Low-temperature silver-coated copper paste applied to heterojunction solar cell

Through the preparation of low-temperature silver-covered copper paste, combined with the combination of ultrafine silver powder, antioxidant silver-covered copper powder and resin, the problem of reduced conductivity of silver-covered copper powder is solved, cost reduction and performance improvement are achieved, and heterogeneity is ensured. High efficiency conductivity and stability of junction solar cells.

CN118969359APending Publication Date: 2024-11-15JIAXING GUOLV NEW MATERIAL CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411338172.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The decrease in silver content in silver-clad copper powder leads to a decrease in conductivity and weakening of oxidation resistance, increasing the contact resistance of the silver-copper interface, thereby reducing the performance and cost-effectiveness of heterojunction solar cells.

Method used

Using low-temperature silver-covered copper paste, silver with excellent conductivity and oxidation resistance is prepared by combining ultrafine silver powder, antioxidant silver-covered copper powder, resin, curing agent and solvent, combined with specific stirring and rolling processes. Copper-covered powder reduces the use of silver content, while improving the uniformity and stability of silver-covered copper powder.

Benefits of technology

While reducing the silver content, the oxidation resistance of silver-clad copper powder is maintained, the conductivity decreases, production costs are reduced, and the conductivity and stability of silver-clad copper paste are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969359A_ABST
    Figure CN118969359A_ABST
Patent Text Reader

Abstract

The invention discloses a low-temperature silver-coated copper paste applied to a heterojunction solar cell. The low-temperature silver-coated copper paste with low silver content comprises 10-40 parts of superfine silver powder; 50-91 parts of antioxidant silver coated copper powder; 0.5-4 parts of resin; 0-1 part of a curing agent; 3-6 parts of a solvent; and 0-2 parts of an auxiliary agent. By means of the preparation method, the silver powder can be wrapped on the surface of the copper powder more evenly, the oxidation resistance of the silver-coated copper powder is improved, more silver powder is not needed, the production cost is saved, meanwhile, increase of the contact resistance of a silver-copper interface is avoided, and the conductivity of silver-coated copper slurry cannot be reduced due to introduction of the silver-coated copper powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer-based conductive materials, and in particular to a low-temperature silver-coated copper slurry applied to heterojunction solar cells. Background Art

[0002] With the development of the photovoltaic industry, heterojunction solar cells (HJT or SHJ solar cells) have attracted the attention of many leading companies and institutions due to their advantages such as high conversion efficiency, low temperature coefficient and low carbon emissions. They will gradually replace PERC cells and become the main force in the photovoltaic industry.

[0003] Silver-coated copper paste is specially used for heterojunction solar cells. It is used to replace pure silver paste in heterojunction solar cells and reduce the cost of mass production of heterojunction solar cells. Silver-coated copper paste is generally composed of conductive fillers and organic polymers. The conductive filler is generally silver-coated copper powder, which mainly plays the role of conducting electrons and determines the conductive properties of heterojunction silver paste. Organic polymers are mainly composed of a variety of composite resins, solvents, curing agents and other additives. Resins such as epoxy resins and polyurethanes, after curing, serve as the molecular structure skeleton, connecting the left and right, and determining physical properties such as bonding strength. Solvents and additives are mainly used to adjust the viscosity and leveling of the paste and determine the printability of the paste. The curing agent is mainly used to cure the collective bonding phase.

[0004] The raw material components are made into a uniform slurry through high-speed stirring and three-roll grinding. The silver paste for heterojunction is screen-printed on the battery cell, and then dried and solidified to obtain the metal grid line.

[0005] As the price of silver continues to rise, the silver content in silver-coated copper powder continues to decrease, the silver layer coating the outer layer of copper powder becomes thinner and thinner, the unevenness of the silver-coated copper slurry increases significantly, and the oxidation resistance of the silver-coated copper powder decreases. The oxidation resistance of the silver-coated copper powder directly affects the performance of the final electrode material. Copper is less conductive than silver, and the increase in contact resistance at the silver-copper interface means that the introduction of silver-coated copper powder will reduce the conductivity of the silver-coated copper slurry. Summary of the invention

[0006] The object of the present invention is to provide a low-temperature silver-coated copper slurry for heterojunction solar cells, which has the advantages of solving the above problems.

[0007] The above technical objectives of the present invention are achieved through the following technical solutions: A low-temperature silver-coated copper slurry applied to a heterojunction solar cell, the low-temperature silver-coated copper slurry comprising, in proportion, 10-40 parts of ultrafine silver powder; 50-91 parts of antioxidant silver-coated copper powder; 0.5-4 parts of resin; 0-1 parts of curing agent; 3-6 parts of solvent; and 0-2 parts of auxiliary agent.

[0008] Preferably, the ultrafine silver powder includes one of D50: 20-200, D50: 200-350, D50: 350-500, D50: 500-700 or a mixture of several powders, and the specific surface area of ​​the ultrafine silver powder is 0.8-2 m 2 / g, spherical or quasi-spherical with a rough surface.

[0009] Preferably, the average particle size of the silver-coated copper powder is 2.5-5 and the specific surface area is 0.2-0.6 m 2 / g, the silver content in the silver-coated copper powder is 6-15%.

[0010] Preferably, the antioxidant silver-coated copper powder is coated or modified by coating with one or a combination of at least two of the coating agents stearic acid, oleic acid, methyl oleate, ethyl oleate, lauric acid, and silane coupling agent.

[0011] Preferably, the preparation method of the antioxidant silver-coated copper powder comprises: mixing the silver-coated copper powder and acetic acid solution at a constant temperature for 30-60 minutes, the concentration of the acetic acid solution is 0.5-10%, the constant temperature is 20-80°C, and after completion, washing with deionized water and filtering with filter paper for standby use. The filtered silver-coated copper powder and the solution prepared with the coating agent are stirred and dispersed at a constant temperature for 30-610 minutes, the coating agent concentration ratio is 0.2-2% alcohol solution, the constant temperature is 20-40°C, and the antioxidant silver-coated copper powder is obtained by direct filtration or washing with alcohol 1-3 times and filtering and drying, and the drying temperature is 30-50°C.

[0012] Preferably, the resin includes any one of a polyurethane prepolymer with an average molecular weight of 1000-5000, an epoxy resin with an epoxy equivalent of 100-280, an acrylic resin with a functionality of 4-15, and a polyester resin with an average molecular weight of 10000-50000, or a mixture of at least two of them.

[0013] Preferably, the curing agent includes any one of anhydride curing agents, imidazole curing agents, amine curing agents, blocked fluorine-containing borates, blocked fluorine-containing phosphates, blocked fluorine-containing sulfonates, blocked iodonium salts, and blocked isocyanate curing agents, or a combination of at least two thereof.

[0014] Preferably, the solvent includes one or a combination of at least two of diethylene glycol butyl ether, diethylene glycol butyl ether acetate, alcohol ester dodecahydrate, alcohol ester hexadecane, dimethyl adipate, dimethyl glutarate, tributyl citrate, acetyl tributyl citrate, triethylene glycol butyl ether, tripropylene glycol monomethyl ether, tripropylene glycol butyl ether, diethylene glycol monoethyl ether acetate, dibutyl phthalate, dioctyl phthalate, and terpineol.

[0015] Preferably, the auxiliary agent includes a dispersant, a leveling agent, and a defoaming agent; the dispersant includes oleic acid, a carbon chain of C15 -C 25 Fatty acids with carbon chains of C 15 -C 25 The present invention relates to a kind of fatty acid ester, organic silane, organic titanium, sodium polyacrylate, polyacrylamide, styrene-maleic anhydride copolymer, sodium phosphate, sodium silicate, sodium carbonate, sodium metasilicate, sodium citrate, sodium humate or a combination of at least two thereof; the leveling agent comprises any one of polydimethylsiloxane, polyether polyester modified organic siloxane, butyl cellulose, polyacrylic acid or turpentine or a combination of at least two thereof; the defoaming agent comprises any one of linear polyether, polyether with alcohol or ammonia as initiator, terminal esterified polyether derivative, dimethylsiloxane, ether modified siloxane, 3-8 carbon chain modified siloxane or a combination of at least two thereof.

[0016] Preferably, the preparation method of the ultra-low silver content low-temperature silver-coated copper slurry comprises: first weighing 0.5-4 of resin, 3-6 of solvent, and 0-2 of auxiliary agent in proportion, and then dispersing them for 15-30 seconds with a gravity mixer at 500-800 revolutions or stirring them for 10-20 minutes with a planetary mixer at 50-90 revolutions, step 2: adding 10-40 of ultrafine silver powder, and repeating the gravity stirring or planetary dispersion step. Step 3: adding 50-91 of antioxidant silver-coated copper powder, and repeating the gravity stirring or planetary stirring step; step 4: finally adding 0-1 of curing agent, and then dispersing them for 20-30 seconds with a gravity mixer at 500-800 revolutions or stirring them for 20-30 minutes with a planetary mixer at 50-90 revolutions; step 5: rolling the slurry obtained in step 4 with a three-roll mill for 3-6 times until the fineness is less than 10 μm, thus preparing the low-temperature silver-coated copper slurry for heterojunction solar cells.

[0017] In summary, the preparation method can reduce the silver content in the silver-coated copper powder without changing the oxidation resistance of the silver-coated copper powder, thereby reducing the production cost, while avoiding the increase of the contact resistance of the silver-copper interface, so that the introduction of the silver-coated copper powder will not reduce the conductivity of the silver-coated copper slurry. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Attached Figure 1 : 1000 times electron microscope image of 10% silver-coated stearic acid-coated silver-coated copper powder; Attached Figure 2 : 2000 times electron microscope image of 10% silver-containing stearic acid-coated silver-coated copper powder; Attached Figure 3 : This is a 2000x electron microscope image of the front side of the low-temperature conductive silver paste test line resistor in Experiment 4; Attached Figure 4 : This is a 2000x electron microscope image of the conductive electrode cross section when testing the photoelectric conversion efficiency of low-temperature conductive silver paste in Experiment 4. DETAILED DESCRIPTION

[0019] The following is only a preferred embodiment of the present invention, and the protection scope is not limited to this embodiment. All technical solutions under the concept of the present invention should belong to the protection scope of the present invention. At the same time, it should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

[0020] See Figures 1 to 4 Experiment 1: The present invention is a low-temperature silver-coated copper conductive paste for heterojunction solar cells, and its composition is calculated by mass percentage, D50 is 2.58 μm, SSA is 0.45 m 2 / g of uncoated silver-coated copper powder 47.78g, the silver content of the silver-coated copper powder is 10%; D50 is 0.30μm, SSA is 1.92m 2 / g submicron silver powder 45.22g; alicyclic epoxy resin with epoxy equivalent of 100-280 4g; solvent diethylene glycol butyl ether acetate 5.2g; curing agent blocked fluorine-containing phosphate 0.2g; long carbon chain fatty acid dispersant 0.6g; according to the process described in product preparation method 1, the conductive paste is dispersed and rolled for use.

[0021] Experiment 2: The composition of the low-temperature silver-clad copper conductive paste of the present invention is calculated by mass percentage, and D50 is 2.63 μm and SSA is 0.47 μm. 2 / g of uncoated silver-coated copper powder 61.43g, the silver content of the silver-coated copper powder is 30%; D50 is 0.29μm, SSA is 2.05m 2 / g submicron silver powder 31.57g; alicyclic epoxy resin with epoxy equivalent of 100-280 4g; solvent diethylene glycol butyl ether acetate 5.2g; curing agent blocked fluorine-containing phosphate 0.2g; long carbon chain fatty acid dispersant 0.6g; according to the process described in product preparation method 1, the conductive paste is dispersed and rolled for use.

[0022] Experiment 3: The composition of the low-temperature silver-clad copper conductive paste of the present invention is calculated by mass percentage, and D50 is 2.51 μm and SSA is 0.42 m 2 / g of uncoated silver-coated copper powder 86g, the silver content of the silver-coated copper powder is 50%; D50 is 0.31μm, SSA is 1.96m 2 / g submicron silver powder 7g; alicyclic epoxy resin with epoxy equivalent of 100-280 4g; solvent diethylene glycol butyl ether acetate 5.2g; curing agent blocked fluorine-containing phosphate 0.2g; long carbon chain fatty acid dispersant 0.6g; according to the process described in product preparation method 1, the conductive paste is dispersed and rolled for use.

[0023] Experiment 4: The composition of the low-temperature silver-clad copper conductive paste of the present invention is calculated by mass percentage, and D50 is 2.59 μm and SSA is 0.41 m 2 / g of silver-coated copper powder 47.78g, the silver-coated copper powder according to the method of product preparation method 2, using stearic acid coating agent for anti-oxidation treatment, the silver content of the silver-coated copper powder is 10%; D50 is 0.3μm, SSA is 1.9m 2 / g submicron silver powder 45.22g; alicyclic epoxy resin with epoxy equivalent of 100-280 4g; solvent diethylene glycol butyl ether acetate 5.2g; curing agent blocked fluorine-containing phosphate 0.2g; long carbon chain fatty acid dispersant 0.6g; according to the process described in product preparation method 1, the conductive paste is dispersed and rolled for use.

[0024] Experimental method 1: The low-temperature silver-coated copper paste prepared by this patent is used for anti-aging test of line resistance. First, the silver-coated copper paste is printed on the HJT battery cell by screen printing. The printing speed is 350mm / s. The printed pattern is a specific serpentine diagram. The wet weight detection is calculated by the difference method to detect the weight change of a single piece before and after printing. 4 pieces are measured and the average value is taken to control the wet weight at 32-38mg. After printing, the battery cell is cured at 200℃-10min. This experiment uses a box-type drying oven for curing. The cured battery cell is then placed in a constant temperature and humidity aging box for aging treatment. After reaching the set conditions / time, the line resistance value is tested. The data is recorded as follows: Data Characterization 1: Silver content% Coating treatment Wet weight / mg R line - 0h R line - 24h R line - 48h R line - 72h Experiment 1 10% Unwrapped 36 28.1mΩ 32.1mΩ 36.3mΩ 48.8mΩ Experiment 2 30% Unwrapped 35 24.6mΩ 24.8mΩ 25.4mΩ 27.3mΩ Experiment 3 50% Unwrapped 36 23.5mΩ 23.6mΩ 23.9mΩ 24.5mΩ Experiment 4 10% Wrap 34 27.3mΩ 27.6mΩ 28.3mΩ 29.9mΩ Experimental method 2: The low-temperature silver-coated copper paste prepared by this patent is used for anti-aging test of line resistance. First, the silver-coated copper paste is printed on the HJT battery cell by screen printing. The printing speed is 400mm / s, and the printed pattern is a normal 110-line west grid line pattern. The wet weight detection is calculated by detecting the weight change of a single piece before and after printing by the differential method. 15 pieces are measured and the average value is taken to control the wet weight at 15-20mg. After printing, the battery cell is cured at 200℃-7min. This experiment uses a Maxwell infrared sintering furnace for curing. The cured battery cell is then placed in a constant temperature and humidity aging box for aging treatment. After reaching the set conditions / time, its photoelectric conversion efficiency is tested. The photoelectric conversion efficiency is measured by Maxwell's HJT screen printing equipment. 15 pieces are measured and the average value is taken. The data is recorded as follows: Data Standard 2: Silver content% Coating treatment Wet weight / mg Efficiency - 0h Efficiency - 24h Efficiency - 48h Efficiency - 72h Experiment 1 10% Unwrapped 36 23.80% 22.63% 20.71% 18.15% Experiment 2 30% Unwrapped 35 24.57% 24.52% 23.47% 23.02% Experiment 3 50% Unwrapped 36 24.62% 24.59% 24.59% 24.56% Experiment 4 10% Wrap 34 24.03% 24.00% 23.89% 23.71% Data analysis: In the uncoated experimental group, as the silver content decreased from 50% to 10%, the line resistance showed a significant upward trend, especially from 30% to 10%, the line resistance increased significantly, and the increase ratio was much higher than when it decreased from 50% to 30%. At different aging times, as the aging time increased, the line resistance showed a significant increasing trend, and the lower the silver content, the more obvious the increase trend was. When the silver content was 10%, the line resistance increased by 10.7mΩ before and after aging, which was much higher than 1mΩ when the silver content was 50%. In the uncoated experimental group, the photoelectric conversion efficiency also showed a similar law to the line resistance. As the silver content decreased, the photoelectric conversion efficiency decreased from the original 24.62% to 23.80%. When the silver content decreased from 30% to 10%, the efficiency decrease ratio was much higher than when it decreased from 50% to 30%. Comparing before and after different aging times, when the silver content was 10%, the efficiency dropped from 23.80% to 18.15%, a decrease of 5.65%, which was very obvious. When the silver content exceeded 50%, it dropped from 24.62% to 24.56%, a decrease of 0.06%. After coating, the line resistance decreased slightly, and the photoelectric efficiency increased slightly. The difference between line resistance and efficiency before and after aging was significantly reduced, indicating that the coating has a very obvious improvement in the anti-aging ability of silver-coated copper powder.

Claims

1. A low-temperature silver-coated copper slurry for heterojunction solar cells, characterized in that: The low-temperature silver-coated copper slurry comprises, in proportion, 10-40 parts of ultrafine silver powder, 50-91 parts of antioxidant silver-coated copper powder, 0.5-4 parts of resin, 0-1 parts of curing agent, 3-6 parts of solvent, and 0-2 parts of auxiliary agent.

2. The low-temperature silver-coated copper slurry for heterojunction solar cells according to claim 1, characterized in that: The ultrafine silver powder comprises one of D50: 20-200, D50: 200-350, D50: 350-500, D50: 500-700 or a mixture of several powders, and the specific surface area of ​​the ultrafine silver powder is 0.8-2 m 2 / g, spherical or quasi-spherical with a rough surface.

3. The low-temperature silver-coated copper slurry for heterojunction solar cells according to claim 1, characterized in that: The silver-coated copper powder has an average particle size of 2.5-5 and a specific surface area of ​​0.2-0.6 m 2 / g, the silver content in the silver-coated copper powder is 6-15%.

4. The low-temperature silver-coated copper slurry for heterojunction solar cells according to claim 1, characterized in that: The antioxidant silver-coated copper powder is coated or modified by coating or modifying with one or a combination of at least two of the coating agents stearic acid, oleic acid, methyl oleate, ethyl oleate, lauric acid and silane coupling agent.

5. The low-temperature silver-coated copper slurry for heterojunction solar cells according to claim 5, characterized in that: The preparation method of the antioxidant silver-coated copper powder comprises: mixing the silver-coated copper powder and acetic acid solution at a constant temperature for 30-60 minutes, wherein the concentration of the acetic acid solution is 0.5-10%, and the constant temperature is 20-80°C. After completion, the silver-coated copper powder is cleaned with deionized water and filtered with filter paper for standby use. The filtered silver-coated copper powder and the solution prepared with the coating agent are stirred and dispersed at a constant temperature for 30-60 minutes, wherein the coating agent concentration ratio is 0.2-2% alcohol solution, and the constant temperature is 20-40°C. The antioxidant silver-coated copper powder is obtained by direct filtration or filtration and drying after washing with alcohol 1-3 times, and the drying temperature is 30-50°C.

6. The low-temperature silver-coated copper slurry for heterojunction solar cells according to claim 1, characterized in that: The resin includes any one of a polyurethane prepolymer with an average molecular weight of 1000-5000, an epoxy resin with an epoxy equivalent of 100-280, an acrylic resin with a functionality of 4-15, and a polyester resin with an average molecular weight of 10000-50000, or a mixture of at least two of them.

7. The low-temperature silver-coated copper slurry for heterojunction solar cells according to claim 1, characterized in that: The curing agent includes any one of anhydride curing agents, imidazole curing agents, amine curing agents, blocked fluorine-containing borates, blocked fluorine-containing phosphates, blocked fluorine-containing sulfonates, blocked iodonium salts, and blocked isocyanate curing agents, or a combination of at least two of them.

8. The low-temperature silver-coated copper slurry for heterojunction solar cells according to claim 1, characterized in that: The solvent includes one or a combination of at least two of diethylene glycol butyl ether, diethylene glycol butyl ether acetate, alcohol ester dodecahydrate, alcohol ester hexadecane, dimethyl adipate, dimethyl glutarate, tributyl citrate, acetyl tributyl citrate, triethylene glycol butyl ether, tripropylene glycol monomethyl ether, tripropylene glycol butyl ether, diethylene glycol monoethyl ether acetate, dibutyl phthalate, dioctyl phthalate, and terpineol.

9. The low-temperature silver-coated copper slurry for heterojunction solar cells according to claim 1, characterized in that: The auxiliary agent includes a dispersant, a leveling agent, and a defoaming agent; the dispersant includes one or a combination of at least two of oleic acid, fatty acids with a carbon chain of C15-C25, fatty acid esters with a carbon chain of C15-C25, organic silane, organic titanium, sodium polyacrylate, polyacrylamide, styrene-maleic anhydride copolymer, sodium phosphate, sodium silicate, sodium carbonate, sodium metasilicate, sodium citrate, and sodium humate; the leveling agent includes any one or a combination of at least two of polydimethylsiloxane, polyether polyester modified organic siloxane, butyl cellulose, polyacrylic acid, or turpentine; the defoaming agent includes any one or a combination of at least two of linear polyether, polyether with alcohol or ammonia as initiator, terminal esterified polyether derivatives, dimethylsiloxane, ether-modified siloxane, and 3-8 carbon chain modified siloxane.

10. The low-temperature silver-coated copper slurry for heterojunction solar cells according to claim 1, characterized in that: The preparation method of the ultra-low silver content low-temperature silver-coated copper slurry includes: first weighing 0.5-4 of resin, 3-6 of solvent, and 0-2 of auxiliary agent in proportion, and then dispersing them for 15-30 seconds with a gravity mixer at 500-800 revolutions or stirring them for 10-20 minutes with a planetary mixer at 50-90 revolutions, step 2: adding 10-40 of ultrafine silver powder, and repeating the gravity stirring or planetary dispersing steps. Step 3: adding 50-91 of antioxidant silver-coated copper powder, and repeating the gravity stirring or planetary stirring steps; step 4: finally adding 0-1 of curing agent, and then dispersing them for 20-30 seconds with a gravity mixer at 500-800 revolutions or stirring them for 20-30 minutes with a planetary mixer at 50-90 revolutions; step 5: rolling the slurry obtained in step 4 with a three-roll mill for 3-6 times until the fineness is less than 10 μm, thus preparing the low-temperature silver-coated copper slurry applied to heterojunction solar cells.

Citation Information

Cited By

  • Low-temperature conductive paste and application thereof

    CN122158225A

  • A low-temperature silver-coated copper paste for heterojunction cells and a preparation method thereof

    CN122677220A