Low-temperature stable negative electrode electrolyte for vanadium battery

By adding vanadium ions, acid solution and polyoxygenate to the all-vana liquid flow battery electrolyte, the polyoxygenate is synthesized by acid extraction method, the stability of the electrolyte at low temperature is solved and the battery is improved Capacity retention and energy efficiency extend the battery life.

CN118970128AInactive Publication Date: 2024-11-15HANGZHOU DEHAI AIKE ENERGY TECH CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202411420900.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The use of all vanadium flow batteries in extremely cold areas is limited, because V(II) and V(III) are prone to precipitation of crystals at low temperatures, resulting in an increase in the polarization resistance of the electrolyte and rapid attenuation of capacity, which affects the long-term stability of the battery. and reliability.

Method used

Using a combination of vanadium ions, acid solution and polyoxygenate additives, polyoxygenate is synthesized by acid extraction, increasing the structural stability of the electrolyte and the solubility of vanadium ions, reducing the freezing point, and passing phosphorus atoms and vanadium ions Coordination complex forms a stable intermediate, improving battery efficiency and capacity.

Benefits of technology

在低温条件下显著提高了电解液的容量保持率和电池的能量效率,延长了电池的使用寿命,并改善了电解液的热稳定性能。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970128A_ABST
    Figure CN118970128A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of all-vanadium redox flow battery electrolyte, and discloses a low-temperature stable negative electrode electrolyte for a vanadium battery, which comprises vanadium ions, an acid solution and a polyoxometallate additive. The preparation method of the polyoxometallate comprises the following steps: preparing transition oxometallate; preparing a polyoxometallate; the synthesized polyoxometallate has high structural stability, the freezing point of the electrolyte is reduced, the solubility of vanadium ions at low temperature is improved, the polyoxometallate is suitable for the field of vanadium battery electrolyte preparation, the low-temperature stability of an all-vanadium redox flow battery is improved, phosphorus, molybdenum and tungsten atoms are high in coordination capacity and can form new chemical bonds with vanadium, and the stability of the electrolyte is improved. The electrochemical activity of the electrolyte is improved, so that the performance of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrolytes for all-vanadium liquid flow batteries, in particular to a low-temperature stable negative electrode electrolyte for vanadium batteries. Background Art

[0002] As an important component of vanadium batteries, the concentration and volume of electrolyte determine the capacity of the battery, affecting the stability and reliability of the battery's long-term operation. However, due to the limited solubility of V(Ⅱ) and V(Ⅲ) in sulfuric acid, crystals are easily precipitated when the temperature is below 0°C, resulting in an increase in the polarization resistance of the electrolyte and a rapid decay of the capacity, which affects the long-term service life of the battery. This greatly limits the normal operation of all-vanadium liquid flow batteries in extremely cold regions, hindering the widespread application of all-vanadium liquid flow batteries. Therefore, it is very necessary to develop a negative electrode additive that can enable the electrolyte to operate stably at low temperatures, which is of great significance to the development of vanadium battery technology. Summary of the invention

[0003] In order to solve the above problems, the present invention provides a low-temperature stable negative electrode electrolyte for a vanadium battery.

[0004] A low-temperature stable negative electrode electrolyte for a vanadium battery comprises vanadium ions, an acid solution and a polyoxometalate additive.

[0005] Preferably, the vanadium ion is one or more of divalent vanadium ion and trivalent vanadium ion; and the concentration in the electrolyte is 1-3 mol / L.

[0006] Preferably, the acid solution is one of a sulfuric acid solution and a hydrochloric acid solution; and the concentration of the acid solution in the electrolyte is 3-9 mol / L.

[0007] Preferably, the polyoxometalate additive is one of sodium phosphomolybdate, potassium phosphomolybdate, lithium phosphomolybdate, sodium phosphotungstate, potassium phosphotungstate, and lithium phosphotungstate; and the concentration in the electrolyte is 2-5 mmol / L.

[0008] A method for preparing a polyoxometalate additive comprises the following steps: Step S1: adding a high oxidation state transition metal salt, hydrochloric acid and phosphoric acid to ultrapure water, heating and stirring, reflux at 40-80° C. for 6-24 hours, and cooling to room temperature to obtain a mixed solution; Step S2: adding ammonium salt to the mixed solution, stirring to generate a precipitate, washing and drying the precipitate, and then dispersing it into ultrapure water at 20-80° C. to obtain a dispersion; Step S3: adding hydrochloric acid and ether to the dispersion to obtain an extract, standing the extract to separate layers, taking out the bottom layer of liquid, and evaporating the liquid to dryness at 40-50° C. to obtain a solid powder; mixing the solid powder, ultrapure water, and concentrated nitric acid in a mass ratio of 1: (5-10): (0.1-0.6), and then evaporating the mixture at 30-50° C. to obtain a polyoxometalate; Step S4: dissolving polyoxometallic acid and strong base in ultrapure water, wherein the concentration of polyoxometallic acid in the obtained solution is 0.01-0.05 mol / L, the concentration of strong base is 0.06-0.3 mol / L, and the molar concentration ratio of polyoxometallic acid to strong base is 1:6, reacting at 30-50°C for 1-3h, and rotary evaporation to obtain polyoxometallate.

[0009] Preferably, the high oxidation state transition metal salt in step S1 is any one of sodium molybdate, potassium molybdate, sodium tungstate and potassium tungstate.

[0010] Preferably, in the mixed solution in step S1, the concentration of the high oxidation state transition metal salt is 0.1-0.5 mol / L, the concentration of the hydrochloric acid is 1-3 mol / L, and the concentration of the phosphoric acid is 1-3 mol / L.

[0011] Preferably, the ammonium salt in step S2 is any one of ammonium chloride and ammonium sulfate, wherein the molar concentration ratio of ammonium ions to high oxidation state transition metal salt is (1.2-1.5):1; and the concentration of the precipitate in the dispersion is 50-100 g / L.

[0012] Preferably, the extract in step S3 contains hydrochloric acid at a concentration of 1-3 mol / L and ether at a concentration of 1-2 mol / L.

[0013] Preferably, the strong base in step S4 is any one of sodium hydroxide, potassium hydroxide and lithium hydroxide.

[0014] The beneficial effects of the present invention are: 1. The present invention adopts an acid extraction method to synthesize polyoxometalates, which have the characteristics of electron sponges, can accommodate multiple electrons without structural changes, and have strong structural stability.

[0015] 2. The polyoxometalate surface of the present invention has abundant oxygen atoms, which can interact with hydrogen atoms in water molecules, reduce hydrogen bonds between water molecules, lower the freezing point of the electrolyte, and increase the solubility of vanadium ions at low temperatures, thereby improving the capacity retention rate of the electrolyte.

[0016] 3. The core phosphorus atom of the present invention can coordinate and complex with water and vanadium ions in the electrolyte 1 to form a more stable VOP intermediate. The reaction activation energy is lower than that of the VOV intermediate, which reduces the generation selectivity of vanadium precipitation and further improves the efficiency and capacity of the battery.

[0017] 4. The molybdenum atoms and tungsten atoms of the present invention have similar properties to vanadium. Molybdates and tungstates contain multiple oxygen atoms and have strong coordination ability. They can form new chemical bonds with vanadium, improve the electrochemical activity of the electrolyte, increase the kinematic viscosity of the electrolyte, and improve the thermal stability of the electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The effect diagram of the electrolyte of Example 1 of the present invention after adding polyoxometalate and standing at -10°C for 20 days. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below through the accompanying drawings and embodiments. However, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0020] A low-temperature stable negative electrode electrolyte for a vanadium battery comprises vanadium ions, an acid solution, and a polyoxometalate additive; the vanadium ions are one or more of divalent vanadium ions and trivalent vanadium ions; the concentration of the vanadium ions in the electrolyte is 1-3 mol / L; the acid solution is one of a sulfuric acid solution and a hydrochloric acid solution; the concentration of the polyoxometalate additive in the electrolyte is 3-9 mol / L; the polyoxometalate additive is one of sodium phosphomolybdate, potassium phosphomolybdate, lithium phosphomolybdate, sodium phosphotungstate, potassium phosphotungstate, and lithium phosphotungstate; the concentration of the polyoxometalate additive in the electrolyte is 2-5 mmol / L.

[0021] A method for preparing a polyoxometalate additive comprises the following steps: Step S1: adding a high oxidation state transition metal salt, hydrochloric acid and phosphoric acid to ultrapure water, heating and stirring, reflux at 40-80° C. for 6-24 hours, cooling to room temperature, and obtaining a mixed solution; the high oxidation state transition metal salt is any one of sodium molybdate, potassium molybdate, sodium tungstate and potassium tungstate; the concentration of the high oxidation state transition metal salt in the mixed solution is 0.1-0.5 mol / L, the concentration of hydrochloric acid is 1-3 mol / L, and the concentration of phosphoric acid is 1-3 mol / L.

[0022] Step S2: adding ammonium salt to the mixed solution, stirring to generate a precipitate, washing and drying the precipitate, and dispersing it into ultrapure water at 20-80° C. to obtain a dispersion; the ammonium salt is any one of ammonium chloride and ammonium sulfate, wherein the molar concentration ratio of ammonium ion to high oxidation state transition metal salt is (1.2-1.5):1; the concentration of the precipitate in the dispersion is 50-100 g / L.

[0023] Step S3: adding hydrochloric acid and ether to the dispersion to obtain an extract, standing the dispersion to separate layers, taking out the bottom layer of liquid, and evaporating to dryness at 40-50° C. to obtain a solid powder; mixing the solid powder, ultrapure water, and concentrated nitric acid in a mass ratio of 1: (5-10): (0.1-0.6), and then evaporating at 30-50° C. to obtain a polyoxometallic acid; the extract contains 1-3 mol / L hydrochloric acid and 1-2 mol / L ether.

[0024] Step S4: dissolving polymetallic acid and strong base in ultrapure water, wherein the concentration of polymetallic acid in the obtained solution is 0.01-0.05 mol / L, the concentration of strong base is 0.06-0.3 mol / L, and the molar concentration ratio of polymetallic acid to strong base is 1:6, reacting at 30-50°C for 1-3h, and rotary evaporation and drying to obtain polymetallic acid salt; the strong base is any one of sodium hydroxide, potassium hydroxide and lithium hydroxide.

[0025] Embodiment 1: This embodiment is specifically obtained by the following operations: (1) Preparation of polyoxometalate additives: Step S1: Add sodium molybdate, hydrochloric acid and phosphoric acid into ultrapure water, heat and stir, reflux at 65°C for 18 hours, and cool to room temperature to obtain a mixed solution, wherein the concentration of sodium molybdate is 0.4 mol / L, the concentration of hydrochloric acid is 2 mol / L, and the concentration of phosphoric acid is 2 mol / L.

[0026] Step S2: adding ammonium chloride to the mixed solution so that the molar concentration ratio of ammonium ions to high oxidation state transition metal salt is 1.3:1, stirring to generate a precipitate, washing and drying the precipitate, and dispersing it into 55° C. ultrapure water to obtain a dispersion in which the concentration of the precipitate is 80 g / L.

[0027] Step S3: Add hydrochloric acid and ether to the dispersion to obtain an extract, wherein the concentration of hydrochloric acid is 2 mol / L and the concentration of ether is 1.5 mol / L. Let stand to separate the layers, take out the bottom layer of liquid, and evaporate to dryness at 45°C to obtain a solid powder. Then, mix the solid powder, ultrapure water, and concentrated nitric acid in a mass ratio of 1:8:0.4, and then evaporate at 45°C to obtain a polyoxometalate.

[0028] Step S4: dissolving polyoxometallic acid and sodium hydroxide in ultrapure water to obtain a solution having a polyoxometallic acid concentration of 0.03 mol / L and a sodium hydroxide concentration of 0.12 mol / L, and a molar concentration ratio of polyoxometallic acid to strong base of 1:6. The solution is reacted at 45°C for 2h, and rotary evaporated to obtain a polyoxometalate additive.

[0029] (2) Preparation of negative electrode electrolyte: The polyoxometalate additive prepared in (1) is added to an electrolyte containing 1.6 mol / L divalent vanadium ions and 5 mol / L sulfuric acid solution and mixed evenly to make the concentration of the polyoxometalate additive 4 mmol / L, thereby obtaining a low-temperature stable negative electrode electrolyte for vanadium batteries.

[0030] Embodiment 2: This embodiment is specifically obtained by the following operations: (1) Preparation of polyoxometalate additives: Step S1: Add potassium molybdate, hydrochloric acid and phosphoric acid into ultrapure water, heat and stir, reflux at 40°C for 6 hours, and cool to room temperature to obtain a mixed solution, wherein the concentration of potassium molybdate is 0.1 mol / L, the concentration of hydrochloric acid is 1 mol / L, and the concentration of phosphoric acid is 1 mol / L.

[0031] Step S2: adding ammonium sulfate to the mixed solution so that the molar concentration ratio of ammonium ions to high oxidation state transition metal salt is 1.2-1.5:1, stirring to generate a precipitate, washing and drying the precipitate, and dispersing it into 20° C. ultrapure water to obtain a dispersion in which the concentration of the precipitate is 50 g / L.

[0032] Step S3: Add hydrochloric acid and ether to the dispersion to obtain an extract, wherein the concentration of hydrochloric acid is 1 mol / L and the concentration of ether is 1 mol / L. Let stand to separate the layers, take out the bottom layer of liquid, and evaporate to dryness at 40°C to obtain a solid powder. Then, mix the solid powder, ultrapure water, and concentrated nitric acid in a mass ratio of 1:5:0.1, and then evaporate at 30°C to obtain a polyoxometalate.

[0033] Step S4: dissolving polyoxometallic acid and potassium hydroxide in ultrapure water, wherein the concentration of polyoxometallic acid in the obtained solution is 0.01 mol / L, the concentration of potassium hydroxide is 0.06 mol / L, and the molar concentration ratio of polyoxometallic acid to strong base is 1:6. The mixture is reacted at 30° C. for 1 h, and rotary evaporated to dry to obtain a polyoxometalate additive.

[0034] (2) Preparation of negative electrode electrolyte: The polyoxometalate additive prepared in (1) is added to an electrolyte containing 3 mol / L vanadium ions or one of the trivalent vanadium ions and 9 mol / L hydrochloric acid solution and mixed evenly to make the concentration of the polyoxometalate additive 5 mmol / L, thereby obtaining a low-temperature stable negative electrode electrolyte for vanadium batteries.

[0035] Embodiment 3: This embodiment is obtained by the following operations: (1) Preparation of polyoxometalate additives: Step S1: Add sodium tungstate, hydrochloric acid and phosphoric acid into ultrapure water, heat and stir, reflux at 80°C for 24h, cool to room temperature to obtain a mixed solution, wherein the concentration of sodium tungstate is 0.5mol / L, the concentration of hydrochloric acid is 3mol / L, and the concentration of phosphoric acid is 3mol / L.

[0036] Step S2: adding ammonium sulfate to the mixed solution so that the molar concentration ratio of ammonium ions to high oxidation state transition metal salts is 1.5:1, stirring to generate a precipitate, washing and drying the precipitate, and dispersing it into 80° C. ultrapure water to obtain a dispersion in which the concentration of the precipitate is 100 g / L.

[0037] Step S3: Add hydrochloric acid and ether to the dispersion to obtain an extract, wherein the concentration of hydrochloric acid is 3 mol / L and the concentration of ether is 2 mol / L. Let stand to separate the layers, take out the bottom layer of liquid, and evaporate to dryness at 50°C to obtain a solid powder. Then, mix the solid powder, ultrapure water, and concentrated nitric acid in a mass ratio of 1:10:0.1, and then evaporate at 50°C to obtain a polyoxometalate.

[0038] Step S4: dissolving polyoxometalate and lithium hydroxide in ultrapure water, wherein the concentration of polyoxometalate in the obtained solution is 0.05 mol / L, the concentration of lithium hydroxide is 0.3 mol / L, and the molar concentration ratio of polyoxometalate to strong base is 1:6. The mixture is reacted at 50° C. for 3 h, and dried by rotary evaporation to obtain a polyoxometalate additive.

[0039] (2) Preparation of negative electrode electrolyte: The polyoxometalate additive prepared in (1) is added to an electrolyte containing 1 mol / L vanadium ions (0.5 mol / L for both divalent vanadium ions and trivalent vanadium ions) and 5 mol / L sulfuric acid solution and mixed evenly to make the concentration of the polyoxometalate additive 3 mmol / L, thereby obtaining a low-temperature stable negative electrode electrolyte for vanadium batteries.

[0040] Embodiment 4: This embodiment is specifically obtained by the following operations: (1) Preparation of polyoxometalate additives: Step S1: Add potassium tungstate, hydrochloric acid and phosphoric acid into ultrapure water, heat and stir, reflux at 65°C for 18h, and cool to room temperature to obtain a mixed solution, wherein the concentration of potassium tungstate is 0.4mol / L, the concentration of hydrochloric acid is 2mol / L, and the concentration of phosphoric acid is 2mol / L.

[0041] Step S2: adding ammonium chloride to the mixed solution so that the molar concentration ratio of ammonium ions to high oxidation state transition metal salt is 1.3:1, stirring to generate a precipitate, washing and drying the precipitate, and dispersing it into 55° C. ultrapure water to obtain a dispersion in which the concentration of the precipitate is 80 g / L.

[0042] Step S3: Add hydrochloric acid and ether to the dispersion to obtain an extract, wherein the concentration of hydrochloric acid is 2 mol / L and the concentration of ether is 1.5 mol / L. Let stand to separate the layers, take out the bottom layer of liquid, and evaporate to dryness at 45°C to obtain a solid powder. Then, mix the solid powder, ultrapure water, and concentrated nitric acid in a mass ratio of 1:8:0.4, and then evaporate at 45°C to obtain a polyoxometalate.

[0043] Step S4: dissolving polyoxometallic acid and sodium hydroxide in ultrapure water to obtain a solution having a polyoxometallic acid concentration of 0.03 mol / L and a sodium hydroxide concentration of 0.12 mol / L, and a molar concentration ratio of polyoxometallic acid to strong base of 1:6. The solution is reacted at 45°C for 2h, and rotary evaporated to obtain a polyoxometalate additive.

[0044] (2) Preparation of negative electrode electrolyte: The polyoxometalate additive prepared in (1) is added to an electrolyte containing 2 mol / L divalent vanadium ions and 5 mol / L sulfuric acid solution and mixed evenly to make the concentration of the polyoxometalate additive 4 mmol / L, thereby obtaining a low-temperature stable negative electrode electrolyte for vanadium batteries.

[0045] Comparative Example 1: This comparative example is a blank control group, i.e. no additives were added to the electrolyte.

[0046] Comparative Example 2: Only phosphoric acid was added to the electrolyte of this comparative example.

[0047] Comparative Example 3: Only sodium molybdate was added to the electrolyte of this comparative example.

[0048] Comparative Example 4: Only potassium tungstate was added to the electrolyte of this comparative example.

[0049] The electrolytes of Examples 1-4 and Comparative Examples 1-3 were left to stand for several days at the same ambient temperature, and the crystallization of the electrolytes was recorded. The results of the low temperature stability of the electrolytes are shown in Table 1: Table 1 Summary of electrolyte low temperature stability results

[0050] Combined with Table 1 Figure 1 , compared with Example 1, Examples 1-4 are more stably stored at low temperatures, indicating that the polyoxometalate surface of the present invention has abundant oxygen atoms, which can interact with the hydrogen atoms in water molecules, reduce the hydrogen bonds between water molecules, lower the freezing point of the electrolyte, and increase the solubility of vanadium ions at low temperatures, thereby improving the capacity retention rate of the electrolyte.

[0051] The polyoxometalate prepared in Examples 1-4 was added to the negative electrode electrolyte and the electrolyte of Comparative Examples 1-3, and the battery stack was assembled and charged and discharged under the same test conditions. The coulombic efficiency, voltage efficiency, energy efficiency and capacity retention rate after 50 cycles of operation of the battery at -10°C were recorded. The test results are shown in Table 2: Table 2 Performance test results of electrolytes of examples and comparative examples at -10°C

[0052] As can be seen from Table 2, compared with Examples 1-4 and Comparative Examples 3-4, Examples 1-4 have higher energy efficiency and capacity retention, indicating that the phosphorus atoms of the present invention can coordinate and complex with water and vanadium ions in the electrolyte 1 to form a more stable VOP intermediate, and the reaction activation energy is lower than that of the VOV intermediate, which reduces the generation selectivity of vanadium precipitation and further improves the efficiency and capacity of the battery. Compared with Comparative Example 2, Examples 1-4 have higher energy efficiency and capacity retention, indicating that molybdenum atoms and tungsten atoms have similar vanadium properties, molybdates and tungstates contain multiple oxygen atoms, have strong coordination ability, can form new chemical bonds with vanadium, improve the electrochemical activity of the electrolyte, increase the kinematic viscosity of the electrolyte, and improve the thermal stability of the electrolyte. Compared with Comparative Examples 3-4, Examples 1-4 have higher energy efficiency and capacity retention, indicating that the polyoxometalate synthesized by the acid extraction method of the present invention has the characteristics of an electron sponge, can accommodate multiple electrons without structural changes, and has strong structural stability.

[0053] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A low-temperature stable negative electrode electrolyte for a vanadium battery, comprising vanadium ions, an acid solution, and a polyoxometalate additive.

2. A low temperature stable negative electrode electrolyte for vanadium battery according to claim 1, characterized in that: The vanadium ion is one or more of divalent vanadium ion and trivalent vanadium ion; and the concentration in the electrolyte is 1-3 mol / L.

3. A low temperature stable negative electrode electrolyte for vanadium battery according to claim 1, characterized in that: The acid solution is one of a sulfuric acid solution and a hydrochloric acid solution; and the concentration of the acid solution in the electrolyte is 3-9 mol / L.

4. A low temperature stable negative electrode electrolyte for vanadium battery according to claim 1, characterized in that: The polyoxometalate additive is one of sodium phosphomolybdate, potassium phosphomolybdate, lithium phosphomolybdate, sodium phosphotungstate, potassium phosphotungstate, and lithium phosphotungstate; and the concentration in the electrolyte is 2-5 mmol / L.

5. A method for preparing a polyoxometalate additive, comprising the following steps: Step S1: adding a high oxidation state transition metal salt, hydrochloric acid and phosphoric acid to ultrapure water, heating and stirring, reflux at 40-80° C. for 6-24 hours, and cooling to room temperature to obtain a mixed solution; Step S2: adding ammonium salt to the mixed solution, stirring to generate a precipitate, washing and drying the precipitate, and then dispersing it into ultrapure water at 20-80° C. to obtain a dispersion; Step S3: adding hydrochloric acid and ether to the dispersion to obtain an extract, standing the extract to separate layers, taking out the bottom layer of liquid, and evaporating the liquid to dryness at 40-50° C. to obtain a solid powder; mixing the solid powder, ultrapure water, and concentrated nitric acid in a mass ratio of 1: (5-10): (0.1-0.6), and then evaporating the mixture at 30-50° C. to obtain a polyoxometalate; Step S4: dissolving polyoxometallic acid and strong base in ultrapure water, wherein the concentration of polyoxometallic acid in the obtained solution is 0.01-0.05 mol / L, the concentration of strong base is 0.06-0.3 mol / L, and the molar concentration ratio of polyoxometallic acid to strong base is 1:6, reacting at 30-50°C for 1-3h, and rotary evaporation to obtain polyoxometallate.

6. The method for preparing a polyoxometalate additive according to claim 5, characterized in that: In step S1, the high oxidation state transition metal salt is any one of sodium molybdate, potassium molybdate, sodium tungstate and potassium tungstate.

7. The method for preparing a polyoxometalate additive according to claim 5, characterized in that: In step S1, the concentration of the high oxidation state transition metal salt in the mixed solution is 0.1-0.5 mol / L, the concentration of hydrochloric acid is 1-3 mol / L, and the concentration of phosphoric acid is 1-3 mol / L.

8. The method for preparing a polyoxometalate additive according to claim 5, characterized in that: In step S2, the ammonium salt is any one of ammonium chloride and ammonium sulfate, wherein the molar concentration ratio of ammonium ions to high oxidation state transition metal salt is (1.2-1.5):1; and the concentration of the precipitate in the dispersion is 50-100 g / L.

9. The method for preparing a polyoxometalate additive according to claim 5, characterized in that: The extract in step S3 contains hydrochloric acid at a concentration of 1-3 mol / L and ether at a concentration of 1-2 mol / L.

10. The method for preparing a polyoxometalate additive according to claim 5, characterized in that: In step S4, the strong base is any one of sodium hydroxide, potassium hydroxide and lithium hydroxide.

Citation Information

Patent Citations

  • Low-temperature electrolyte for LiFePO4 (lithium iron phosphate) lithium-ion batteries

    CN102983362A

  • Method for preparing Dawson heteropolyphosphatotungstate

    CN103613082A

  • Vanadium battery electrolyte containing inorganic molybdate and vanadium battery

    CN106299434A

  • Flow battery

    CN106611867A

  • Vanadium cell electrolyte

    CN107658487A