Negative electrode material and preparation method thereof, negative electrode plate and secondary battery
By introducing the pre-improved carbon film and sp2 carbon layer of ultramicro-pores on the surface of the hard carbon material, the channel structure of the secondary battery is optimized, the problem of SEI film formation on the surface of the hard carbon material is solved, and the performance and life of the battery are improved.
Patent Information
- Application Number
- CN202411051518.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-15
AI Technical Summary
The existing hard carbon materials are prone to form organic SEI films in secondary batteries, resulting in active ion loss and capacity attenuation, affecting battery life.
The introduction of pre-formed carbon film with ultramicro-pores on the surface of hard carbon materials optimizes the pore structure, allows positive electrode ions and fluorine ions to pass through, blocks organic solvent molecules, reduces the formation of harmful SEI films, and normalizes the surface through the sp2 carbon layer to reduce the Growth of SEI membrane.
It improves the diffusion performance of the positive electrode ions, reduces the deposition of inactive ions, extends the service life of the battery, and significantly improves the first-time efficiency and cycle capacity retention rate.
Smart Images

Figure CN118970049A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to a negative electrode material and a preparation method thereof, a negative electrode sheet, and a secondary battery. Background Art
[0002] With the development of science and technology, the demand for secondary batteries is increasing, so the technology of secondary batteries has also been vigorously developed. The negative electrode material of a secondary battery is the raw material that constitutes the negative electrode in the battery. Its main function is to transport the active ions in the positive electrode material to the negative electrode through the electrolyte and store them. In the prior art, common negative electrode materials include hard carbon, graphite, mesophase carbon microbeads, petroleum coke, carbon fiber, pyrolytic resin carbon, etc.
[0003] Among them, hard carbon materials are one of the negative electrode materials of secondary batteries. Hard carbon presents a twisted graphene sheet stacking structure, is cheap, has rich active groups and natural pores, and is conducive to structural regulation. However, the surface pores of existing hard carbon negative electrode materials are prone to form SEI films and lose active ions, so how to reduce the SEI film on the surface of hard carbon materials has become a key issue. Summary of the invention
[0004] The purpose of the present application is to provide a negative electrode material and a preparation method thereof, a negative electrode plate, and a secondary battery to solve the problem that a SEI film is easily formed on the surface of hard carbon materials.
[0005] To achieve the purpose of this application, this application provides the following technical solutions:
[0006] In a first aspect, the present invention provides a negative electrode material, comprising a carbon matrix and a pre-processed carbon film, wherein the pre-processed carbon film is coated on the outer surface of the carbon matrix, and the pre-processed carbon film has ultra-micro pores, and the ultra-micro pores are used for exchanging ions.
[0007] The present invention introduces a pre-processed carbon film with ultra-micropores into the negative electrode material as an exclusive diffusion channel for positive electrode ions, optimizes the pore structure of the negative electrode material, and improves the diffusion performance of the positive electrode ions; and the ultra-micropores can selectively allow positive electrode ions and fluoride ions to pass through, blocking organic solvent molecules in the electrolyte; the pre-processed carbon film utilizes osmotic pressure and fluid static pressure to induce spontaneous pre-dissolution of ultra-micro nanopores, thereby achieving efficient positive electrode ion screening, isolating electrolytes, directionally reducing the formation of harmful organic SEI films, increasing the formation of beneficial inorganic SEI films, and effectively reducing the deposition of inactive ions; the optimized ultra-micropores help to slow down the capacity decay of the material, greatly extending the service life of the secondary battery; and the pre-processed carbon film can be regarded as a pre-ionized film, and the thickness of the SEI film grown on the surface of the pre-processed carbon film will not grow too thick.
[0008] In one embodiment, the negative electrode material further includes an sp2 carbon layer, the pre-processed carbon film is coated on the outer surface of the carbon matrix, and the sp2 carbon layer is coated on the outer surface of the pre-processed carbon film.
[0009] In one embodiment, the negative electrode material further includes a sp2 carbon layer, the sp2 carbon layer is coated on the outer surface of the carbon matrix, and the pre-treated carbon film is coated on the outer surface of the sp2 carbon layer.
[0010] In one embodiment, the density of the sp2 carbon layer is greater than or equal to 98%.
[0011] In one embodiment, the thickness of the sp2 carbon layer is 10 nm to 20 nm.
[0012] In one embodiment, the interlayer spacing of the sp2 carbon layer is 0.35nm to 0.4nm.
[0013] In one embodiment, the mass ratio of the pre-treated carbon film to the sp2 carbon layer is (1-5):1.
[0014] In one embodiment, a portion of the surface of the carbon matrix is modified to sp2 hybridized carbon.
[0015] In one embodiment, the pre-treated carbon film is doped with fluoride ions and sodium ions, and at least a portion of the fluoride ions and the sodium ions are contained in the ultra-micro channels.
[0016] In one embodiment, the carbon matrix comprises hard carbon.
[0017] In one embodiment, the diameter of the ultramicrochannel is 0.4 nm to 1.2 nm.
[0018] In one embodiment, the volume of the ultramicrochannel is 0.01 cm 3 / g~0.05cm 3 / g.
[0019] In one embodiment, the particle size D50 of the carbon matrix is 2 μm to 10 μm.
[0020] In one embodiment, the pre-carbon film has a thickness of 10 nm to 100 nm.
[0021] In one embodiment, the mass ratio of the carbon matrix to the pre-processed carbon film is 100:(1-10).
[0022] In a second aspect, the present invention provides a method for preparing a negative electrode material, comprising: preparing a carbon matrix; mixing a first carbon precursor with the carbon matrix so that the first carbon precursor is coated on the outer layer of the carbon matrix, and converting the first carbon precursor into a pre-processed carbon film after heat treatment, wherein the pre-processed carbon film has ultra-micro pores, and the ultra-micro pores are used for exchanging ions.
[0023] In one embodiment, the preparation method includes: mixing the carbon matrix with a second carbon precursor so that the second carbon precursor is coated on the outer surface of the carbon matrix, and converting the second carbon precursor into a sp2 carbon layer after heat treatment; mixing the carbon matrix coated with the sp2 carbon layer with the first carbon precursor so that the first carbon precursor is coated on the outer surface of the sp2 carbon layer.
[0024] In a third aspect, the present invention provides a negative electrode plate, comprising the negative electrode material as described in the various embodiments of the first aspect, or the negative electrode material prepared by the aforementioned method for preparing the negative electrode material.
[0025] In a fourth aspect, the present invention provides a secondary battery comprising a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode and the negative electrode are arranged in the electrolyte, and the negative electrode comprises the negative electrode plate as described in the third aspect; if an electrolyte is used, a diaphragm must be arranged between the positive and negative electrodes, and if a solid electrolyte is used, no diaphragm is required. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0027] Figure 1 is a schematic diagram of a cross-sectional structure of a negative electrode material according to an embodiment;
[0028] Figure 2 is a schematic diagram of an embodiment without a pre-processed carbon film and with a pre-processed carbon film;
[0029] Figure 3 is a schematic diagram of a cross-sectional structure of a negative electrode material including a sp2 carbon layer in an embodiment;
[0030] Figure 4 is a schematic diagram of a cross-sectional structure of a negative electrode material including an sp2 carbon layer in another embodiment;
[0031] Figure 5 is a partial enlarged view of a negative electrode material including a sp2 carbon layer according to an embodiment;
[0032] Figure 6 is a TEM (transmission electron microscope) image of an sp2 carbon layer according to an embodiment;
[0033] Figure 7 is a TEM image of a negative electrode material including a pre-carbon film and an sp2 carbon layer in an embodiment;
[0034] Figure 8 is a selected area electron diffraction pattern of an sp2 carbon layer according to an embodiment;
[0035] Fig. 9 is a schematic diagram of sodium ions and fluoride ions filling ultramicrochannels according to an embodiment;
[0036] Fig.10 is a flow chart of a method for preparing a negative electrode material according to an embodiment;
[0037] Fig.11 is the XRD characterization spectrum of the negative electrode material of Example 1;
[0038] Fig.12 is the first charge and discharge curve of the battery of Example 1;
[0039] Fig.13 This is a graph showing the capacity retention rate of the battery of Example 1 after 100 cycles. DETAILED DESCRIPTION
[0040] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0041] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in this application and in the specification are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more of the related listed items.
[0042] In conjunction with the accompanying drawings, some embodiments of the present application are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0043] The present invention provides a negative electrode material, please refer to Figure 1 and Figure 2, including a carbon matrix 10 and a pre-processed carbon film 20, wherein the pre-processed carbon film 20 is coated on the outer surface of the carbon matrix 10, and the pre-processed carbon film 20 is provided with ultra-micro pores 21, and the ultra-micro pores 21 are used for exchanging ions.
[0044] Specifically, the negative electrode material provided by the present invention is applied to the negative electrode of a secondary battery, which is a sodium ion battery or a lithium ion battery, and can of course also be applied to other rechargeable batteries (such as potassium ion batteries). Among them, a sodium ion battery is a rechargeable battery with sodium ions as charge carriers, and its working principle and structure are similar to those of a lithium ion battery, but lithium is replaced by sodium in the same group of the periodic table and with similar chemical properties. During the charge and discharge process, sodium ions are intercalated and removed back and forth between the positive electrode and the negative electrode, and the negative electrode material is used to store sodium ions from the positive electrode.
[0045] Optionally, in a specific embodiment, the carbon matrix 10 is biomass hard carbon. In secondary batteries, especially sodium ion batteries, the radius of sodium ions is larger than that of lithium ions, making it difficult for sodium ions to be effectively deintercalated in graphite materials. On the contrary, hard carbon will not be completely graphitized at high temperatures, and its internal structure has more free space, so it becomes the preferred material for the negative electrode of secondary batteries.
[0046] The carbon matrix 10 may be in the form of particles, specifically in the form of spheres, quasi-spheres, ellipsoids, polyhedral surfaces or irregular particles. The outer surface of the carbon matrix 10 may have a plurality of pores, which are mainly used to store positive electrode ions (such as sodium ions or lithium ions) from the positive electrode. The pore structure on the carbon matrix 10 significantly affects the performance of the secondary battery. A suitable pore structure can ensure the diffusion kinetics of the positive electrode ions during the insertion / extraction process and provide ion storage sites. However, in the prior art, please refer to Figure 2 1), the substances stored in the pores include not only positive electrode ions, but also fluoride ions in the electrolyte and organic solvent molecules in the electrolyte (AC in the figure). During the first discharge of the secondary battery, the organic solvent molecules and positive electrode ions will form an organic SEI film on the surface of the pores of the hard carbon. The organic SEI film consumes a large amount of positive electrode ions and electrolytes, and the active ions in the battery are converted into inactive ions (commonly known as "dead sodium" or "dead lithium"). The positive electrode ions coated by the organic SEI film are generally difficult to escape (due to the high degree of polymerization of organic matter), resulting in a decrease in the initial efficiency of the secondary battery. In the prior art, the formation of organic SEI film can be reduced by optimizing various film layers, but the optimized film layers of the prior art also make it difficult for positive electrode ions to pass through, and the organic SEI film will be formed on the surface of the film layer, and the thickness of the formed SEI film is too high.
[0047] Therefore, the present invention sets a pre-carbon film 20 on the outer surface of the carbon substrate 10, please refer to Figure 22), the pre-processed carbon film 20 is coated on the outer surface of the carbon substrate 10 to close the pores of the carbon substrate 10. Then, the pre-processed carbon film 20 is provided with ultra-micro channels 21 penetrating the pre-processed carbon film 20, such as Figure 1 As shown, the ultra-micropores 21 connect the surface of the carbon matrix 10 with the external space of the negative electrode material. In the structure of the negative electrode material provided in this embodiment, the positive electrode ions and fluoride ions can enter the pores of the carbon matrix 10 through the ultra-micropores 21. However, since the pore size of the ultra-micropores 21 is smaller than the pore size, the organic solvent molecules with a larger volume cannot enter the ultra-micropores 21 and are isolated outside the pre-carbon film 20.
[0048] It needs to be explained that the sodium ion battery storage model in the prior art divides the discharge curve into two regions: the slope region and the platform region. These two regions correspond to two sodium ion storage modes. The former is the graphite domain. Hard carbon is formed by random stacking of a few layers of graphene, usually formed by sodium ions inserted into the stacked graphene or adsorbed on the defect surface, forming a slope capacity. The latter is the ultra-micropores or nanopores on the hard carbon, which can be regarded as the gaps in the randomly stacked graphite domains. In the prior art, the capacity of the high-voltage slope section can be increased by increasing the number of openings (ultra-micropores or nanopores) and defects, which is beneficial to the improvement of rate performance. However, during the charging stage, sodium ions need to migrate from the openings. During this process, a large number of quasi-metallic sodium clusters cannot migrate out, resulting in a low initial efficiency of the material. Therefore, it is necessary to propose a new type of hard carbon composite material to overcome the limitations of traditional methods. The present invention constructs exclusive diffusion and screening channels for sodium ions on the surface of the carbon matrix 10, optimizes the pore structure of the negative electrode material, improves the diffusion performance of sodium ions, and reduces the deposition of "dead sodium". Ultimately, without the need for additional pre-sodiumization technology, the initial efficiency of the hard carbon material in the sodium battery negative electrode is greatly improved (greater than 96%).
[0049] The present invention introduces a pre-processed carbon film 20 with ultrafine pores 21 into the negative electrode material as an exclusive diffusion channel for positive electrode ions, thereby optimizing the pore structure of the negative electrode material and improving the diffusion performance of the positive electrode ions; and the ultrafine pores 21 can selectively allow positive electrode ions and fluoride ions to pass through, blocking the organic solvent molecules in the electrolyte; the pre-processed carbon film 20 utilizes the spontaneous pre-dissolution induced by osmotic pressure and fluid static pressure on ultrafine nanopores, thereby achieving efficient positive electrode ion screening, isolating electrolytes, and directionally reducing the formation of harmful organic SEI films and increasing the formation of beneficial inorganic SEI films, effectively reducing the deposition of inactive ions; the optimized ultrafine pores 21 help to slow down the capacity decay of the material and greatly extend the service life of the secondary battery; and the pre-processed carbon film 20 can be regarded as a pre-ionized film, and the thickness of the SEI film grown on the surface of the pre-processed carbon film 20 will not grow excessively thick.
[0050] In one embodiment, the precursor of the pre-carbon film 20 can be a ZIF material (Zeolitic Imidazolate Frameworks) or a MOF material (Metal organic Framework). It is understandable that ZIF materials and MOF materials generally have high specific surface area, high porosity and adjustable pore size. When the two are carbonized, the carbide obtained can retain a rich pore structure, which becomes the ultra-micro pores 21 of the pre-carbon film 20.
[0051] In one implementation, please refer to Figure 3 , Figure 6 , Figure 7 and Figure 8 The negative electrode material also includes an sp2 carbon layer 30 , the pre-treated carbon film 20 is coated on the outer surface of the carbon matrix, and the sp2 carbon layer 30 is coated on the outer surface of the pre-treated carbon film 20 .
[0052] Specifically, sp2 hybridized carbon is a carbon atom that hybridizes with two p orbitals and one s orbital to form a planar triangular molecular structure, which contains three sp2 hybrid orbitals and one p orbital that does not participate in hybridization. Figure 3 As shown, the outer surface of the pre-carbon film 20 is coated with multiple layers of stacked sp2 hybridized carbon (similar to the stacked graphene structure), and the multiple layers of stacked sp2 hybridized carbon form an sp2 carbon layer 30.
[0053] In the prior art, the surface of hard carbon will form irregular concave and convex surfaces, which increase the growth probability of SEI film, resulting in the formation of SEI film on the surface of pre-carbon film 20 to consume positive electrode ions even when coated with pre-carbon film 20.
[0054] Therefore, in order to solve the problem of irregular surface of carbon matrix, especially hard carbon, the present invention also covers the outer layer of carbon matrix with sp2 carbon layer 30; based on the regular and dense structure of p2 hybridized carbon, the surface of negative electrode material presents a regular arc surface, which is beneficial to reduce the formation of organic SEI film and accelerate the passage of positive electrode ions and fluoride ions.
[0055] In one implementation, please refer to Figure 4 and Figure 5 , the sp2 carbon layer 30 is coated on the outer surface of the carbon matrix, and the pre-carbon film 20 is coated on the outer surface of the sp2 carbon layer 30 .
[0056] Specifically, based on the above embodiment, the sp2 carbon layer 30 can also be arranged between the pre-processed carbon film 20 and the carbon substrate. The advantage of this arrangement is that before coating the pre-processed carbon film 20, the surface of the carbon substrate is coated with the sp2 carbon layer 30, i.e., a regular arc surface is formed, which is beneficial to the coating of the pre-processed carbon film 20, and the ultra-micro pores 21 of the pre-processed carbon film 20 are located at the outermost side, which is beneficial to improve the efficiency of ions passing through the ultra-micro pores.
[0057] In one embodiment, the density of the sp2 carbon layer 30 is greater than or equal to 98%. Optionally, the density of the sp2 carbon layer 30 can be 98%, 98.5%, 99%, 99.5%, or 100%.
[0058] The density of the sp2 carbon layer 30 is greater than or equal to the above range in order to prevent the organic solvent molecules from entering the pores of the carbon matrix 10 through the sp2 carbon layer 30, thereby ensuring the diffusion of the positive electrode ions and effectively isolating the organic solvent molecules.
[0059] In one embodiment, the thickness of the sp2 carbon layer 30 is 10 nm to 20 nm. Optionally, the thickness of the sp2 carbon layer 30 may be 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, or 20 nm.
[0060] The thickness of the sp2 carbon layer 30 is within the above range in order to avoid affecting the capacity of the carbon matrix 10 for storing positive electrode ions and to ensure that the irregular concave and convex surfaces on the surface of the carbon matrix 10 are reduced.
[0061] In one embodiment, the interlayer spacing of the sp2 carbon layer is 0.35 nm to 0.4 nm. Optionally, the sp2 carbon layer has multiple carbon layers, and the spacing between the multiple carbon layers can be 0.35 nm, 0.36 nm, 0.37 nm, 0.38 nm, 0.39 nm, or 0.4 nm.
[0062] The interlayer spacing of the sp2 carbon layer 30 is within the above range in order to ensure the electrical conductivity of the sp2 carbon layer 30 and to form a smooth coating carbon layer structure and reduce the irregular concave-convex structure on the surface of the carbon substrate.
[0063] In one embodiment, the mass ratio of the pre-treated carbon film 20 to the sp2 carbon layer 30 is (1-5): 1. Optionally, the mass ratio of the pre-treated carbon film 20 to the sp2 carbon layer 30 can be 1: 1, 2: 1, 3: 1, 4: 1, 5: 1. The mass ratio of the pre-treated carbon film 20 to the sp2 carbon layer 30 is within the above range to ensure that both can give full play to their own advantages and functions, and avoid that part of the carbon substrate 10 is not covered with the pre-treated carbon film 20 or the sp2 carbon layer 30.
[0064] In one embodiment, part of the surface of the carbon matrix is modified to sp2 hybridized carbon. Specifically, based on the above embodiment, since sp2 hybridized carbon has a relatively regular molecular structure, modifying part of the surface of the carbon matrix to sp2 hybridized carbon can improve the regularity of the surface of the carbon matrix, thereby reducing the formation of the organic SEI film and accelerating the passage of positive electrode ions and fluoride ions.
[0065] In one implementation, please refer to Fig. 9 , the pre-treated carbon film 20 is doped with fluoride ions and sodium ions, and at least part of the fluoride ions and sodium ions are contained in the ultra-micro pores 21. Specifically, fluoride ions and sodium ions (such as sodium hexafluorophosphate) can be introduced into the pre-treated carbon film 20 during the preparation process, so that the obtained pre-treated carbon film 20 is doped with fluoride ions and sodium ions. Sodium ions and fluoride ions can be combined in the pre-treated carbon film 20, specifically contained in the ultra-micro pores 21. The sodium ions and fluoride ions in the ultra-micro pores 21 can increase the diffusion rate of sodium ions and fluoride ions from the electrolyte, enhance the permeability of the pre-treated carbon film 20, and thereby improve the diffusion performance of the pre-treated carbon film 20 to the carbon matrix 10.
[0066] By constructing specific ion screening channels in the pre-carbon membrane 20, the passage of organic macromolecules is isolated, and a beneficial inorganic SEI membrane is constructed inside the ultramicropores 21 by doping sodium ions and fluoride ions. The ultramicropores 21 have a high degree of selective permeability, enhance the desolvation ability of the solute, and ensure the full storage and release of sodium ions during the charge and discharge process.
[0067] In one embodiment, the proportion of fluorine ions and sodium ions in the pre-treated carbon film 20 is 5% to 10%. Optionally, the proportion of fluorine ions and sodium ions in the pre-treated carbon film 20 can be 5%, 6%, 7%, 8%, 9%, or 10%.
[0068] The ratio of fluoride ions and sodium ions in the pre-processed carbon film 20 is within the above range in order to effectively improve the diffusion rate and ensure the conductivity and structural stability of the pre-processed carbon film 20. When the ratio of the two is less than the above range, the content of sodium ions and fluoride ions filled in the ultra-micro pores 21 is low, and even some ultra-micro pores 21 are not filled with the two ions, resulting in a decrease in the diffusion rate of ions in the ultra-micro pores 21. When the ratio of the two is greater than the above range, the content of sodium ions and fluoride ions in the pre-processed carbon film 20 is high, which affects the conductivity of the pre-processed carbon film 20, and the sodium ions and fluoride ions occupy the spatial position of carbon atoms, resulting in the deterioration of the structural stability of the pre-processed carbon film 20.
[0069] In one embodiment, the diameter of the ultramicrochannel 21 is 0.4 nm to 1.2 nm. Optionally, the diameter of the ultramicrochannel 21 can be 0.4 nm, 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, 0.9 nm, 1 nm, 1.1 nm, or 1.2 nm.
[0070] When the diameter of the ultra-micropores 21 is within the above range, it can be ensured that the pre-carbon film 20 fully exerts its screening effect. When the diameter of the ultra-micropores 21 is smaller than the above range, the ultra-micropores 21 have an enhanced blocking effect on positive electrode ions and fluoride ions, and it is difficult for positive electrode ions and fluoride ions to pass through the ultra-micropores 21, resulting in a decrease in the reversible capacity of the negative electrode material, and the difficulty of preparing the ultra-micropores 21 that are too small is also increased, which is not conducive to industrial production. When the diameter of the ultra-micropores 21 is larger than the above range, it is difficult for the ultra-micropores 21 to effectively screen the organic solvent molecules, resulting in the formation of a small amount of organic SEI film in the pores, which reduces the initial efficiency of the material.
[0071] In one embodiment, the volume of the ultra-microchannel 21 is 0.01 cm 3 / g~0.05cm 3 Optionally, the volume of the ultra-microchannel 21 can be 0.01 cm 3 / g, 0.02cm 3 / g, 0.03cm 3 / g, 0.04cm 3 / g, 0.05cm 3 / g.
[0072] When the volume of the ultra-micropores 21 is within the above range, it can ensure that the pre-carbon film 20 fully exerts its screening effect and provides additional ion storage space. When the volume of the ultra-micropores 21 is less than the above range, the ultra-micropores 21 have an enhanced blocking effect on positive electrode ions and fluoride ions, and it is difficult for positive electrode ions and fluoride ions to pass through the ultra-micropores 21. The number of ultra-micropores 21 decreases, and some holes are not connected to the ultra-micropores 21, resulting in a decrease in the capacity of the negative electrode material. When the volume of the ultra-micropores 21 is greater than the above range, it is difficult for the ultra-micropores 21 to effectively screen organic solvent molecules, resulting in the formation of a small amount of organic SEI film in the holes, reducing the initial efficiency of the material.
[0073] In one embodiment, the particle size D50 of the carbon matrix 10 is 2 μm to 10 μm. Optionally, the particle size D50 of the carbon matrix 10 can be 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, or 10 μm.
[0074] When the particle size of the carbon matrix 10 is within the above range, the particle size of the carbon matrix 10 can well balance the comprehensive electrochemical properties of the negative electrode material, which is beneficial to improving the tap density of the negative electrode material. When the particle size of the carbon matrix 10 is too small, the compaction density of the negative electrode sheet is small, the specific surface area is large, and the first efficiency is low; when the particle size of the carbon matrix 10 is too large, the rate performance of the negative electrode material is poor.
[0075] In one embodiment, the thickness of the pre-treated carbon film 20 is 10 nm to 100 nm. Optionally, the thickness of the pre-treated carbon film 20 may be 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, or 100 nm.
[0076] When the thickness of the pre-decomposed carbon film 20 is within the above range, the reversible sodium storage capacity of the negative electrode material can be ensured. When the thickness of the pre-decomposed carbon film 20 is too thin, part of the surface of the carbon matrix 10 will not be covered and an organic SEI film will be formed; when the thickness of the pre-decomposed carbon film 20 is too thick, since the carbon matrix 10 is the main sodium storage material, the proportion of the carbon matrix 10 will be reduced, and the reversible sodium storage capacity of the negative electrode material cannot be guaranteed.
[0077] In one embodiment, the mass ratio of the carbon substrate 10 to the pre-processed carbon film 20 is 100:(1-10). Optionally, the mass ratio of the carbon substrate 10 to the pre-processed carbon film 20 can be 100:1, 100:2, 100:3, 100:4, 100:5, 100:6, 100:7, 100:8, 100:9, 100:10.
[0078] The reversible sodium storage capacity of the negative electrode material can be ensured by satisfying the mass ratio of the carbon matrix 10 and the pre-decomposed carbon film 20 within the above range. When the proportion of the pre-decomposed carbon film 20 is too small, part of the surface of the carbon matrix 10 will not be covered and an organic SEI film will be formed; when the proportion of the pre-decomposed carbon film 20 is too large, since the carbon matrix 10 is the main sodium storage material, the proportion of the carbon matrix 10 will become smaller, thereby failing to ensure the reversible sodium storage capacity of the negative electrode material.
[0079] In one embodiment, the present invention also provides a method for preparing a negative electrode material, please refer to Fig.10 , specifically including the following steps:
[0080] Step S10, preparing a carbon matrix.
[0081] Step S20, mixing a first carbon precursor with a carbon matrix so that the first carbon precursor is coated on the outer surface of the carbon matrix, and converting the first carbon precursor into a pre-carbon film after heat treatment.
[0082] The pre-treated carbon membrane has ultra-micro pores, which are used for exchanging ions.
[0083] In one embodiment, in step S10, preparing the carbon matrix specifically includes the following steps:
[0084] Step S11, providing a biomass raw material, and pre-treating the biomass raw material to obtain a carbon source.
[0085] Step S12, heat-treating the carbon source, cleaning to remove impurities and then drying to obtain a carbon matrix.
[0086] Optionally, in step S11, the provided biomass raw materials include one or more of straw, coconut shell, wood, and enteromorpha. In a specific embodiment, the biomass raw materials may be bamboo, corn stalks, coconut shells, rice stalks, cotton stalks, wood chips, wheat straw, and the like.
[0087] Optionally, in step S11, the biomass raw material is pre-treated, specifically including: crushing and sieving the biomass raw material, immersing the sieved material in a cleaning liquid, and drying after sufficient stirring to obtain a carbon source. It should be explained that there will be a large amount of metal impurities in the biomass raw material. In order to avoid the metal impurities being retained in the final carbon matrix, the biomass raw material needs to be cleaned with a cleaning liquid.
[0088] Optionally, in step S11, the biomass raw material is crushed and sieved to a mesh size of 100 to 400 mesh; the cleaning liquid can be an acid solution or an alkali solution, specifically potassium hydroxide, sodium hydroxide, hydrochloric acid, etc.; the temperature for sufficient stirring in the cleaning liquid can be 50°C to 100°C, and the stirring time can be 3h to 10h; the drying temperature is greater than or equal to 100°C.
[0089] Optionally, in step S12, the carbon source is heat-treated, cleaned to remove impurities and then dried, specifically comprising: placing the carbon source in a tubular furnace for initial carbonization, cleaning the obtained powder with acid solution to remove impurities after cooling to room temperature, and obtaining a carbon matrix after drying and filtering.
[0090] Optionally, in step S12, the heating rate of the initial carbonization is 5°C / min, the initial carbonization temperature is 600°C to 1000°C, the holding time is 2h to 8h, and the cooling rate of the initial carbonization is 10°C / min.
[0091] In one embodiment, in step S20, a first carbon precursor is mixed with a carbon matrix so that the first carbon precursor is coated on the outer layer of the carbon matrix, and the first carbon precursor is converted into a pre-carbon film after heat treatment, which specifically includes the following steps:
[0092] Step S21, mix and dissolve precursor A and precursor B to obtain solution A, add precursor C to solution A, stir thoroughly to obtain solution B, mix solution B with a solvent to obtain solution C, solution B is a pre-carbon film precursor, mix the carbon matrix into solution C, stir thoroughly and mix thoroughly to obtain a mixture.
[0093] Step S22, heat-treating the mixture, crushing and screening it to obtain a negative electrode material.
[0094] Optionally, in step S21, precursor A may be furfuryl alcohol (PFA), precursor B may be oxalic acid dihydrate, precursor C may be polyethylene glycol (PEG, molecular weight 8000), and solvent may be NMP (N-methylpyrrolidone). The purpose of using the above three as pre-carbon film precursors is that the carboxyl group on oxalic acid dihydrate can react with the hydroxyl groups on furfuryl alcohol and polyethylene glycol, so that solution B forms a cross-linked structure, so that ultra-micropores can be obtained after carbonization.
[0095] Optionally, in step S21, the precursor A and the precursor B are mixed and dissolved to obtain solution A, which specifically includes: mixing the precursor A and the precursor B, and stirring them in a hot water bath. The water bath temperature can be 50° C. to 80° C., and the stirring time is 8 h to 12 h.
[0096] Optionally, in step S21, solution B is mixed with a solvent to obtain solution C, and the carbon matrix is mixed into solution C, specifically comprising: mixing solution B and the solvent in a preset ratio and heating to form a stable solution C, and then adding the carbon matrix thereto and mixing and stirring until the solution is dried. The ratio of solution B to the solvent may be 1:(10-30), and the stirring temperature may be 80°C-120°C.
[0097] Optionally, in step S22, the mixture is heat treated and crushed and sieved, specifically comprising: placing the mixture in a tubular furnace for carbonization, and after cooling to room temperature, crushing and sieving the obtained product to obtain the negative electrode material.
[0098] Optionally, in step S22, the carbonization heating rate is 2°C / min, the initial carbonization temperature is 1000°C to 1500°C, the insulation time is 2h to 8h, the initial carbonization cooling rate is 10°C / min, and the sieving mesh size is 100 mesh to 400 mesh.
[0099] In one embodiment, in step S21, precursor A may be furfuryl alcohol (PFA), precursor B may be sodium hexafluorophosphate (NaPF6), precursor C may be polyethylene glycol (PEG, molecular weight 8000), and the solvent may be NMP (N-methylpyrrolidone). The purpose of using the above three as pre-carbon film precursors is to introduce sodium ions and fluoride ions into the pre-carbon film.
[0100] Optionally, in step S21, the carbon matrix mixed into the solution C may be glucose, and the solution C includes sodium hexafluorophosphate.
[0101] Optionally, in step S22, the mixture is heat treated and crushed and sieved, specifically including: placing the mixture in a high-pressure reactor, washing and drying after initial heat treatment, and then placing the product in a tubular furnace for carbonization, and after cooling to room temperature, crushing and sieving the product to obtain the negative electrode material.
[0102] Optionally, in step S22, the temperature of the initial heat treatment is 200℃~300℃, the time of the initial heat treatment is 5h~10h, the carbonization heating rate is 2℃ / min, the initial carbonization temperature is 1000℃~1500℃, the insulation time is 2h~8h, and the initial carbonization cooling rate is 10℃ / min.
[0103] In one embodiment, the negative electrode material further includes an sp2 carbon layer, and the preparation method of the negative electrode material includes:
[0104] Step A10, preparing a carbon substrate.
[0105] Step A20, mixing the carbon matrix with the second carbon precursor so that the second carbon precursor is coated on the outer surface of the carbon matrix, and converting the second carbon precursor into an sp2 carbon layer after heat treatment.
[0106] Step A30: mixing the carbon substrate coated with the sp2 carbon layer with the first carbon precursor, so that the first carbon precursor is coated on the outer surface of the sp2 carbon layer.
[0107] Wherein, step A10 and step A30 can refer to step S10 and step S20 in the above embodiment, and will not be described in detail here. Step A20, mixing the carbon matrix with the second carbon precursor so that the second carbon precursor is coated on the outer surface of the carbon matrix, and converting the second carbon precursor into an sp2 carbon layer after heat treatment, comprises:
[0108] Step A21, dissolving precursor D to obtain solution D, solution D is a pre-carbon film precursor, adding precursor E and precursor F to solution D to obtain solution E, mixing solution E into the carbon matrix, and drying after sufficient stirring and mixing to obtain a mixture.
[0109] Step A22, heat-treating the mixture, and obtaining a carbon matrix coated with an sp2 carbon layer after crushing and screening.
[0110] Optionally, in step A21, precursor D can be a phenolic resin, the solvent of precursor D is ethanol, precursor E is copper acetate, and precursor F is ammonia water. Copper hydroxide particles can be obtained by reacting copper acetate and ammonia water, and the copper hydroxide particles are attached to the resin skeleton. The copper hydroxide particles act as a catalyst to induce cross-linking of the phenolic resin.
[0111] Optionally, in step A21, solution E is mixed into the carbon matrix and mixed by sufficient stirring, specifically comprising: dispersing the carbon matrix in ethanol, then adding solution E thereto, and obtaining a mixture by hot stirring. The hot stirring temperature is 50° C. to 80° C., and the stirring time is 2 h to 4 h.
[0112] Optionally, in step A22, the mixture is heat treated and crushed and sieved, specifically comprising: placing the mixture in a tubular furnace for carbonization, acid-washing the obtained product after cooling to room temperature, and crushing and sieving to obtain the negative electrode material.
[0113] Optionally, in step A22, the carbonization heating rate is 2°C / min, the initial carbonization temperature is 1000°C to 1500°C, the insulation time is 2h to 8h, the initial carbonization cooling rate is 10°C / min, and the sieving mesh size is 100 mesh to 400 mesh.
[0114] The preparation method of the negative electrode material provided by the present invention can prepare a negative electrode material with an ion screening channel suitable for the negative electrode. The negative electrode material includes a carbon matrix and a pre-formed carbon film coated on the carbon matrix. The ultra-micro pores on the pre-formed carbon film serve as diffusion and screening channels exclusively for positive electrode ions, ensuring that the positive electrode ions can be fully desolvated and diffused into the ultra-micro pores, while effectively isolating the organic solvent molecules in the electrolyte, reducing the formation of the organic SEI film in the first discharge process, reducing the consumption of positive electrode ions, and finally achieving the ultra-high first efficiency of the material.
[0115] In one embodiment, the present invention further provides a negative electrode plate, the negative electrode plate comprising the negative electrode material provided in the above embodiment or the negative electrode material prepared by the preparation method provided in the above embodiment. In other embodiments, the negative electrode plate further comprises a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, the negative electrode film layer comprising the negative electrode material provided in the above embodiment.
[0116] In one embodiment, the present invention also provides a secondary battery, including a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode and the negative electrode are arranged in the electrolyte, and the negative electrode includes the negative electrode plate provided in the above embodiment. Optionally, the electrolyte includes a liquid electrolyte or a solid electrolyte. If a solid electrolyte is used, no diaphragm is required. If a liquid electrolyte is used, a diaphragm is arranged between the positive and negative electrodes. During the battery charge and discharge process, the active positive electrode ions are embedded and removed back and forth between the positive electrode and the negative electrode. The electrolyte plays the role of conducting positive electrode ions between the positive electrode and the negative electrode. The diaphragm is arranged between the positive electrode and the negative electrode, mainly to prevent the positive and negative electrodes from short-circuiting, and at the same time to allow the positive electrode ions to pass through.
[0117] The technical solution of the present invention is described in detail below through specific embodiments.
[0118] Example 1
[0119] This embodiment provides a negative electrode material, which includes a carbon matrix (hard carbon) and a pre-processed carbon film. The pre-processed carbon film is coated on the outer surface of the carbon matrix, and ultra-micro pores are opened on the pre-processed carbon film.
[0120] The diameter of the ultramicropores is 0.4nm to 1nm, and the volume of the ultramicropores is 0.02cm 3 / g, the particle size of the carbon matrix is 6 μm, the thickness of the pre-treated carbon film is 20 nm, and the mass ratio of the carbon matrix to the pre-treated carbon film is 100:5.
[0121] The preparation method of the negative electrode material comprises the following steps:
[0122] 1) Preparation of carbon source for carbon matrix: Bamboo was selected as raw material, the bamboo was crushed through a 300 mesh sieve, 100 g of the bamboo was taken and immersed in 300 mL of 0.1 M potassium hydroxide solution, stirred at 90° C. for 6 h to make the material uniform, and then transferred to a 120° C. oven for drying.
[0123] 2) Preparation of carbon matrix: The dried material is transferred to a tubular furnace for primary carbonization, the temperature is raised to 800°C at a rate of 5°C / min, kept at this temperature for 2 hours, and then cooled to room temperature at a rate of 10°C / min. The powder obtained by calcination is decontaminated with a hydrochloric acid solution, and a porous carbon matrix is obtained after drying and filtration.
[0124] 3) Prepare a mixture of pre-carbon film precursor and carbon matrix: Measure 100mL of furfuryl alcohol and pour it into a three-necked flask, then add 1g of dihydrated oxalic acid, stir in a water bath at 60°C for 10h, and the stirrer speed is 300rpm. Then add 10g of polyethylene glycol (molecular weight of 8000) and continue stirring for 30min, pour it into a beaker for use. Mix the polyfurfuryl alcohol / polyethylene glycol (PFA / PEG) mixture precursor with NMP at a mass ratio of 1:20 to form a uniform and stable mixed solution, then pour the hard carbon matrix material into the polymer solution and stir at 100°C for 24h until the solution is dried.
[0125] 4) Preparation of negative electrode material: The solid dried in step 3) is transferred to a tubular furnace for calcination, the temperature is increased to 1100°C at a rate of 2°C / min, kept at this temperature for 2 hours, and then cooled to room temperature at a rate of 10°C / min; the calcined product is crushed through a 300-mesh sieve to obtain the negative electrode material.
[0126] from Fig.11 It can be clearly seen from the XRD characterization spectrum of the negative electrode material of Example 1 provided that the negative electrode material has obvious peaks located at 26° and 43°, which correspond to the planes (002) and (101) of the carbon material. This also shows that a hard carbon negative electrode material with a pre-cured carbon film is prepared in Example 1.
[0127] Example 2
[0128] This embodiment provides a negative electrode material, which includes a carbon matrix (hard carbon) and a pre-processed carbon film. The pre-processed carbon film is coated on the outer surface of the carbon matrix, and ultra-micro pores are opened on the pre-processed carbon film.
[0129] The diameter of the ultramicropores is 0.4nm to 0.8nm, and the volume of the ultramicropores is 0.01cm 3 / g, the particle size of the carbon matrix is 2μm, the thickness of the pre-treated carbon film is 20nm, and the mass ratio of the carbon matrix to the pre-treated carbon film is 100:8.
[0130] The preparation steps of this embodiment are the same as those of embodiment 1.
[0131] Example 3
[0132] This embodiment provides a negative electrode material, which includes a carbon matrix (hard carbon) and a pre-processed carbon film. The pre-processed carbon film is coated on the outer surface of the carbon matrix, and ultra-micro pores are opened on the pre-processed carbon film.
[0133] The diameter of the ultramicropores is 0.8nm to 1.2nm, and the volume of the ultramicropores is 0.05cm 3 / g, the particle size of the carbon matrix is 10μm, the thickness of the carbon film is 80nm, and the mass ratio of the carbon matrix to the carbon film is 100:4.
[0134] The preparation steps of this embodiment are the same as those of embodiment 1.
[0135] Example 4
[0136] This embodiment provides a negative electrode material, which includes a carbon matrix (hard carbon) and a pre-processed carbon film. The pre-processed carbon film is coated on the outer surface of the carbon matrix, and ultra-micro pores are opened on the pre-processed carbon film.
[0137] The diameter of the ultramicropores is 0.4nm to 0.8nm, and the volume of the ultramicropores is 0.02cm 3 / g, the particle size of the carbon matrix is 5μm, the thickness of the pre-treated carbon film is 10nm, and the mass ratio of the carbon matrix to the pre-treated carbon film is 100:2.
[0138] The preparation steps of this embodiment are the same as those of embodiment 1.
[0139] Example 5
[0140] This embodiment provides a negative electrode material, which includes a carbon matrix (hard carbon) and a pre-processed carbon film. The pre-processed carbon film is coated on the outer surface of the carbon matrix, and ultra-micro pores are opened on the pre-processed carbon film.
[0141] The diameter of the ultramicropores is 0.4nm to 1nm, and the volume of the ultramicropores is 0.02cm 3 / g, the particle size of the carbon matrix is 10, the thickness of the pre-treated carbon film is 100nm, and the mass ratio of the carbon matrix to the pre-treated carbon film is 100:10.
[0142] The preparation steps of this embodiment are the same as those of embodiment 1.
[0143] Example 6
[0144] This embodiment provides a negative electrode material, which includes a carbon matrix (hard carbon) and a pre-processed carbon film, wherein the pre-processed carbon film is coated on the outer surface of the carbon matrix, and ultra-micro pores are formed on the pre-processed carbon film, and sodium ions and fluoride ions are doped in the pre-processed carbon film.
[0145] The diameter of the ultramicropores is 0.4nm to 1nm, and the volume of the ultramicropores is 0.04cm 3 / g, the particle size of the carbon matrix is 6μm, the thickness of the pre-treated carbon film is 20nm, and the mass ratio of the carbon matrix to the pre-treated carbon film is 100:4. The proportion of fluoride ions and sodium ions in the pre-treated carbon film is 5%.
[0146] The preparation method of the negative electrode material comprises the following steps:
[0147] 1) Measure 100 mL of furfuryl alcohol and pour it into a three-necked flask, then add 2 g of NaPF6, stir in a water bath at 60°C for 10 h, and the stirrer speed is 300 rpm. Then add 10 g of polyethylene glycol (molecular weight 8000) and continue stirring for 30 min, pour it into a beaker for use. The polyfurfuryl alcohol / polyethylene glycol (PFA / PEG) mixture precursor is mixed with NMP at a mass ratio of 1:20 to form a uniform and stable mixed solution, and then 10 g of glucose is dissolved in 40 mL of the above mixed solution to obtain a mixture.
[0148] 2) The mixture in step 1) was transferred to a 100 mL autoclave reactor and reacted at 200° C. for 6 h. After the reaction, the solid product was separated by filtration and washed three times with deionized water and anhydrous ethanol in sequence. The obtained solid was vacuum dried at 100° C. overnight, and the obtained sample was carbonized at 1300° C. for 2 h in an argon atmosphere.
[0149] Example 7
[0150] This embodiment provides a negative electrode material, which includes a carbon matrix (hard carbon) and a pre-processed carbon film, wherein the pre-processed carbon film is coated on the outer surface of the carbon matrix, and ultra-micro pores are formed on the pre-processed carbon film, and sodium ions and fluoride ions are doped in the pre-processed carbon film.
[0151] The diameter of the ultramicropores is 0.4nm to 1nm, and the volume of the ultramicropores is 0.04cm 3 / g, the particle size of the carbon matrix is 6μm, the thickness of the pre-carbon film is 20nm, and the mass ratio of the carbon matrix to the pre-carbon film is 100:4. The proportion of fluoride ions and sodium ions in the pre-carbon film is 10%.
[0152] The preparation steps of this embodiment are the same as those of embodiment 6.
[0153] Example 8
[0154] This embodiment provides a negative electrode material, which includes a carbon matrix (hard carbon), a pre-processed carbon film and an sp2 carbon layer, wherein the pre-processed carbon film is coated on the outer surface of the carbon matrix, and ultra-micro pores are opened on the pre-processed carbon film. The sp2 carbon layer is coated on the outer surface of the pre-processed carbon film.
[0155] The diameter of the ultramicropores is 0.4nm to 1nm, and the volume of the ultramicropores is 0.02cm 3 / g, the particle size of the carbon matrix is 6μm, the thickness of the pre-treated carbon film is 20nm, the mass ratio of the carbon matrix and the pre-treated carbon film is 100:2, the interlayer spacing of the sp2 carbon layer is 0.35nm, and the mass ratio of the pre-treated carbon film and the sp2 carbon layer is 1:1.
[0156] The preparation method of the negative electrode material comprises the following steps:
[0157] 1) Prepare a mixture of pre-carbon film precursor and carbon matrix: Measure 100mL of furfuryl alcohol and pour it into a three-necked flask, then add 1g of dihydrated oxalic acid, stir in a water bath at 60°C for 10h, and the stirrer speed is 300rpm. Then add 10g of polyethylene glycol (molecular weight of 8000) and continue stirring for 30min, pour it into a beaker for use. Mix the polyfurfuryl alcohol / polyethylene glycol (PFA / PEG) mixture precursor with NMP at a mass ratio of 1:20 to form a uniform and stable mixed solution, and then disperse 10g of porous carbon matrix in 40mL of the above mixed solution to obtain a mixture. Transfer the mixture to a 100mL autoclave reactor and react at 200°C for 6h. After the reaction is completed, filter and separate the solid product, and wash it three times with deionized water and anhydrous ethanol in turn.
[0158] 2) Prepare sp2 carbon layer precursor: Measure 10 grams of phenolic resin and dissolve it in 100 mL of ethanol solution, stir at 60 ° C for 6 hours to fully dissolve the resin, then add 1 gram of copper acetate to the solution, continue stirring until the metal salt is completely dissolved, add ammonia water dropwise to form copper hydroxide particles attached to the resin skeleton, then filter and wash to obtain sp2 carbon layer precursor. Take 10g of the solid obtained in step 1) and disperse it in 100 mL of ethanol, then add 0.5g of sp2 carbon layer precursor, stir at 60 ° C for 2 hours, the stirrer speed is 300 rpm, and then stir at 100 ° C for 4 hours until the solution is dried.
[0159] 3) Then, the solid dried in step 2) is transferred to a tube furnace for calcination, and the temperature is raised to 1100°C at a rate of 2°C / min, kept at this temperature for 2 hours, and then cooled to room temperature at a rate of 10°C / min. The calcined product is dissolved with hydrochloric acid to remove the metal catalyst, washed and dried, and then crushed through a 300-mesh sieve to obtain a negative electrode material.
[0160] Example 9
[0161] This embodiment provides a negative electrode material, which includes a carbon matrix (hard carbon), a pre-treated carbon film and a sp2 carbon layer. The sp2 carbon layer is coated on the outer surface of the carbon matrix, the pre-treated carbon film is coated on the outer surface of the sp2 carbon layer, and ultra-micro pores are opened on the pre-treated carbon film.
[0162] The diameter of the ultramicropores is 0.4nm to 1nm, and the volume of the ultramicropores is 0.02cm 3 / g, the particle size of the carbon matrix is 6μm, the thickness of the pre-treated carbon film is 40nm, the mass ratio of the carbon matrix to the pre-treated carbon film is 100:4. The interlayer spacing of the sp2 carbon layer is 0.35nm, and the mass ratio of the pre-treated carbon film to the sp2 carbon layer is 4:1.
[0163] The preparation method of the negative electrode material comprises the following steps:
[0164] 1) Measure 10 grams of phenolic resin and dissolve it in 100 mL of ethanol solution, stir at 60°C for 6 hours to fully dissolve the resin, then add 1 gram of copper acetate to the solution, continue stirring until the metal salt is completely dissolved, add ammonia water dropwise to form copper hydroxide particles attached to the resin skeleton, and then filter and wash to obtain the modified resin. Then, mix 10g of glucose and 0.5g of modified resin and dissolve them in 40mL, transfer them to a 100mL autoclave reactor, and react at 200°C for 6 hours. After the reaction is completed, filter and separate the solid product, and wash it three times with deionized water and anhydrous ethanol in sequence.
[0165] 2) Measure 100mL of furfuryl alcohol and pour it into a three-necked flask, stir in a water bath at 60°C for 10h, and the stirrer speed is 300rpm. Then add 10g of polyethylene glycol (molecular weight is 8000) thereto, continue stirring for 30min, and pour it into a beaker for use. The polyfurfuryl alcohol / polyethylene glycol (PFA / PEG) mixture precursor is mixed with NMP in a mass ratio of 1:20 to form a uniform and stable mixed solution, and then 10g of the solid product prepared in step 1) is added thereto, stirred at 60°C for 2h, the stirrer speed is 300rpm, and then stirred at 100°C for 4h until the solution is dried.
[0166] 3) Then, the solid dried in step 2) is transferred to a tube furnace for calcination, and the temperature is raised to 1100°C at a rate of 2°C / min, kept at this temperature for 2 hours, and then cooled to room temperature at a rate of 10°C / min. The calcined product is dissolved with hydrochloric acid to remove the metal catalyst, washed and dried, and then crushed through a 300-mesh sieve to obtain a negative electrode material.
[0167] Example 10
[0168] This embodiment provides a negative electrode material, which includes a carbon matrix (hard carbon), a pre-processed carbon film and an sp2 carbon layer, wherein the pre-processed carbon film is coated on the outer surface of the carbon matrix, and ultra-micro pores are opened on the pre-processed carbon film. The sp2 carbon layer is coated on the outer surface of the pre-processed carbon film.
[0169] The diameter of the ultramicropores is 0.4nm to 1nm, and the volume of the ultramicropores is 0.02cm 3 / g, the particle size of the carbon matrix is 6μm, the thickness of the pre-treated carbon film is 100nm, the mass ratio of the carbon matrix and the pre-treated carbon film is 100:10, the interlayer spacing of the sp2 carbon layer is 0.35nm, and the mass ratio of the pre-treated carbon film and the sp2 carbon layer is 5:1.
[0170] Comparative Example 1
[0171] This comparative example provides a negative electrode material, which is common hard carbon.
[0172] Comparative Example 2
[0173] This comparative example provides a negative electrode material, which is a microporous hard carbon material coated with an amorphous carbon layer.
[0174] The preparation method of the negative electrode material comprises the following steps:
[0175] 1) Take 5g of bamboo and place it in a tube furnace. In a 50mL / min nitrogen atmosphere, heat it to 800℃ at 5℃ / min, keep it warm for 2h, and cool it to room temperature to obtain bamboo charcoal powder; heat the bamboo charcoal powder to 1300℃ at 5℃ / min in a 50mL / min nitrogen atmosphere, keep it warm for 4h. After cooling to room temperature, hard carbon powder is obtained.
[0176] 2) Weigh 0.5g dopamine monomer and dissolve it in 50mL of 0.1mol / L sodium hydroxide-ethanol solution to obtain 10mg / mL DA dispersion. Perform polymerization reaction at 40°C at 90 rpm with stirring for 1h. Then transfer the reaction solution into a dialysis bag, place it in deionized water, and dialyze until the pH value of the liquid outside the bag is neutral; vacuum dry the material in the bag to obtain PDA nanoparticles with an average particle size of 1nm.
[0177] 3) Weigh 0.2g of hard carbon from step 1) and 0.3g of PDA nanoparticles from step 2), disperse them in 30mL of sodium bicarbonate buffer (0.1mol / L) containing hydrogen peroxide (H2O2, 1mg / mL), and react at 40°C at 120 rpm while stirring for 1h; separate the hard carbon with PDA in the pores from the dispersion of PDA nanoparticles by suction filtration and wash with deionized water. Transfer the hard carbon with PDA in the pores into a tubular furnace, heat it to 1100°C at 5°C / min in a nitrogen atmosphere, and keep it warm for 2h. Cool it to room temperature to obtain a microporous hard carbon material with an amorphous carbon layer on the surface.
[0178] Comparative Example 3
[0179] This comparative example provides a negative electrode material, which is a hard carbon material modified by 4A type molecular sieve.
[0180] The preparation method of the negative electrode material comprises the following steps:
[0181] First, the commercial 4A molecular sieve is sand-milled (the Na / Si molar ratio of 4A molecular sieve is about 1:1) to a particle size of 200 nanometers. Then, the commercial hard carbon and the sand-milled 4A molecular sieve are evenly mixed in a weight ratio of 100:1. The molecular sieve is uniformly, completely and conformally coated on the surface of the hard carbon particles by mechanical fusion. Finally, the mixture is heated at 400°C in argon for 3 hours to obtain a surface-modified hard carbon material.
[0182] The negative electrode material parameters provided by Examples 1 to 10 and Comparative Examples 1 to 3 are shown in Table 1:
[0183] Table 1 Negative electrode material parameters provided in Examples and Comparative Examples
[0184]
[0185]
[0186] In Table 1, parameter A is the diameter of the ultramicrochannel, parameter B is the volume of the ultramicrochannel, parameter C is the particle size of the carbon matrix, parameter D is the thickness of the pre-treated carbon film, parameter E is the mass ratio of the carbon matrix to the pre-treated carbon film, parameter F is the proportion of fluoride ions and sodium ions, parameter G is the interlayer spacing of the sp2 carbon layer, and parameter H is the mass ratio of the pre-treated carbon film to the sp2 carbon layer.
[0187] The negative electrode materials provided in the above-mentioned Examples 1 to 10 and the negative electrode materials provided in Comparative Examples 1 to 3 are respectively assembled into negative electrode sheets and sodium ion batteries according to the following methods:
[0188] Negative electrode sheet: The negative electrode material is mixed with carboxymethyl cellulose (CMC), SBR and SP in a mass ratio of 95.8:1.2:2:1, and the negative electrode slurry is obtained by ball milling. The negative electrode slurry is coated on the surface of copper foil, and vacuum dried at 110° C. overnight to obtain a negative electrode sheet;
[0189] Positive electrode: metal sodium sheet;
[0190] Electrolyte: Ethylene carbonate and ethyl methyl carbonate were mixed in a volume ratio of 3:7, and NaPF6 was added to form an electrolyte. The concentration of NaPF6 was 1 mol / L.
[0191] Diaphragm: polypropylene microporous diaphragm;
[0192] Sodium ion battery assembly: Assemble button-type sodium ion batteries in an inert atmosphere glove box in the order of negative electrode sheet-diaphragm-electrolyte-positive electrode sheet.
[0193] The electrochemical performance of each sodium ion battery assembled in the above sodium ion battery embodiment was tested as shown in Table 2, and the test results are shown in Table 2 below:
[0194] Table 2 Formation test results of the assembled batteries of the embodiments and comparative examples
[0195]
[0196]
[0197] From the test results of Examples 1 to 10 and Comparative Examples 1 to 3 in Table 1 and Table 2, it can be seen that the initial charge and discharge capacity, coulomb efficiency and cycle capacity retention rate of the negative electrode materials prepared in the examples are higher than those of the comparative examples; this indicates that the negative electrode materials provided by the present invention have better electrochemical properties than the existing ordinary hard carbon materials or the existing modified hard carbon materials. Fig.12 and Fig.13 It can be clearly seen from the first charge and discharge curve of the battery of Example 1 and the 100-cycle cycle capacity retention rate graph that the negative electrode material provided in Example 1 can reach more than 360mAh / g during the first charge and discharge process, far exceeding the ordinary hard carbon provided in Comparative Example 1; and the 100-cycle cycle capacity retention rate can also exceed 99%. It should be noted that Fig.13 The 100-cycle capacity retention rate of Example 1 provided is calculated from the second cycle of the battery after the first cycle of charge and discharge, and during the cycle from the 2nd cycle to the 100th cycle, the capacity retention rate of the battery is in the range of 99% to 100%, and the capacity retention rate is close to a straight line, indicating that the negative electrode material provided by the present invention has a stable ring capacity retention rate.
[0198] From the test results of Examples 1 to 3 in Tables 1 and 2, it can be seen that the initial charge and discharge capacity of the negative electrode material is positively correlated with the diameter and volume of the ultra-micropores, and the coulombic efficiency and cycle capacity retention rate are negatively correlated with the diameter and volume of the ultra-micropores. This is because the larger the volume of the ultra-micropores, the easier it is to accommodate positive electrode ions, but the larger diameter also causes organic solvent molecules to enter after multiple cycles, resulting in performance degradation. Therefore, the diameter and volume of the ultra-micropores of the negative electrode material need to be controlled within an appropriate range to avoid being too large or too small.
[0199] From the test results of Example 1, Example 4 and Example 5 in Table 1 and Table 2, it can be seen that the thickness of the pre-carbon film on the negative electrode material needs to be controlled within an appropriate range. Since the pre-carbon film is not the main ion storage material, a pre-carbon film that is too thick will lead to a decrease in the material's ion storage capacity (capacity decrease), while a pre-carbon film that is too thin will not have the corresponding effect and will also lead to a decrease in capacity. However, the thicker the pre-carbon film, the stronger its ability to inhibit the formation of the SEI film, so the higher the cycle capacity retention rate of the battery.
[0200] It can be seen from the test results of Example 1, Example 6 and Example 7 in Table 1 and Table 2 that by doping sodium ions and fluoride ions in the pre-treated carbon film, the electrochemical performance of the negative electrode material is more favorable, thereby improving the capacity and the first coulombic efficiency of the battery. However, it can be seen from the test results of Example 7 that the doping amount of sodium ions and fluoride ions needs to be controlled within a suitable range, otherwise the sodium ions and fluoride ions will affect the effect of the pre-treated carbon film.
[0201] From the test results of Example 1, Example 8-Example 10 in Table 1 and Table 2, it can be known that a sp2 carbon layer can be further added to the carbon matrix, and the sp2 carbon layer can improve the first coulomb efficiency and cycle retention rate of the battery, so that the sp2 carbon layer can improve the cycle stability of the negative electrode material. And it can be seen from Example 8 and Example 9 that different positions of the sp2 carbon layer (inside or outside the pre-processed carbon film) can improve the performance of the negative electrode material.
[0202] In the description of the embodiments of the present application, it should be noted that the orientation or positional relationship of terms such as "center", "up", "down", "left", "right", "vertical", "horizontal", "inside" and "outside" are based on the orientation or positional relationship described in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.
[0203] What is disclosed above is only a preferred embodiment of the present application, and it certainly cannot be used to limit the scope of rights of the present application. Ordinary technicians in this field can understand that all or part of the processes of implementing the above embodiment and equivalent changes made according to the claims of the present application are still within the scope covered by the present application.
Claims
1. A negative electrode material, characterized in that: The invention comprises a carbon matrix and a pre-processed carbon film, wherein the pre-processed carbon film is coated on the outer surface of the carbon matrix, and the pre-processed carbon film is provided with ultra-micro pores, and the ultra-micro pores are used for exchanging ions.
2. The negative electrode material according to claim 1, characterized in that The negative electrode material also includes an sp2 carbon layer, the pre-treated carbon film is coated on the outer surface of the carbon matrix, and the sp2 carbon layer is coated on the outer surface of the pre-treated carbon film; or, the sp2 carbon layer is coated on the outer surface of the carbon matrix, and the pre-treated carbon film is coated on the outer surface of the sp2 carbon layer.
3. The negative electrode material according to claim 2, characterized in that The density of the sp2 carbon layer is greater than or equal to 98%; and / or The thickness of the sp2 carbon layer is 10nm to 20nm; and / or The interlayer spacing of the sp2 carbon layer is 0.35nm to 0.4nm; and / or The mass ratio of the pre-treated carbon film to the sp2 carbon layer is (1-5):
1.
4. The negative electrode material according to claim 1, characterized in that Part of the surface layer of the carbon matrix is modified into sp2 hybridized carbon.
5. The negative electrode material according to claim 1, characterized in that The pre-treated carbon film is doped with fluorine ions and sodium ions, and at least a portion of the fluorine ions and the sodium ions are contained in the ultra-micro pores.
6. The negative electrode material according to any one of claims 1 to 5, characterized in that: The carbon matrix comprises hard carbon; and / or The diameter of the ultramicrochannel is 0.4nm to 1.2nm; and / or The volume of the ultra-microchannel is 0.01 cm 3 / g~0.05cm 3 / g; and / or The particle size D50 of the carbon matrix is 2 μm to 10 μm; and / or The thickness of the pre-carbon film is 10nm to 100nm; and / or The mass ratio of the carbon matrix to the pre-processed carbon film is 100:(1-10).
7. A method for preparing a negative electrode material, characterized in that: include: preparing a carbon matrix; Mixing a first carbon precursor with the carbon matrix so that the first carbon precursor is coated on the outer layer of the carbon matrix, and converting the first carbon precursor into a pre-carbon film after heat treatment; Wherein, the pre-treated carbon film is provided with ultra-micro pores, and the ultra-micro pores are used for exchanging ions.
8. The method for preparing the negative electrode material according to claim 7, characterized in that: The preparation method comprises: The carbon matrix is mixed with a second carbon precursor so that the second carbon precursor is coated on the outer surface of the carbon matrix, and the second carbon precursor is converted into an sp2 carbon layer after heat treatment; The carbon matrix coated with the sp2 carbon layer is mixed with the first carbon precursor so that the first carbon precursor is coated on the outer surface of the sp2 carbon layer.
9. A negative electrode plate, characterized in that: The invention comprises the negative electrode material as described in any one of claims 1 to 6, or the negative electrode material prepared by the method for preparing the negative electrode material as described in claim 7 or 8.
10. A secondary battery, characterized in that: It comprises a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode and the negative electrode are arranged in the electrolyte, and the negative electrode comprises the negative electrode sheet as claimed in claim 9.