, such as Figure 2 , 3 .

[0035] (4) Rigid patch for descaling roller: To drive the descaling roller to rotate and avoid the serious circumferential deformation of the descaling roller during the simulation process, resulting in a "singular point" and causing the simulation to not converge, a cylindrical rigid patch with a size of As shown in the figure Figure 2 , 3 The two rigid patches are set as rigid bodies and are bound to the two end faces of the descaling roller.

[0036] Step 2.2, establishing a constitutive model of the geometric model;

[0037] Based on the geometric model in step 2.1, material properties are assigned and cell division is performed to form a constitutive model. Then, the finite element system is used to simulate and calculate the constitutive model and output the analysis results. According to the simulation requirements, two models are established: the 42CrMo "rolling contact fatigue" constitutive model and the WC45 "rolling contact fatigue" constitutive model.

[0038] Table 1 Material parameter assignments of the two constitutive models

[0039]

[0040] Fatigue analysis model: According to the working condition of the descaling roller, its static friction fatigue damage belongs to multi-axis high-cycle fatigue (multi-axis: the descaling roller is subjected to loads in more than two directions, high cycle: through on-site investigation, the life cycle of the descaling roller is more than 10 4 times, less than 10 7 times). The mainstream criteria for high cycle fatigue life prediction mainly include NormalStress criterion and Brownmiller criterion. NormalStress criterion is applicable to most tough materials, since WC coating is not a tough material. Brownmiller algorithm of Morrow mean stress correction criterion is more suitable for the prediction of descaling roller fatigue life, so this criterion is selected as the fatigue life evaluation criterion.

[0041] The "stress-life curve (SN curve)" of the material in Figure 1 expresses the relationship between the fatigue strength and fatigue life of the material under certain cycle characteristics, and is the material damage parameter for fatigue analysis. According to the existing technology, the SN curves of 42CrMo and WC are obtained, as shown in Figure 1. The curves are converted into data and directly imported into the fatigue analysis system, as shown in Table 2.

[0042] Table 2 Material SN data

[0043]

[0044] Step 3, model accuracy verification: After investigation, it was found that when the descaling roller worked continuously for six months, it transported a total of 121783.4776 slabs. For each slab transported, the descaling roller rotated 7.3549 times (the descaling roller contacted the slab 8 times at some positions, so the worst case was taken). When a certain point on the descaling roller worked for six months, it contacted the slab 974267.8208 times, that is, the life of the descaling roller under the original working condition was 974267.8208 times. Figure 4 As shown in the figure, according to the model analysis, under the original working condition, the fatigue life of the descaling roller is 10 5.984 times, that is 963829.0236 times. After calculation, the error is 0.0107145.

[0045] Step 4: Analysis of coating rolling contact fatigue life: Figure 5 is the fatigue life of WC45 coating. It can be seen from the figure that the life after adding coating is 10 6.568 times, that is 3698281.798 times.

[0046] And from Figure 4 It can be observed that the fatigue damage under the original working condition is mainly concentrated in the symmetry center and the edge where the slab contacts the descaling roller. Figure 5It can be seen that after adding the coating, the location of fatigue failure has improved, but it is still concentrated in the symmetrical center. The life of the descaling roller under the original working condition is 6 months. After adding the coating, the life is increased from 6 months to 22.88 months (about two years).

[0047] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that various changes may be made to the present invention in form and detail without departing from the scope defined by the claims of the present invention.

Claims

1. A method for predicting the life of a nickel-based surface coating of a descaling roller, characterized in that: The following steps are involved: Step 1, obtaining material stress-life curves of the base material 42CrMO and the surface coating WC45 of the descaling roller; Step 2: Establish a life prediction finite element model: Step 2.1, according to the shape and size of the descaling roller and the plate and the relative friction relationship in the original working condition, the 42CrMO rolling contact fatigue damage geometric model and the WC45 rolling contact fatigue damage geometric model are established respectively; Step 2.2, on the basis of the 42CrMO rolling contact fatigue damage geometric model and the WC45 rolling contact fatigue damage geometric model, assign material properties and perform meshing to form a 42CrMO rolling contact fatigue damage constitutive model and a WC45 rolling contact fatigue damage constitutive model, and perform finite element simulation calculation on the 42CrMO rolling contact fatigue damage constitutive model and the WC45 rolling contact fatigue damage constitutive model, select a fatigue life prediction method and convert the stress-life curves of the substrate 42CrMO and the surface coating WC45 in step 1 into data and import them into a finite element analysis system, and obtain the calculated life of the rolling contact fatigue damage of the substrate 42CrMO and the surface coating WC45 through finite element simulation calculation and analysis; Step 3: Model accuracy correction and optimization: The actual life of the descaling roller is obtained by observing the actual working condition of the descaling roller without coating, and the calculated life of the substrate 42CrMO is obtained according to the analysis in step 2.2, and the actual life and calculated life of the substrate 42CrMO are compared and the error is calculated; Step 4: Obtain the service life curve and calculate the predicted service life: According to the calculation error obtained in step 3, combined with the calculated life of coating WC45 obtained in step 2.2, the predicted life of the descaling roller after coating the surface coating WC45 is calculated.

2. The life prediction method of the nickel-based surface coating of the descaling roller according to claim 1, characterized in that: The 42CrMO rolling contact fatigue damage geometric model and the WC45 rolling contact fatigue damage geometric model established in the step 2.1 are respectively symmetrical models with the plane of the diameter where the midpoint of the axis of the descaling roller is located, and the left half or the right half of the 42CrMO rolling contact fatigue damage geometric model and the WC45 rolling contact fatigue damage geometric model are taken to perform the step 2.

2.

3. The life prediction method of the nickel-based surface coating of the descaling roller according to claim 2, characterized in that: In the step 2.1, rigid patches are set on the left and right end surfaces of the descaling roller in the half-obtained 42CrMO rolling contact fatigue damage geometric model and the WC45 rolling contact fatigue damage geometric model.

4. The method for predicting the rolling contact fatigue life of a mechanical component coating according to claim 3, characterized in that: The size of the rigid patch is Ø200×50 mm.

5. The life prediction method of the nickel-based surface coating of the descaling roller according to claim 1, characterized in that: In step 2.1, the diameter of the descaling roller in the 42CrMO rolling contact fatigue damage geometric model and the diameter of the descaling roller in the WC45 rolling contact fatigue damage geometric model are both Ø400 mm, but the outermost 7 mm layer of the descaling roller in the WC45 rolling contact fatigue damage geometric model is the surface coating.