Manufacturing process for ultrathin power chip

By using a high-temperature and acid-resistant UV protective film and a vacuum adsorption tray in the manufacturing process of ultra-thin power chips, the problems of wafer shaking and breakage during vacuum mounting have been solved, and low-cost ultra-thin chip manufacturing has been achieved.

CN118969596APending Publication Date: 2024-11-15SHAANXI ELECTRONIC CORE IND TIMES TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410851878.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the manufacturing of ultra-thin power chips, existing technologies often result in wafers shaking during vacuum bonding, leading to problems such as excessive gas rings, bubbles, or even wafer cracking. Furthermore, the temporary bonding and debonding processes have high equipment and material costs.

Method used

A power chip ultra-thin manufacturing process is adopted, including front-end process, front-end film bonding, back-end pre-thinning, back-end Taiko thinning, back-end wet etching, back-end metal deposition, front-end UV irradiation, Taiko vacuum bonding, front-end film peeling and Taiko ring cutting. A high temperature and acid resistant UV protective film is used as the support material, and a vacuum adsorption tray is used during Taiko vacuum bonding to avoid wafer shaking.

Benefits of technology

It effectively reduced the breakage rate, lowered equipment and material costs, solved the problem of wafer wobbling during vacuum bonding, and enabled low-cost manufacturing of ultra-thin power chips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969596A_ABST
    Figure CN118969596A_ABST
Patent Text Reader

Abstract

The invention provides a power chip ultra-thin manufacturing process, which comprises the following steps: a front-end front process, a front film pasting process, a back pre-thinning process, a back Taiko thinning process, a back wet etching process, a back metal deposition process, a front UV irradiation process, a Taiko vacuum surface mounting process, a front film tearing process and a Taiko girdling process, and finally an ultra-thin sheet product is produced. The invention provides a power chip ultra-thin manufacturing process, which is inspired by a wafer thinning back gold process which is always provided with a protective carrier so as to effectively reduce the fragment rate and by a process of firstly pasting a chip and then tearing a film of a currently used thinning chip-pasting film-tearing integrated device. And a high-temperature-resistant and acid-resistant UV protective film material is added as a supporting and protecting material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of chips, and in particular to a manufacturing process for ultra-thin power chips. Background Art

[0002] With the continuous development of power chips, the demand for ultra-thin chips is getting higher and higher. The thickness requirement for power chips has reached 50um and thinner. At present, the thinning back gold process of 50um and below wafers is mainly achieved by Taiko thinning process or temporary bonding and debonding process.

[0003] The Taiko process refers to leaving an unthinned area of ​​about 3mm on the edge when thinning the back of the wafer, which can support the ultra-thin wafer for subsequent processing. When producing ultra-thin wafers, the traditional Taiko process is prone to cracks at the connection between the high and low Taiko steps during thinning and subsequent process steps (such as Taiko film tearing, wafer back wet etching, back metal deposition, vacuum bonding, etc.). The crack rate increases with the thinner the wafer thickness. The Taiko process generally removes the front protective film before vacuum bonding. At this time, in order to avoid the vacuum bonding table directly contacting the front circuit of the wafer, the equipment generally uses a Bernoulli table that does not contact the wafer surface. However, because the wafer is too thin, it is easy to shake during vacuum bonding, which leads to quality problems such as excessive air rings, bubbles and even cracks in the bonding.

[0004] In order to address the many problems of traditional Taiko process in manufacturing ultra-thin wafers, a temporary bonding and debonding process has been developed. The temporary bonding and debonding process refers to bonding a material with strong support properties of a carrier (glass wafer, etc.) to the wafer through a bonding glue, and completing subsequent processing such as wafer thinning, wet etching, and metal deposition with the support of the carrier. Finally, the carrier is peeled off by laser and other means to obtain an ultra-thin wafer. This process method can effectively reduce the breakage rate of ultra-thin wafers. At present, temporary bonding and debonding equipment has extremely high requirements on wafer alignment accuracy, the process is relatively complex, and the equipment is expensive. In addition, the bonding materials and cleaning materials have photosensitive or temperature characteristics, so the material prices are also expensive, which makes the overall cost of the temporary bonding and debonding process relatively high.

[0005] Therefore, it is necessary to provide a manufacturing process for ultra-thin power chips to solve the above technical problems. Summary of the invention

[0006] The present invention provides a manufacturing process for ultra-thin power chips, which solves the problem that current equipment generally uses a Bernoulli table that does not contact the surface of the wafer, but the wafer is too thin and is prone to shaking during vacuum chip mounting, resulting in the chip being prone to excessive air rings, bubbles, and even cracks.

[0007] In order to solve the above technical problems, the present invention provides a manufacturing process for ultra-thin power chips, comprising the following steps:

[0008] S1, front-end front process;

[0009] S2, front film laminating process;

[0010] S3, backside pre-thinning process;

[0011] S4, back Taiko thinning process;

[0012] S5, back side wet etching process;

[0013] S6, back metal deposition process;

[0014] S7, front UV irradiation process;

[0015] S8, Taiko vacuum patch process;

[0016] S9, front film tearing process;

[0017] S10, Taiko circumferential cutting process;

[0018] S11, finally producing ultra-thin sheet products.

[0019] Preferably, the front-end process in S1 reduces the thermal stress and mechanical stress of the wafer by controlling the temperature uniformity, temperature gradient and temperature change rate of the heating and cooling process of the front-end process, the uniformity and thickness design of various film layers, etc., so as to achieve the effect of reducing the wafer warpage;

[0020] The front film laminating process in S2 uses the low-tension film laminating mode of the film laminating equipment to reduce the tension of the protective film, optimizes the tension caused by the protective film on the wafer after laminating by controlling the film laminating pressure and speed, and reduces the warping and deformation degree of the wafer after thinning. The film laminating process uses a UV protective film with good acid resistance, high temperature resistance, and low viscosity after ultraviolet light irradiation.

[0021] Preferably, the backside pre-thinning process in S3 reduces the residual stress after wafer thinning by controlling the spindle feed speed, spindle speed and table speed of the plane thinning equipment. The pre-thinning process only needs to completely grind off the device back seal layer and reach the step height difference required by the Taiko step liner of the Taiko ring cutting equipment. The smaller the pre-thinning grinding amount, the smaller the warping degree of the subsequent Taiko wafer.

[0022] The back Taiko thinning process in S4 uses Taiko thinning equipment to leave an area of ​​about 3mm on the edge of the wafer without thinning during thinning. In this process, the bevel Taiko ring manufacturing process is used to effectively solve the problem of cracking in the thick-thin connection area, improve the wafer support force and effectively reduce the warpage. The residual stress after wafer thinning is reduced by controlling the spindle feed speed, spindle speed and table speed of the Taiko thinning equipment. The fine grinding spindle selects a grinding wheel model with a larger mesh number to reduce mechanical stress. The thinnest Taiko thinning is recommended to be 75um, and the remaining thinning thickness is carried out by a wet etching process.

[0023] Preferably, the backside wet etching process in S5 uses Spin D etching solution, Spin E etching solution, DHF and other chemicals of the backside wet etching equipment to wet-thinn the backside of the wafer and roughen the surface, eliminate the residual stress of the wafer, and improve the metal adhesion on the backside. In this process, Spin D etching solution is first used to quickly thinn the wafer to remove the grinding damage layer, and then Spin E etching solution is used to continue thinning to reach the required thickness of the final device and meet the roughness requirements, and then DHF and DIW are used to clean the backside of the wafer, and finally spin-drying or N2 drying is performed. The protective film needs to be able to withstand the mixed acid corrosion of this process;

[0024] The back metal deposition process in S6 realizes the sequential deposition of multiple layers of metals such as Ti, Ni, Ag, etc. on the back side of the wafer by back sputtering or evaporation coating. This process reduces the wafer warping and metal peeling problems by optimizing the thickness configuration of the multi-layer metal. Stress optimization can be performed by step-by-step deposition and N2 injection during Ni deposition. The maximum temperature of the process is generally 200°C to 250°C, so the temperature resistance of the protective film is required to be higher than 250°C. Since the temperature resistance time of the protective film is generally not too long, it is more appropriate to use a back sputtering metal deposition process with a short single-wafer process time.

[0025] Preferably, the front UV irradiation process in S7 irradiates the front protective film of the wafer through a UV irradiation device to reduce the viscosity of the protective film to an extremely low level, and the UV irradiation time or total energy and the table temperature need to be set in accordance with the characteristics of the protective film used;

[0026] The Taiko vacuum mounting process in S8 uses Taiko vacuum mounting equipment to attach the Taiko wafer to the iron ring through the dicing film. General Taiko vacuum mounting equipment uses a Bernoulli platen to avoid the platen from contacting the front of the wafer. At this time, the Taiko wafer is prone to shaking during mounting, resulting in abnormal mounting or even cracking. In the process flow of this patent, the front of the wafer is still provided with a protective film during Taiko vacuum mounting, so the equipment can use a vacuum adsorption platen, and use vacuum to vacuum adsorb the front of the Taiko wafer with a UV protective film, thereby solving the problem of wafer shaking caused by the use of a Bernoulli platen, and the presence of the protective film greatly reduces the breakage rate of this process step.

[0027] Preferably, the front film tearing process in S9 uses a Taiko wafer vacuum adsorption table to adsorb the back of the wafer on the table, and tear the film in a certain direction by applying a very small pulling force. Since the UV irradiation process has been carried out, this process is easy to carry out. The tearing direction refers to the characteristics of the protective film, and the pulling force and speed need to be controlled to avoid residual glue and broken pieces.

[0028] The Taiko ring cutting process in S10 uses the Taiko ring cutting equipment to cut and remove the 4.5mm area on the edge of the wafer, and the ultra-thin area in the middle is left on the dicing film. The device thinning back gold process is completed. This process requires extremely high wafer positioning accuracy of the equipment. Because the wafer is ultra-thin, a slight collision when removing the ring will cause edge collapse or even cracking. The ring cutting of ultra-thin wafers is not suitable for using the Taiko ring lifting function when removing the ring. It is easy to cause ultra-thin area cracks when lifting the Taiko ring. The size of the Taiko step liner needs to adapt to the height difference of the Taiko step.

[0029] Preferably, an irradiation device is required in S7, and the irradiation device includes an equipment body, a plurality of drawers are arranged inside the equipment body, a plurality of placement components are arranged inside the drawers, and the placement component includes a fixed rod, a plurality of rotating sleeves are sequentially sleeved on the surface of the fixed rod from top to bottom, the surface of the rotating sleeve is connected to a placement rack through a connecting block, and the fixed components are symmetrically arranged on the left and right sides of the placement rack.

[0030] Preferably, the fixing assembly includes a movable rod, one end of which is connected to an arc-shaped fixing block, a limiting block is arranged inside the movable rod, a limiting hole matching the limiting block is opened on the surface of the movable rod, and one end of the movable rod is connected to a stopper.

[0031] Preferably, a fixing piece is provided between the fixing rod and the drawer.

[0032] Preferably, a storage component is provided on one side of the surface of the device body, and the storage component includes a connecting frame, a mounting frame is connected to the bottom of the connecting frame, a plurality of storage plates are provided inside the mounting frame, and a connecting piece is provided between the connecting frame and the device body.

[0033] Compared with the related art, the ultra-thin manufacturing process of a power chip provided by the present invention has the following beneficial effects:

[0034] The invention provides a manufacturing process for ultra-thin power chips. The invention is inspired by the fact that a protective carrier is always carried during a wafer thinning back gold process, which can effectively reduce the fragmentation rate, and the process of first patching and then tearing the film in currently used integrated thinning patch and film tearing equipment. A high-temperature and acid-resistant UV protective film material is added as a supporting protective material. The UV protective film is used from before thinning until after patching and then torn off, so as to protect the entire process of ultra-thin power chips to the greatest extent. Compared with the temporary bonding and debonding process currently used for ultra-thin chips, the invention has great advantages in equipment cost and material cost. The front UV protective film of the Taiko wafer is innovatively retained to complete the Taiko vacuum patch process. The Taiko vacuum patch equipment uses a vacuum adsorption table instead of a Bernoulli table, which effectively solves the shaking problem of ultra-thin wafers during patching and reduces patch abnormalities and fragmentation losses. The invention is an innovative, low-cost manufacturing method for ultra-thin power chip wafers with a reduced fragmentation rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A schematic structural diagram of a first embodiment of a manufacturing process for ultra-thin power chips provided by the present invention; Figure 2 for Figure 1 A second schematic diagram of the manufacturing process shown; Figure 3 for Figure 1 A third schematic diagram of the manufacturing process shown; Figure 4 A schematic structural diagram of a second embodiment of a manufacturing process for ultra-thin power chips provided by the present invention; Figure 5 for Figure 4 An enlarged schematic diagram of part A is shown; Figure 6 for Figure 5 An enlarged schematic diagram of part B is shown; Figure 7 for Figure 4 A schematic diagram of the overall three-dimensional structure of the device shown; Figure 8 A schematic structural diagram of a third embodiment of a manufacturing process for ultra-thin power chips provided by the present invention.

[0043] Numbers in the figure: 1. Equipment body, 2. Drawer, 3. Placement assembly, 31. Fixed rod, 32. Rotating sleeve, 33. Placement rack, 4. Fixed assembly, 41. Movable rod, 42. Arc-shaped fixed block, 43. Limit block, 44. Limit hole, 45. Stopper, 5. Fixing part, 6. Storage assembly, 61. Connecting rack, 62. Mounting rack, 63. Storage plate, 64. Connecting part. DETAILED DESCRIPTION

[0044] The present invention will be further described below in conjunction with the accompanying drawings and implementation modes.

[0045] First embodiment

[0046] Please refer to Figure 1 , Figure 2 and Figure 3 ,in, Figure 1 A schematic structural diagram of a first embodiment of a manufacturing process for ultra-thin power chips provided by the present invention; Figure 2 for Figure 1 A second schematic diagram of the manufacturing process shown; Figure 3 for Figure 1 A third schematic diagram of the manufacturing process shown. A manufacturing process for ultra-thin power chips, comprising the following steps:

[0047] S1, front-end front process;

[0048] S2, front film laminating process;

[0049] S3, backside pre-thinning process;

[0050] S4, back Taiko thinning process;

[0051] S5, back side wet etching process;

[0052] S6, back metal deposition process;

[0053] S7, front UV irradiation process;

[0054] S8, Taiko vacuum patch process;

[0055] S9, front film tearing process;

[0056] S10, Taiko circumferential cutting process;

[0057] S11, finally producing ultra-thin sheet products.

[0058] The front-end process in S1 reduces the thermal stress and mechanical stress of the wafer by controlling the temperature uniformity, temperature gradient and temperature change rate of the heating and cooling process of the front-end process, the uniformity and thickness design of various film layers, etc., so as to achieve the effect of reducing the wafer warpage;

[0059] The front film laminating process in S2 uses the low-tension film laminating mode of the film laminating equipment to reduce the tension of the protective film, optimizes the tension caused by the protective film on the wafer after laminating by controlling the film laminating pressure and speed, and reduces the warping and deformation degree of the wafer after thinning. The film laminating process uses a UV protective film with good acid resistance, high temperature resistance, and low viscosity after ultraviolet light irradiation.

[0060] The backside pre-thinning process in S3 reduces the residual stress after wafer thinning by controlling the spindle feed speed, spindle speed and table speed of the plane thinning equipment. The pre-thinning process only needs to completely grind off the device back seal layer and reach the step height difference required by the Taiko step liner of the Taiko ring cutting equipment. The smaller the pre-thinning grinding amount, the smaller the warping degree of the subsequent Taiko wafer;

[0061] The back Taiko thinning process in S4 uses Taiko thinning equipment to leave an area of ​​about 3mm on the edge of the wafer without thinning during thinning. In this process, the bevel Taiko ring manufacturing process is used to effectively solve the problem of cracking in the thick-thin connection area, improve the wafer support force and effectively reduce the warpage. The residual stress after wafer thinning is reduced by controlling the spindle feed speed, spindle speed and table speed of the Taiko thinning equipment. The fine grinding spindle selects a grinding wheel model with a larger mesh number to reduce mechanical stress. The thinnest Taiko thinning is recommended to be 75um, and the remaining thinning thickness is carried out by a wet etching process.

[0062] The backside wet etching process in S5 uses Spin D etching solution, Spin E etching solution, DHF and other chemicals of the backside wet etching equipment to wet-thinn the backside of the wafer and roughen the surface, eliminate the residual stress of the wafer, and improve the metal adhesion on the backside. In this process, Spin D etching solution is first used to quickly thinn the wafer to remove the grinding damage layer, and then Spin E etching solution is used to continue thinning to reach the required thickness of the final device and meet the roughness requirements, and then DHF and DIW are used to clean the backside of the wafer, and finally spin-dry or N2 blow-dry, and the protective film needs to be able to withstand the mixed acid corrosion of this process;

[0063] The back metal deposition process in S6 realizes the sequential deposition of multiple layers of metals such as Ti, Ni, Ag, etc. on the back side of the wafer by back sputtering or evaporation coating. This process reduces the wafer warping and metal peeling problems by optimizing the thickness configuration of the multi-layer metal. Stress optimization can be performed by step-by-step deposition and N2 injection during Ni deposition. The maximum temperature of the process is generally 200°C to 250°C, so the temperature resistance of the protective film is required to be higher than 250°C. Since the temperature resistance time of the protective film is generally not too long, it is more appropriate to use a back sputtering metal deposition process with a short single-wafer process time.

[0064] The front UV irradiation process in S7 irradiates the front protective film of the wafer through a UV irradiation device to reduce the viscosity of the protective film to an extremely low level. The UV irradiation time or total energy and the table temperature need to be set in accordance with the characteristics of the protective film used.

[0065] The Taiko vacuum mounting process in S8 uses Taiko vacuum mounting equipment to attach the Taiko wafer to the iron ring through the dicing film. General Taiko vacuum mounting equipment uses a Bernoulli platen to avoid the platen from contacting the front of the wafer. At this time, the Taiko wafer is prone to shaking during mounting, resulting in abnormal mounting or even cracking. In the process flow of this patent, the front of the wafer is still provided with a protective film during Taiko vacuum mounting, so the equipment can use a vacuum adsorption platen, and use vacuum to vacuum adsorb the front of the Taiko wafer with a UV protective film, thereby solving the problem of wafer shaking caused by the use of a Bernoulli platen, and the presence of the protective film greatly reduces the breakage rate of this process step.

[0066] The front film tearing process in S9 uses a Taiko wafer vacuum adsorption table to adsorb the back of the wafer on the table, and tear the film in a certain direction by applying a very small pulling force. Since the UV irradiation process has been carried out, this process is easy to carry out. The tearing direction refers to the characteristics of the protective film. The pulling force and speed need to be controlled to avoid residual glue and broken pieces.

[0067] The Taiko ring cutting process in S10 uses the Taiko ring cutting equipment to cut and remove the 4.5mm area on the edge of the wafer, and the ultra-thin area in the middle is left on the dicing film. The device thinning back gold process is completed. This process requires extremely high wafer positioning accuracy of the equipment. Because the wafer is ultra-thin, a slight collision when removing the ring will cause edge collapse or even cracking. The ring cutting of ultra-thin wafers is not suitable for using the Taiko ring lifting function when removing the ring. It is easy to cause ultra-thin area cracks when lifting the Taiko ring. The size of the Taiko step liner needs to adapt to the height difference of the Taiko step.

[0068] Embodiment 1

[0069] 1. Low-tension lamination is performed on the wafers that have completed front-side circuit manufacturing, using a high-temperature and acid-resistant UV protective film;

[0070] 2. Use a full-surface thinning machine to pre-thin the back of the wafer, removing 50um. Taking an 8-inch wafer as an example, the initial thickness is reduced from 725um to 675um;

[0071] 3. Use Taiko thinning machine to perform Taiko thinning on the back of the wafer. The final thickness of the thinning is 75um. The thinning process uses the bevel Taiko ring manufacturing process. The top width of the Taiko ring is 3mm.

[0072] 4. Use Spin D etching solution, Spin E etching solution, 100:1DHF and other chemicals to perform wet chemical etching on the back of the wafer. Among them, Spin D etching solution is used for smooth surface treatment and removes 20um thickness, Spin E etching solution is used for rough surface treatment and removes 5um thickness, 100:1DHF removes the surface oxide layer, and then rinses with deionized water, and uses N2 to blow dry the back of the wafer to obtain a wafer with a middle thin film area thickness of 50um and an edge Taiko ring height of about 625um;

[0073] 5. Use the back metal sputtering process to sputter three layers of metal, Ti, NiV, and Ag, on the back of the wafer in sequence, with the metal thicknesses of 1000A, 2000A, and 10000A respectively;

[0074] 6. Place the wafer on the vacuum stage of the UV irradiator and irradiate the UV protective film on the front of the wafer;

[0075] 7. Perform vacuum bonding on the wafer, use a vacuum table to completely adsorb the front side of the wafer on the table, so that the wafer has no warping or deformation, and then use the pressure difference of the vacuum chamber to make the cutting film adhere to the back side of the wafer evenly, and obtain a Taiko wafer with an iron ring;

[0076] 8. Place the wafer on the vacuum stage, start vacuum adsorption on the iron ring and Taiko ring area, and remove the UV protective film on the front side;

[0077] 9. Perform Taiko ring cutting and ring removal on the wafer. Use a ring cutting blade to ring cut the 4.5mm position of the wafer edge and perform subsequent ring removal. At this time, the equipment is equipped with a Taiko step liner with a thickness of 575um. The Taiko ring lifting function is not used in the ring removal process;

[0078] 10. Obtain ultra-thin wafers with a thickness of 50um.

[0079] Embodiment 2

[0080] 1. Low-tension lamination is performed on the wafers that have completed front-side circuit manufacturing, using a high-temperature and acid-resistant UV protective film;

[0081] 2. Use a full-surface thinning machine to pre-thin the back of the wafer, removing 50um. Taking an 8-inch wafer as an example, the initial thickness is reduced from 725um to 675um;

[0082] 3. Use Taiko thinning machine to perform Taiko thinning on the back of the wafer. The final thickness of the thinning is 75um. The thinning process uses the right-angle double-step Taiko ring manufacturing process. The top width of the Taiko ring is 3mm.

[0083] 4. Use Spin D etching solution, Spin E etching solution, 100:1DHF and other chemicals to perform wet chemical etching on the back of the wafer. Among them, Spin D etching solution is used for smooth surface treatment, removing a thickness of 20um; Spin E etching solution is used for rough surface treatment, removing a thickness of 5um, 100:1DHF removes the surface oxide layer, and then rinses with deionized water, and uses N2 to blow dry the back of the wafer to obtain a wafer with a middle thin film area thickness of 50um and an edge Taiko ring height of about 625um;

[0084] 5. Use the back metal sputtering process to sputter three layers of metal, Ti, NiV, and Ag, on the back of the wafer in sequence, with the metal thicknesses of 1000A, 2000A, and 10000A respectively;

[0085] 6. Place the wafer on the vacuum stage of the UV irradiator and irradiate the UV protective film on the front of the wafer;

[0086] 7. Perform vacuum bonding on the wafer, use a vacuum table to completely adsorb the front side of the wafer on the table, so that the wafer has no warping or deformation, and then use the pressure difference of the vacuum chamber to make the cutting film adhere to the back side of the wafer evenly, and obtain a Taiko wafer with an iron ring;

[0087] 8. Place the wafer on the vacuum stage, start vacuum adsorption on the iron ring and Taiko ring area, and remove the UV protective film on the front side;

[0088] 9. Perform Taiko ring cutting and ring removal on the wafer. Use a ring cutting blade to ring cut the 4.5mm position of the wafer edge and perform subsequent ring removal. At this time, the equipment is equipped with a Taiko step liner with a thickness of 575um. The Taiko ring lifting function is not used in the ring removal process;

[0089] 10. Obtain ultra-thin wafers with a thickness of 50um.

[0090] Embodiment 3

[0091] 1. Low-tension lamination is performed on the wafers that have completed front-side circuit manufacturing, using a high-temperature and acid-resistant UV protective film;

[0092] 2. Use a full-surface thinning machine to pre-thin the back of the wafer, removing 50um. Taking an 8-inch wafer as an example, the initial thickness is reduced from 725um to 675um;

[0093] 3. Use Taiko thinning machine to perform Taiko thinning on the back of the wafer. The final thickness of the thinning is 75um. The thinning process uses the bevel Taiko ring manufacturing process. The top width of the Taiko ring is 3mm.

[0094] 4. Use Spin D etching solution, Spin E etching solution, 100:1DHF and other chemicals to perform wet chemical etching on the back of the wafer. Among them, Spin D etching solution is used for smooth surface treatment and removes 20um thickness, Spin E etching solution is used for rough surface treatment and removes 5um thickness, 100:1DHF removes the surface oxide layer, and then rinses with deionized water, and uses N2 to blow dry the back of the wafer to obtain a wafer with a middle thin film area thickness of 50um and an edge Taiko ring height of about 625um;

[0095] 5. Use the back metal sputtering process to sputter three layers of metal, Ti, NiV, and Ag, on the back of the wafer in sequence, with the metal thicknesses of 1000A, 2000A, and 10000A respectively;

[0096] 6. Perform vacuum bonding on the wafer, use a vacuum table to completely adsorb the front side of the wafer on the table, so that the wafer has no warping or deformation, and then use the pressure difference of the vacuum chamber to make the cutting film adhere to the back side of the wafer evenly, and obtain a Taiko wafer with an iron ring;

[0097] 7. Place the wafer on the vacuum stage of the UV irradiator, start vacuum adsorption on the iron ring and Taiko ring area, use a light shielding plate to shield the area outside the wafer, and only irradiate the UV protective film area on the front of the wafer. Then remove the light shielding plate and tear off the UV protective film on the front.

[0098] 8. Perform Taiko ring cutting and ring removal on the wafer. Use a ring cutting blade to cut the 4.5mm position of the wafer edge and then remove the ring. At this time, the equipment is equipped with a Taiko step liner with a thickness of 575um. The Taiko ring lifting function is not used in the ring removal process.

[0099] 9. Obtain ultra-thin wafers with a thickness of 50um.

[0100] Embodiment 4

[0101] 1. Low-tension lamination is performed on the wafers that have completed front-side circuit manufacturing, using a high-temperature and acid-resistant UV protective film;

[0102] 2. Use a full-surface thinning machine to pre-thin the back of the wafer, removing 50um. Taking an 8-inch wafer as an example, the initial thickness is reduced from 725um to 675um;

[0103] 3. Use Taiko thinning machine to perform Taiko thinning on the back of the wafer. The final thickness of the thinning is 75um. The thinning process uses the right-angle double-step Taiko ring manufacturing process. The top width of the Taiko ring is 3mm.

[0104] 4. Use Spin D etching solution, Spin E etching solution, 100:1DHF and other chemicals to perform wet chemical etching on the back of the wafer. Among them, Spin D etching solution is used for smooth surface treatment and removes 20um thickness, Spin E etching solution is used for rough surface treatment and removes 5um thickness, 100:1DHF removes the surface oxide layer, and then rinses with deionized water, and uses N2 to blow dry the back of the wafer to obtain a wafer with a middle thin film area thickness of 50um and an edge Taiko ring height of about 625um;

[0105] 5. Use the back metal sputtering process to sputter three layers of metal, Ti, NiV, and Ag, on the back of the wafer in sequence, with the metal thicknesses of 1000A, 2000A, and 10000A respectively;

[0106] 6. Perform vacuum bonding on the wafer, use a vacuum table to completely adsorb the front side of the wafer on the table, so that the wafer has no warping or deformation, and then use the pressure difference of the vacuum chamber to make the cutting film adhere to the back side of the wafer evenly, and obtain a Taiko wafer with an iron ring;

[0107] 7. Place the wafer on the vacuum stage of the UV irradiator, start vacuum adsorption on the iron ring and Taiko ring area, use a light shielding plate to shield the area outside the wafer, and only irradiate the UV protective film area on the front of the wafer. Then remove the light shielding plate and tear off the UV protective film on the front.

[0108] 8. Perform Taiko ring cutting and ring removal on the wafer. Use a ring cutting blade to cut the 4.5mm position of the wafer edge and then remove the ring. At this time, the equipment is equipped with a Taiko step liner with a thickness of 575um. The Taiko ring lifting function is not used in the ring removal process.

[0109] 9. Obtain ultra-thin wafers with a thickness of 50um.

[0110] Compared with the related art, the ultra-thin manufacturing process of a power chip provided by the present invention has the following beneficial effects:

[0111] The invention provides a manufacturing process for ultra-thin power chips. The invention is inspired by the fact that a protective carrier is always carried during a wafer thinning back gold process, which can effectively reduce the fragmentation rate, and the process of first patching and then tearing the film in currently used integrated thinning patch and film tearing equipment. A high-temperature and acid-resistant UV protective film material is added as a supporting protective material. The UV protective film is used from before thinning until after patching and then torn off, so as to protect the entire process of ultra-thin power chips to the greatest extent. Compared with the temporary bonding and debonding process currently used for ultra-thin chips, the invention has great advantages in equipment cost and material cost. The front UV protective film of the Taiko wafer is innovatively retained to complete the Taiko vacuum patch process. The Taiko vacuum patch equipment uses a vacuum adsorption table instead of a Bernoulli table, which effectively solves the shaking problem of ultra-thin wafers during patching and reduces patch abnormalities and fragmentation losses. The invention is an innovative, low-cost manufacturing method for ultra-thin power chip wafers with a reduced fragmentation rate.

[0112] Second embodiment

[0113] Please refer to Figure 4 , Figure 5 , Figure 6 and Figure 7 Based on the ultra-thin manufacturing process of a power chip provided by the first embodiment of the present application, the second embodiment of the present application proposes another ultra-thin manufacturing process of a power chip. The second embodiment is only a preferred method of the first embodiment, and the implementation of the second embodiment will not affect the independent implementation of the first embodiment.

[0114] Specifically, the second embodiment of the present application provides an ultra-thin manufacturing process for power chips, which is different in that, in an ultra-thin manufacturing process for power chips, an irradiation device is required in S7, and the irradiation device includes an equipment body 1, and a plurality of drawers 2 are arranged inside the equipment body 1, and a plurality of placement components 3 are arranged inside the drawer 2, and the placement component 3 includes a fixed rod 31, and a plurality of rotating sleeves 32 are sequentially sleeved on the surface of the fixed rod 31 from top to bottom, and the surface of the rotating sleeve 32 is connected to a placement rack 33 through a connecting block, and the left and right sides of the placement rack 33 are symmetrically provided with fixed components 4.

[0115] The fixing part 5 is composed of a threaded block and a threaded sleeve. A circular block is connected to the bottom end of the fixing rod 31. A mounting through hole compatible with the threaded block is opened on the surface of the circular block. The rotating sleeve 32 is connected to the fixing rod 31 through a bearing to facilitate the rotation of the placement frame 33. A movable through hole compatible with the movable rod 41 is opened on the placement frame 33. The shape of the limit block 43 is U-shaped, and the limit hole 44 can be opened on the surface of the movable rod 41 and at the left and right sides of the placement frame 33.

[0116] The fixing assembly 4 includes a movable rod 41, one end of which is connected to an arc-shaped fixing block 42, a limiting block 43 is arranged inside the movable rod 41, a limiting hole 44 adapted to the limiting block 43 is opened on the surface of the movable rod 41, and one end of the movable rod 41 is connected to a stopper 45.

[0117] A fixing member 5 is provided between the fixing rod 31 and the drawer 2 .

[0118] The working principle of the manufacturing process for ultra-thin power chips provided by the present invention is as follows:

[0119] When in use, first rotate the placement rack 33 to the outside by rotating the sleeve 32, and then place the wafer inside the placement rack 33. After the wafer is placed, push the movable plate 41 to drive the arc-shaped fixing block 42 to move to squeeze and fix the wafer. After the wafer is fixed, use the limit block 43 to connect with the limit hole 44 on the surface of the movable rod 41, and then the entire device can be installed inside the drawer 2 through the fixing part 5 and pushed to the inside of the equipment body 1 for processing.

[0120] Compared with the related art, the ultra-thin manufacturing process of a power chip provided by the present invention has the following beneficial effects:

[0121] The present invention provides a manufacturing process for ultra-thin power chips. A plurality of fixing rods 31 with rotating sleeves 32, a plurality of placement racks 33 and fixing components 4 are arranged inside a drawer 2 for use, which can increase the number of wafers placed in a device body 1 when the wafers are subjected to UV irradiation.

[0122] Third embodiment

[0123] Please refer to Figure 8 Based on the ultra-thin manufacturing process of a power chip provided in the first embodiment of the present application, the third embodiment of the present application proposes another ultra-thin manufacturing process of a power chip. The third embodiment is only a preferred method of the first embodiment, and the implementation of the third embodiment will not affect the independent implementation of the first embodiment.

[0124] Specifically, the difference of the ultra-thin manufacturing process of power chips provided in the third embodiment of the present application is that, in an ultra-thin manufacturing process of power chips, a storage component 6 is provided on one side of the surface of the device main body 1, and the storage component 6 includes a connecting frame 61, and the bottom of the connecting frame 61 is connected to a mounting frame 62, and a plurality of storage plates 63 are provided inside the mounting frame 62, and a connecting member 64 is provided between the connecting frame 61 and the device main body 1.

[0125] Compared with the related art, the ultra-thin manufacturing process of a power chip provided by the present invention has the following beneficial effects:

[0126] The present invention provides a manufacturing process for ultra-thin power chips, in which a storage component 6 is arranged on one side of the surface of a device body 1 to temporarily store wafers.

[0127] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A manufacturing process for ultra-thin power chips, characterized in that: The following steps are involved: S1, front-end front process; S2, front film laminating process; S3, backside pre-thinning process; S4, back Taiko thinning process; S5, back side wet etching process; S6, back metal deposition process; S7, front UV irradiation process; S8, Taiko vacuum patch process; S9, front film tearing process; S10, Taiko circumferential cutting process; S11, finally producing ultra-thin sheet products.

2. The manufacturing process for ultra-thin power chip according to claim 1, characterized in that: The front-end process in S1 reduces the thermal stress and mechanical stress of the wafer by controlling the temperature uniformity, temperature gradient and temperature change rate of the heating and cooling process of the front-end process, the uniformity and thickness design of various film layers, etc., so as to achieve the effect of reducing the wafer warpage; The front film laminating process in S2 uses the low-tension film laminating mode of the film laminating equipment to reduce the tension of the protective film, optimizes the tension caused by the protective film on the wafer after laminating by controlling the film laminating pressure and speed, and reduces the warping and deformation degree of the wafer after thinning. The film laminating process uses a UV protective film with good acid resistance, high temperature resistance, and low viscosity after ultraviolet light irradiation.

3. The manufacturing process for ultra-thin power chip according to claim 1, characterized in that: The backside pre-thinning process in S3 reduces the residual stress after wafer thinning by controlling the spindle feed speed, spindle speed and table speed of the plane thinning equipment. The pre-thinning process only needs to completely grind off the device back seal layer and reach the step height difference required by the Taiko step liner of the Taiko ring cutting equipment. The smaller the pre-thinning grinding amount, the smaller the warping degree of the subsequent Taiko wafer; The back Taiko thinning process in S4 uses Taiko thinning equipment to leave an area of ​​about 3mm on the edge of the wafer without thinning during thinning. In this process, the bevel Taiko ring manufacturing process is used to effectively solve the problem of cracking in the thick-thin connection area, improve the wafer support force and effectively reduce the warpage. The residual stress after wafer thinning is reduced by controlling the spindle feed speed, spindle speed and table speed of the Taiko thinning equipment. The fine grinding spindle selects a grinding wheel model with a larger mesh number to reduce mechanical stress. The thinnest Taiko thinning is recommended to be 75um, and the remaining thinning thickness is carried out by a wet etching process.

4. The manufacturing process for ultra-thin power chip according to claim 1, characterized in that: The backside wet etching process in S5 uses Spin D etching solution, Spin E etching solution, DHF and other chemicals of the backside wet etching equipment to wet-thinn the backside of the wafer and roughen the surface, eliminate the residual stress of the wafer, and improve the metal adhesion on the backside. In this process, Spin D etching solution is first used to quickly thinn the wafer to remove the grinding damage layer, and then Spin E etching solution is used to continue thinning to reach the required thickness of the final device and meet the roughness requirements, and then DHF and DIW are used to clean the backside of the wafer, and finally spin-dry or N2 blow-dry, and the protective film needs to be able to withstand the mixed acid corrosion of this process; The back metal deposition process in S6 realizes the sequential deposition of multiple layers of metals such as Ti, Ni, Ag, etc. on the back side of the wafer by back sputtering or evaporation coating. This process reduces the wafer warping and metal peeling problems by optimizing the thickness configuration of the multi-layer metal. Stress optimization can be performed by step-by-step deposition and N2 injection during Ni deposition. The maximum temperature of the process is generally 200°C to 250°C, so the temperature resistance of the protective film is required to be higher than 250°C. Since the temperature resistance time of the protective film is generally not too long, it is more appropriate to use a back sputtering metal deposition process with a short single-wafer process time.

5. The manufacturing process for ultra-thin power chip according to claim 1, characterized in that: The front UV irradiation process in S7 irradiates the front protective film of the wafer through a UV irradiation device to reduce the viscosity of the protective film to an extremely low level. The UV irradiation time or total energy and the table temperature need to be set in accordance with the characteristics of the protective film used. The Taiko vacuum mounting process in S8 uses Taiko vacuum mounting equipment to attach the Taiko wafer to the iron ring through the dicing film. General Taiko vacuum mounting equipment uses a Bernoulli platen to avoid the platen from contacting the front of the wafer. At this time, the Taiko wafer is prone to shaking during mounting, resulting in abnormal mounting or even cracking. In the process flow of this patent, the front of the wafer is still provided with a protective film during Taiko vacuum mounting, so the equipment can use a vacuum adsorption platen, and use vacuum to vacuum adsorb the front of the Taiko wafer with a UV protective film, thereby solving the problem of wafer shaking caused by the use of a Bernoulli platen, and the presence of the protective film greatly reduces the breakage rate of this process step.

6. The manufacturing process for ultra-thin power chip according to claim 1, characterized in that: The front film tearing process in S9 uses a Taiko wafer vacuum adsorption table to adsorb the back of the wafer on the table, and tear the film in a certain direction by applying a very small pulling force. Since the UV irradiation process has been carried out, this process is easy to carry out. The tearing direction refers to the characteristics of the protective film. The pulling force and speed need to be controlled to avoid residual glue and broken pieces. The Taiko ring cutting process in S10 uses the Taiko ring cutting equipment to cut and remove the 4.5mm area on the edge of the wafer, and the ultra-thin area in the middle is left on the dicing film. The device thinning back gold process is completed. This process requires extremely high wafer positioning accuracy of the equipment. Because the wafer is ultra-thin, a slight collision when removing the ring will cause edge collapse or even cracking. The ring cutting of ultra-thin wafers is not suitable for using the Taiko ring lifting function when removing the ring. It is easy to cause ultra-thin area cracks when lifting the Taiko ring. The size of the Taiko step liner needs to adapt to the height difference of the Taiko step.

7. The manufacturing process for ultra-thin power chip according to claim 1, characterized in that: An irradiation device is required in S7, and the irradiation device includes an equipment body, a plurality of drawers are arranged inside the equipment body, a plurality of placement components are arranged inside the drawers, and the placement component includes a fixed rod, a plurality of rotating sleeves are sequentially sleeved on the surface of the fixed rod from top to bottom, and the surface of the rotating sleeve is connected to a placement rack through a connecting block, and the fixed components are symmetrically arranged on the left and right sides of the placement rack.

8. The manufacturing process for ultra-thin power chip according to claim 7, characterized in that: The fixing assembly comprises a movable rod, one end of which is connected to an arc-shaped fixing block, a limiting block is arranged inside the movable rod, a limiting hole matched with the limiting block is opened on the surface of the movable rod, and one end of the movable rod is connected to a stopper.

9. The manufacturing process for ultra-thin power chip according to claim 7, characterized in that: A fixing piece is arranged between the fixing rod and the drawer.

10. The manufacturing process for ultra-thin power chip according to claim 7, characterized in that: A storage component is arranged on one side of the surface of the device body, and the storage component comprises a connecting frame, a mounting frame is connected to the bottom of the connecting frame, a plurality of storage plates are arranged inside the mounting frame, and a connecting piece is arranged between the connecting frame and the device body.

Citation Information

Cited By

  • Wafer thinning method