Unsealing method of plastic package GaAs device

Through the combination method of corrosion liquid 1 and corrosion liquid 2, the GaAs device chip is gradually exposed, which solves the problem of chip damage during the opening process in the prior art, and achieves the effect of protecting the chip, ensuring the safety and observation convenience of the opening process.

CN118969673APending Publication Date: 2024-11-15CHONGQING SAIBAO IND TECH RES INST CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411042997.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing plastic-sealed GaAs device unpacking method can easily lead to damage to the chip passivation layer and metallization layer, affecting observation and device functions.

Method used

The combination method of corrosion liquid 1 and corrosion liquid 2 is used to corrode the device by water bath heating and acid dropping method, gradually expose the chip, and clean and dry it with cleaning liquid and deionized water to protect the chip body and avoid damage.

Benefits of technology

It effectively protects the chip body, avoids damage during the opening process, and achieves safe chip exposure and observation, making it easier to use later.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969673A_ABST
    Figure CN118969673A_ABST
Patent Text Reader

Abstract

The invention discloses an unsealing method for a plastic package GaAs device. The unsealing method comprises the following steps: S1, thinning a plastic package material on the surface of a device chip; s2, heating the corrosive liquid 1 in a water bath to 75-90 DEG C, and corroding the device by using the corrosive liquid 1 until a chip of the device is exposed; s3, cleaning with a cleaning solution, then cleaning with deionized water, and drying; s4, corroding the device by using the corrosive liquid 2, wherein the corrosion time is 5-15 seconds; and S5, cleaning with a cleaning solution, and then cleaning with deionized water. By adopting the unsealing method of the plastic-packaged GaAs device designed by the scheme, a passivation layer and a metallization layer of a chip of the device cannot be damaged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of integrated circuits, and in particular relates to a method for unsealing a plastic-sealed GaAs device. Background Art

[0002] Integrated circuit packaging can be roughly divided into glass-metal sealing, ceramic-metal packaging, low-melting glass-ceramic sealing and plastic packaging. Currently, plastic packaging is still the main packaging form of integrated circuits due to the constraints of cost, process and convenience of automated production.

[0003] GaAs devices are one type of integrated circuits. Existing plastic-encapsulated GaAs devices have the characteristics of large bandgap and high electron mobility. They are widely used in the fields of radio frequency, wireless communication and optoelectronics. However, due to the material properties of GaAs chips, it is difficult to unseal plastic-encapsulated GaAs devices, which can easily damage the passivation layer and metallization layer of the device chip. Therefore, it is necessary to propose a new method for unsealing plastic-encapsulated GaAs devices. Summary of the invention

[0004] In view of the problem that the unsealing failure in the above-mentioned existing unsealing technology causes chip damage and affects observation, the present invention provides a method for unsealing a plastic-sealed GaAs device, which neither affects observation nor damages its passivation layer and metallization layer after the device is unsealed.

[0005] The present invention provides a method for unsealing a plastic-sealed GaAs device, comprising the following steps: S1, thinning the plastic sealing material on the surface of the device chip; S2, heating the etching solution 1 in a water bath to 75° C.-90° C., and then etching the device with the etching solution 1 until the device chip is exposed; S3, cleaning with a cleaning solution, and then cleaning with deionized water, and drying;

[0006] S4, the device is corroded by the etching solution 2, and the etching time is 5s to 15s; S5, the device is cleaned by the cleaning solution, and then cleaned by the deionized water; wherein the composition of the etching solution 1, by volume ratio, includes sulfuric acid: fuming nitric acid: glacial acetic acid: deionized water = 4 (3.5-5): 1.5 (1.3-1.8): 2 (1.8-2.3): 1 (0.8-1.4); the composition of the etching solution 2, by volume ratio, includes sulfuric acid: deionized water = 9 (8.5-10): 1 (0.5-2).

[0007] Furthermore, the composition of the cleaning solution in step S3 includes carbon tetrachloride:acetone=3(2.5-4):1(0.8-1.5) in volume ratio.

[0008] Furthermore, the composition of the etching solution 1 includes sulfuric acid: fuming nitric acid: glacial acetic acid: deionized water = 4:1.5:2:1 in volume ratio.

[0009] Furthermore, the composition of the etching solution 2 includes sulfuric acid: deionized water=9:1 in volume ratio.

[0010] Furthermore, in step S2, the etching solution 1 is heated to 80°C in a water bath.

[0011] Furthermore, in step S4, the etching time of the device using the etching solution 2 is 10 seconds.

[0012] Furthermore, in step S3, ultrasonic cleaning is performed using a cleaning solution for 10 seconds.

[0013] Further, in step S5, ultrasonic cleaning is performed using a cleaning solution for 10 seconds.

[0014] Furthermore, in step S1, the plastic packaging material on the surface of the chip is thinned using an optical decapsulation machine, and the process stops when the bonding wires are exposed.

[0015] Furthermore, in step S2, the device is corroded by the etching solution 1 using a dripping acid method until the device chip is exposed.

[0016] The invention has the advantages that the device chip can be exposed by corroding the plastic sealing material on the device surface through the corrosive liquid 1, thus effectively realizing the protection of the chip body by the corrosive liquid during the unsealing process.

[0017] Under the action of the etching liquid 1, the chip body and bonding can be protected while removing the plastic sealing material on the chip surface; that is, it effectively avoids the chip body being damaged and unable to work normally due to unsealing. The PI glue on the chip surface is corroded by the protective liquid 2, exposing the chip for easy observation. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 Schematic diagram before and after using the etching solution 1 in Example 2 of the method of the present invention.

[0020] Figure 2 Schematic diagram of the method of the present invention before and after the use of the etching solution 2 in Example 2.

[0021] Figure 3 It is a schematic diagram of the opening effect of the prior art.

[0022] Figure 4 It is a schematic diagram of the unsealing effect of Example 2 of the method of the present invention. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1

[0025] A method for unsealing a plastic-sealed GaAs device comprises the following steps:

[0026] S1. Use a laser decapsulator to thin the plastic packaging material on the chip surface and stop when the bonding wire is exposed.

[0027] S2, heating the etching solution 1 to 75° C. in a water bath, and then using the acid dripping method to etch the device with the etching solution 1 until the device chip is exposed; wherein the etching solution 1 is composed of sulfuric acid: fuming nitric acid: glacial acetic acid: deionized water = 3.5:1.3:1.8:0.8 in volume ratio;

[0028] S3. Ultrasonic cleaning with a cleaning solution for 10 seconds, then cleaning with deionized water, and drying; wherein the cleaning solution comprises, by volume ratio, carbon tetrachloride: acetone = 2.5:0.8.

[0029] S4, the device is corroded by the etching solution 2 for 5 seconds; wherein the etching solution 2 is composed of sulfuric acid: deionized water=8.5:0.5 in volume ratio.

[0030] S5. Ultrasonic cleaning with a cleaning solution for 10 seconds, and then cleaning with deionized water; wherein the composition of the cleaning solution, in terms of volume ratio, includes carbon tetrachloride:acetone=2.5:0.8.

[0031] Example 2

[0032] A method for unsealing a plastic-sealed GaAs device comprises the following steps:

[0033] S1. Use a laser decapsulator to thin the plastic packaging material on the chip surface and stop when the bonding wire is exposed.

[0034] S2, heating the etching solution 1 to 80° C. in a water bath, and then using the acid dripping method to etch the device with the etching solution 1 until the device chip is exposed; wherein the etching solution 1 is composed of sulfuric acid: fuming nitric acid: glacial acetic acid: deionized water = 4:1.5:2:1 in volume ratio;

[0035] S3. Ultrasonic cleaning with a cleaning solution for 10 seconds, then cleaning with deionized water, and drying; wherein the cleaning solution comprises, by volume ratio, carbon tetrachloride: acetone = 3:1.

[0036] S4, the device is corroded by the etching solution 2, and the etching time is 10 seconds; wherein the composition of the etching solution 2 is mixed by volume ratio, including sulfuric acid: deionized water = 9:1.

[0037] S5. Ultrasonic cleaning with a cleaning solution for 10 seconds, and then cleaning with deionized water; wherein the cleaning solution has a composition, by volume ratio, of carbon tetrachloride:acetone = 3:1.

[0038] like Figure 1 , Figure 2 and Figure 4 As shown, the chip unsealing effect of the plastic-sealed GaAs device unsealing method of the present invention is much better than that of the prior art unsealing method. The chip body is well protected during the unsealing process, and no damage is caused to the chip body after the unsealing is completed.

[0039] Example 3

[0040] A method for unsealing a plastic-sealed GaAs device comprises the following steps:

[0041] S1. Use a laser decapsulator to thin the plastic packaging material on the chip surface and stop when the bonding wire is exposed.

[0042] S2, heating the etching solution 1 to 90° C. in a water bath, and then using the acid dripping method to etch the device with the etching solution 1 until the device chip is exposed; wherein the etching solution 1 is composed of sulfuric acid: fuming nitric acid: glacial acetic acid: deionized water = 5:1.8:2.3:1.4 in volume ratio;

[0043] S3. Ultrasonic cleaning with a cleaning solution for 10 seconds, then cleaning with deionized water, and drying; wherein the cleaning solution comprises, by volume ratio, carbon tetrachloride:acetone=4:1.5.

[0044] S4, the device is corroded by the etching solution 2, and the etching time is 15s; wherein the composition of the etching solution 2 is mixed by volume ratio, including sulfuric acid: deionized water = 10:2.

[0045] S5. Ultrasonic cleaning with a cleaning solution for 10 seconds, and then cleaning with deionized water; wherein the cleaning solution comprises, by volume ratio, carbon tetrachloride:acetone=4:1.5.

[0046] Example 4

[0047] A method for unsealing a plastic-sealed GaAs device comprises the following steps:

[0048] S1. Use a laser decapsulator to thin the plastic packaging material on the chip surface and stop when the bonding wire is exposed.

[0049] S2, heating the etching solution 1 to 80° C. in a water bath, and then using the acid dripping method to etch the device with the etching solution 1 until the device chip is exposed; wherein the etching solution 1 is composed of sulfuric acid: fuming nitric acid: glacial acetic acid: deionized water = 3.5:1.5:2:1 in volume ratio;

[0050] S3. Ultrasonic cleaning with a cleaning solution for 10 seconds, then cleaning with deionized water, and drying; wherein the cleaning solution comprises, by volume ratio, carbon tetrachloride: acetone = 3:1.5.

[0051] S4. The device is corroded by the etching solution 2 for 10 seconds. The etching solution 2 is composed of sulfuric acid and deionized water in a volume ratio of 9:1.5.

[0052] S5. Ultrasonic cleaning is performed with a cleaning solution for 10 seconds, and then cleaning is performed with deionized water; wherein the cleaning solution comprises, by volume ratio, carbon tetrachloride:acetone=3:1.5.

[0053] Example 5

[0054] A method for unsealing a plastic-sealed GaAs device comprises the following steps:

[0055] S1. Use a laser decapsulator to thin the plastic packaging material on the chip surface and stop when the bonding wire is exposed.

[0056] S2, heating the etching solution 1 to 85° C. in a water bath, and then using the acid dripping method to etch the device with the etching solution 1 until the device chip is exposed; wherein the etching solution 1 is composed of sulfuric acid: fuming nitric acid: glacial acetic acid: deionized water = 5:1.5:2:1.4 in volume ratio;

[0057] S3. Ultrasonic cleaning with a cleaning solution for 10 seconds, then cleaning with deionized water, and drying; wherein the cleaning solution comprises, by volume ratio, carbon tetrachloride:acetone=3.5:1.

[0058] S4, the device is corroded by the etching solution 2, and the etching time is 12 seconds; wherein the composition of the etching solution 2 is mixed by volume ratio, including sulfuric acid: deionized water = 9:1.5.

[0059] S5. Ultrasonic cleaning with a cleaning solution for 10 seconds, and then cleaning with deionized water; wherein the composition of the cleaning solution, in terms of volume ratio, includes carbon tetrachloride:acetone=2.5:1.5.

Claims

1. A method for unsealing a plastic-sealed GaAs device, comprising the following steps: S1, thinning the plastic packaging material on the surface of the device chip; S2, heating the etching solution 1 in a water bath to 75°C-90°C, and then etching the device with the etching solution 1 until the device chip is exposed; S3, washing with a cleaning solution, then washing with deionized water, and drying; S4, the device is corroded by the corrosive solution 2, and the corrosion time is 5s to 15s; S5, washing with cleaning solution, and then washing with deionized water; The composition of the etching solution 1 is calculated by volume ratio, including sulfuric acid: fuming nitric acid: glacial acetic acid: deionized water = 4 (3.5-5): 1.5(1.3-1.8):2(1.8-2.3):1(0.8-1.4); The composition of the etching solution 2 includes sulfuric acid: deionized water = 9 (8.5-10): 1 (0.5-2) in volume ratio.

2. A method for unsealing a plastic-sealed GaAs device according to claim 1, Features: The composition of the cleaning solution in step S3 includes carbon tetrachloride:acetone=3(2.5-4):1(0.8-1.5) in volume ratio.

3. A method for unsealing a plastic-sealed GaAs device according to claim 1, Features: The composition of the etching solution 1 is calculated by volume ratio, including sulfuric acid: fuming nitric acid: glacial acetic acid: deionized water = 4:1.5:2:

1.

4. A method for unsealing a plastic-sealed GaAs device according to claim 1, Features: The composition of the etching solution 2 includes sulfuric acid: deionized water = 9:1 in volume ratio.

5. A method for unsealing a plastic-sealed GaAs device according to claim 1, Features: In step S2, the etching solution 1 is heated to 80°C in a water bath.

6. A method for unsealing a plastic-sealed GaAs device according to claim 1, Features: In step S4, the etching time of the device using the etching solution 2 is 10 seconds.

7. A method for unsealing a plastic-sealed GaAs device according to claim 2, Features: In step S3, ultrasonic cleaning is performed using a cleaning solution for 10 seconds.

8. A method for unsealing a plastic-sealed GaAs device according to claim 2, Features: In step S5, ultrasonic cleaning is performed using a cleaning solution for 10 seconds.

9. A method for unsealing a plastic-sealed GaAs device according to claim 1, Features: In step S1, a laser decapsulator is used to thin the plastic packaging material on the chip surface, and the process stops when the bonding wire is exposed.

10. The method according to claim 1, Features: In step S2, the device is corroded by etching solution 1 using a dripping acid method until the device chip is exposed.

Citation Information

Cited By

  • Chip unsealing method

    CN120453203A