Composite current collector and preparation method thereof, electrode, battery and battery application

By adding organic porous membrane layer and conductor to the current collector of the lithium battery to form a composite liquid collector, the thermal runaway problem of lithium battery in puncture conditions and high temperature environments is solved, and the safety and energy density of the battery are improved.

CN118970057APending Publication Date: 2024-11-15CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310542615.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Lithium batteries are prone to thermal runaway in abnormal environments such as puncture conditions and high temperatures, resulting in safety accidents. The existing technology mainly focuses on packaging quality and diaphragm improvements, and pays less attention to the improvement of current collectors to improve safety.

Method used

A composite fluid collection, including a metal matrix and an organic porous membrane layer, is used to fill the pores of the membrane layer to form a conductive bonding layer, enhancing structural stability and conductivity, and reducing the risk of thermal runaway.

Benefits of technology

Effectively reduce the risk of thermal runaway in puncture conditions and high temperature environments, improve the safety performance and energy density of the battery, and enhance structural stability and conductive properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970057A_ABST
    Figure CN118970057A_ABST
Patent Text Reader

Abstract

The invention discloses a composite current collector and a preparation method thereof, an electrode, a battery and battery application. The composite current collector provided by the embodiment of the invention comprises a metal matrix and an organic porous film layer. The organic porous film layer is attached to the surface of the metal base layer, pores of the organic porous film layer are filled with electric conductors, and the electric conductors are electrically connected with the surface of the metal base layer. The electrode and the battery both contain the composite current collector. According to the composite current collector, through compounding of the organic porous film layer and the metal matrix, the risk of thermal failure of the battery caused by factors such as a puncture working condition can be effectively reduced or relieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of batteries, and in particular to a composite current collector and a preparation method thereof, an electrode, a battery and battery applications. Background Art

[0002] Lithium-ion batteries have rapidly become popular in the fields of automotive power supply, 3C electronic products, and energy storage devices due to their high energy density and low self-discharge. As the application of lithium batteries becomes more and more popular, the safety of lithium batteries has received more and more attention, and the safety requirements have become higher and higher.

[0003] However, lithium batteries are prone to thermal runaway under electrical, thermal, and mechanical failures such as internal and external short circuits, overcharging, thermal abuse, and mechanical abuse, which can easily cause safety accidents. At present, in order to alleviate the thermal runaway of lithium batteries and reduce the hazards of safety accidents caused by them, the focus is on improving the quality of lithium battery packaging and improving the diaphragm and electrolyte. There are relatively few improvements to the current collector to alleviate the thermal runaway of lithium batteries and improve the safety of lithium batteries. Summary of the invention

[0004] In view of the above problems, the present application provides a composite current collector and a preparation method thereof, an electrode, a battery and applications thereof, which can effectively alleviate the risk of thermal runaway of the battery including that caused by puncture conditions to improve the safety of the lithium battery.

[0005] In a first aspect, an embodiment of the present application provides a composite current collector. The composite current collector of the embodiment of the present application includes:

[0006] A metal substrate having at least one surface;

[0007] The organic porous membrane layer is laminated on the surface of the metal substrate, and the pores of the organic porous membrane layer are filled with a conductor, and the conductor is electrically connected to the surface of the metal substrate.

[0008] The composite current collector in the embodiment of the present application can effectively reduce or alleviate the risk of thermal failure of the battery caused by factors such as puncture conditions, and improve the safety performance of the battery, by compounding the organic porous membrane layer and the metal matrix.

[0009] In some embodiments, the organic porous membrane layer includes at least one of the following (1) to (4):

[0010] (1) The thickness of the organic porous membrane layer laminated on the surface is 0.1 μm to 6 μm, and can be 0.5 μm to 3 μm;

[0011] (2) The porosity of the organic porous membrane layer is 40% to 95%, and can be 60% to 90%;

[0012] (3) The pores contained in the organic porous membrane layer have a pore size of 200 to 5000 nm, and can be optionally 500 nm to 2500 nm.

[0013] (4) The tensile strength of the organic porous membrane layer is higher than 50 MPa.

[0014] By further controlling the thickness, porosity and pore size of the organic porous membrane layer and the mechanical properties, the elastic deformation capacity and resistance to physical puncture of the composite current collector can be further improved, so as to further reduce or alleviate the thermal failure of the battery. At the same time, the stability of the composite current collector in the processing or application process of the embodiment of the application is improved.

[0015] In some embodiments, the material of the organic porous membrane layer includes at least one of ethylene, polyimide, polypropylene, and polytetrafluoroethylene. The membrane layers of these materials have good mechanical properties such as elastic deformation capacity, which can further reduce or alleviate factors such as physical puncture or high temperature that cause thermal runaway of the battery, and further improve the mechanical properties of the composite current collector of the embodiment of the present application.

[0016] In some embodiments, the material of the conductor includes a conductive adhesive.

[0017] In some embodiments, the conductor is filled in the pores to a depth of 4 / 5 to 5 / 5 of the thickness of the organic porous membrane layer.

[0018] In some embodiments, the organic porous membrane layer is bonded to the surface of the metal base layer via a conductive adhesive layer.

[0019] In some embodiments, the thickness of the conductive adhesive layer is 0.05 μm to 1 μm, and may be 0.1 μm to 0.5 μm; and / or

[0020] In some embodiments, the conductor is formed by extending from the surface of the conductive adhesive layer into the pores of the organic porous membrane layer.

[0021] In the embodiment, the electrical conductivity of the conductor is 10 3 S / m~6×10 7 S / m.

[0022] In the embodiment, the conductivity of the conductive adhesive layer is 10 3 S / m~10 4 S / m.

[0023] By selecting the conductive material as a conductive adhesive and controlling its conductivity, the conductivity of the composite current collector of the embodiment of the present application can be effectively improved and the internal resistance can be reduced. By adding a conductive adhesive layer between the organic porous film layer and the metal base layer and controlling the conductivity of the conductive adhesive layer, the structural strength of the composite current collector of the embodiment of the present application can be effectively enhanced and the conductivity can be improved.

[0024] In some embodiments, the metal substrate is a metal film layer having two surfaces arranged opposite to each other, and the two surfaces are both provided with the organic porous film layer. The organic porous film layer is added to the two surfaces of the metal film layer, which can further reduce the risk of thermal failure caused by environments including puncture conditions, high temperature thermal anomalies, etc.

[0025] In some embodiments, the metal substrate is a metal film layer, and the thickness of the metal film layer is 4 μm to 15 μm, and can be 6 μm to 12 μm. The metal film layer and the organic porous film layer of this thickness can improve the mechanical properties of the composite current collector and can effectively reduce the weight of the composite current collector.

[0026] In some embodiments, the total thickness of the composite current collector is 6 μm to 18 μm, and can be 8 μm to 14 μm.

[0027] In some embodiments, the sheet resistance of the composite current collector is greater than 0, less than or equal to 5Ω, and can be selected to be 0.005Ω to 1Ω.

[0028] The composite current collector of this thickness can effectively reduce or alleviate the risk of thermal runaway of the battery caused by physical puncture or high temperature, and has a stable structure and stable processing and operation. At the same time, it gives the composite current collector of the embodiment of the present application good conductivity.

[0029] In a second aspect, the present invention also provides a method for preparing a composite current collector. The method for preparing a composite current collector in the present invention comprises the following steps:

[0030] Providing a metal substrate and an organic porous membrane, wherein the metal substrate has at least one surface;

[0031] The organic porous membrane is attached to the surface of the metal substrate, and at the same time, a conductor is filled in the pores of the organic porous membrane, and the conductor is electrically connected to the surface of the metal substrate to form a composite current collector.

[0032] The composite current collector prepared by the preparation method of the composite current collector of the embodiment of the present application contains an organic porous film layer, which can be hot-melted to form a closed film layer when elastic deformation and abnormal environment such as high temperature occur in the puncture working condition, thereby relieving or preventing the chemical reaction inside the battery from continuing, thereby effectively reducing or relieving the thermal failure of the battery and improving the safety performance of the battery. In addition, the prepared composite current collector has excellent conductive properties and a stable structure.

[0033] In some embodiments, the method of attaching the organic porous membrane to the surface of the metal substrate comprises the following steps:

[0034] forming a conductive adhesive wet coating on the surface of the organic porous membrane and / or the surface of the metal substrate;

[0035] Laminating the organic porous membrane to the surface of the metal substrate, and allowing the formed conductive adhesive wet coating to be disposed between the organic porous membrane and the metal substrate to form a composite current collector blank;

[0036] The composite current collector blank is subjected to a pressing process, and the conductive adhesive part in the conductive adhesive wet coating is squeezed into the pores contained in the organic porous membrane, and then a drying process is performed.

[0037] This method can form a conductive bonding layer between the organic porous film and the metal substrate, and can form a conductor in the organic porous film, thereby enhancing the stability of the prepared composite current collector structure and the good conductivity.

[0038] In an embodiment, the pressing process includes first performing a first pressing process and then performing a second pressing process; wherein the pressure of the first pressing process is less than the pressure of the second pressing process.

[0039] In an embodiment, the first lamination process comprises a roller pressing process, and a surface of a pressing roller in the roller pressing process has a convex-concave structure.

[0040] In the embodiment, the pressure of the second pressing process is 0.5 MPa to 5 MPa, and can be optionally 1 MPa to 3 MPa.

[0041] In an embodiment, the second lamination process is performed more than twice.

[0042] The lamination treatment method and conditions can improve the uniformity of the conductive adhesive layer and the ability of the conductor to be fully filled in the pores of the organic porous film, thereby enhancing the structural stability and conductivity of the prepared composite current collector.

[0043] In a third aspect, the present application also provides an electrode. The present application embodiment electrode comprises a current collector and an active layer combined with the current collector, wherein the current collector comprises the composite current collector of the above application embodiment or a composite current collector prepared by the composite current collector preparation method of the above application embodiment.

[0044] The battery thermal failure caused by the electrode in the embodiment of the present application in the puncture condition and / or abnormal high temperature environment is significantly reduced, and the electrode has excellent conductivity. Or further has high energy density and stable structure.

[0045] In some embodiments, the electrode is at least one of a positive electrode and a negative electrode.

[0046] In a fourth aspect, the present application also provides a battery. The battery of the present application comprises an electrode, which is the electrode of the above-mentioned application.

[0047] The battery of the embodiment of the present application can significantly reduce or alleviate the occurrence of thermal runaway under abnormal conditions such as puncture conditions or high temperatures, or reduce the harm caused by thermal runaway, thereby effectively improving the safety performance of the battery of the embodiment of the present application. In addition, since the electrode structure of the above-mentioned text application is firm and stable, the cycle performance of the battery of the embodiment of the present application is significantly improved.

[0048] In some embodiments, the battery includes any one of a battery cell, a battery module, and a battery pack.

[0049] In a fifth aspect, the embodiments of the present application also provide an electric device. The electric device of the embodiments of the present application includes a power supply unit or an energy storage unit, and the power supply unit or energy storage unit contains a battery, and the battery includes the battery of the above embodiments of the present application. The power supply unit or energy storage unit of the electric device of the embodiments of the present application has high safety and long service life, and the electric device of the embodiments of the present application has a long standby or battery life.

[0050] In a sixth aspect, the present application also provides an energy storage device, including an energy storage unit, wherein the energy storage unit contains a battery, wherein the battery includes the battery of the above-mentioned application embodiment. The energy storage device has high safety, long service life, and further high energy density.

[0051] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the drawings:

[0053] Figure 1 This is a schematic diagram of the structure of the composite current collector in some embodiments of the present application;

[0054] Figure 2 Schematic diagrams of the structures of composite current collectors in other embodiments of the present application;

[0055] Figure 3 This is a schematic structural diagram of an implementation of a battery cell according to an embodiment of the present application;

[0056] Figure 4 for Figure 3 An exploded schematic diagram of the battery cell shown;

[0057] Figure 5 This is a schematic structural diagram of an implementation scheme of a battery module according to an embodiment of the present application;

[0058] Figure 6 This is a schematic structural diagram of an implementation scheme of a battery pack according to an embodiment of the present application;

[0059] Figure 7 for Figure 6 A schematic diagram of the exploded structure of the battery pack shown;

[0060] Figure 8 A schematic diagram of an embodiment of an electrical device including a battery according to an embodiment of the present application as a power source;

[0061] The reference numerals in the specific implementation manner are as follows:

[0062] 1-metal substrate, 2-organic porous membrane layer, 3-conductor, 4-conductive bonding layer;

[0063] 30-battery cell, 31-housing, 32-electrode assembly, 33-cover plate;

[0064] 40-battery module;

[0065] 50-battery pack, 51-box, 52-lower box. DETAILED DESCRIPTION

[0066] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0067] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0068] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0069] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0070] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0071] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0072] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.

[0073] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.

[0074] At present, from the perspective of market development, the application of power batteries is becoming more and more extensive. Power batteries are not only used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, but also widely used in electric vehicles such as electric bicycles, electric motorcycles, electric vehicles, as well as military equipment and aerospace and other fields. With the continuous expansion of the application field of power batteries, the market demand is also constantly expanding. Lithium-ion batteries have rapidly become popular in the fields of automotive power supplies, 3C electronic products and energy storage devices due to their advantages such as high energy density and low self-discharge. With the popularization of lithium batteries, the safety of lithium batteries has received more and more attention, and the safety requirements are getting higher and higher.

[0075] Based on the current structure of lithium batteries, lithium batteries are prone to thermal runaway under electrical, thermal, and mechanical failures such as internal and external short circuits, overcharging, thermal abuse, and mechanical abuse, which can easily cause safety accidents. Existing measures to improve the safety of the battery body are mainly focused on improving the lithium battery packaging process, electrolyte, and diaphragm, such as providing lithium battery packaging technology, adding flame retardants to the electrolyte, and improving the diaphragm to reduce lithium battery thermal runaway and the hazards it causes. However, improving the lithium battery packaging process involves upgrading the production system and equipment, and the improvement of flame retardants and diaphragms will affect the energy density of the battery.

[0076] In order to effectively reduce the thermal runaway of lithium batteries and the hazards caused by them, and improve the safety performance of lithium batteries, it has been found through research that the creative addition of an organic porous membrane layer on the surface of the current collector can effectively reduce or delay the risk of thermal runaway of the battery, including puncture conditions, thereby improving the safety performance of the battery. Based on this, the following technical solutions are proposed in the embodiments of the present application.

[0077] Composite current collector

[0078] In a first aspect, the embodiments of the present application provide a composite current collector. In some embodiments, the structure of the composite current collector of the embodiments of the present application is as follows: Figure 1 to Figure 2As shown, it comprises a metal substrate 1 and an organic porous membrane layer 2. The metal substrate 1 has at least one surface; the organic porous membrane layer 2 is laminated on the surface of the metal substrate 1, and the pores of the organic porous membrane layer 2 are filled with a conductor 3, and the conductor 3 is electrically connected to the surface of the metal substrate 1.

[0079] In the composite current collector of the embodiment of the present application, the metal substrate 1 constitutes the support layer of the organic porous film layer 2, which should be conductive, such as the metal material of the current collector. The surface bonding arrangement of the organic porous film layer 2 and the metal substrate 1 refers to that one surface of the organic porous film layer 2 is bonded to the surface of the metal substrate 1, so that the organic porous film layer 2 is stacked on the surface of the metal substrate 1. The organic porous film layer 2 refers to an organic film containing pores. The conductor 3 refers to a component with conductive properties, which is filled in the pores of the organic porous film layer 2 to form a conductive path in the organic porous film layer 2, which is used to collect the charge of the electrode active layer and transfer it to the metal substrate 1.

[0080] The composite current collector of the embodiment of the present application is provided with an organic porous film layer 2 attached to the surface of the metal substrate 1. In the normal working environment of the battery, the charge of the electrode active layer can be collected by the conductor 3 filled in the pores of the organic porous film layer 2, and transferred and converged to the metal substrate 1. When the composite current collector of the embodiment of the present application is in a puncture condition, the organic porous film layer 2 has elastic deformation ability, and the organic porous film layer 2 can effectively deform to significantly reduce or alleviate the physical puncture and cause a short circuit inside the battery; in an abnormal temperature such as a high temperature environment, the organic porous film layer 2 can also be hot-melted to form a closed film layer, thereby reducing or relieving the chemical reaction that continues inside the battery. Therefore, the composite current collector of the embodiment of the present application can effectively reduce or alleviate the thermal failure of the battery and improve the safety performance of the battery through the compounding of the organic porous film layer 2 and the metal substrate 1.

[0081] In the embodiment, the metal substrate 1 may have one surface or two surfaces arranged opposite to each other. When the metal substrate 1 has two surfaces arranged opposite to each other, the metal substrate 1 may be a metal film layer. The surface of the metal substrate 1 refers to the surface for attaching the organic porous film layer 2. When the metal substrate 1 has two surfaces arranged opposite to each other, the organic porous film layer 2 may be attached to only one of the surfaces, such as Figure 1 Of course, the organic porous membrane layer 2 can also be attached to the two surfaces arranged opposite to each other, such as Figure 2 When the composite current collector of the present application embodiment is as follows Figure 2 When the organic porous membrane layer 2 is respectively attached to two opposite surfaces of the metal substrate 1, an electrode active layer can be provided on the surfaces of the two organic porous membrane layers 2 facing away from the metal substrate 1, thereby increasing the energy density of the battery.

[0082] Regardless of the composite current collector of the present application embodiment Figure 1 The structure shown is Figure 2 As shown in the structure, since the composite current collector of the embodiment of the present application contains an organic porous film layer 2, and the pores of the organic porous film layer 2 are filled with a conductor 3 electrically connected to the surface of the metal substrate 1. Therefore, in some embodiments, the thickness of the metal substrate 1 can be significantly thinner than the thickness of the conventional current collector. For example, in the embodiment, the metal substrate 1 is a metal film layer. In this case, the thickness of the metal film layer is set as follows: Figure 1 The d1 shown in the figure can be 4-15μm, and can further be 6-12μm. In the examples, the thickness can be 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, etc., which are typical but not limiting.

[0083] Taking the existing conventional current collector aluminum foil as 10μm and copper foil as 6μm, the existing conventional current collector accounts for about 7% and 9% of the mass in the battery core; this is because if the thickness of the existing conventional current collector is reduced, the tensile strength will be reduced, which will affect the coating thickness and significantly increase the incidence of the problem of broken bands. In the composite current collector of the embodiment of the present application, due to the presence of the organic porous film layer 2 contained in the composite current collector, the thickness of the metal matrix 1 contained therein can be significantly reduced. In this way, on the basis of effectively playing the role of the composite current collector of the embodiment of the present application in reducing or alleviating the risk of thermal runaway of the battery, the thickness of the metal matrix 1 can be effectively reduced, and the weight of the composite current collector of the embodiment of the present application can be effectively reduced, thereby significantly improving the energy density of the battery. Moreover, due to the mechanical properties such as toughness of the organic porous film layer 2, even if the thickness of the metal matrix 1 is reduced, it will not cause undesirable phenomena such as broken bands during its processing or application.

[0084] In the exemplary embodiment, the material of the metal substrate 1 can be a metal material with good conductivity, such as a commonly used positive electrode current collector metal material, such as aluminum; or a commonly used negative electrode current collector metal material, such as copper.

[0085] In order to improve the role of the organic porous film layer 2 in the composite current collector of the embodiment of the present application, further reduce the risk of thermal failure caused by puncture conditions, high temperature thermal anomalies and other environments, and improve the safety performance of the battery, in some embodiments, the organic porous film layer 2 has at least one or more of the following properties:

[0086] As in the embodiment, the thickness of the organic porous membrane layer 2 attached to one surface of the metal substrate 1 is set as follows: Figure 1As shown in d2, the d2 is 0.1 μm to 6 μm, and can be 0.5 μm to 3 μm. In the exemplary embodiment, the thickness of the organic porous membrane layer 2 may include a typical but not limited thickness range of 0.1 μm to 0.5 μm, 0.5 μm to 1 μm, 1 μm to 2 μm, 2 μm to 3 μm, 3 μm to 4 μm, 4 μm to 5 μm, 5 μm to 6 μm, etc. Among them, the thickness of the organic porous membrane layer 2 refers to Figure 1 The distance from one surface to the other surface of the organic porous membrane layer 2 is shown in . By adjusting the thickness of the organic porous membrane layer 2, such as controlling it within this thickness range, it has good elastic deformation ability, thereby significantly reducing or alleviating the thermal runaway of the battery caused by factors such as physical puncture or high temperature, and can also improve the mechanical properties of the composite current collector of the embodiment of the present application, reduce or avoid the occurrence of undesirable phenomena such as broken bands during its processing or application.

[0087] In the embodiment, the porosity of the organic porous membrane layer 2 may be 40% to 95%, and may be 60% to 90%. The porosity of the organic porous base membrane 11 may include a typical but non-exclusive porosity range of 40% to 45%, 45% to 50%, 50% to 55%, 55% to 60%, 60% to 65%, 65% to 70%, 70% to 75%, 75% to 80%, 80% to 85%, 85% to 90%, 90% to 95%, etc. Among them, the porosity refers to the percentage of the pore volume contained in the organic porous membrane layer 2 per unit volume.

[0088] In the embodiment, the pores contained in the organic porous membrane layer 2 have a pore size of 200 to 5000 nm, and can be optionally 500 nm to 2500 nm. In the exemplary embodiment, the pore size of the organic porous membrane layer 2 may include typical but not exclusive limiting pore size ranges such as 200 nm to 500 nm, 500 nm to 1000 nm, 1000 nm to 1500 nm, 1500 nm to 2000 nm, 2000 nm to 2500 nm, 2500 nm to 3000 nm, 3000 nm to 3500 nm, 3500 nm to 4000 nm, 4000 nm to 4500 nm, and 4500 nm to 5000 nm.

[0089] By continuing to select and control the porosity and pore size of the organic porous film layer 2, if controlled within the above range, the elastic deformation capacity of the organic porous film layer 2 can be further improved, that is, the elastic deformation capacity and other mechanical properties of the composite current collector of the embodiment of the present application can be further improved, thereby further reducing or alleviating factors such as physical puncture or high temperature that cause thermal runaway of the battery, improving battery safety, and further improving the stability of the composite current collector of the embodiment of the present application during processing or application. In addition, the porosity in the above range can also adjust the amount and morphology of the conductor 3 filled in the pores of the organic porous film layer 2, thereby improving the overall conductivity of the composite current collector of the embodiment of the present application.

[0090] In the embodiment, the organic porous membrane layer 2 has the following mechanical properties: a tensile strength higher than 50 MPa.

[0091] The organic porous membrane layer 2 with such mechanical properties has good elastic deformation ability and the ability to resist puncture by physical factors, so as to further reduce or alleviate the thermal failure of the battery, and at the same time improve the stability of the composite current collector in the processing or application process of the embodiment of the present application.

[0092] In the embodiments, the organic porous membrane layer 2 in the above embodiments can be an organic straight pore membrane. Among them, the straight pore membrane is a through hole in the membrane layer from one surface of the membrane layer to the other surface. In this way, the conductor 3 filled in the pores of the organic porous membrane layer 2 can be effectively filled in the pores, and one end can be electrically connected to the surface of the metal substrate 1, and the other end extends to the surface of the organic porous membrane layer 2 away from the metal substrate 1, so as to be electrically connected to the electrode active layer bonded to the surface of the organic porous membrane layer 2, thereby reducing the resistance of the contact interface between the electrode active layer and the composite current collector of the embodiment of the present application.

[0093] In the exemplary embodiments, the material of the organic porous film layer 2 in the above-mentioned embodiments may include at least one of polyethylene (PE), polyimide (PI), polypropylene (PP), and polytetrafluoroethylene (PTFE). For example, it may be any organic porous film of PE porous film, PI porous film, PP porous film, PTFE porous film, etc., and it may be a composite porous film in which two or more film layers are stacked. Of course, it may also be a porous film formed by a mixture of these materials. The film layers of these materials have good mechanical properties such as elastic deformation ability, which can further reduce or alleviate factors such as physical puncture or high temperature that cause thermal runaway of the battery, and further improve the mechanical properties of the composite current collector of the embodiment of the present application, and improve its stability during processing or application.

[0094] The conductor 3 contained in the composite current collector of the embodiment of the present application, specifically the conductor 3 filled in the pores of the organic porous membrane layer 2 in the above-mentioned embodiments, plays a conductive role, and is electrically connected to the surface of the metal substrate 1 that is bonded to the organic porous membrane layer 2. When the electrode active layer is bonded to the surface of the organic porous membrane layer 2, the conductor 3 is electrically connected to the electrode active layer. Therefore, at this time, the conductor 3 plays a role in electrically connecting the electrode active layer and the metal substrate 1 in the organic porous membrane layer 2, so that the charge of the electrode active layer can be effectively transferred to the metal substrate 1.

[0095] In some embodiments, the electrical conductivity of the conductor 3 is 10 3 S / m~6×10 7 S / m, optional 10 3 S / m~10 4 S / m or 3×10 7 S / m~6×10 7 S / m, the higher the conductivity of the conductor 3, the better. When the conductor 3 is formed by extending and filling the pores of the conductive adhesive layer 4 below into the organic porous membrane layer 2, the conductivity of the conductor 3 can be the same as or close to the conductivity of the conductive adhesive layer 4 below. When the conductor 13 contains a high-conductivity material, such as a metal filler, the conductivity of the conductor 3 will increase, such as up to 3×10 7 S / m~6×10 7 S / m, or greater than 6×10 7 The conductor 3 within this range has good conductivity and low internal resistance, and can effectively collect the charges in the electrode active layer and transfer them to the metal substrate 1, thereby improving the conductivity of the composite current collector of the embodiment of the present application and reducing the internal resistance of the battery.

[0096] In some embodiments, the depth of the conductor 3 filled in the pores of the organic porous membrane layer 2 is 4 / 5 to 5 / 5 of the thickness of the organic porous membrane layer 2. In the exemplary embodiment, the ratio may include 4 to 4.2:5, 4.2 to 4.5:5, 4.5 to 4.8:5, 4.8 to 5:5, etc., which are typical but not limited. By controlling the filling depth of the conductor 3, the electrical contact between the composite current collector and the electrode active layer of the embodiment of the present application can be enhanced, and the internal resistance of the electrode can be reduced.

[0097] In some embodiments, the material of the conductor 3 may include a conductive adhesive. The conductive adhesive has good mechanical properties such as good elasticity on the basis of good electrical conductivity, can be bonded with the organic porous film layer 2 to form a whole, enhance the mechanical energy such as elastic deformation capacity of the organic porous film layer 2, and can further reduce or alleviate factors such as physical puncture or high temperature that cause thermal runaway of the battery. Moreover, the electrical connection with the surface of the metal substrate 1 is stable, which improves the processing and working stability of the composite current collector. Of course, other materials with conductive properties can also be used, as long as they can cooperate with the organic porous film layer 2 to have good elasticity and a conductive material with a stable electrical connection with the surface of the metal substrate 1, they are all within the scope disclosed in the embodiments of this application.

[0098] In some embodiments, Figure 1 and Figure 2 As shown, the organic porous film layer 2 in the above-mentioned embodiments is bonded to the surface of the metal base layer 1 through the conductive adhesive layer 4. The organic porous film layer 2 and the metal base layer 1 are bonded by the conductive adhesive layer 4, which effectively enhances the stability of the composite current collector structure of the embodiment of the present application; more importantly, the conductive adhesive layer 4 also has good elasticity, which can cooperate with the elasticity of the organic porous film layer 2 to enhance the elastic deformation capacity and other mechanical properties of the organic layer composed of the organic porous film layer 2 and the conductive adhesive layer 4, so as to further reduce or alleviate the thermal runaway of the battery caused by factors such as physical puncture or high temperature; at the same time, the conductive adhesive layer 4 also has good conductivity, which can collect the charge in the electrode active layer of the conductor 3 and finally transfer it to the metal substrate 1, thereby improving the conductive performance of the composite current collector of the embodiment of the present application and reducing the internal resistance of the battery.

[0099] In the embodiment, the thickness of the conductive adhesive layer 4 is as follows: Figure 1 and Figure 2 As shown, the single-layer conductive adhesive layer 4 is configured as follows Figure 1 The d3 shown in the figure can be 0.05μm to 1μm, and can be 0.1μm to 0.5μm. In the exemplary embodiment, it can be 0.05μm to 0.1μm, 0.1μm to 0.3μm, 0.3μm to 0.5μm, 0.5μm to 0.7μm, 0.7μm to 0.9μm, 0.9μm to 1μm, etc. Typical but not the only limited thickness range. Controlling the thickness of the conductive adhesive layer 4 within the range can effectively enhance the bonding strength between the conductive adhesive layer 4 and the surface of the metal substrate 1, and can further enhance the mechanical properties such as the elastic deformation capacity of the organic layer composed of the organic porous membrane layer 2 and the conductive adhesive layer 4, so as to further reduce or alleviate the thermal runaway of the battery caused by factors such as physical puncture or high temperature; and reduce the resistance of the composite current collector.

[0100] In some embodiments, the conductivity of the conductive adhesive layer 4 may be 10 3 S / m~10 4S / m, the higher the conductivity of the conductive adhesive layer 2, the better. For example, by selecting the material of the conductive adhesive layer 4, its conductivity can also be greater than 10 4 The conductive adhesive layer 4 within this range has good conductivity and low internal resistance, which improves the conductivity of the composite current collector in the embodiment of the present application and reduces the internal resistance of the battery.

[0101] When the conductor 3 filled in the pores of the organic porous membrane layer 2 contains a conductive binder, the conductive binder contained in the conductive adhesive layer 4 may be the same as the conductive binder of the conductor 3, or may be different.

[0102] In the embodiment, the conductive adhesive contained in the conductor 3 and the conductive adhesive contained in the conductive adhesive layer 4 may be the same or different, including an adhesive base and a conductive filler dispersed in the adhesive base. Wherein, the adhesive base may be a commonly used adhesive in the battery field, such as but not limited to at least one of polyimide (Polyimide, abbreviated as PI), polyamide (Polyamide, PA), polypropylene, and polyvinylidene fluoride (PVDF). The conductive agent may include but is not limited to at least one of conductive carbon black conductive agent (SP), Ketjen black, carbon nanotubes (CNT), graphene, etc. Wherein, the amount of the conductive agent added can make the conductivity of the conductive adhesive layer 4 and the conductor 3 within the above range. Of course, if the adhesive base itself has good conductivity, the content of the conductive agent can also be controlled to 0, that is, the conductive agent can be added.

[0103] In the embodiment, when the conductive binder contained in the conductor 3 is the same as the conductive binder contained in the conductive adhesive layer 4 , the conductor 3 may be formed by extending from the surface of the conductive adhesive layer 4 into the pores of the organic porous membrane layer 2 .

[0104] Based on the metal base layer 1, organic porous film layer 2 and conductor 3 contained in the composite current collector of the above-mentioned embodiments, or the conductive adhesive layer 4 further contained, in some embodiments, the total thickness of the composite current collector of the present application embodiment can be 6μm to 18μm, and can be 8μm to 14μm. In the exemplary embodiment, the total thickness of the composite current collector can include typical but not limited thickness ranges such as 6μm to 8μm, 8μm to 10μm, 10μm to 12μm, 12μm to 14μm, 14μm to 16μm, and 16μm to 18μm. Among them, the total thickness of the composite current collector is the distance from one surface of the current collector to the other surface, such as Figure 1 As shown in d1+d2+d3; Figure 2 The sum of the thicknesses of the two organic porous membrane layers 2, the metal base layer 1, and the two conductive adhesive layers 4 shown.

[0105] The composite current collector of this thickness can effectively reduce or alleviate the risk of thermal runaway of the battery caused by factors such as physical puncture or high temperature, and the structure is stable, and its processing and operation are stable. At the same time, the composite current collector of the embodiment of the present application is endowed with good conductivity and low internal resistance. For example, in some embodiments, the diaphragm resistance of the composite current collector of the embodiment of the present application can be greater than 0, less than or equal to 5Ω, and can be selected as 0.005Ω~1Ω. In the exemplary embodiment, the composite current collector has a typical but not exclusive diaphragm resistance range of 0.001Ω~0.005Ω, 0.005Ω~0.01Ω, 0.01Ω~0.05Ω, 0.05Ω~0.1Ω, 0.1Ω~1Ω, 1Ω~2Ω, 2Ω~3Ω, 3Ω~4Ω, 4Ω~5Ω, etc. Among them, the diaphragm resistance refers to the resistance value measured along the thickness direction of the composite current collector.

[0106] Preparation method of composite current collector

[0107] In a second aspect, the present invention also provides a method for preparing a composite current collector, comprising the following steps:

[0108] S10: providing a metal substrate and an organic porous membrane, wherein the metal substrate has at least one surface;

[0109] S20: laminating the organic porous membrane on the surface of the metal substrate, and simultaneously filling the pores of the organic porous membrane with a conductor, and making the conductor electrically connected to the surface of the metal substrate to form a composite current collector.

[0110] Step S10:

[0111] The metal substrate in step S10 may be Figure 1 and Figure 2 The metal substrate 1 contained in the composite current collector of the above application example is shown, then, the metal substrate can have one surface, or can be a metal film layer, that is, has two surfaces arranged oppositely. Similarly, the organic porous membrane can be the organic porous membrane layer 2 contained in the composite current collector of the above application example.

[0112] Step S20:

[0113] The conductor filled in the pores of the organic porous film constitutes the conductor 3 contained in the composite current collector of the above embodiment of the application. Therefore, the conductor is electrically connected to the surface of the metal substrate.

[0114] Therefore, the composite current collector prepared by the preparation method of the composite current collector of the embodiment of the present application contains an organic porous film layer, which can undergo elastic deformation during puncture conditions to significantly reduce or alleviate the physical puncture and cause short circuits inside the battery; at the same time, in abnormal environments such as high temperature, the organic porous film layer can also be hot-melted to form a closed film layer to alleviate or prevent the chemical reaction inside the battery from continuing; therefore, the composite current collector of the embodiment of the present application can effectively reduce or alleviate battery thermal failure and improve the safety performance of the battery. In addition, the conductor filled in the pores of the organic porous film and the metal matrix construct a conductive system in the composite current collector, giving the composite current collector excellent conductive properties and low internal resistance. Secondly, the process conditions of the preparation method of the composite current collector of the embodiment of the present application are controllable, which can ensure the stability of the quality and other properties of the prepared composite current collector.

[0115] In some embodiments, the method of laminating the organic porous membrane on the surface of the metal substrate in step S20 may include the following steps:

[0116] S21: first forming a conductive adhesive wet coating on the surface of at least one of the organic porous film and the metal substrate;

[0117] S22: laminating the organic porous membrane to the surface of the metal substrate, and allowing the formed conductive adhesive wet coating to be disposed between the organic porous membrane and the metal substrate to form a composite current collector blank;

[0118] S23: pressing the composite current collector blank, and squeezing the conductive adhesive part in the conductive adhesive wet coating into the pores contained in the organic porous membrane, and then drying it.

[0119] Wherein, the conductive adhesive wet coating formed in step S21 can be formed only on the surface of the organic porous film, can be formed only on the surface of the metal substrate, or can be formed on the surfaces of the organic porous film and the metal substrate at the same time. It should be understood that the formation of the conductive adhesive wet coating on the surface of the organic porous film and / or the metal substrate is combined with the formation of the conductive adhesive wet coating on the surface where the organic porous film and the metal substrate are attached to achieve the bonding of the organic porous film and the metal substrate.

[0120] In addition, the thickness of the conductive adhesive wet coating formed should at least ensure that during the pressing process in step 23, the conductive adhesive wet coating is partially squeezed into the pores of the organic porous membrane, and a conductive adhesive layer is formed between the surfaces of the organic porous membrane and the metal substrate. The thickness of the conductive adhesive layer can be the thickness of the conductive adhesive layer 4 contained in the composite current collector in the above-mentioned application embodiment.

[0121] The surface bonding of the organic porous membrane and the metal substrate in step S22 should be carried out according to the following steps: Figure 1 or Figure 2The bonding sequence shown enables the organic porous film to be bonded to one surface or two oppositely disposed surfaces of the metal substrate.

[0122] The pressing treatment in step S23 is to enhance the bonding strength between the organic porous membrane and the metal substrate and enhance the bonding stability between the two. At the same time, during the pressing process, the conductive adhesive wet coating disposed between the organic porous membrane and the metal substrate is squeezed by pressure, so that part of the conductive adhesive wet coating enters along the pores of the organic porous membrane and fills the pores, and the remaining conductive adhesive wet coating remains between the organic porous membrane and the metal substrate.

[0123] The lamination process refers to applying pressure on the surface of the organic porous membrane and / or the metal substrate. In an embodiment, the lamination process includes the steps of first performing a first lamination process and then performing a second lamination process; wherein the pressure of the first lamination process is less than the pressure of the second lamination process.

[0124] In this way, the first lamination process plays the role of initial lamination, which can ensure that the organic porous film and the metal substrate are fitted to meet the position requirements, and can reduce the obvious displacement of the conductive adhesive wet coating during the lamination process, thereby enhancing the conductive adhesive wet coating to maintain a relatively uniform distribution during the lamination process. In the embodiment, the first lamination process includes a roller pressing process, and the roller surface of the roller pressing process has a convex-concave structure. By setting a convex-concave structure on the roller surface, the conductive adhesive in the conductive adhesive wet coating can be partially squeezed to the concave structure of the roller surface under the action of pressure during the first lamination process. In this way, after the first lamination process, the uniformity of the conductive adhesive wet coating distributed between the organic porous film and the metal substrate interface can be significantly improved, and the conductive adhesive wet coating can be significantly displaced as the roller is advanced by rolling the roller with a smooth surface. Of course, the conductive adhesive part in the conductive adhesive wet coating can also be filled into the pores along the pores of the organic porous film. At the same time, the roller can achieve continuous operation and improve the efficiency of lamination. Based on the purpose of the first pressing process, the pressure of the first pressing process only needs to be able to effectively ensure that the wet coating of the conductive adhesive is relatively evenly distributed.

[0125] The second pressing process is to make the organic porous membrane and the metal substrate fit closely, enhance the strength and stability of the bonding between the two, and at the same time allow part of the conductive adhesive in the conductive adhesive wet coating to continue to be squeezed into the pores of the organic porous membrane to form a conductor.

[0126] In an embodiment, the pressure of the second pressing treatment may be 0.5 MPa to 5 MPa, and may be optionally 1 MPa to 3 MPa. In a demonstrative example, the pressure of the second pressing treatment may include typical but not exclusive pressure ranges such as 0.5 MPa to 1.5 MPa, 1.5 MPa to 2 MPa, 2 MPa to 2.5 MPa, 2.5 MPa to 3 MPa, 3 MPa to 3.5 MPa, 3.5 MPa to 4 MPa, 4 MPa to 4.5 MPa, and 4 MPa.5 to 5 MPa.

[0127] By selectively controlling the pressure of the second pressing treatment, the bonding strength between the organic porous membrane and the metal substrate can be effectively enhanced, the structure and quality stability of the prepared composite current collector can be improved, and it can be effectively ensured that the pores of the organic porous membrane are filled with a conductive binder to form a conductor.

[0128] In an embodiment, the second pressing treatment may be performed multiple times, such as more than twice. In a demonstration example, the second pressing treatment may be performed 2 to 5 times, so that the bonding strength between the organic porous membrane and the metal substrate can be further enhanced, thereby further enhancing the stability of the structure and quality of the prepared composite current collector.

[0129] The drying process in step S23 is to solidify and dry the conductive adhesive wet coating remaining between the organic porous membrane and the metal substrate after the lamination process and the conductive adhesive squeezed and filled in the organic porous membrane. After the drying process, the conductive adhesive squeezed and filled in the organic porous membrane solidifies to form a conductor, specifically forming a conductive body such as Figure 1 and Figure 2 The conductor 3 contained in the composite current collector of the above-mentioned application embodiment; the conductive adhesive wet coating remaining between the organic porous membrane and the metal substrate is cured to form a conductive adhesive layer, specifically forming a conductive adhesive layer as shown in FIG. Figure 1 and Figure 2 The composite current collector in the above-mentioned application embodiment contains a conductive adhesive layer 4.

[0130] electrode

[0131] In a third aspect, the present invention also provides an electrode. The electrode of the present invention comprises a current collector and an electrode active layer coupled to the current collector.

[0132] Wherein, the current collector is the composite current collector of the above text application embodiment. The electrode active layer is an electrode material active layer containing electrode material, therefore, the active layer can be an active layer containing positive electrode material, or it can be an active layer containing negative electrode material. When the active layer is an active layer containing positive electrode material, the electrode of the present application embodiment is a positive electrode; when the active layer is an active layer containing negative electrode material, the electrode of the present application embodiment is a negative electrode. It should be understood that the electrode active layer contained in the electrode of the present application embodiment is electrically connected to the conductor filled in the pores of the organic porous membrane layer contained in the composite current collector of the above text application embodiment.

[0133] Based on the structure and performance of the composite current collector of the embodiment of the present application, the composite current collector of the embodiment of the present application contains an organic porous film layer, and it has good elastic deformation ability, which can significantly reduce or alleviate the battery thermal failure of the electrode of the embodiment of the present application in the puncture condition and / or abnormal environment of excessive high temperature, and improve the safety performance of the battery. At the same time, the electrode of the embodiment of the present application has excellent conductivity.

[0134] In the embodiment, since the weight of the composite current collector contained in the electrode of the embodiment of the present application can be significantly reduced (such as effectively reducing the thickness of the metal matrix contained in the composite current collector), the weight of the electrode of the embodiment of the present application can be significantly reduced, that is, the energy density can be significantly improved.

[0135] In the embodiment, since the electrode active layer contained in the electrode of the embodiment of the present application is directly combined with the organic porous membrane layer contained in the composite current collector, the porous structure of the organic porous membrane layer gives the organic porous membrane layer a convex-concave surface, and the convex-concave surface increases the contact area with the electrode active layer and increases the mechanical riveting strength with the electrode active layer, thereby significantly enhancing the bonding strength between the electrode active layer and the composite current collector and improving the cycle performance of the electrode.

[0136] Battery

[0137] In a fourth aspect, the present application also provides a battery. The battery of the present application comprises an electrode, and the electrode is the electrode of the above-mentioned application, specifically, an electrode containing a composite current collector of the above-mentioned application.

[0138] Among them, when the positive electrode of the battery of the embodiment of the present application is the electrode of the embodiment of the above text application, then at this time, the electrode of the embodiment of the above text application is the positive electrode, and the composite current collector contained therein is the positive electrode current collector (the metal matrix contained in the composite current collector is the positive electrode current collector matrix), and the electrode active layer is the positive electrode active layer; when the negative electrode of the battery of the embodiment of the present application is the electrode of the embodiment of the above text application, then at this time, the electrode of the embodiment of the above text application is the negative electrode, and the composite current collector contained therein is the negative electrode current collector (the metal matrix contained in the composite current collector is the negative electrode current collector matrix), and the electrode active layer is the negative electrode active layer. Then the positive electrode and the negative electrode of the battery can be the electrodes of the embodiment of the above text application at the same time.

[0139] Since the electrodes of the battery of the present application are the electrodes of the above application, the battery of the present application can significantly reduce or alleviate the occurrence of thermal runaway under abnormal conditions such as puncture conditions or high temperatures, or reduce the harm caused by thermal runaway, thereby effectively improving the safety performance of the battery of the present application. Moreover, since the electrodes of the above application have a firm structure and good stability, the cycle performance of the battery of the present application is significantly improved.

[0140] In the embodiment, when the thickness of the metal matrix contained in the composite current collector of the electrode contained in the battery of the embodiment of the present application is set to be significantly smaller than the thickness of the existing conventional current collector, the energy density of the electrode is significantly increased. At this time, the energy density of the battery of the embodiment of the present application is also significantly improved.

[0141] In an embodiment, the battery of the embodiment of the present application may include any one of a battery cell, a battery module, and a battery pack.

[0142] The battery cell refers to a battery housing and an electrode assembly encapsulated in the battery housing. The shape of the battery cell is not particularly limited, and it can be cylindrical, square, or any other shape. In an exemplary embodiment, the battery cell can be Figure 3 The battery cell 30 shown has a square structure.

[0143] In some embodiments, Figure 4 As shown, the outer packaging of the battery cell 30 may include a shell 31 and a cover plate 33. The shell 31 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 31 has an opening connected to the receiving cavity, and the cover plate 33 is used to cover the opening to close the receiving cavity. The positive electrode, the separator and the negative electrode contained in the battery cell 30 of the embodiment of the present application can form an electrode assembly 32 through a winding process and / or a lamination process. The electrode assembly 32 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 32. The number of electrode assemblies 32 contained in the battery cell 30 may be one or more, which can be adjusted according to actual needs.

[0144] The preparation method of the battery cell 30 is well known. In some embodiments, the positive electrode, the separator, the negative electrode and the electrolyte can be assembled to form the battery cell 30. As an example, the positive electrode, the separator and the negative electrode can be formed into an electrode assembly 32 through a winding process or a lamination process, and the electrode assembly 32 is placed in an outer package, dried and injected with electrolyte, and then vacuum packaged, left to stand, formed, shaped and other processes are performed to obtain the battery cell 30.

[0145] The battery module is assembled from the battery cells 30 , that is, it may contain a plurality of the battery cells 30 , and the specific number can be adjusted according to the application and capacity of the battery module.

[0146] In some embodiments, Figure 5 FIG. 4 is a schematic diagram of a battery module 40 as an example. Figure 5 As shown, in the battery module 50, the plurality of battery cells 30 may be arranged in sequence along the length direction of the battery module 40. Of course, they may also be arranged in any other manner. Further, the plurality of battery cells 30 may be fixed by fasteners.

[0147] Optionally, the battery module 40 may further include a housing having an accommodation space, and the plurality of battery cells 30 may be accommodated in the accommodation space.

[0148] A battery pack is composed of the above-mentioned battery cells 30, that is, it may contain multiple battery cells 30, wherein multiple battery cells 30 may be assembled into the above-mentioned battery module 50. The specific number of battery cells 30 or battery modules 40 contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0149] As in the embodiment, Figure 6 and Figure 7 is a schematic diagram of an example battery pack 50. The battery pack 50 may include a battery box and a plurality of battery modules 40 disposed in the battery box. The battery box includes an upper box body 51 and a lower box body 52, wherein the upper box body 51 is used to cover the lower box body 52 and form a closed space for accommodating the battery modules 40. The plurality of battery modules 40 may be arranged in the battery box in any manner.

[0150] Electrical devices

[0151] In the fifth aspect, the embodiments of the present application also provide an electric device. The electric device in the embodiments of the present application includes a power supply unit or an energy storage unit, and of course may also include other auxiliary components or necessary components. Among them, the power supply unit or energy storage unit contains the battery of the above-mentioned embodiment of the text application. The battery contained in the power supply unit or energy storage unit may be one or more. When there are multiple batteries, multiple batteries can form a battery module or battery pack. Since the electric device in the embodiments of the present application contains the battery of the above-mentioned embodiment of the text application, the power supply unit or energy storage unit of the electric device in the embodiments of the present application has high safety and long service life, and the standby or battery life of the electric device in the embodiments of the present application is long.

[0152] Figure 8 Schematic diagram of an electric device as an example. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the requirements of the electric device for high power and high energy density, a battery pack or a battery module may be used.

[0153] As another example, the electric device may be a mobile phone, a tablet computer, a notebook computer, etc. The electric device is usually required to be light and thin, and a secondary battery may be used as a power source.

[0154] Energy storage device

[0155] In a sixth aspect, the embodiments of the present application also provide an energy storage device, which includes an energy storage unit and, of course, other auxiliary components or necessary components. Among them, the energy storage unit contains the battery of the above-mentioned embodiment of the text application. The battery contained in the energy storage unit may be one or more. When there are multiple batteries, multiple batteries can form a battery module or battery pack. Since the energy storage device of the embodiment of the present application contains the battery of the above-mentioned embodiment of the text application, the energy storage device has high safety, long service life, and further high energy density.

[0156] Example

[0157] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0158] 1. Composite current collector and preparation method thereof

[0159] Example A1

[0160] An embodiment of the present application provides a composite positive electrode current collector, comprising an aluminum foil layer and a PE porous film layer, wherein the PE porous film layer is bonded to two opposite surfaces of the aluminum foil layer through a conductive adhesive layer, and the surface of the conductive adhesive layer extends and fills the pores of the PE porous film layer.

[0161] Among them, the total thickness of the composite positive electrode collector is 14μm, the thickness of the aluminum foil layer is 6μm, and the thickness of the PE porous film layer arranged on the surface of the aluminum foil layer is 2.5μm; the porosity of the PE porous film layer is 60%, the pore size is 600nm, and the depth of the conductive adhesive layer filled into the pores of the PE porous film layer is 2μm on average; the adhesive of the conductive adhesive layer includes a PI adhesive and a conductive agent doped in the PI adhesive, the conductive agent is SP, and the weight content in the conductive adhesive layer is 30%.

[0162] The method for preparing the composite positive electrode current collector of the present application embodiment comprises the following steps:

[0163] S1: coating a conductive adhesive for forming the conductive adhesive layer on one surface of the PE porous film and two oppositely disposed surfaces of the aluminum foil layer to form conductive adhesive wet film layers respectively;

[0164] S2: Laminating the conductive adhesive wet film layer to obtain a composite current collector blank;

[0165] S3: The composite current collector blank is subjected to a micro-concave rubber roller pressing process, and then subjected to 4 steel roller / rubber roller pressing processes, and then subjected to a drying process (to dry the conductive adhesive), and then rolled up to obtain a composite positive electrode current collector; wherein, the pressure of the micro-concave rubber roller pressing is controlled to be less than the pressure of the steel roller / rubber roller pressing, and the pressure of the steel roller / rubber roller pressing is 3MPa.

[0166] Example A2

[0167] The embodiment of the present application provides a composite positive electrode current collector, which is different from the composite positive electrode current collector in Example A1 in that: the porosity of the PE porous film layer is 90%, and the pore size is 1500nm; the depth of the conductive adhesive layer filled into the pores of the PE porous film layer is the same as the thickness of the PE porous film layer, that is, the pores are filled.

[0168] The preparation method of the composite positive electrode current collector of the embodiment of the present application refers to the preparation method steps and conditions in Example A1, and is adjusted in combination with the composite positive electrode current collector of the present embodiment.

[0169] Example A3

[0170] The present embodiment provides a composite positive electrode current collector, which is different from the composite positive electrode current collector in embodiment A1 in that a PE porous film layer is bonded to only one surface of the aluminum foil layer, that is, a PE porous film layer is not bonded to the other opposite surface of the aluminum foil layer, and a conductive adhesive layer is not provided. Other aspects are the same as those of the composite positive electrode current collector in embodiment A1.

[0171] The preparation method of the composite positive electrode current collector of the embodiment of the present application refers to the preparation method steps and conditions in Example A1, and is adjusted in combination with the composite positive electrode current collector of the present embodiment.

[0172] Example A4

[0173] The embodiment of the present application provides a composite positive electrode current collector, which is different from the composite positive electrode current collector in Example A1 in that: the thickness of the aluminum foil layer is 5 μm; the PE porous film layer is replaced by a PI porous film layer, and the thickness of the PI porous film layer is 3 μm, the porosity of the PI porous film layer is 80%, the pore size is 1500 nm, and the depth of the conductive adhesive layer filled into the pores of the PI porous film layer is 2.8 μm on average.

[0174] The preparation method of the composite positive electrode current collector of the embodiment of the present application refers to the preparation method steps and conditions in Example A1, and is adjusted in combination with the composite positive electrode current collector of the present embodiment.

[0175] Example A5

[0176] The embodiment of the present application provides a composite positive electrode current collector, which is different from the composite positive electrode current collector in Example A2 in that the thickness of the PI porous film layer is 2.5 μm, the porosity of the PI porous film layer is 40%, the pore size is 800 nm, and the depth of the conductive adhesive layer filled into the pores of the PI porous film layer is 2 μm on average.

[0177] The preparation method of the composite positive electrode current collector of the embodiment of the present application refers to the preparation method steps and conditions in Example A1, and is adjusted in combination with the composite positive electrode current collector of the present embodiment.

[0178] Example A6

[0179] An embodiment of the present application provides a composite negative electrode current collector, comprising a copper foil layer and a PE porous film layer, wherein the PE porous film layer is bonded to two opposite surfaces of the copper foil layer through a conductive adhesive layer, and the surface of the conductive adhesive layer extends and fills the pores of the PE porous film layer.

[0180] Among them, the total thickness of the composite positive electrode collector is 6μm, the thickness of the copper foil layer is 2μm, the thickness of the PE porous film layer set on the surface of the copper foil layer is 1.5μm; the porosity of the PE porous film layer is 85%; the adhesive of the conductive adhesive layer is the same as that in Example A1.

[0181] The preparation method of the composite positive electrode current collector of the embodiment of the present application refers to the preparation method steps and conditions in Example A1, and is adjusted in combination with the composite negative electrode current collector of the present embodiment.

[0182] The steps include:

[0183] The present application embodiment provides a composite negative electrode current collector,

[0184] The total thickness of the composite positive electrode collector is 14 μm, the thickness of the aluminum foil layer is 5 μm, and the thickness of the PE porous film layer set on one surface of the aluminum foil layer is 3 μm; the porosity of the PE porous film layer is 80%, and the depth of the conductive adhesive layer filled into the pores of the PE porous film layer is about 2.8 μm.

[0185] The preparation method of the composite positive electrode current collector in the embodiment of the present application is prepared according to the method of Example A1.

[0186] Comparative Example A1

[0187] Aluminum foil with a thickness of 14 μm was used as the positive electrode current collector;

[0188] Comparative Example A2

[0189] A copper foil with a thickness of 6 μm was used as the negative electrode current collector.

[0190] The composite current collectors provided in the above-mentioned Examples A1 to A7 and the current collectors provided in Comparative Examples A1 to A2 were respectively subjected to the relevant performance tests shown in Table 1 below.

[0191] The relevant performance test methods are as follows:

[0192] Maximum force and elongation at break test: the above current collector is cut into strips with a width of 2 cm and a length of 10 cm, and stretched using a tensile machine at a stretching speed of 50 mm / min, and the maximum force and elongation at break are recorded;

[0193] Adhesion force test: Prepare the pole piece according to the method described in (2. Secondary battery monomer example) below, and after cold pressing, use a tensile machine to stretch it at a stretching speed of 50 mm / min, and record the 180° peeling adhesion force;

[0194] Current collector density test:

[0195] Cut samples of standard area, weigh them, measure their thickness, and then calculate the current collector density.

[0196] The test results are shown in Table 1 below:

[0197] Table 1

[0198]

[0199] From the data in Table 1, it can be seen from the comparison of Examples A1 to A5 with Comparative Example A1, and Example A6 with Comparative Example A2 that the tensile strength of the composite current collector of the embodiment of the present application reaches the tensile strength of the pure aluminum / copper foil current collector on the basis of the same total thickness, and can even be better than the tensile strength of the pure metal current collector; and the elongation at break of the composite current collector of the embodiment of the present application has been significantly improved, and the density has also been significantly reduced, which has contributed to reducing the risk of thermal failure of the battery and improving the energy density. At the same time, due to the presence of the organic porous film layer of the composite current collector of the present application, the bonding force between it and the electrode active layer has been significantly improved, so that the bonding force of the electrode containing the composite current collector of the present application is significantly higher than the bonding force of the electrode containing the pure aluminum / copper foil current collector.

[0200] 2. Secondary battery cell example

[0201] Example B1 to Example B7 and Comparative Example B1 to Comparative Example B2;

[0202] Embodiments B1 to B7 and Comparative Examples B1 to B2 each provide a secondary battery cell. Each secondary battery cell includes an electrode assembly formed of a positive electrode, a separator, and a negative electrode, and also includes an electrolyte.

[0203] The composite current collectors provided in Examples A1 to A5 and the pure aluminum foil provided in Comparative Example A1 were respectively prepared as positive electrodes of lithium iron phosphate batteries, and the composite current collectors provided in Example A6 and the pure copper foil provided in Comparative Example A2 were respectively prepared as negative electrodes of lithium iron phosphate batteries. The prepared electrodes were sequentially denoted as M1 to M6 and N1 to N2.

[0204] Battery assembly: According to the pairing relationship of the positive electrode sheet and the negative electrode sheet in Table 2 below, the hard shell cells of each lithium iron phosphate battery are assembled according to the battery assembly requirements and process.

[0205] Secondary battery monomer related performance test:

[0206] Each battery provided in Examples B1 to B7 and Comparative Examples B1 to B2 was subjected to a needle puncture test, wherein the needle puncture test refers to GB / T 31485-2015. The diameter of the steel needle is 8 mm, the puncture speed is 30 mm / s, and it is considered to have passed if there is no fire or explosion;

[0207] The acupuncture test results are shown in Table 2 below:

[0208] Table 2

[0209]

[0210] From the data in Table 2, it can be seen that the puncture test of the battery containing the composite current collector of the embodiment of the present application was passed, while the comparative example B1 did not pass the puncture test because it used a conventional pure metal current collector. It can be seen that the battery of the embodiment of the present application contains the composite current collector of the embodiment of the present application, and under puncture conditions, including abnormal environments such as high temperature, the thermal failure of the battery of the embodiment of the present application can be significantly improved, and the safety performance is significantly improved.

[0211] At the same time, the electrode containing the composite current collector of the embodiment of the present application in Table 1 has a significantly reduced density and a significantly improved structural strength. Therefore, the energy density and cycle performance of the battery of the embodiment of the present application are also significantly improved.

[0212] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. A composite current collector, characterized in that: include: A metal substrate having at least one surface; The organic porous membrane layer is laminated on the surface of the metal substrate, and the pores of the organic porous membrane layer are filled with a conductor, and the conductor is electrically connected to the surface of the metal substrate.

2. The composite current collector according to claim 1, characterized in that: The organic porous membrane layer includes at least one of the following (1) to (4): (1) The thickness of the organic porous membrane layer laminated on the surface is 0.1 μm to 6 μm, and can be 0.5 μm to 3 μm; (2) The porosity of the organic porous membrane layer is 40% to 95%, and can be 60% to 90%; (3) The pores contained in the organic porous membrane layer have a pore size of 200 to 5000 nm, and can be optionally 500 nm to 2500 nm; (4) The tensile strength of the organic porous membrane layer is higher than 50 MPa.

3. The composite current collector according to claim 1 or 2, characterized in that: The material of the organic porous membrane layer includes at least one of polyethylene, polyimide, polypropylene and polytetrafluoroethylene.

4. The composite current collector according to any one of claims 1 to 3, characterized in that: The material of the conductor includes a conductive adhesive; and / or The depth of the conductor filled in the pores is 4 / 5 to 5 / 5 of the thickness of the organic porous membrane layer; and / or The organic porous membrane layer is bonded to the surface of the metal base layer via a conductive adhesive layer.

5. The composite current collector according to claim 4, characterized in that: The thickness of the conductive adhesive layer is 0.05 μm to 1 μm, and can be 0.1 μm to 0.5 μm; and / or The conductor is formed by extending from the surface of the conductive adhesive layer to the pores of the organic porous membrane layer.

6. The composite current collector according to claim 4 or 5, characterized in that: The electrical conductivity of the conductor is 10 3 S / m~6×10 7 S / m; and / or The conductivity of the conductive adhesive layer is 10 3 S / m~10 4 S / m.

7. The composite current collector according to any one of claims 1 to 6, characterized in that: The metal substrate is a metal film layer having two surfaces arranged opposite to each other, and the organic porous film layer is bonded to both surfaces.

8. The composite current collector according to any one of claims 1 to 7, characterized in that: The metal substrate is a metal film layer, and the thickness of the metal film layer is 4 μm to 15 μm, and can be 6 μm to 12 μm.

9. The composite current collector according to any one of claims 1 to 8, characterized in that: The total thickness of the composite current collector is 6 μm to 18 μm, and can be 8 μm to 14 μm; and / or The sheet resistance of the composite current collector is greater than 0 and less than or equal to 5Ω, and can be selected to be 0.005Ω to 1Ω.

10. A method for preparing a composite current collector, characterized in that: The steps include: Providing a metal substrate and an organic porous membrane, wherein the metal substrate has at least one surface; The organic porous membrane is attached to the surface of the metal substrate, and at the same time, a conductor is filled in the pores of the organic porous membrane, and the conductor is electrically connected to the surface of the metal substrate to form a composite current collector.

11. The preparation method according to claim 10, characterized in that: The method for attaching the organic porous membrane to the surface of the metal substrate comprises the following steps: forming a conductive adhesive wet coating on the surface of the organic porous membrane and / or the surface of the metal substrate; Laminating the organic porous membrane to the surface of the metal substrate, and allowing the formed conductive adhesive wet coating to be disposed between the organic porous membrane and the metal substrate to form a composite current collector blank; The composite current collector blank is subjected to a pressing process, and the conductive adhesive part in the conductive adhesive wet coating is squeezed into the pores contained in the organic porous membrane, and then a drying process is performed.

12. The preparation method according to claim 11, characterized in that: The lamination process includes first performing a first lamination process and then performing a second lamination process; wherein the pressure of the first lamination process is less than the pressure of the second lamination process.

13. The preparation method according to claim 12, characterized in that: The first lamination process includes a roller pressing process, and the surface of the roller in the roller pressing process has a convex-concave structure; and / or The pressure of the second pressing process is 0.5 MPa to 5 MPa, and can be optionally 1 MPa to 3 MPa; and / or The second lamination process may be performed twice or more.

14. An electrode comprising a current collector and an active layer combined with the current collector, characterized in that: The current collector is the composite current collector according to any one of claims 1 to 9 or a composite current collector prepared by the preparation method according to any one of claims 10 to 13.

15. The electrode according to claim 14, characterized in that The electrode is at least one of a positive electrode and a negative electrode.

16. A battery, characterized in that: The battery comprises the electrode according to claim 14 or 15.

17. The battery according to claim 16, characterized in that The battery includes any one of a battery cell, a battery module, and a battery pack.

18. An electrical device, characterized in that: It comprises a power supply unit or an energy storage unit, wherein the power supply unit or the energy storage unit contains a battery, wherein the battery comprises the battery according to claim 16 or 17.

19. An energy storage device, characterized in that: An energy storage unit is included, the energy storage unit comprising a battery, the battery comprising the battery of claim 16 or 17.

Citation Information

Patent Citations

  • Composite current collector, preparation method thereof and lithium battery pole piece

    CN111883777A

  • Current collector and application thereof

    CN112993263A

  • High-performance flame-retardant composite current collector, preparation method thereof, electrode and battery

    CN116093334A

  • Collector for bipolar battery

    JP2010277862A

  • Flexible current collector, method for manufacturing same, and secondary battery using same

    WO2015020338A1