Electrolyte and lithium battery using same

By using trimethylphosphorus tetrafluoroborate and ether solvents in the lithium battery electrolyte, the problems of uneven heat production and electrolyte decomposition during the fast charging of lithium batteries are solved, and a stable SEI film is formed, which improves the lithium battery. fast charging performance and capacity retention rate.

CN118970182APending Publication Date: 2024-11-15EVE ENERGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411035918.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the fast charging process, existing lithium batteries have problems of uneven heat production and electrolyte decomposition, resulting in increased impedance and unstable SEI film, affecting fast charging performance.

Method used

Using an electrolytetrafluoroborate containing trimethylphosphate tetrafluoroborate and an ether organic solvent, the Li+ transport performance is improved by the combination of F, B and P elements, and the ether solvent is used to promote the formation of dense and protective SEI on the negative electrode surface. film, reducing interface resistance and impedance.

Benefits of technology

It significantly improves the fast charging performance and capacity retention rate of lithium batteries, reduces impedance, realizes rapid transmission of lithium ions and the stability of SEI film, and avoids lithium evolution problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004971650710000021
    Figure BDA0004971650710000021
  • Figure BDA0004971650710000031
    Figure BDA0004971650710000031
  • Figure BDA0004971650710000051
    Figure BDA0004971650710000051
Patent Text Reader

Abstract

The invention provides an electrolyte and a lithium battery using the electrolyte. The electrolyte comprises a first additive and an organic solvent, wherein the mass fraction of the first additive in the electrolyte is 0.2-1%; the first additive is trimethylphosphonium tetrafluoroborate; the organic solvent comprises an ether solvent. According to the electrolyte provided by the invention, the first coulombic efficiency of the lithium battery applying the electrolyte is improved, a more stable SEI film is formed on the surface of a negative electrode of the lithium battery, meanwhile, the condition of electrolyte decomposition caused by non-uniform heat production of the lithium battery in a rapid charging process is improved, the impedance of the lithium battery is reduced, rapid transmission of lithium ions is realized, and the service life of the lithium battery is prolonged. And finally, the fast charging performance of the lithium battery is improved, so that the constant-current charging ratio and the cycle capacity retention ratio of the lithium battery during fast charging are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to an electrolyte and a lithium battery using the electrolyte. Background Art

[0002] Lithium batteries are widely used in 3C digital products, electric vehicles, military and aerospace fields due to their high operating voltage, high energy density, long cycle life and environmental friendliness. With the popularization and application of smart digital products and the widespread application of new energy vehicles, people's demand for the fast charging performance of lithium batteries has become more urgent. In order to alleviate the problem of long charging time, the development of fast charging technology has become one of the main directions of the industry. High-rate charging can further reduce the time required for charging, thereby achieving the purpose of fast charging. There are many factors that affect fast charging, including the design of positive and negative electrode materials and electrolytes. Among them, the performance of the electrolyte has a key influence on fast charging.

[0003] At present, the fast charging requirements of lithium-ion batteries are met by adding various additives to the electrolyte. However, the fast charging process of lithium batteries using existing electrolytes will result in uneven heat generation and electrolyte decomposition, which will increase the impedance of the lithium battery, and the SEI film formed on the surface of the negative electrode will easily become loose, unstable or even dissolved under high-rate charging, which will cause the capacity of the lithium battery to decay too quickly, affecting the fast charging performance of the lithium battery. Therefore, it is urgent to develop an electrolyte for lithium batteries suitable for fast charging. Summary of the invention

[0004] In order to solve the problems of uneven heat generation during fast charging of lithium batteries using existing electrolytes and increased impedance of lithium batteries due to decomposition of the electrolyte, and to improve the stability of the SEI film formed on the surface of the negative electrode and the fast charging performance of the lithium battery, the present invention provides an electrolyte and a lithium battery using the electrolyte.

[0005] According to a first aspect of the present invention, an electrolyte is provided, which includes a first additive and an organic solvent, wherein the mass fraction of the first additive in the electrolyte is 0.2-1%; the first additive is trimethylphosphoborate tetrafluoroborate; and the organic solvent includes an ether solvent.

[0006] The electrolyte provided by the present invention comprises a first additive trimethylphosphine tetrafluoroborate and an ether organic solvent. First, the first additive trimethylphosphine tetrafluoroborate contains three elements: F, B and P. The F element has a lower lithium ion solvation ability, and the B element has electron deficiency and can capture anions as an anion receptor, so that more free Li is present in the electrolyte. + , improved Li +The transmission performance of the lithium battery is improved, thereby improving the rate performance of the lithium battery, and the P element can make the SEI film formed on the negative electrode surface of the lithium battery have a lower impedance; secondly, an ether solvent is used as the organic solvent in the electrolyte. After being matched with the first additive as a component of the electrolyte, it can promote the formation of a denser, more protective and more conductive SEI film on the negative electrode surface, which not only reduces the interface resistance on the negative electrode surface, but also improves the interface stability on the negative electrode surface, improves the first coulomb efficiency of the lithium battery, and can better protect the silicon-carbon negative electrode during the fast charging of the lithium battery, effectively solving the problem of continuous production and rupture of the SEI film caused by the expansion of the silicon-carbon negative electrode during the fast charging of the lithium battery, significantly improving the fast charging performance of the lithium battery, and increasing the transmission speed of lithium ions in the electrolyte and the negative electrode surface, so that lithium ions can be deintercalated in time at the silicon-carbon negative electrode, avoiding the problem of lithium precipitation due to untimely deintercalation of lithium ions. The electrolyte provided by the present invention forms a more stable SEI film on the surface of the negative electrode of the lithium battery through the above-mentioned two effects, thereby improving the initial coulombic efficiency of the lithium battery, and at the same time improving the decomposition of the electrolyte due to uneven heat generation during the fast charging process of the lithium battery, thereby reducing the impedance of the lithium battery, realizing the rapid transmission of lithium ions, and ultimately improving the fast charging performance of the lithium battery, so that the constant current charging ratio of the lithium battery during fast charging and the capacity retention rate during the cycle process are significantly improved.

[0007] Preferably, the ether solvent includes at least one of n-propyl ether, ethyl butyl ether, n-butyl ether, isobutyl ether, n-pentyl ether and isopentyl ether.

[0008] Preferably, the electrolyte further comprises a second additive, the mass fraction of the second additive in the electrolyte is 0.2-0.8%; the structure of the second additive is as shown in Formula I;

[0009]

[0010] A contains at least one of a P atom and a B atom;

[0011] R1, R2, R3 are independently selected from -H, One of the .

[0012] Preferably, the structure of the second additive is as shown in Formula II;

[0013]

[0014] Adding the second additive with a structure as shown in Formula II to the above electrolyte can promote the formation of a more compact, uniform and stable CEI film on the positive electrode surface, and the second additive can be oxidized preferentially before other components in the electrolyte, thereby forming a CEI film with better protection effect on the positive electrode interface, and can also effectively inhibit the decomposition of the electrolyte and the dissolution of transition metals. The electrolyte provided by this scheme forms a more stable CEI film and SEI film on the surface of the positive and negative electrodes of the lithium battery by adding the first additive, the second additive and the ether organic solvent at the same time, thereby improving the first coulomb efficiency of the lithium battery, and at the same time improving the electrolyte decomposition caused by uneven heat generation during the fast charging process of the lithium battery, reducing the impedance of the lithium battery, realizing the rapid transmission of lithium ions, and finally improving the fast charging performance of the lithium battery, so that the constant current charging ratio of the lithium battery during fast charging and the capacity retention rate during the cycle process are significantly improved.

[0015] Preferably, the electrolyte further comprises a lithium salt additive, and the mass fraction of the lithium salt additive in the electrolyte is 1 to 3%.

[0016] Preferably, the lithium salt additive includes at least one of lithium bis(fluorosulfonyl)imide (LiFSI) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).

[0017] Preferably, the lithium salt additive is a mixture of lithium bis(fluorosulfonyl)imide (LiFSI) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) in a mass ratio of 0.5-5:0.2-2.

[0018] Preferably, the above-mentioned organic solvent also includes a carbonate solvent.

[0019] Preferably, the carbonate solvent includes at least one of propylene carbonate (PC), ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), and vinylene carbonate (VC).

[0020] Preferably, the organic solvent is a mixture of ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), fluoroethylene carbonate (FEC), n-butyl ether and isoamyl ether in a mass ratio of 15-25:35-45:5-15:3-8:12-17:5-15.

[0021] The first additive and the second additive are compounded with a low-polarity ether solvent, a carbonate solvent, and a lithium salt additive to form an electrolyte, and the electrolyte is applied to a lithium battery. This is beneficial for forming a stable CEI film and a SEI film at the positive electrode and the negative electrode, respectively, and can reduce the binding energy between the solvent and the lithium ions in the electrolyte, thereby reducing the battery impedance, achieving rapid transmission of lithium ions, and ultimately improving the fast charging performance of the lithium battery.

[0022] Preferably, the electrolyte further comprises a lithium salt, and the concentration of the lithium salt in the electrolyte is 1 to 1.5 mol / L.

[0023] Preferably, the lithium salt includes at least one of lithium hexafluorophosphate and lithium tetrafluoroborate.

[0024] According to a second aspect of the present invention, a lithium battery is provided, the lithium battery comprising the above-mentioned electrolyte.

[0025] The electrolyte provided by the present invention is applied to lithium batteries to give the lithium batteries excellent fast charging performance.

[0026] Preferably, the lithium battery further comprises a negative electrode sheet, the negative electrode sheet comprising a negative electrode current collector and a negative electrode active coating disposed on at least one surface of the negative electrode current collector, the negative electrode active coating comprising a silicon-based material

[0027] Preferably, the silicon-based material includes at least one of silicon monoxide and silicon carbon materials. DETAILED DESCRIPTION

[0028] The following is a further clear and complete description of the technical features in the technical solution provided by the present invention in conjunction with the specific implementation methods. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] A lithium battery is prepared by the following steps:

[0031] 1. Preparation of positive electrode

[0032] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2, conductive agent acetylene black and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3 and added to a solvent N-methylpyrrolidone (NMP). The mixture is evenly mixed to obtain a positive electrode slurry with a solid content of 45%. The positive electrode slurry is coated on both surfaces of the positive electrode current collector aluminum foil to form a positive electrode active coating. After vacuum drying, a positive electrode sheet is obtained.

[0033] 2. Preparation of negative electrode

[0034] Silicon carbon (SiC) negative electrode active material, conductive carbon black (SP) and binder polyacrylic acid (PAA) were mixed in a mass ratio of 95:2:3 and added into deionized water solvent, mixed evenly to prepare a negative electrode slurry with a solid content of 45%, the negative electrode slurry was coated on both surfaces of the negative electrode current collector copper foil to form a negative electrode active coating, and after vacuum drying, a negative electrode sheet was prepared;

[0035] 3. Preparation of Diaphragm

[0036] Celgard 2400 diaphragm produced by Celgard Diaphragm Co., Ltd. of the United States is used.

[0037] 4. Preparation of Electrolyte

[0038] The electrolyte comprises a first additive, a second additive, a lithium salt additive, an organic solvent and a lithium salt, wherein the mass fraction of the first additive in the electrolyte is 0.5%, the mass fraction of the second additive in the electrolyte is 0.5%, and the mass fraction of the lithium salt additive in the electrolyte is 2%;

[0039] The first additive is trimethylphosphine tetrafluoroborate; the structure of the second additive is shown in Formula II;

[0040]

[0041] The lithium salt additive is prepared by mixing lithium bis(fluorosulfonyl)imide LiFSI and lithium bis(trifluoromethanesulfonyl)imide LiTFSI in a mass ratio of 2:1.

[0042] The organic solvent is prepared by mixing ethylene carbonate EC, dimethyl carbonate DMC, diethyl carbonate DEC, fluoroethylene carbonate FEC, n-butyl ether and isoamyl ether in a mass ratio of 20:40:10:5:15:10;

[0043] The electrolyte used in this embodiment is prepared by the following steps: dissolving the lithium salt LiPF6 in an organic solvent to prepare a lithium salt solution with a concentration of 1.3 mol / L, adding the first additive, the second additive and the lithium salt additive to the lithium salt solution, mixing them evenly, to prepare the electrolyte.

[0044] 5. Assembly of lithium batteries

[0045] The positive electrode sheet, separator and negative electrode sheet are stacked in order, so that the separator is placed between the positive and negative electrode sheets to play an isolating role, and then wound to obtain a bare battery cell, which is placed in an outer packaging shell, dried and injected with the above-mentioned electrolyte, and subjected to vacuum packaging, standing, forming, shaping and other processes to obtain a lithium battery.

[0046] Example 2

[0047] This embodiment provides a lithium battery. Compared with the embodiment 1, the difference in structure is: the content and ratio of each component in the electrolyte are different;

[0048] The electrolyte used in this embodiment includes a first additive, a second additive, a lithium salt additive, an organic solvent and a lithium salt, the mass fraction of the first additive in the electrolyte is 0.2%, the mass fraction of the second additive in the electrolyte is 0.8%, and the mass fraction of the lithium salt additive in the electrolyte is 3%;

[0049] The first additive is trimethylphosphine tetrafluoroborate; the structure of the second additive is shown in Formula II;

[0050]

[0051] The lithium salt additive is a mixture of LiFSI and LiTFSI in a mass ratio of 0.5:2;

[0052] The organic solvent is a mixture of EC, DMC, DEC, FEC, n-butyl ether, and isoamyl ether in a mass ratio of 15:45:5:3:17:15;

[0053] The electrolyte used in this embodiment is prepared by the following steps: dissolving the lithium salt LiPF6 in an organic solvent to prepare a lithium salt solution with a concentration of 1 mol / L, adding the first additive, the second additive and the lithium salt additive to the lithium salt solution, mixing them evenly, to prepare the electrolyte.

[0054] Except for the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.

[0055] Example 3

[0056] This embodiment provides a lithium battery. Compared with the embodiment 1, the difference in structure is: the content and ratio of each component in the electrolyte are different;

[0057] The electrolyte used in this embodiment includes a first additive, a second additive, a lithium salt additive, an organic solvent and a lithium salt, the mass fraction of the first additive in the electrolyte is 1%, the mass fraction of the second additive in the electrolyte is 0.2%, and the mass fraction of the lithium salt additive in the electrolyte is 1%;

[0058] The first additive is trimethylphosphine tetrafluoroborate; the structure of the second additive is shown in Formula II;

[0059]

[0060] The lithium salt additive is a mixture of lithium bis(fluorosulfonyl)imide (LiFSI) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) in a mass ratio of 5:0.2.

[0061] The organic solvent is a mixture of EC, DMC, DEC, FEC, n-butyl ether, and isoamyl ether in a mass ratio of 25:35:15:8:12:5;

[0062] The electrolyte used in this embodiment is prepared by the following steps: dissolving the lithium salt LiPF6 in an organic solvent to prepare a lithium salt solution with a concentration of 1.5 mol / L, adding the first additive, the second additive and the lithium salt additive to the lithium salt solution, mixing them evenly, to obtain an electrolyte.

[0063] Except for the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.

[0064] Example 4

[0065] This embodiment provides a lithium battery, which is different from that of embodiment 1 in that: the structure of the second additive contained in the electrolyte is as shown in formula III;

[0066]

[0067] Except for the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.

[0068] Example 5

[0069] This embodiment provides a lithium battery, which is different from that of embodiment 1 in that: the structure of the second additive contained in the electrolyte is as shown in formula IV;

[0070]

[0071] Except for the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in Example 1.

[0072] Example 6

[0073] This embodiment provides a lithium battery, and compared with the embodiment 1, the difference in structure is: the first additive is used in an equal amount to replace the second additive. Except for the above difference, the materials, formula ratio and preparation operation used in this comparative example are strictly consistent with those in the embodiment 1.

[0074] Example 7

[0075] This embodiment provides a lithium battery, and compared with the embodiment 1, the difference in structure is that the mass fraction of the second additive in the electrolyte is 0.1%. In addition to the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.

[0076] Example 8

[0077] This embodiment provides a lithium battery, and compared with the embodiment 1, the difference in structure is that the mass fraction of the second additive in the electrolyte is 1.0%. In addition to the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.

[0078] Example 9

[0079] This embodiment provides a lithium battery, and compared with the embodiment 1, the difference in structure is that the mass fraction of the lithium salt additive in the electrolyte is 0.5%. In addition to the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.

[0080] Example 10

[0081] This embodiment provides a lithium battery, and compared with the embodiment 1, the difference in structure is that the mass fraction of the lithium salt additive in the electrolyte is 3.5%. In addition to the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.

[0082] Embodiment 11

[0083] This embodiment provides a lithium battery, and compared with the embodiment 1, the difference in structure is that the lithium salt additive in the electrolyte is LiFSI. In addition to the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.

[0084] Example 12

[0085] This embodiment provides a lithium battery. Compared with the embodiment 1, the difference in structure is that the lithium salt additive in the electrolyte is LiTFSI. In addition to the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.

[0086] Embodiment 13

[0087] This embodiment provides a lithium battery, and compared with the embodiment 1, the difference in structure is that the organic solvent in the electrolyte is a mixture of n-butyl ether and isoamyl ether in a mass ratio of 60:40. In addition to the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.

[0088] Embodiment 14

[0089] This embodiment provides a lithium battery. Compared with the embodiment 1, the difference in structure is that the organic solvent in the electrolyte is a mixture of EC, DMC, EMC, n-butyl ether, and isoamyl ether in a mass ratio of 20:40:15:15:10. Except for the above differences, the materials, formula ratios, and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.

[0090] Embodiment 15

[0091] This embodiment provides a lithium battery. Compared with the embodiment 1, the difference in structure is that the organic solvent in the electrolyte is a mixture of EC, DMC, DEC, FEC, and n-butyl ether in a mass ratio of 20:40:10:5:25. Except for the above differences, the materials, formula ratios, and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.

[0092] Example 16

[0093] This embodiment provides a lithium battery. Compared with the embodiment 1, the difference in structure is that the organic solvent in the electrolyte is a mixture of EC, DMC, DEC, FEC, n-propyl ether, and n-pentyl ether in a mass ratio of 20:40:10:5:15:10. Except for the above differences, the materials, formula ratios, and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.

[0094] Embodiment 17

[0095] This embodiment provides a lithium battery. Compared with the embodiment 1, the difference in structure is that the components of the electrolyte are different. Specifically, the organic solvent is a mixture of EC, DMC, DEC, FEC, n-butyl ether, and isoamyl ether in a mass ratio of 20:35:10:5:10:20. Except for the above differences, the materials, formula ratios, and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.

[0096] Embodiment 18

[0097] This embodiment provides a lithium battery. Compared with the embodiment 1, the difference in structure is that the components of the electrolyte are different. Specifically, the organic solvent is a mixture of EC, DMC, DEC, FEC, n-butyl ether, and isoamyl ether in a mass ratio of 20:40:10:7:20:3. Except for the above differences, the materials, formula ratios, and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.

[0098] Embodiment 19

[0099] This embodiment provides a lithium battery. Compared with the embodiment 1, the difference in structure is that the components of the electrolyte are different. Specifically, the organic solvent is a mixture of EC, DMC, DEC, FEC, n-butyl ether, and isoamyl ether in a mass ratio of 20:30:20:10:15:10. Except for the above differences, the materials, formula ratios, and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.

[0100] Embodiment 20

[0101] This embodiment provides a lithium battery. Compared with the embodiment 1, the difference in structure is that the components of the electrolyte are different. Specifically, the organic solvent is a mixture of EC, DMC, DEC, FEC, n-butyl ether, and isoamyl ether in a mass ratio of 20:40:3:12:15:10. Except for the above differences, the materials, formula ratios, and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.

[0102] Comparative Example 1

[0103] This comparative example provides a lithium battery, which is different from Example 1 in that the electrolyte does not contain the first additive and the second additive. Except for the above differences, the materials, formula ratios and preparation operations used in this comparative example are strictly consistent with those in Example 1.

[0104] Comparative Example 2

[0105] This comparative example provides a lithium battery, which is different from Example 1 in that an equal amount of the second additive is used to replace the first additive. Except for the above differences, the materials, formula ratios and preparation operations used in this comparative example are strictly consistent with those in Example 1.

[0106] Comparative Example 3

[0107] This comparative example provides a lithium battery. Compared with Example 1, the difference in composition is that the organic solvent in the electrolyte is a mixture of EC, DMC, DEC, and FEC in a mass ratio of 25:45:15:15. Except for the above differences, the materials, formula ratios, and preparation operations used in this comparative example are strictly consistent with those in Example 1.

[0108] Comparative Example 4

[0109] This comparative example provides a lithium battery, which is different from Example 1 in that the mass fraction of the first additive in the electrolyte is 0.1%. Except for the above differences, the materials, formula ratios and preparation operations used in this comparative example are strictly consistent with those in Example 1.

[0110] Comparative Example 5

[0111] This comparative example provides a lithium battery, which is different from Example 1 in that the mass fraction of the first additive in the electrolyte is 1.2%. Except for the above differences, the materials, formula ratios and preparation operations used in this comparative example are strictly consistent with those in Example 1.

[0112] Test Case

[0113] 1. Participants

[0114] In this test example, the lithium batteries prepared in Examples 1 to 20 and Comparative Examples 1 to 5 were used as test objects to conduct relevant performance tests.

[0115] 2. Test content

[0116] (1) First Coulomb efficiency

[0117] At 25°C, the lithium battery was charged to 4.2V at a constant current and constant voltage rate of 0.33C and allowed to stand for 10 minutes. Then, the lithium battery was discharged to 2.5V at a constant current rate of 0.33C and allowed to stand for 10 minutes. The first coulombic efficiency of the lithium battery was calculated.

[0118] First coulombic efficiency (%) = total capacity of lithium battery discharged at 0.33C for the first time / total capacity of lithium battery charged at 0.33C for the first time × 100%.

[0119] (2) Capacity retention rate after 900 cycles at 1C / 1C at room temperature

[0120] At 25°C, the lithium battery was charged at a constant current and constant voltage rate of 1C to 4.2V, cut off at 0.05C, and allowed to stand for 10 minutes. Then, the lithium battery was discharged at a constant current rate of 1C to 2.5V and allowed to stand for 10 minutes. This was considered one charge and discharge cycle. The lithium battery was charged and discharged for 900 cycles according to the above method, and the capacity retention rate of the lithium battery after 900 cycles of charge and discharge at 1C / 1C was calculated.

[0121] The capacity retention rate (%) of a lithium battery after N cycles = (discharge capacity at the Nth cycle / first discharge capacity) × 100%, where N is the number of cycles of the lithium battery.

[0122] (3) 6C rate performance at room temperature

[0123] At 25°C, the lithium battery was discharged at a constant current rate of 1C to 2.5V and allowed to stand for 10 minutes. Then, the lithium battery was charged at a constant current and constant voltage rate of 6C to 4.2V, with a cut-off current of 0.05C and allowed to stand for 10 minutes. The constant current charging capacity Q1, the constant current and constant voltage charging total capacity Q2 and the highest temperature during fast charging (i.e., the highest temperature during 6C rate charging) of the lithium battery were recorded. The 6C rate charging constant current charging ratio was calculated according to the following formula: 6C rate charging constant current charging ratio = constant current charging capacity Q1 / constant current and constant voltage charging total capacity Q2 × 100%, wherein, the constant current and constant voltage charging total capacity Q2 = constant current charging capacity + constant voltage charging capacity.

[0124] 3. Experimental results

[0125] Table 1. Test results of relevant performance of lithium battery

[0126]

[0127]

[0128] The relevant performance test results of the lithium batteries prepared in Examples 1 to 20 and Comparative Examples 1 to 5 are shown in Table 1.

[0129] Compared with Comparative Examples 1 to 5, the electrolyte of the lithium battery provided in Examples 1 to 20 contains the first additive trimethylphosphine tetrafluoroborate and uses an ether solvent as the organic solvent. The test results show that the first coulombic efficiency, the capacity retention rate of 900 cycles of 1C / 1C cycles at room temperature and the 6C rate performance of the lithium battery provided in Examples 1 to 20 are better than those of Comparative Examples 1 to 5, while the maximum temperature of 6C rate charging is lower than that of Comparative Examples 1 to 5. The reason for the above phenomenon is that the synergistic effect between the first additive trimethylphosphine tetrafluoroborate and the ether organic solvent contained in the electrolyte of the lithium battery provided in Examples 1 to 20 forms a more stable SEI film on the surface of the negative electrode of the lithium battery, thereby improving the initial coulombic efficiency of the lithium battery. At the same time, it improves the decomposition of the electrolyte due to uneven heat generation during the fast charging process of the lithium battery, thereby reducing the maximum temperature of 6C rate charging, reducing the impedance of the lithium battery, and realizing the rapid transmission of lithium ions, thereby ultimately improving the fast charging performance of the lithium battery, and significantly improving the constant current charging ratio of the lithium battery during fast charging and the capacity retention rate during the cycle.

[0130] The electrolyte in the lithium battery provided in Example 1 contains, in addition to the first additive trimethylphosphine tetrafluoroborate and an ether organic solvent, a second additive as shown in Ⅱ, and the mass fraction of the second additive is controlled within the range of 0.2 to 0.8%. Compared with Example 1, Example 6 contains only the first additive but does not contain the second additive. The test results show that the first coulombic efficiency, the capacity retention rate of 900 cycles of 1C / 1C cycles at room temperature, and the 6C rate performance of the lithium battery provided in Example 6 are worse than those in Example 1, and the maximum temperature of 6C rate charging is higher than that in Example 1. This is mainly because: the lithium battery provided in Example 1 can promote the formation of a more dense, uniform, and stable CEI film on the positive electrode surface by adding the second additive with a structure as shown in Formula Ⅱ to the electrolyte, and the second The additive can be oxidized before other components in the electrolyte, thereby forming a CEI film with better protection effect on the positive electrode interface, and can also effectively inhibit the decomposition of the electrolyte and the dissolution of transition metals. The synergistic effect between the first additive, the second additive and the ether organic solvent enables the surfaces of the positive and negative electrodes of the lithium battery to form more stable CEI film and SEI film, respectively, thereby improving the first coulombic efficiency of the lithium battery, and at the same time improving the decomposition of the electrolyte caused by uneven heat generation during the fast charging process of the lithium battery, thereby reducing the maximum temperature of 6C rate charging, reducing the impedance of the lithium battery, realizing the rapid transmission of lithium ions, and ultimately improving the fast charging performance of the lithium battery, so that the constant current charging ratio of the lithium battery during fast charging and the capacity retention rate during the cycle process are significantly improved.

[0131] Compared with Example 1, the mass fractions of the second additive in the electrolyte of the lithium batteries provided in Examples 7 and 8 are 0.1% and 1.0%, respectively; the mass fractions of the lithium salt additive in the electrolyte of the lithium batteries provided in Examples 9 and 10 are 0.5% and 3.5%, respectively; the electrolytes of the lithium batteries provided in Examples 11 and 12 contain only one lithium salt additive. The test results show that the first coulombic efficiency, the capacity retention rate of 900 cycles of 1C / 1C cycles at room temperature, and 6C rate performance of the lithium batteries provided in Examples 7 to 12 are worse than those in Example 1, and the maximum temperature of 6C rate charging is higher than that in Example 1.

[0132] Compared with Example 1, the organic solvent in the electrolyte of the lithium battery provided in Examples 13 to 20 does not meet the condition that "the organic solvent is composed of ethylene carbonate, dimethyl carbonate, diethyl carbonate, fluoroethylene carbonate, n-butyl ether, and isopentyl ether in a mass ratio of 15 to 25:35 to 45:5 to 15:3 to 8:12 to 17:5 to 15". The test results show that the first coulomb efficiency, the capacity retention rate of 900 cycles of 1C / 1C cycles at room temperature, and 6C rate performance of the lithium batteries provided in Examples 13 to 20 are worse than those in Example 1, and the maximum temperature of 6C rate charging is higher than that in Example 1.

[0133] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.

Claims

1. An electrolyte, characterized in that: The electrolyte comprises a first additive and an organic solvent, wherein the mass fraction of the first additive in the electrolyte is 0.2 to 1%; The first additive is trimethylphosphine tetrafluoroborate; The organic solvent includes an ether solvent.

2. The electrolyte according to claim 1, characterized in that: The ether solvent includes at least one of n-propyl ether, ethyl butyl ether, n-butyl ether, isobutyl ether, n-pentyl ether and isopentyl ether.

3. The electrolyte according to claim 1, characterized in that: The electrolyte further comprises a second additive, wherein the mass fraction of the second additive in the electrolyte is 0.2 to 0.8%; The structure of the second additive is shown in Formula I; A contains at least one of a P atom and a B atom; R1, R2, R3 are independently selected from One of the .

4. The electrolyte according to claim 3, characterized in that: The structure of the second additive is shown in Formula II; 5. The electrolyte according to claim 1, characterized in that: The electrolyte further comprises a lithium salt additive, wherein the mass fraction of the lithium salt additive in the electrolyte is 1 to 3%; The lithium salt additive includes at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethanesulfonyl)imide.

6. The electrolyte according to claim 2, characterized in that: The organic solvent also includes a carbonate solvent; The carbonate solvent includes at least one of propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, fluoroethylene carbonate, ethyl methyl carbonate, and vinylene carbonate.

7. The electrolyte according to claim 6, characterized in that: The organic solvent is prepared by mixing ethylene carbonate, dimethyl carbonate, diethyl carbonate, fluoroethylene carbonate, n-butyl ether and isopentyl ether in a mass ratio of 15-25:35-45:5-15:3-8:12-17:5-15.

8. The electrolyte according to claim 1, characterized in that: The electrolyte further comprises a lithium salt, wherein the concentration of the lithium salt in the electrolyte is 1 to 1.5 mol / L; The lithium salt includes at least one of lithium hexafluorophosphate and lithium tetrafluoroborate.

9. A lithium battery, characterized in that: The lithium battery comprises the electrolyte according to any one of claims 1 to 8.

10. The lithium battery according to claim 9, characterized in that: The lithium battery further includes a negative electrode sheet, which includes a negative electrode collector and a negative electrode active coating disposed on at least one surface of the negative electrode collector, wherein the negative electrode active coating contains a silicon-based material.

Citation Information

Patent Citations

  • Lithium ion battery electrolytic solution and lithium ion battery

    CN111653829A

  • Electrolytic solution and lithium ion battery containing same

    CN112271338A

  • Lithium secondary battery electrolyte, lithium secondary battery and electric equipment

    CN115799636A

  • Electrolyte and lithium ion battery

    CN116247301A

  • Electrolyte, electrolytic solution for lithium ion secondary battery comprising the electrolyte, and lithium ion secondary battery using the electrolytic solution

    KR1020090052870A