OLED display structure and manufacturing method

By introducing a reflective film layer, a prism layer, and a diffusion layer into the OLED display, and designing a PVA+TAC layer on the color filter layer, the problems of insufficient brightness and contrast are solved, achieving higher light utilization and uniformity, making it suitable for high-brightness application scenarios.

CN118973305APending Publication Date: 2024-11-15广西自贸区睿显科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411014283.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing OLED displays have room for improvement in brightness, light uniformity, and contrast, especially due to uneven light and dark caused by the gaps between anode pixels and the impact of light reflection from metallic materials on contrast.

Method used

In the OLED display structure, a reflective film layer, a prism layer, and a diffusion layer are introduced. The light reflection and diffusion performance are improved by optimizing the process. A PVA+TAC layer is designed on the color filter layer to reduce ambient light interference. Specific materials and processes such as spin coating, exposure, development, and atomic layer deposition technology are used to stack the layers one by one.

Benefits of technology

It significantly improves the brightness and contrast of the display, enhances light utilization and uniformity, reduces the impact of ambient light, and performs particularly well in high-brightness applications, while extending the device's battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973305A_ABST
    Figure CN118973305A_ABST
Patent Text Reader

Abstract

The invention provides an OLED display structure and a manufacturing method thereof. The OLED display structure comprises a CMOS IC layer located at the bottom; a reflecting layer is laid on the CMOS IC layer, and the reflecting layer comprises a reflecting film layer and a reflecting medium layer which are stacked from bottom to top; a CMOS IC layer is attached to the bottom surface of the reflective film layer, and an anode layer is laid on the top surface of the reflective dielectric layer; the anode layer is formed by stripping Al and ITO materials, and a gap Pitch exists between the Al and ITO materials; a light-emitting layer is laid on the anode layer, and the light-emitting layer comprises a hole injection layer, a hole transport layer, an EML light-emitting lamination layer, an electron transport layer and an electron injection layer which are stacked from bottom to top; an anode layer is attached to the bottom surface of the hole injection layer, a cathode layer is laid on the electron injection layer, and the cathode layer comprises a cathode material layer and an aluminum oxide film layer which are stacked from bottom to top; the prism Lens layer covers the top surface of the aluminum oxide film layer; the prism Lens layer is covered with an upper diffusion layer, and the upper diffusion layer is covered with a color film layer; and an optical film layer covers the color film layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of display technology and relates to a silicon-based OLED, in particular to an OLED display structure and a manufacturing method. Background Art

[0002] OLED performance requirements are gradually increasing to match different terminal application scenarios. The most important indicators are brightness, light uniformity, and contrast. Given the technical bottleneck of improving the luminous efficiency of existing materials, improving it through structural optimization is the most effective and direct way to improve it at this stage.

[0003] Since the gap between anode pixels is an invalid non-luminous Pitch area, there will be a certain light and dark unevenness problem, and the structure can be optimized. Similarly, when the single-color light emission brightness is relatively high, because the metal material in the structure has a certain reflection of the ambient light, it will affect the contrast to a certain extent.

[0004] The existing technology still needs to be further improved in terms of the comprehensiveness of display effects such as reflectivity, brightness, uniformity and contrast. Summary of the invention

[0005] The purpose of the present invention is to solve the above problems in the prior art and to propose an OLED display structure and a manufacturing method.

[0006] The object of the present invention can be achieved by the following technical scheme: an OLED display structure, comprising a CMOS IC layer at the bottom; a reflective layer is laid on the CMOS IC layer, and the reflective layer comprises a reflective film layer and a reflective medium layer stacked from bottom to top; the bottom surface of the reflective film layer is attached to the CMOS IC layer; IC layer, an anode layer is laid on the top surface of the reflective medium layer; the anode layer is made of Al and ITO material and there is a gap Pitch after peeling; a light-emitting layer is laid on the anode layer, and the light-emitting layer includes a hole injection layer, a hole transport layer, an EML light-emitting stack, an electron transport layer and an electron injection layer stacked from bottom to top; the bottom surface of the hole injection layer is covered with the anode layer, and a cathode layer is laid on the electron injection layer, and the cathode layer includes a cathode material layer and an aluminum oxide film layer stacked from bottom to top; the top surface of the aluminum oxide film layer is covered with a prism Lens layer; the prism Lens layer is covered with an upper diffusion layer, and the upper diffusion layer is covered with a color filter layer, and the color filter layer is formed by R color filter pixel points, B color filter pixel points, and G color filter pixel points arranged in sequence; the color filter layer is covered with an optical film layer.

[0007] A method for manufacturing an OLED display structure, the manufacturing method is applied to the above-mentioned OLED display structure, and the manufacturing method comprises the following steps:

[0008] S1: After cleaning the silicon substrate, a CMOS IC layer is fabricated on the silicon substrate using photolithography and etching processes, which serves as a switch for individually controlling the hole transmission of the corresponding pixel anode.

[0009] S2 makes the reflection layer:

[0010] a. The reflective film layer is manufactured by using a spin coating process, an exposure process and a development process in sequence; the coating of the reflective film layer contains magnesium and silver;

[0011] b. A reflective dielectric layer is manufactured on the reflective film layer through a spin coating process, an exposure process and a development process in sequence; the reflective dielectric layer is made of a non-conductive and reflective material, which can effectively reflect the light emitted downward by the anode Pitch and the light transmitted through the anode layer upward, thereby improving the utilization rate of the light emission, and the reflectivity of the reflective layer reaches more than 95%.

[0012] S3: Making the anode layer: Making the anode layer by sequentially using the ITO evaporation process and the AL evaporation process;

[0013] S4 makes the light-emitting layer: uses a high-precision mask to evaporate the organic material to make the light-emitting layer;

[0014] S5: Preparation of cathode layer: Use a high-precision mask to evaporate the cathode material, which is a mixture of magnesium, silver and lutetium, to obtain a cathode material layer; after the evaporation, use trimethylaluminum and water as materials, use atomic layer deposition technology on the cathode material layer to prepare an aluminum oxide film layer, and then complete the cathode layer preparation;

[0015] S6 covers the prism lens layer: spin coating, exposure and development processes are used in sequence to make the entire prism lens layer on the aluminum oxide film layer of the cathode layer;

[0016] S7 covers the diffusion layer: a diffusion layer is formed on the entire surface of the prism lens layer by using a spin coating process and a coating process in sequence;

[0017] The optical diffusion layer is prepared by hydrolysis and polycondensation reaction of aminopropyl trimethoxysilane, vinyl trimethoxysilane and phenyl triethoxysilane to produce an organosilicon microsphere precursor core, and further in-situ growth of nano ZnO / CeO2 / Al2O3 on the surface thereof, and the core-shell light diffusion microspheres are grafted and copolymerized with polyurethane acrylate by chemical cross-linking of glutaraldehyde intermediate and amino group, thereby significantly improving the stability of the light diffusion layer; a layer of randomly dispersed micron-structured diffusion particles is grown on the surface, so that the light undergoes multiple refraction, reflection and diffraction phenomena through the diffusion layer, so as to correct the light into a uniform surface light source, achieve the effect of optical diffusion, make the light display more uniform and soft, and thus improve the optical problem of pitch brightness non-uniformity;

[0018] Because nano ZnO / CeO2 / Al2O3 is unevenly distributed on the surface of silicone microspheres, when light is projected into the light diffusion layer, refraction and diffuse reflection occur at different angles and directions, which significantly improves the diffusion performance of the diffusion film for visible light. The transmittance of visible light is more than 98%, the transmittance of ultraviolet light is less than 12%, and the transmittance of 400nm~460nm short-wave blue light is less than 15%.

[0019] S8 covered with color film layer:

[0020] Production of R color film pixels: spin coating, exposure and development processes are used in sequence to produce R color film at the anode CD position;

[0021] Production of pixel points of B color film: At the anode CD position adjacent to the R color film, the B color film is produced by sequentially adopting the spin coating process, exposure process and development process;

[0022] G color film pixel production: At the anode CD position adjacent to the B color film, the G color film is produced by using the spin coating process, exposure process and development process in sequence;

[0023] S9 covers the optical film layer: a PVA film layer is made on the entire surface of the color film layer by spin coating or printing transfer, and then a TAC film layer is made on the entire surface of the PVA film layer by spin coating or printing transfer as a protective layer to complete the production of the optical film layer.

[0024] The optical film layer can effectively resist ambient light, reduce display interference, and improve contrast. The tested contrast can be improved by 3 to 5 times, and the greater the brightness, the greater the improvement ratio.

[0025] An OLED display structure includes a CMOS IC layer at the bottom; the CMOS A reflective layer is laid on the IC layer, and the reflective layer includes a reflective film layer and a reflective medium layer stacked from bottom to top; the bottom surface of the reflective film layer is covered with the CMOSIC layer, and the top surface of the reflective medium layer is laid with an anode layer; the anode layer is made of Al and ITO materials, and there is a gap Pitch after peeling; a light-emitting layer is laid on the anode layer, and the light-emitting layer includes a hole injection layer, a hole transport layer, an EML light-emitting stack, an electron transport layer and an electron injection layer stacked from bottom to top; the bottom surface of the hole injection layer is covered with the anode layer, and a cathode layer is laid on the electron injection layer, and the cathode layer includes a cathode material layer and an aluminum oxide film layer stacked from bottom to top; the top surface of the aluminum oxide film layer covers the first prism Lens layer; the first prism Lens layer is covered with an upper diffusion layer, and the upper diffusion layer is covered with a color filter layer, and the color filter layer is formed by R color filter pixel points, B color filter pixel points, and G color filter pixel points arranged alternately in sequence; the color filter layer covers the second prism Lens layer, and the second prism Lens layer is covered with an optical film layer.

[0026] A method for manufacturing an OLED display structure, the manufacturing method is applied to the above-mentioned OLED display structure, and the manufacturing method comprises the following steps:

[0027] S1: After cleaning the silicon substrate, a CMOS IC layer is fabricated on the silicon substrate using photolithography and etching processes, which serves as a switch for individually controlling the hole transmission of the corresponding pixel anode.

[0028] S2 makes the reflection layer:

[0029] a. The reflective film layer is manufactured by using a spin coating process, an exposure process and a development process in sequence; the coating of the reflective film layer contains magnesium and silver;

[0030] b. A reflective dielectric layer is manufactured on the reflective film layer through a spin coating process, an exposure process and a development process in sequence; the reflective dielectric layer is made of a non-conductive and reflective material, which can effectively reflect the light emitted downward by the anode Pitch and the light transmitted through the anode layer upward, thereby improving the utilization rate of the light emission, and the reflectivity of the reflective layer reaches more than 95%.

[0031] S3: Making the anode layer: Making the anode layer by sequentially using the ITO evaporation process and the AL evaporation process;

[0032] S4 makes the light-emitting layer: uses a high-precision mask to evaporate the organic material to make the light-emitting layer;

[0033] S5: Preparation of cathode layer: Use a high-precision mask to evaporate the cathode material, which is a mixture of magnesium, silver and lutetium, to obtain a cathode material layer; after the evaporation, use trimethylaluminum and water as materials, use atomic layer deposition technology on the cathode material layer to prepare an aluminum oxide film layer, and then complete the cathode layer preparation;

[0034] S6: Covering the first prism lens layer: using a spin coating process, an exposure process and a development process in sequence to manufacture the entire first prism lens layer on the aluminum oxide film layer of the cathode layer;

[0035] S7: Spin coating and coating are used to form a diffusion layer on the entire surface of the first prism lens layer;

[0036] The optical diffusion layer is prepared by hydrolysis and polycondensation reaction of aminopropyl trimethoxysilane, vinyl trimethoxysilane and phenyl triethoxysilane to produce an organosilicon microsphere precursor core, and further in-situ growth of nano ZnO / CeO2 / Al2O3 on the surface thereof, and the core-shell light diffusion microspheres are grafted and copolymerized with polyurethane acrylate by chemical cross-linking of glutaraldehyde intermediate and amino group, thereby significantly improving the stability of the light diffusion layer; a layer of randomly dispersed micron-structured diffusion particles is grown on the surface, so that the light undergoes multiple refraction, reflection and diffraction phenomena through the diffusion layer, so as to correct the light into a uniform surface light source, achieve the effect of optical diffusion, make the light display more uniform and soft, and thus improve the optical problem of pitch brightness non-uniformity;

[0037] Because nano ZnO / CeO2 / Al2O3 is unevenly distributed on the surface of silicone microspheres, when light is projected into the light diffusion layer, refraction and diffuse reflection occur at different angles and directions, which significantly improves the diffusion performance of the diffusion film for visible light. The transmittance of visible light is more than 98%, the transmittance of ultraviolet light is less than 12%, and the transmittance of 400nm~460nm short-wave blue light is less than 15%.

[0038] S8 covered with color film layer:

[0039] Production of R color film pixels: spin coating, exposure and development processes are used in sequence to produce R color film at the anode CD position;

[0040] Production of pixel points of B color film: At the anode CD position adjacent to the R color film, the B color film is produced by sequentially adopting the spin coating process, exposure process and development process;

[0041] G color film pixel production: At the anode CD position adjacent to the B color film, the G color film is produced by using the spin coating process, exposure process and development process in sequence;

[0042] S9 covers the second prism Lens layer: the entire second prism Lens layer is made on the color film layer using spin coating, exposure and development processes;

[0043] S10 covers the optical film layer: a PVA film layer is formed on the entire surface of the second prism Lens layer by spin coating or printing transfer, and then a TAC film layer is formed on the entire surface of the PVA film layer by spin coating or printing transfer as a protective layer to complete the production of the optical film layer.

[0044] The optical film layer can effectively resist ambient light, reduce display interference, and improve contrast. The tested contrast can be improved by 3 to 5 times, and the greater the brightness, the greater the improvement ratio.

[0045] Preferably, the thickness of the reflective film layer in step S2 is The thickness of the reflective medium layer is The thicker design of the reflective film layer is to maximize the light reflection efficiency, thereby improving the brightness and energy efficiency of the display screen; the relatively thin thickness of the reflective medium layer helps to maintain good optical performance without increasing the thickness of the overall structure too much; in step S3, the thickness of the anode layer is This thickness range is to balance the conductivity and transparency. Too thick will affect its transparency, thus affecting the display effect. In step S4, the thickness of the light-emitting layer is 2000-2900nm, which helps to achieve uniform and efficient light emission to ensure uniform distribution of light and effective light emission. In step S5, the thickness of the cathode material layer is The thickness of the aluminum oxide film is The cathode material layer is designed to be thin to ensure good electron injection and transparency, while the thickness of the aluminum oxide film layer is designed to protect the OLED material from corrosion by oxygen and moisture. This film layer determines the life of the organic layer without excessively increasing the overall thickness.

[0046] Preferably, the preparation process of the aluminum oxide film layer is as follows:

[0047] 1) Surface preparation stage: After the cathode material layer is made, the silicon substrate is placed in the reaction chamber for pretreatment to ensure that the surface of the silicon substrate is covered with hydroxyl groups -OH;

[0048] 2) Trimethylaluminum treatment: Trimethylaluminum vapor is introduced into the reaction chamber under controlled temperature and pressure conditions; the contact time of the trimethylaluminum vapor on the surface is maintained to ensure sufficient surface coverage, and the hydrogen atoms on the surface are removed and replaced with methyl groups through the reaction of hydroxyl -OH and trimethylaluminum, and aluminum-containing compounds are formed on the surface;

[0049] 3) Inert gas purging treatment: Introduce inert gas to purge the remaining trimethylaluminum and byproducts in the reaction chamber to clean the reaction chamber;

[0050] 4) Water vapor treatment: Introduce water vapor into the reaction chamber; control the contact time of water vapor on the surface, the hydrogen atoms of water molecules react with the methyl groups on the surface to form more methane, and the oxygen atoms in the water molecules combine with aluminum atoms to form hydroxyl groups to achieve the growth of aluminum oxide film;

[0051] 5) Repeating the cycle: cyclically performing trimethylaluminum treatment, inert gas purge treatment, and water vapor treatment to build an aluminum oxide film layer by layer, and controlling the number of cycles to achieve a desired aluminum oxide film thickness.

[0052] Preferably, in step S6, the thickness of the prism Lens layer is 1200-3500nm, which helps to achieve the wavelength boosting effect of white light to ensure effective light emission; in step S7, the thickness of the upper diffusion layer is 600-2500nm, which helps to achieve uniform and efficient light emission to ensure uniform distribution of light and effective light emission; in step S8, the thickness of the R color film is 700-1500nm; the thickness of the B color film is 700-1500nm; the thickness of the G color film is 700-1500nm, and these thicknesses are intended to optimize the luminous efficiency and color purity of each color.

[0053] Preferably, in step S6, the thickness of the first prism Lens layer is 1200-3500nm; in step S7, the thickness of the upper diffusion layer is 600-2500nm; in step S8, the thickness of the R color film is 700-1500nm; the thickness of the B color film is 700-1500nm; the thickness of the G color film is 700-1500nm; in step S9, the thickness of the second prism Lens layer is 2000-3000nm. This thickness helps to cooperate with the first prism Lens layer to achieve the wavelength assist effect of light, avoid the standing wave effect, and ensure the effective increase of light by 15%-35%.

[0054] Preferably, in step S9, the thickness of the PVA film layer and the TAC film layer in the optical film layer is 500-1000nm, specifically, the thickness of the PVA film layer is 300-600nm, and the thickness of the TAC film layer is 200-400nm; and the PVA film layer covers the AA area, and the TAC film layer covers the cathode ring area, ensuring that the PVA function of protecting the optical film layer is maximized, and the optical film layer can effectively absorb the ambient light outside the structure, prevent the ambient light from entering the structure, and reflect the metal layer, causing contrast distortion. The PVA film layer is polyvinyl alcohol, which has carbon, hydrogen and oxygen light atoms; the composition of the TAC film layer is triacetate cellulose film.

[0055] The PVA film layer has high transparency and good extensibility, good iodine adsorption and film-forming properties. When the PVA film layer is extended and oriented, the iodine molecules on it are also orderly distributed, and the two-way absorption molecules adsorbed by iodine are extended and aligned, so that the PVA film layer has the function of polarization, thereby determining its polarization performance, transmittance, color tone and other key optical indicators; because the PVA film layer is easily affected by water and fades and reduces the optical performance, a layer of TAC film with uniform optical properties and good transparency is used to protect it from moisture and air.

[0056] Preferably, in step S10, the thickness of the PVA film layer and the TAC film layer in the optical film layer is 500-1000nm, specifically, the thickness of the PVA film layer is 300-600nm, and the thickness of the TAC film layer is 200-400nm; and the PVA film layer covers the AA area, and the TAC film layer covers the cathode ring area, ensuring that the PVA function of protecting the optical film layer is maximized, and the optical film layer can effectively absorb the ambient light outside the structure, avoiding the ambient light from entering the structure, reflecting the metal layer, and causing contrast distortion. The PVA film layer is polyvinyl alcohol, which has carbon, hydrogen and oxygen light atoms; the composition of the TAC film layer is triacetate cellulose film.

[0057] The PVA film layer has high transparency and good extensibility, good iodine adsorption and film-forming properties. When the PVA film layer is extended and oriented, the iodine molecules on it are also orderly distributed, and the two-way absorption molecules adsorbed by iodine are extended and aligned, so that the PVA film layer has the function of polarization, thereby determining its polarization performance, transmittance, color tone and other key optical indicators; because the PVA film layer is easily affected by water and fades and reduces the optical performance, a layer of TAC film with uniform optical properties and good transparency is used to protect it from moisture and air.

[0058] Compared with the prior art, the OLED display structure and manufacturing method have the following beneficial effects:

[0059] 1. This display structure first adds a reflective film layer process to the bottom layer of the anode: by optimizing this process, the brightness performance of the product is improved, the reflectivity of the film layer can reach 95% or more, and the overall brightness can be increased by 5%-15%.

[0060] 2. The display structure adds a prism layer process above the light-emitting layer: Through this additional optimization process, the brightness can be increased by 15-30%.

[0061] 3. The display structure adds a diffusion layer process above the prism layer: By adding this optimized design, the uniformity and contrast of the light output can be improved. The transmittance of the diffusion film layer to visible light is more than 98%, the transmittance of ultraviolet light is less than 12%, and the transmittance of 400nm~460nm short-wave blue light is less than 15%. The harmful blue light wavelength is mainly in the 415-455nm segment. The diffusion layer acts as a blue light protection film, which is greatly beneficial for eye protection.

[0062] 4. The display structure uses a PVA+TAC layer process designed above the color film layer: Through optimized design, the PVA film layer is one-way light-transmitting when the product is outdoors or in areas with high ambient brightness. This can prevent ambient light from entering the metal layer inside the product and reflecting during product use, similar to an anti-peep film, to improve the contrast of the product. After testing, the contrast is increased by 3-5%, and the greater the original brightness, the greater the improvement.

[0063] 5. The above features can also achieve higher brightness and contrast at the same power consumption level. Improved brightness and contrast without changing power consumption: This improvement improves the visual effect of the display, especially in applications with high brightness of 15,000 nit and above. It is particularly important for improving the energy efficiency of the device and extending the battery life, especially on portable and low-power devices.

[0064] In summary, the present invention has made a significant contribution to improving the performance of silicon-based OLED displays. Through its unique design and process innovation, it not only improves the display effect, but also improves the overall performance of the device while maintaining low power consumption. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Figure 1 It is a structural diagram of embodiment 1 of the present invention.

[0066] In the figure, a, CMOS IC layer; b, reflective layer; c, anode layer; d, light-emitting layer; e, cathode layer; f, prism lens layer; g, upper diffusion layer; h, color filter layer; i, optical film layer.

[0067] Figure 2 It is a structural diagram of embodiment 2 of the present invention.

[0068] In the figure, 1, CMOS IC layer; 2, reflective layer; 3, anode layer; 4, light-emitting layer; 5, cathode layer; 6, first prism Lens layer; 7, upper diffusion layer; 8, color filter layer; 9, second prism Lens layer; 10, optical film layer.

[0069] Figure 3 Schematic diagram of the color filter layer in the present invention. DETAILED DESCRIPTION

[0070] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0071] Embodiment 1

[0072] like Figure 1As shown, the OLED display structure includes a CMOS IC layer a at the bottom; a reflective layer b is laid on the CMOS IC layer a, and the reflective layer b includes a reflective film layer and a reflective medium layer stacked from bottom to top; the bottom surface of the reflective film layer is attached to the CMOS IC layer a, and the top surface of the reflective medium layer is paved with an anode layer c; the anode layer c is made of Al and ITO materials, and there is a gap Pitch after peeling, Pitch: the interval between sub-pixels (sub-pixels); a light-emitting layer d is laid on the anode layer c, and the light-emitting layer d includes a hole injection layer, a hole transport layer, an EML light-emitting stack, an electron transport layer and an electron injection layer stacked from bottom to top; the bottom surface of the hole injection layer is attached to the anode layer c, and a cathode layer e is laid on the electron injection layer, and the cathode layer e includes a cathode material layer and an aluminum oxide film layer stacked from bottom to top; the top surface of the aluminum oxide film layer is covered with a prism lens layer f (Mirco Lens Array is a process for improving brightness); the prism Lens layer f is covered with an upper diffusion layer g, the upper diffusion layer g is covered with a color film layer h, and the color film layer h is formed by the R color film pixel points, the B color film pixel points, and the G color film pixel points arranged alternately in sequence; the color film layer h is covered with an optical film layer i.

[0073] A method for manufacturing an OLED display structure, the manufacturing method is applied to the above-mentioned OLED display structure, and the manufacturing method comprises the following steps:

[0074] S1: After cleaning the silicon substrate, a CMOS IC layer a is fabricated on the silicon substrate by using photolithography and etching processes in sequence, which serves as a switch for individually controlling the hole transmission of the corresponding pixel anode;

[0075] S2 makes reflection layer b:

[0076] a. The reflective film layer is manufactured by using a spin coating process, an exposure process and a development process in sequence; the coating of the reflective film layer contains magnesium and silver; the thickness of the reflective film layer is

[0077] The reflective film layer reflects light absorbed by the back of the screen so that it can re-enter the luminous layer d, directly contributing to the brightness of the screen; this reflection not only increases the overall brightness of the screen, but also improves energy efficiency because more light is effectively used rather than wasted; the reflective film layer containing magnesium and silver can increase the reflectivity and enhance the luminous efficiency.

[0078] b. A reflective medium layer is manufactured on the reflective film layer through a spin coating process, an exposure process and a development process in sequence; the thickness of the reflective medium layer is The reflective dielectric layer is made of a non-conductive and reflective material. The non-conductive material is to ensure the correct flow of current and avoid short circuits. The reflective dielectric layer can effectively reflect the light emitted downward by the anode Pitch and the light transmitted by the anode layer c upward, thereby improving the utilization rate of light emission. The reflectivity of the reflective layer b reaches more than 95%.

[0079] The thicker design of the reflective film layer is to maximize the light reflection efficiency, thereby improving the brightness and energy efficiency of the display; the relatively thin thickness of the reflective dielectric layer helps to maintain good optical performance without excessively increasing the thickness of the overall structure.

[0080] S3: Prepare anode layer c: Prepare anode layer c by magnetron sputtering evaporation ITO process and AL evaporation process in sequence; the thickness of anode layer c is The anode layer c can greatly improve the regularity of the pixel edge, improve the uniformity and tightness of the film layer, and cooperate with the transmission layer to increase the transmission efficiency and density of holes, thereby maximizing the anode performance.

[0081] Since the anode layer c is a relatively thin ITO layer, it is transparent to a certain extent, and the anode gap Pitch will cause light leakage from the luminous pixel area to the bottom. A reflective film layer is designed at the bottom of this structure to effectively converge and reflect the downward light from the luminous layer d upward, ensuring that each pixel displays its predetermined brightness more accurately. The reflectivity of the reflective layer b here is as high as 95% or above, and the brightness can be increased by 5-15%.

[0082] In the design of the reflective film layer, the reflected light will interfere with or enhance the light waves emitted upward by the light-emitting layer d. Therefore, DOE is used to verify the optimal thickness of the reflective layer b. When the thickness is adjusted to the point where the peaks of the light waves are superimposed, the color gamut and brightness are greatly improved.

[0083] S4: preparing the light-emitting layer d: using a high-precision mask to evaporate the organic material to prepare the light-emitting layer d; the thickness of the light-emitting layer d is 2000-2900nm;

[0084] S5: Prepare cathode layer e: Use a high-precision mask to evaporate the cathode material, which is a mixture of magnesium, silver and lutetium, to obtain a cathode material layer; the thickness of the cathode material layer is After the evaporation, trimethylaluminum and water were used as materials, and the atomic layer deposition technology was used on the cathode material layer to make an aluminum oxide film layer. The thickness of the aluminum oxide film layer was Complete the cathode layer e; trimethylaluminum and water are selected because they can be carried out at relatively low temperatures, which is particularly important for protecting sensitive materials of OLED display structures from thermal damage. Atomic layer deposition technology can produce a very uniform and dense aluminum oxide film layer.

[0085] The preparation process of the aluminum oxide film layer is as follows:

[0086] 1) Surface preparation stage: After the cathode material layer is made, the silicon substrate is placed in the reaction chamber for pretreatment to ensure that the surface of the silicon substrate is covered with hydroxyl groups -OH;

[0087] 2) Trimethylaluminum treatment: Trimethylaluminum vapor is introduced into the reaction chamber; through the reaction of hydroxyl -OH and trimethylaluminum, hydrogen atoms on the surface are removed and replaced with methyl groups, and aluminum-containing compounds are formed on the surface;

[0088] 3) Inert gas purging treatment: Introduce inert gas to purge the remaining trimethylaluminum and byproducts in the reaction chamber to clean the reaction chamber;

[0089] 4) Water vapor treatment: Water vapor is introduced into the reaction chamber, and the hydrogen atoms of the water molecules react with the methyl groups on the surface to form methane, while the oxygen atoms in the water molecules combine with the aluminum atoms to form hydroxyl groups to achieve the growth of aluminum oxide film;

[0090] 5) Repeating the cycle: cyclically performing trimethylaluminum treatment, inert gas purge treatment, and water vapor treatment to build an aluminum oxide film layer by layer, and controlling the number of cycles to achieve a desired aluminum oxide film thickness.

[0091] The design of the aluminum oxide film layer helps to improve the electron injection efficiency and optimize the electron transmission performance of the entire device. At the same time, the aluminum oxide film layer acts as a protective layer to protect the cathode material from oxygen and moisture, thereby improving the stability of the OLED display structure.

[0092] S6 covers the prism Lens layer f: spin coating process, exposure process and development process are used in sequence to make the entire prism Lens layer f on the aluminum oxide film layer of the cathode layer e; the thickness of the prism Lens layer f is 1200-3500nm; the prism Lens layer f can be made into a whole surface pattern or a pixel pattern, and the pixel pattern has higher requirements for the development PGMEA concentration process.

[0093] The thickness requirement of the prism lens layer f is also affected by the spectrum of organic light emission. For example, the design film thickness of white light can be 2.5μm or above for best effect, and the brightness can be increased by 15-30%. Proper film thickness of the prism layer can improve the light focusing ability and help improve the efficiency of OLED light emission upward.

[0094] S7: Covering the upper diffusion layer g: using the spin coating process and the coating process in sequence to form the entire diffusion layer g on the prism lens layer f; the thickness of the upper diffusion layer g is 600-2500nm;

[0095] The optical diffusion layer g is prepared by hydrolysis and polycondensation reaction of aminopropyl trimethoxysilane, vinyl trimethoxysilane and phenyl triethoxysilane to produce an organic silicon microsphere precursor core, and further in situ growth of nano ZnO / CeO2 / Al2O3 on its surface, and the core-shell type light diffusion microspheres and polyurethane acrylate are grafted and copolymerized by chemical cross-linking of glutaraldehyde intermediate and amino group, thereby significantly improving the stability of the light diffusion layer; a layer of randomly dispersed micron-structured diffusion particles is grown on the surface, so that the light undergoes multiple refraction, reflection and diffraction phenomena through the diffusion layer, so as to correct the light into a uniform surface light source, achieve the effect of optical diffusion, make the light display more uniform and soft, and thus improve the optical problem of pitch brightness non-uniformity;

[0096] Because nano ZnO / CeO2 / Al2O3 is unevenly distributed on the surface of the silicone microspheres, when light is projected into the light diffusion layer g, refraction and diffuse reflection occur at different angles and directions, which significantly improves the diffusion performance of the diffusion film for visible light. The transmittance of visible light is more than 98%, the transmittance of ultraviolet light is less than 12%, and the transmittance of 400nm~460nm short-wave blue light is less than 15%.

[0097] The upper diffusion layer g can be made into a pixel pattern or cover the entire surface, and its thickness can be designed to be half of the prism lens layer f, so that the light can be diffused more evenly and the light loss caused by the diffusion layer can be avoided. According to the test, the loss is 2% at best and 8% at the highest. After passing through the upper diffusion layer g, the prism lens layer f emits convergent light, which helps to improve the uniformity of light emission, convert point light into surface light, and improve contrast.

[0098] like Figure 3 As shown, S8 covers the color filter layer h:

[0099] Production of R color film pixels: The R color film is produced by sequentially using spin coating, exposure and development processes at the anode CD position; the thickness of the R color film is 700-1500nm;

[0100] Production of B color film pixels: At the anode CD position adjacent to the R color film, the B color film is produced by sequentially adopting the spin coating process, exposure process and development process; the thickness of the B color film is 700-1500nm;

[0101] Production of G color film pixels: At the anode CD position adjacent to the B color film, the G color film is produced by sequentially adopting the spin coating process, the exposure process and the development process; the thickness of the G color film is 700-1500nm.

[0102] After repeated preparation of colored glue, exposure and development, a regular RGB arrangement is obtained.

[0103] S9 covers the optical film layer i: a PVA film layer is made on the entire surface of the color film layer h by spin coating or printing transfer, and then a TAC film layer is made on the entire surface of the PVA film layer as a protective layer by spin coating or printing transfer, completing the production of the optical film layer i. The thickness of the PVA film layer and the TAC film layer in the optical film layer i is 500-1000nm; the PVA film layer is polyvinyl alcohol, which has carbon, hydrogen and oxygen light atoms; the composition of the TAC film layer is triacetate cellulose film.

[0104] The PVA film layer has high transparency and good extensibility, good iodine adsorption and film-forming properties. When the PVA film layer is extended and oriented, the iodine molecules on it are also orderly distributed, and the two-way absorption molecules adsorbed by iodine are extended and aligned, so that the PVA film layer has the function of polarization, thereby determining its polarization performance, transmittance, color tone and other key optical indicators; because the PVA film layer is easily affected by water and fades and reduces the optical performance, a layer of TAC film with uniform optical properties and good transparency is used to protect it from moisture and air.

[0105] The core of the optical film layer i is a polarizing film layer that can effectively absorb the ambient light outside the structure, preventing the ambient light from entering the structure and reflecting from the metal layer, causing contrast distortion. The optical film layer i effectively resists ambient light and reduces interference in the display, which can improve the contrast. The tested contrast can be improved by 3 to 5 times, and the greater the brightness, the greater the improvement ratio.

[0106] Embodiment 2

[0107] like Figure 2 As shown, the OLED display structure includes a CMOS IC layer 1 at the bottom; a reflective layer 2 is laid on the CMOS IC layer 1, and the reflective layer 2 includes a reflective film layer and a reflective medium layer stacked from bottom to top; the bottom surface of the reflective film layer is covered with a CMOS IC layer. IC layer 1, an anode layer 3 is laid on the top surface of the reflective medium layer; the anode layer 3 is made of Al and ITO material and there is a gap Pitch after peeling; the light-emitting layer 4 is laid on the anode layer 3, and the light-emitting layer 4 includes a hole injection layer, a hole transport layer, an EML light-emitting stack, an electron transport layer and an electron injection layer stacked from bottom to top; the bottom surface of the hole injection layer is covered with the anode layer 3, and the cathode layer 5 is laid on the electron injection layer, and the cathode layer 5 includes a cathode material layer and an aluminum oxide film layer stacked from bottom to top; the top surface of the aluminum oxide film layer is covered with a first prism Lens layer 6; the first prism Lens layer 6 is covered with an upper diffusion layer 7, and the upper diffusion layer 7 is covered with a color film layer 8, and the color film layer 8 is formed by R color film pixel points, B color film pixel points, and G color film pixel points arranged alternately in sequence; the color film layer 8 is covered with a second prism Lens layer 9, and the second prism Lens layer 9 is covered with an optical film layer 10.

[0108] A method for manufacturing an OLED display structure, the manufacturing method is applied to the above-mentioned OLED display structure, and the manufacturing method comprises the following steps:

[0109] S1: After cleaning the silicon substrate, a CMOS IC layer 1 is fabricated on the silicon substrate by using a photolithography process and an etching process in sequence, which serves as a switch for individually controlling the hole transmission of the corresponding pixel anode;

[0110] S2 makes reflection layer 2:

[0111] a. The reflective film layer is manufactured by using a spin coating process, an exposure process and a development process in sequence; the coating of the reflective film layer contains magnesium and silver; the thickness of the reflective film layer is

[0112] The reflective film layer reflects light absorbed by the back of the screen so that it can re-enter the luminous layer 4 and directly contribute to the brightness of the screen; this reflection not only increases the overall brightness of the screen, but also improves energy efficiency because more light is effectively used rather than wasted; the reflective film layer containing magnesium and silver can increase the reflectivity and enhance the luminous efficiency.

[0113] b. A reflective medium layer is manufactured on the reflective film layer through a spin coating process, an exposure process and a development process in sequence; the thickness of the reflective medium layer is The reflective dielectric layer is made of a non-conductive and reflective material. The non-conductive material is to ensure the correct flow of current and avoid short circuit. The reflective dielectric layer can effectively reflect the light emitted by the anode Pitch downward and the light transmitted by the anode layer 3 upward, thereby improving the utilization rate of light emission. The reflectivity of the reflective layer 2 reaches more than 95%.

[0114] The thicker design of the reflective film layer is to maximize the light reflection efficiency, thereby improving the brightness and energy efficiency of the display; the relatively thin thickness of the reflective dielectric layer helps to maintain good optical performance without excessively increasing the thickness of the overall structure.

[0115] S3: Prepare anode layer 3 by magnetron sputtering ITO evaporation process and AL evaporation process in sequence; the thickness of anode layer 3 is The anode layer 3 can greatly improve the regularity of the pixel edge, improve the uniformity and compactness of the film layer, and cooperate with the transmission layer to increase the transmission efficiency and density of holes, thereby maximizing the anode performance.

[0116] Since the anode layer 3 is a relatively thin ITO layer, it is transparent to a certain extent, and the anode gap Pitch will cause light leakage from the luminous pixel area to the bottom. A reflective layer 2 is designed at the bottom of this structure to effectively converge and reflect the downward light from the luminous layer 4 upward, ensuring that each pixel displays its predetermined brightness more accurately. The reflectivity of the reflective layer 2 here is as high as 95% or more, and the brightness can be increased by 5-15%.

[0117] In the design of the reflective film layer, the reflected light will interfere with or enhance the light waves emitted upward by the light-emitting layer 4. Therefore, DOE is used to verify the optimal thickness of the reflective layer 2. When the thickness is adjusted to the point where the light wave peaks are superimposed, the color gamut and brightness are greatly improved.

[0118] S4: preparing the light-emitting layer 4: using a high-precision mask to evaporate the organic material to prepare the light-emitting layer 4; the thickness of the light-emitting layer 4 is 2000-2900nm;

[0119] S5 Preparation of cathode layer 5: Use a high-precision mask to evaporate the cathode material. The cathode material is a mixture of magnesium, silver and lutetium. The combination of magnesium, silver and lutetium provides excellent electron injection and transmission capabilities, which helps to improve the electro-optical conversion efficiency of OLED; the thickness of the cathode material layer is After the evaporation, trimethylaluminum and water were used as materials, and the atomic layer deposition technology was used on the cathode material layer to make an aluminum oxide film layer. The thickness of the aluminum oxide film layer was The cathode layer 5 is fabricated; trimethylaluminum and water are selected because they can be carried out at a relatively low temperature, which is particularly important for protecting sensitive materials of the OLED display structure from thermal damage. Atomic layer deposition technology can produce a very uniform and dense aluminum oxide film layer.

[0120] The preparation process of the aluminum oxide film layer is as follows:

[0121] 1) Surface preparation stage: After the cathode material layer is made, the silicon substrate is placed in the reaction chamber for pretreatment to ensure that the surface of the silicon substrate is covered with hydroxyl groups -OH;

[0122] 2) Trimethylaluminum treatment: Trimethylaluminum vapor is introduced into the reaction chamber; through the reaction of hydroxyl -OH and trimethylaluminum, hydrogen atoms on the surface are removed and replaced with methyl groups, and aluminum-containing compounds are formed on the surface;

[0123] 3) Inert gas purging treatment: Introduce inert gas to purge the remaining trimethylaluminum and byproducts in the reaction chamber to clean the reaction chamber;

[0124] 4) Water vapor treatment: Water vapor is introduced into the reaction chamber, and the hydrogen atoms of the water molecules react with the methyl groups on the surface to form methane, while the oxygen atoms in the water molecules combine with the aluminum atoms to form hydroxyl groups to achieve the growth of aluminum oxide film;

[0125] 5) Repeating the cycle: cyclically performing trimethylaluminum treatment, inert gas purge treatment, and water vapor treatment to build an aluminum oxide film layer by layer, and controlling the number of cycles to achieve a desired aluminum oxide film thickness.

[0126] The design of the aluminum oxide film layer helps to improve the electron injection efficiency and optimize the electron transmission performance of the entire device. At the same time, the aluminum oxide film layer acts as a protective layer to protect the cathode material from oxygen and moisture, thereby improving the stability of the OLED display structure.

[0127] S6 covers the first prism Lens layer 6: spin coating process, exposure process and development process are used in sequence to make the entire first prism Lens layer 6 on the aluminum oxide film layer of the cathode layer 5; the thickness of the first prism Lens layer 6 is 1200-3500nm; the prism Lens layer can be made into a whole surface pattern or a pixel pattern, and the pixel pattern has higher requirements for the development PGMEA concentration process.

[0128] The thickness requirement of the prism lens layer is also affected by the spectrum of organic light emission. For example, the design film thickness of white light can be 2.5μm or above for best effect, and the brightness can be increased by 15-30%. Proper film thickness of the prism layer can improve the light focusing ability and help improve the efficiency of OLED light emission upward.

[0129] S7: Covering the upper diffusion layer 7: using the spin coating process and the coating process in sequence to form the entire diffusion layer 7 on the first prism lens layer 6; the thickness of the upper diffusion layer 7 is 600-2500nm;

[0130] The optical diffusion layer 7 is prepared by hydrolysis and polycondensation reaction of aminopropyl trimethoxysilane, vinyl trimethoxysilane and phenyl triethoxysilane to produce an organic silicon microsphere precursor core, and further in situ grows nano ZnO / CeO2 / Al2O3 on its surface, and utilizes the chemical cross-linking effect of glutaraldehyde intermediate and amino group to make core-shell type light diffusion microspheres and polyurethane acrylate undergo graft copolymerization, thereby significantly improving the stability of the light diffusion layer; a layer of randomly dispersed micron structured diffusion particles is grown on the surface, so that the light undergoes multiple refraction, reflection and diffraction phenomena through the diffusion layer, so as to correct the light into a uniform surface light source, achieve the effect of optical diffusion, make the light display more uniform and soft, and thus improve the optical problem of pitch brightness non-uniformity;

[0131] Since nano ZnO / CeO2 / Al2O3 is unevenly distributed on the surface of the silicone microspheres, when light is projected into the light diffusion layer 7, refraction and diffuse reflection occur at different angles and directions, which significantly improves the diffusion performance of the diffusion film for visible light. The transmittance of visible light is more than 98%, the transmittance of ultraviolet light is less than 12%, and the transmittance of 400nm~460nm short-wave blue light is less than 15%.

[0132] The upper diffusion layer 7 can be made into a pixel pattern or a full-surface cover, and its thickness can be designed to be half of the prism lens layer, so that the light can be diffused more evenly and the light loss of the diffusion layer can be avoided. According to the test, the loss is 2% at best and 8% at best. After passing through the upper diffusion layer 7, the prism lens layer emits convergent light, which helps to improve the uniformity of light emission, convert point light into surface light, and improve contrast.

[0133] like Figure 3 As shown, S8 covers the color filter layer 8:

[0134] Production of R color film pixels: The R color film is produced by sequentially using spin coating, exposure and development processes at the anode CD position; the thickness of the R color film is 700-1500nm;

[0135] Production of B color film pixels: At the anode CD position adjacent to the R color film, the B color film is produced by sequentially adopting the spin coating process, exposure process and development process; the thickness of the B color film is 700-1500nm;

[0136] Production of G color film pixels: At the anode CD position adjacent to the B color film, the G color film is produced by sequentially adopting the spin coating process, the exposure process and the development process; the thickness of the G color film is 700-1500nm.

[0137] After repeated preparation of colored glue, exposure and development, a regular RGB arrangement is obtained.

[0138] S9 covers the second prism Lens layer 9: the entire second prism Lens layer 9 is made on the color film layer 8 by using a spin coating process, an exposure process and a development process; the thickness of the second prism Lens layer 9 is 2000-3000nm. The prism Lens layer can be made into a whole surface pattern or a pixel pattern, and the pixel pattern has a higher requirement for the development PGMEA concentration process.

[0139] Since the light loss after passing through the color film layer 8 reaches more than 70%, the light intensity can be increased back to 155-35% by adding a prism lens layer. However, it is necessary to cooperate with the first prism lens layer 6 and adjust the appropriate film thickness to ensure that the light waves from the first layer and the second layer can achieve the wave-assisting effect and avoid the standing wave effect. This can enhance the light focusing ability and help improve the efficiency of the OLED's light emission upwards.

[0140] S10 covers the optical film layer 10: a PVA film layer is formed on the entire surface of the second prism Lens layer 9 by spin coating or printing transfer, and then a TAC film layer is formed on the entire surface of the PVA film layer by spin coating or printing transfer as a protective layer, completing the production of the optical film layer 10. The thickness of the PVA film layer and the TAC film layer in the optical film layer 10 is 500-1000nm; the PVA film layer is polyvinyl alcohol, which has carbon, hydrogen and oxygen light atoms; the composition of the TAC film layer is triacetyl cellulose film.

[0141] The PVA film layer has high transparency and good extensibility, good iodine adsorption and film-forming properties. When the PVA film layer is extended and oriented, the iodine molecules on it are also orderly distributed, and the two-way absorption molecules adsorbed by iodine are extended and aligned, so that the PVA film layer has the function of polarization, thereby determining its polarization performance, transmittance, color tone and other key optical indicators; because the PVA film layer is easily affected by water and fades and reduces the optical performance, a layer of TAC film with uniform optical properties and good transparency is used to protect it from moisture and air.

[0142] The core of the optical film layer 10 is a polarizing film layer that can effectively absorb the ambient light outside the structure, preventing the ambient light from entering the structure and reflecting from the metal layer, causing contrast distortion. The optical film layer 10 effectively resists ambient light and reduces interference in display, and can improve the contrast. The tested contrast can be improved by 3 to 5 times, and the greater the brightness, the greater the improvement ratio.

[0143] In summary, the OLED display structure is an upward emitting structure. The upward emitting structure can effectively reduce light loss, improve light utilization, simplify component levels, reduce material and production costs, and provide a clearer and more uniform display effect by directly emitting light upward.

[0144] Table 1 below verifies the corresponding brightness enhancement values ​​measured by the color enhancement spectrometer under different film thicknesses of the lens and diffusion layer.

[0145]

[0146] The specific embodiments described herein are merely examples of the spirit of the present invention. A person skilled in the art of the present invention may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but will not deviate from the spirit of the present invention or exceed the defined scope. Although the present invention is described and described in detail in the drawings and the foregoing description, such descriptions and descriptions are considered to be illustrative or exemplary rather than restrictive. It should be understood that within the scope of the following claims, changes and modifications may be made by a person of ordinary skill. Specifically, the present invention encompasses additional embodiments having any combination of features from the above-mentioned different embodiments. With respect to the use of the expression "generally" or "substantially", this patent application should be understood to disclose that these features and values ​​are also fully satisfied, i.e., there is no aforementioned characterization as "generally" or "substantially".

Claims

1. An OLED display structure, comprising a CMOS IC layer at the bottom; characterized in that: A reflective layer is laid on the CMOS IC layer, and the reflective layer includes a reflective film layer and a reflective medium layer stacked from bottom to top; the bottom surface of the reflective film layer is covered with the CMOS IC layer, and the top surface of the reflective medium layer is laid with an anode layer; the anode layer is made of Al and ITO materials, and there is a gap Pitch after peeling; a light-emitting layer is laid on the anode layer, and the light-emitting layer includes a hole injection layer, a hole transport layer, an EML light-emitting stack, an electron transport layer and an electron injection layer stacked from bottom to top; the bottom surface of the hole injection layer is covered with the anode layer, and a cathode layer is laid on the electron injection layer, and the cathode layer includes a cathode material layer and an aluminum oxide film layer stacked from bottom to top; the top surface of the aluminum oxide film layer is covered with a prism lens layer; the prism lens layer is covered with an upper diffusion layer, and the upper diffusion layer is covered with a color filter layer, and the color filter layer is formed by R color filter pixel points, B color filter pixel points, and G color filter pixel points arranged in sequence; the color filter layer is covered with an optical film layer.

2. A method for manufacturing an OLED display structure, the method being applied to the OLED display structure according to claim 1, characterized in that: The production method comprises the following steps: S1: After cleaning the silicon substrate, a CMOS IC layer is fabricated on the silicon substrate using photolithography and etching processes, which serves as a switch for individually controlling the hole transmission of the corresponding pixel anode. S2 makes the reflection layer: a. The reflective film layer is manufactured by using a spin coating process, an exposure process and a development process in sequence; the coating of the reflective film layer contains magnesium and silver; b. manufacturing a reflective medium layer on the reflective film layer through a spin coating process, an exposure process and a development process in sequence; S3: Making the anode layer: Making the anode layer by sequentially using the ITO evaporation process and the AL evaporation process; S4 makes the light-emitting layer: uses a high-precision mask to evaporate the organic material to make the light-emitting layer; S5: Preparation of cathode layer: Use a high-precision mask to evaporate the cathode material, which is a mixture of magnesium, silver and lutetium, to obtain a cathode material layer; after the evaporation, use trimethylaluminum and water as materials, use atomic layer deposition technology on the cathode material layer to prepare an aluminum oxide film layer, and then complete the cathode layer preparation; S6 covers the prism lens layer: spin coating, exposure and development processes are used in sequence to make the entire prism lens layer on the aluminum oxide film layer of the cathode layer; S7 covers the diffusion layer: a diffusion layer is formed on the entire surface of the prism lens layer by using a spin coating process and a coating process in sequence; The optical diffusion layer is prepared by hydrolysis and polycondensation reaction of aminopropyl trimethoxysilane, vinyl trimethoxysilane and phenyl triethoxysilane to produce an organosilicon microsphere precursor core, and further in-situ growth of nano ZnO / CeO2 / Al2O3 on the surface thereof, and the core-shell light diffusion microspheres are grafted and copolymerized with polyurethane acrylate by chemical cross-linking of glutaraldehyde intermediate and amino group, thereby significantly improving the stability of the light diffusion layer; a layer of randomly dispersed micron-structured diffusion particles is grown on the surface, so that the light undergoes multiple refraction, reflection and diffraction phenomena through the diffusion layer, so as to correct the light into a uniform surface light source, achieve the effect of optical diffusion, make the light display more uniform and soft, and thus improve the optical problem of pitch brightness non-uniformity; S8 covered with color film layer: Production of R color film pixels: spin coating, exposure and development processes are used in sequence to produce R color film at the anode CD position; Production of pixel points of B color film: At the anode CD position adjacent to the R color film, the B color film is produced by sequentially adopting the spin coating process, exposure process and development process; G color film pixel production: At the anode CD position adjacent to the B color film, the G color film is produced by using the spin coating process, exposure process and development process in sequence; S9 covers the optical film layer: a PVA film layer is made on the entire surface of the color film layer by spin coating or printing transfer, and then a TAC film layer is made on the entire surface of the PVA film layer by spin coating or printing transfer as a protective layer to complete the production of the optical film layer.

3. An OLED display structure, comprising a CMOS IC layer at the bottom; characterized in that: A reflective layer is laid on the CMOS IC layer, and the reflective layer includes a reflective film layer and a reflective medium layer stacked from bottom to top; the bottom surface of the reflective film layer is attached to the CMOS IC layer. IC layer, an anode layer is laid on the top surface of the reflective medium layer; the anode layer is made of Al and ITO material and there is a gap Pitch after peeling; a light-emitting layer is laid on the anode layer, and the light-emitting layer includes a hole injection layer, a hole transport layer, an EML light-emitting stack, an electron transport layer and an electron injection layer stacked from bottom to top; the bottom surface of the hole injection layer is covered with the anode layer, and a cathode layer is laid on the electron injection layer, and the cathode layer includes a cathode material layer and an aluminum oxide film layer stacked from bottom to top; the top surface of the aluminum oxide film layer covers the first prism Lens layer; the first prism Lens layer is covered with an upper diffusion layer, and the upper diffusion layer is covered with a color filter layer, and the color filter layer is formed by R color filter pixel points, B color filter pixel points, and G color filter pixel points arranged alternately in sequence; the color filter layer is covered with a second prism Lens layer, and the second prism Lens layer is covered with an optical film layer.

4. A method for manufacturing an OLED display structure, the method being applied to the OLED display structure according to claim 3, characterized in that: The production method comprises the following steps: S1: After cleaning the silicon substrate, a CMOS IC layer is fabricated on the silicon substrate using photolithography and etching processes, which serves as a switch for individually controlling the hole transmission of the corresponding pixel anode. S2 makes the reflection layer: a. The reflective film layer is manufactured by using a spin coating process, an exposure process and a development process in sequence; the coating of the reflective film layer contains magnesium and silver; b. manufacturing a reflective medium layer on the reflective film layer through a spin coating process, an exposure process and a development process in sequence; S3: Making the anode layer: Making the anode layer by sequentially using the ITO evaporation process and the AL evaporation process; S4 makes the light-emitting layer: uses a high-precision mask to evaporate the organic material to make the light-emitting layer; S5: Preparation of cathode layer: Use a high-precision mask to evaporate the cathode material, which is a mixture of magnesium, silver and lutetium, to obtain a cathode material layer; after the evaporation, use trimethylaluminum and water as materials, use atomic layer deposition technology on the cathode material layer to prepare an aluminum oxide film layer, and then complete the cathode layer preparation; S6: Covering the first prism lens layer: using a spin coating process, an exposure process and a development process in sequence to manufacture the entire first prism lens layer on the aluminum oxide film layer of the cathode layer; S7: Spin coating and coating are used to form a diffusion layer on the entire surface of the first prism lens layer; The optical diffusion layer is prepared by hydrolysis and polycondensation reaction of aminopropyl trimethoxysilane, vinyl trimethoxysilane and phenyl triethoxysilane to produce an organosilicon microsphere precursor core, and further in-situ growth of nano ZnO / CeO2 / Al2O3 on the surface thereof, and the core-shell light diffusion microspheres are grafted and copolymerized with polyurethane acrylate by chemical cross-linking of glutaraldehyde intermediate and amino group, thereby significantly improving the stability of the light diffusion layer; a layer of randomly dispersed micron-structured diffusion particles is grown on the surface, so that the light undergoes multiple refraction, reflection and diffraction phenomena through the diffusion layer, so as to correct the light into a uniform surface light source, achieve the effect of optical diffusion, make the light display more uniform and soft, and thus improve the optical problem of pitch brightness non-uniformity; S8 covered with color film layer: Production of R color film pixels: spin coating, exposure and development processes are used in sequence to produce R color film at the anode CD position; Production of pixel points of B color film: At the anode CD position adjacent to the R color film, the B color film is produced by sequentially adopting the spin coating process, exposure process and development process; G color film pixel production: At the anode CD position adjacent to the B color film, the G color film is produced by using the spin coating process, exposure process and development process in sequence; S9 covers the second prism Lens layer: the entire second prism Lens layer is made on the color film layer using spin coating, exposure and development processes; S10 covers the optical film layer: a PVA film layer is formed on the entire surface of the second prism Lens layer by spin coating or printing transfer, and then a TAC film layer is formed on the entire surface of the PVA film layer by spin coating or printing transfer as a protective layer to complete the production of the optical film layer.

5. The method for manufacturing an OLED display structure according to claim 2 or 4, characterized in that: The thickness of the reflective film layer in step S2 is The thickness of the reflective medium layer is In step S3, the thickness of the anode layer is In step S4, the thickness of the light-emitting layer is 2000-2900 nm; in step S5, the thickness of the cathode material layer is The thickness of the aluminum oxide film is 6. The method for manufacturing an OLED display structure according to claim 2 or 4, characterized in that: The preparation process of the aluminum oxide film layer is as follows: 1) Surface preparation stage: After the cathode material layer is made, the silicon substrate is placed in the reaction chamber for pretreatment to ensure that the surface of the silicon substrate is covered with hydroxyl groups -OH; 2) Trimethylaluminum treatment: Trimethylaluminum vapor is introduced into the reaction chamber; through the reaction of hydroxyl -OH and trimethylaluminum, hydrogen atoms on the surface are removed and replaced with methyl groups, and aluminum-containing compounds are formed on the surface; 3) Inert gas purging treatment: Introduce inert gas to purge the remaining trimethylaluminum and byproducts in the reaction chamber to clean the reaction chamber; 4) Water vapor treatment: Water vapor is introduced into the reaction chamber, and the hydrogen atoms of the water molecules react with the methyl groups on the surface to form methane, while the oxygen atoms in the water molecules combine with the aluminum atoms to form hydroxyl groups to achieve the growth of aluminum oxide film; 5) Repeating the cycle: cyclically performing trimethylaluminum treatment, inert gas purge treatment, and water vapor treatment to build an aluminum oxide film layer by layer, and controlling the number of cycles to achieve a desired aluminum oxide film thickness.

7. The method for manufacturing an OLED display structure according to claim 2, wherein: In step S6, the thickness of the prism Lens layer is 1200-3500nm; in step S7, the thickness of the upper diffusion layer is 600-2500nm; in step S8, the thickness of the R color film is 700-1500nm; the thickness of the B color film is 700-1500nm; and the thickness of the G color film is 700-1500nm.

8. The method for manufacturing an OLED display structure according to claim 4, wherein: In step S6, the thickness of the first prism Lens layer is 1200-3500nm; in step S7, the thickness of the upper diffusion layer is 600-2500nm; in step S8, the thickness of the R color film is 700-1500nm; the thickness of the B color film is 700-1500nm; the thickness of the G color film is 700-1500nm; in step S9, the thickness of the second prism Lens layer is 2000-3000nm.

9. The method for manufacturing an OLED display structure according to claim 2, wherein: In step S9, the thickness of the PVA film layer and the TAC film layer in the optical film layer is 500-1000 nm; the PVA film layer is polyvinyl alcohol, which has carbon, hydrogen and oxygen light atoms; and the composition of the TAC film layer is triacetyl cellulose film.

10. The method for manufacturing an OLED display structure according to claim 4, wherein: In step S10, the thickness of the PVA film layer and the TAC film layer in the optical film layer is 500-1000 nm; the PVA film layer is polyvinyl alcohol, which has carbon, hydrogen and oxygen light atoms; and the composition of the TAC film layer is triacetyl cellulose film.