Narrow-groove gas-shielded arc welding method and welding device for narrow-groove gas-shielded arc welding
By adjusting the distance between electrodes, wire diameter and protective gas composition, the problem of high-temperature cracking of the center of the welding metal in multi-electrode welding is solved, and efficient and low-cost multi-layer welding of thick steel plates is achieved, improving welding quality and construction efficiency.
Patent Information
- Application Number
- CN202380030544.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-02-22
- Publication Date
- 2024-11-15
AI Technical Summary
When performing multi-electrode gas-protected arc welding with more than 3 electrodes, high-temperature cracking in the center of the welding metal is prone to occur, and the prior art is difficult to achieve good welding quality and high welding construction efficiency under low-cost bevel processing.
By adjusting the distance between electrodes, wire diameter, electrode configuration method and protective gas composition, the sufficient melting and stability of the welding metal is ensured. Specific measures include: setting the distance between electrodes to 10~100mm, the diameter of welding wire is 1.0~1.6mm, and the electrode configuration. For positive polarity and reverse polarity, protective gas containing more than 60% CO2 is used, and the supply angle and curvature radius of the welding wire are controlled during welding.
Under low-cost bevel processing, it is possible to prevent high-temperature cracking and poor fusion in the center of the welded metal, improve welding construction efficiency and quality, and reduce welding costs. It is especially suitable for multi-layer welding of thick steel plates.
Smart Images

Figure CN118973752A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a gas shielded arc welding method, and to a narrow groove gas shielded arc welding method for thick steel plates and a welding device for narrow groove gas shielded arc welding. The so-called "narrow groove" here means that the groove angle is less than 25° and the minimum groove width between the thick steel plates that become the welded materials is less than 50% of the plate thickness of the thick steel plates. "x to y" indicating a numerical range in this specification means more than x and less than y, that is, the boundary value is included in the range. Background Art
[0002] Gas shielded arc welding used in welding construction of steel is widely used in the manufacturing fields of automobiles, buildings, bridges, electrical equipment, etc. In recent years, with the development of large-scale and thick-walled steel structures, the amount of weld deposited during welding in the manufacturing process, especially the butt welding of steel materials, has increased. In addition, welding construction requires a lot of time. This leads to an increase in construction costs. Therefore, it is considered to apply narrow groove gas shielded arc welding to perform multi-layer welding of grooves with small gaps relative to the plate thickness by gas shielded arc welding. Compared with conventional gas shielded arc welding, narrow groove gas shielded arc welding has less weld deposit, which can achieve efficient and energy-saving welding, and can be expected to reduce construction costs.
[0003] In addition, a technique for performing narrow groove gas shielded arc welding with multiple electrodes has recently been proposed. Multi-electrode welding can increase the amount of deposited metal used to fill the groove, that is, the amount of metal that melts the welding wire and adheres to the groove, according to the number of electrodes, so that higher welding efficiency can be achieved compared to single-electrode welding. Therefore, it has become an effective means to contribute to welding efficiency.
[0004] For example, Patent Document 1 describes a narrow groove gas shielded arc welding method for joining thick steel plates by multi-layer welding of narrow grooves. In the technology described in Patent Document 1, the first layer welding is set as multi-electrode welding with more than two electrodes, the first electrode and the second electrode are set to positions along a predetermined parallel welding line, the distance between the front ends of the welding wires of the first electrode and the second electrode is controlled to be in the range of 5 mm to 16 mm, the angle between the straight line connecting the front ends of the welding wires of the first electrode and the second electrode and the direction orthogonal to the welding line is controlled to be in the range of 45° or less, and the melting depth at the bottom of the thick steel plate in the direction orthogonal to the welding line is set to be 1.5 mm or more. Thus, even when groove processing such as gas cutting and plasma cutting is implemented as groove processing, the effect of no defect generation and improved welding construction efficiency can be obtained.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2015-223605 Summary of the invention
[0008] Problems to be solved by the invention
[0009] However, in the technology described in Patent Document 1, when multi-electrode welding with three or more electrodes is performed, there is a problem that high-temperature cracking occurs in the center of the weld metal.
[0010] The present invention aims to provide a narrow groove gas shielded arc welding technology, wherein, when performing multi-electrode welding of thick steel plates with three or more electrodes, even if low-cost groove processing is performed, there is no need to perform groove surface trimming, etc., and good welding quality and high welding construction efficiency can be achieved. As low-cost groove processing, gas cutting, plasma cutting, etc. can be exemplified. Good welding quality means that defects such as poor fusion and defects such as high-temperature cracking that occur in the center of the weld metal can be suppressed.
[0011] Means for solving problems
[0012] In order to achieve the above-mentioned object, the inventors of the present application have conducted in-depth research on the cause of high-temperature cracking of weld metal in multi-electrode welding with more than three electrodes. As a result, it was found that when the inter-electrode distance after the second electrode deviates from the appropriate range, a welding defect that causes high-temperature cracking occurs in the center of the weld metal. It was also found that if the inter-electrode distance after the second electrode is adjusted to an appropriate range, a solid weld bead, that is, a weld joint with weld metal can be obtained. In addition, it was found that when the multi-layer welding is set as multi-electrode welding with more than three electrodes, the first electrode and the second electrode are arranged at positions along a predetermined parallel welding line, and one of the first electrode and the second electrode is set to positive polarity and the other is set to reverse polarity, and the relative position of the first electrode and the second electrode during welding is adjusted to an appropriate position, the diameter of the welding wire used in all the electrodes in the multi-electrode is set to a thin diameter in the range of 1.0 to 1.6 mm, thereby making the total amount of deposited metal per unit time of all electrodes 200 g / min or more, and the bottom melting depth p of the thick steel plate 1.5 mm or more. Thus, it was found that multi-layer welding of thick steel plates can be achieved with high welding work efficiency.
[0013] The present invention has been completed based on the above findings and further studies. That is, the gist of the present invention is as follows.
[0014] [1] A narrow groove gas shielded arc welding method, wherein the groove angle θ is set to 25° or less, the bottom groove gap G is set to the range of 7 to 18 mm, and thick steel plates with a plate thickness t of 22 mm or more are joined by multi-layer welding of the narrow groove,
[0015] Wherein, the multi-layer welding is set as multi-electrode welding with more than 3 electrodes,
[0016] The first electrode and the second electrode of the plurality of electrodes are arranged at positions along predetermined parallel welding lines, and
[0017] One of the first electrode and the second electrode is set to positive polarity and the other is set to reverse polarity,
[0018] Furthermore, the distance a between the front ends of the welding wires supplied from the power supply electrode tips provided at the front ends of the welding torches of the first electrode and the second electrode is set to a range of 5 to 16 mm, and the angle α formed by the straight line connecting the front ends of the welding wires of the first electrode and the second electrode and the direction orthogonal to the welding line is set to a range of 60° or less,
[0019] Furthermore, the diameter of the welding wire used in all electrodes of the multi-electrode is set to a range of 1.0 to 1.6 mm.
[0020] The distance between the electrodes after the second electrode in the multi-electrode is set to a range of 10 to 100 mm,
[0021] Furthermore, the supply angle φ of each welding wire supplied from the power supply electrode tips of the first electrode and the second electrode to the bottom groove is optionally set to a range of 0 to 15° relative to a perpendicular line of the bottom groove,
[0022] Furthermore, the distance d between the side end of the front end of the welding wire supplied from the first electrode and the second electrode and the groove surface of the thick steel plate is optionally set to a range of 0.5 to 3.0 mm,
[0023] The total amount of deposited metal per unit time of all electrodes is set to 200 g / min or more, and the fusion depth p at the bottom of the thick steel plate in a direction perpendicular to the weld line is set to 1.5 mm or more.
[0024] [2] The narrow groove gas shielded arc welding method according to [1], wherein electrodes after the third electrode are arranged at the center of the groove behind the first electrode and the second electrode.
[0025] [3] The narrow groove gas shielded arc welding method according to [1] or [2], wherein a welding wire bent with a curvature radius in the range of 150 to 300 mm is fed to the power supply electrode tips of the first electrode and the second electrode.
[0026] [4] The narrow groove gas shielded arc welding method according to [1] or [2], wherein a mixed gas containing 60% by volume or more of CO2 gas is used as the shielding gas used in the multi-layer welding.
[0027] [5] A welding device for narrow groove gas shielded arc welding, which is a welding device for narrow groove gas shielded arc welding of thick steel plates for performing narrow groove multilayer welding on thick steel plates with a plate thickness t of 22 mm or more, wherein the narrow groove is a groove with a groove angle θ of 25° or less and a bottom groove gap G in the range of 7 to 18 mm,
[0028] The narrow groove gas shielded arc welding device comprises: a plurality of electrodes with more than three electrodes; a plurality of welding power supplies for supplying welding power to the plurality of electrodes; a power supply electrode head arranged at the front end of the welding torch of the plurality of electrodes; a plurality of welding wire supply units for respectively feeding welding wire to the plurality of electrodes; and a shielding gas supply unit for supplying shielding gas; and a welding table or a welding trolley.
[0029] Furthermore, among the plurality of electrodes, one of the first electrode and the second electrode is connected in a manner of setting the positive polarity and the other of the first electrode and the second electrode to a reverse polarity.
[0030] The power supply electrode tip is configured to supply welding wire in the range of 1.0 to 1.6 mm.
[0031] The first electrode and the second electrode are arranged at positions along a predetermined parallel welding line, and the distance between the first electrode and the second electrode is within a range of 5 to 16 mm as measured by the distance a between the tips of the welding wires supplied from the power supply electrode tips provided at the tips of the welding torches of the electrodes, and further, the first electrode and the second electrode are arranged in such a manner that an angle α formed by a straight line connecting the tips of the welding wires supplied from the power supply electrode tips provided at the tips of the welding torches of the first electrode and the second electrode and a direction orthogonal to the welding line is less than 60°,
[0032] Furthermore, the electrodes after the third electrode are arranged so that the distance between the electrodes after the second electrode is in the range of 10 to 100 mm in terms of the distance from the respective adjacent preceding electrodes.
[0033] Optionally, the power supply electrode tip disposed at the front end of the welding torch of the first electrode and the second electrode has an inclination at the front end thereof in the range of 0 to 15° relative to a vertical line.
[0034] [6] The welding device for narrow groove gas shielded arc welding according to [5], wherein the electrodes after the third electrode are arranged at the center of the groove behind the first electrode and the second electrode.
[0035] [7] The welding device for narrow groove gas shielded arc welding according to [5] or [6], wherein the welding wire supply unit is configured to be able to feed a welding wire bent with a curvature radius in the range of 150 to 300 mm.
[0036] [8] The welding device for narrow groove gas shielded arc welding according to [5] or [6], wherein the shielding gas supply unit is configured to supply a mixed gas containing 60% by volume or more of CO2 gas as the shielding gas.
[0037] Effects of the Invention
[0038] According to the narrow groove gas shielded arc welding method and the welding device for narrow groove gas shielded arc welding of the present invention, even if low-cost groove processing is implemented, there is no need to perform groove surface trimming, etc., and good welding quality and high welding construction efficiency can be achieved. In particular, defects such as poor fusion and defects such as high-temperature cracking in the center of the weld metal can be prevented. Therefore, multi-electrode welding with more than 3 electrodes can be applied to all layers of multi-layer welding, thereby improving welding construction efficiency. If the technology involved in the present invention is used to manufacture welded joints, the welding construction cost can be greatly reduced compared with the manufacture of existing welded joints, which has a significant effect in the industry. In particular, the present invention is particularly suitable for welding construction of general structures such as buildings, bridges and shipbuilding. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] [ Figure 1 ] is a cross-sectional schematic diagram showing the groove shape of a narrow groove gas shielded arc welding method suitable for one embodiment of the present invention.
[0040] [ Figure 2 ] are explanatory diagrams showing the essentials of welding construction using three electrodes involved in the above-mentioned embodiment, (a) shows a front view, and (b) shows a top view.
[0041] [ Figure 3 ] is an explanatory diagram showing an example of a cross-section of a weld joint in which multilayer welding using three electrodes according to the above-mentioned embodiment is performed.
[0042] [ Figure 4 ] are schematic explanatory diagrams showing a welding device for narrow groove gas shielded arc welding involved in other embodiments of the present invention, (a) shows a stereoscopic view, (b) shows a front view, and (c) shows a top view. DETAILED DESCRIPTION
[0043] The following is a detailed description of the embodiments of the present invention. It should be noted that the drawings are schematic and may differ from the actual ones. In addition, the following embodiments illustrate the devices and methods used to concretize the technical concept of the present invention, and do not specifically constitute the following structure. That is, the technical concept of the present invention can be implemented in a variety of ways within the technical scope described in the claims.
[0044] [Bevel shape]
[0045] First, refer to Figure 1 To illustrate the groove shape suitable for the narrow groove gas shielded arc welding method involved in one embodiment of the present invention. In the figure, reference numeral 1 represents a thick steel plate, 2 represents the groove surface of the thick steel plate, symbol θ represents the groove angle, G represents the bottom groove gap, and t represents the plate thickness. The groove used in this embodiment is set as a V-shaped groove (θ>0°) or an I-shaped groove (θ=0°). In the V-shaped groove, the side with a smaller gap in the plate thickness direction is set as the bottom.
[0046] The present embodiment is a narrow groove gas shielded arc welding method, wherein the groove angle θ is set to be less than 25°, the bottom groove gap G is set to be in the range of 7 to 18 mm, and thick steel plates 1, 1 with a plate thickness t of 22 mm or more are joined by multi-layer welding of the narrow groove. Here, "thick steel plate" includes thick wall materials, thick steel materials, etc. in addition to steel plates.
[0047] Thickness t of thick steel plate 1: 22 mm or more
[0048] The plate thickness t of the thick steel plate 1 is set to be 22 mm or more. This is because if the plate thickness of the thick steel plate 1 is less than 22 mm, the groove angle is increased and the groove gap is reduced in the existing レ-shaped groove, resulting in a groove cross-sectional area smaller than the groove targeted by the present invention. Therefore, there is a case where the existing レ-shaped groove becomes a highly efficient welding with a small amount of weld metal.
[0049] It should be noted that even if a special structure is included, the maximum plate thickness of the steel structure is about 200 mm. In this embodiment, it is preferred that the upper limit of the plate thickness t of the thick steel plate 1 is set to 200 mm. In addition, this embodiment can be applied to various thick steel plates from mild steel plates to 980 MPa-level high-tensile steel plates. It can be applied to the welding of 590 MPa-level high-tensile thick steel plates without preheating.
[0050] Groove angle θ: less than 25°
[0051] The groove used in this embodiment is an I-shaped groove or a V-shaped groove.
[0052] The smaller the groove (groove angle), the more efficient welding can be achieved. However, if the groove (groove angle) is small, defects such as poor fusion are likely to occur. From the perspective of reducing the amount of weld metal, it is most effective to set the groove angle θ to 0°, that is, to set the groove to an I-shaped groove. On the other hand, the I-shaped groove closes during welding due to welding thermal strain. Therefore, it is preferable to set the groove angle θ corresponding to the plate thickness t in consideration of the welding thermal strain.
[0053] Specifically, when the plate thickness t is set to a range of 22 to 200 mm, the groove angle θ (°) is preferably set to a range of (0.5×t / 20) to (2.0×t / 20). It is more preferably set to a range of (0.8×t / 20) to (1.8×t / 20). It is further preferred that the upper limit of the groove angle θ is set to 10°.
[0054] On the other hand, the existing welding construction method can be applied to welding using a groove having a groove angle θ exceeding 25°. Therefore, in the present embodiment, the upper limit of the groove angle θ is set to 25°.
[0055] Bottom groove gap G: 7~18mm
[0056] If the bottom groove gap G is less than 7 mm, it becomes difficult to perform multi-electrode welding with more than 3 electrodes from the viewpoint of suppressing the occurrence of welding defects. On the other hand, if the bottom groove gap G exceeds 18 mm, the existing welding construction method can be applied. Therefore, in the present embodiment, the bottom groove gap G is set to a range of 7 to 18 mm. If it is within this range, welding construction under the existing welding construction method is difficult, and by applying the present embodiment, welding construction is expected to be more efficient.
[0057] [Narrow groove gas shielded arc welding method]
[0058] Below, refer to Figure 2 and Figure 3 The narrow groove gas shielded arc welding method according to the present embodiment will be described. Figure 2 It is an explanatory diagram showing the outline of welding work using three electrodes according to the present embodiment. Figure 2 (a) is the main view, Figure 2 (b) is a top view.
[0059] Figure 3 This is an explanatory diagram showing an example of a cross section of a welded joint in which multi-layer welding using three electrodes is performed. In this embodiment, the narrow groove of the above-mentioned shape is used to perform multi-layer welding by multi-electrode welding with three or more electrodes for the first layer welding 21 and the second layer welding 22. Furthermore, welding is performed at a high welding efficiency in a manner such that a welded joint is obtained in which defects such as poor fusion and high-temperature cracking, especially high-temperature cracking in the center of the weld metal, are suppressed.
[0060] In the groove processing of the thick steel plate in this embodiment, processing based on gas cutting, plasma cutting, laser cutting, etc. is performed. However, mechanical processing is not excluded. The required melting depth of the groove surface in narrow groove gas shielded arc welding (described later) Figure 3p) shown is mainly determined by the surface properties of the groove surface 2, especially the depth of the recess and the cleanliness. In the groove processing using the most common gas cutting, except for special steels, stainless steel, etc., the cut surface produced will be quite different depending on the gas flow rate and the choice of the burner during gas cutting. For example, when the gas flow rate and the burner are well adjusted, the depth of the recess on the groove surface is about 0.2 mm or less. However, in special cases, for example, when the flame flow rate is lower than usual due to wear of the burner, etc., a recess depth of more than 1 mm may occur. However, even if such a recess occurs, it does not need to be trimmed in general structures and can be directly used for welding.
[0061] Therefore, in order to effectively prevent defects caused by high temperature cracking, poor fusion, etc., it is necessary to melt the groove surface more deeply during welding, especially the bottom (thick steel plate) in the groove where the temperature during welding is low and the melting depth tends to decrease. In addition, since the cut surface is covered with a thick oxide film generated by processing heat, it is still necessary to melt the groove surface more deeply during welding.
[0062] Based on the above situation, in this embodiment, the melting depth p at the bottom of the groove (thick steel plate) is set to be 1.5 mm or more. It should be noted that it is preferably set to be 2.0 mm or more. However, if the melting depth p exceeds 4 mm, undercut will occur on the upper part of the weld bead of the groove surface 2, which becomes a cause of welding defects. Therefore, the melting depth is preferably 4 mm or less.
[0063] In the present embodiment, it is important to set the melting depth p at the bottom of the groove (thick steel plate) to 1.5 mm or more. In order to achieve this with high welding efficiency, it is very important to appropriately control the welding conditions of the gas shielded arc welding.
[0064] The welding conditions will be described in detail below.
[0065] · Multi-layer welding is set to multi-electrode welding with three or more electrodes, and the first electrode and the second electrode are arranged at positions along a predetermined parallel welding line
[0066] In this embodiment, from the viewpoint of improving high temperature cracking resistance, especially from the viewpoint of suppressing high temperature cracking in the weld metal, the multi-layer welding is set to multi-electrode welding with three or more electrodes. It should be noted that from the viewpoint of improving welding construction efficiency, it is preferably four electrodes or less.
[0067] In multi-layer welding of narrow grooves, when one pass is performed per layer, heat is easily concentrated in the center of the groove in one electrode, so the melting on the groove surface 2 of the thick steel plate 1 is insufficient, which easily leads to defects caused by poor fusion (cold lap) and spatter and slag attached to the groove surface 2. In particular, since the temperature of the thick steel plate 1 in the first layer welding 21 is low and the melting depth p becomes small, defects caused by poor fusion are easily generated. Based on this situation, in the present embodiment, the first electrode and the second electrode of the multi-electrode of more than three electrodes are arranged and welded along a predetermined parallel welding line 8. With respect to the welding direction WD, the numbering starts from the preceding electrode, and the same applies to the following. As an example, in Figure 2 2 shows the construction method of performing multi-layer welding with three electrodes. It is preferred that the first electrode 3 and the second electrode 4 are respectively along mutually parallel welding lines 8 close to different groove surfaces 2.
[0068] One of the first electrode and the second electrode is set to positive polarity and the other is set to reverse polarity
[0069] If the first electrode 3 and the second electrode 4 are set to the same polarity (for example, the first electrode 3 and the second electrode 4 are both connected to the welding wire positively), the mutual arcs will be turned inward due to the electromagnetic force of mutual attraction, and the heat will be concentrated in the center of the groove. Therefore, it is impossible to obtain sufficient melting at the groove surface 2. On the other hand, if one of the first electrode 3 and the second electrode 4 is set to be connected to the welding wire negatively (positive polarity) and the other is set to be connected to the welding wire positively (reverse polarity), and the configuration of the first electrode 3 and the second electrode 4 is appropriately controlled, the magnetic field caused by the mutual welding current will generate a strong outward electromagnetic force, and the arcs will repel each other. As a result, a sufficient melting depth p can be obtained on the groove surface.
[0070] Based on this, in this embodiment, one of the welding wires supplied from the power supply electrode tips at the front ends of the first and second electrodes of the welding torch is connected to the negative wire connection (positive polarity) and the other is connected to the positive wire connection (reverse polarity).
[0071] · Distance a between the front ends of the welding wires supplied from the power supply electrode tips arranged at the front ends of the first and second welding torches: 5 to 16 mm
[0072] The distance a between the tips of the welding wires 3b and 4b supplied from the power supply electrode tips 3a and 4a at the tips of the respective welding torches of the first electrode 3 and the second electrode 4 (see Figure 2 (b), hereinafter also referred to as "the distance between the first and second electrodes") is adjusted to a range of 5 to 16 mm. It should be noted that the "distance between the ends of the welding wires" referred to here refers to the distance between the centers of the ends of the welding wires in each electrode.
[0073] If the distance a between the 1st and 2nd electrodes is less than 5mm, the current (electrons) flows between the electrodes, thereby reducing the heat carried by the arc itself, and it is impossible to obtain sufficient melting of the groove surface 2. On the other hand, if the distance a between the 1st and 2nd electrodes exceeds 16mm, the outward electromagnetic force between the electrodes decreases inversely proportional to the distance. Therefore, it is impossible to obtain an arc repulsive force to overcome the inward electromagnetic force generated by the current flowing on the groove surface 2, and the mutual arcs become inward, and the heat is concentrated in the center of the groove. As a result, it is impossible to obtain sufficient melting at the groove surface 2.
[0074] In addition, in narrow groove welding, the suppression of welding defects caused by the adhesion of spatters to the groove surface 2 has become a problem. In this regard, the first electrode 3 and the second electrode 4 are arranged along predetermined parallel welding lines 8, 8, one of which is set to positive polarity and the other is set to reverse polarity, and the distance a between the first and second electrodes is adjusted to a range of 5 to 16 mm, so that the spatters are absorbed by the respective molten metals. As a result, since the adhesion of spatters to the groove surface 2 is suppressed, a healthy weld can be obtained.
[0075] Based on the above situation, the distance a between the front ends of the welding wires supplied from the power supply electrode tips provided at the front ends of the first electrode 3 and the second electrode 4 is adjusted to a range of 5 to 16 mm. It should be noted that in order to obtain a deeper and more stable melting of the groove surface 2 by stronger arc repulsion, it is preferred to adjust the distance a between the first and second electrodes to a range of 5 to 8 mm.
[0076] Angle α formed by a straight line connecting the ends of the welding wires of the first electrode and the second electrode and a direction perpendicular to the welding line: 60° or less
[0077] In this embodiment, the arc repulsion is used to ensure the melting of the groove surface 2. If the angle α formed by the straight line connecting the tips of the welding wires of the first electrode and the second electrode and the direction perpendicular to the welding line is α (see Figure 2 If (b), hereinafter also referred to as "the 1st-2nd electrode configuration angle") exceeds 60°, sufficient arc repulsion force cannot be obtained. Therefore, sufficient melting cannot be obtained on the groove surface 2. Therefore, the 1st-2nd electrode configuration angle α is limited to a range below 60°. More preferably, it is below 45°. It should be noted that the 1st-2nd electrode configuration angle α can also be 0°.
[0078] Wire diameter D: 1.0~1.6mm
[0079] The welding wire for gas shielded arc welding is usually manufactured in a diameter range of 0.6 to 2.0 mm. When welding with the same welding current, the thinner the welding wire diameter D, the higher the deposition rate can be achieved by utilizing Joule heat. Therefore, in order to achieve efficient welding construction, it is preferred to select a thinner welding wire diameter D. On the other hand, if the welding wire diameter D is too thin, the welding wire softens due to Joule heat, and the welding becomes unstable. Taking these circumstances into consideration, the diameter D of the welding wire is set to the range of 1.0 to 1.6 mm. It should be noted that the diameter D of the welding wire is preferably in the range of 1.2 to 1.4 mm. In the present embodiment, the welding wire used in all electrodes in the multi-electrode is set to the same type.
[0080] It should be noted that the welding wire used in the present embodiment is preferably a steel wire having a diameter D within the above range and corresponding to the steel type of the thick steel plate 1 as a material to be welded, for example, various steel wires specified in JIS Z 3312.
[0081] · Total deposited metal amount per unit time for all electrodes: 200g / min or more
[0082] In order to perform efficient welding construction, it is effective to increase the amount of deposited metal per layer. In the present embodiment, in order to perform efficient welding construction compared with the existing method, the above-mentioned welding wire is used to perform welding in a manner such that the total amount of deposited metal per unit time of all electrodes is 200g / min or more. It should be noted that if the amount of deposited metal per unit time is less than 200g / min, the welding construction time becomes long. In conventional single-electrode gas shielded arc welding, although there are differences caused by the wire diameter D and the welding current, the amount of deposited metal per unit time is about 60 to 160g / min. As for the deposition speed involved in the present embodiment, a deposition speed about twice that of the existing single-electrode welding can be obtained.
[0083] Distance between electrodes after the second electrode: 10 to 100 mm
[0084] It is important to control the arc heat source generated by the electrodes after the third electrode 5 to an appropriate range to prevent the occurrence of high-temperature cracking. If the distance between the electrodes after the second electrode 4 is too small, the heat input is concentrated in the central part of the weld metal, and the possibility of high-temperature cracking during solidification becomes higher. On the other hand, if the distance between the electrodes after the second electrode 4 is too large, the interaction between the electrodes becomes too small, the shape of the molten pool 20 becomes too long or separated, and high-temperature cracking is likely to occur during solidification. Based on this situation, in order to prevent high-temperature cracking, in this embodiment, the distance between the electrodes after the second electrode (inter-electrode distance) is limited to a range of 10 to 100 mm. It should be noted that the preferred range is 20 to 80 mm.
[0085] The above welding conditions are basic welding conditions in this embodiment. By performing welding under such conditions, even if the fusion depth p at the bottom of the thick steel plate in the direction perpendicular to the weld line is 1.5 mm or more and multi-electrode welding with three or more electrodes is performed on each layer, a weld joint that prevents the occurrence of high-temperature cracking of the weld metal portion can be obtained.
[0086] It should be noted that in this embodiment, by further satisfying the following welding conditions in addition to the above-mentioned basic welding conditions, the melting depth p from the groove surface 2 at the bottom of the thick steel plate 1 in the narrow groove can be obtained more deeply and stably.
[0087] · Supply angle φ of each welding wire supplied from the power supply electrode tips of the first electrode and the second electrode to the bottom groove: 0 to 15° relative to the vertical line of the bottom groove
[0088] The arc has directivity and has the property of being easily directed toward the direction indicated by the tip of the electrode (welding wire). In order to effectively use the directivity of the arc for melting the groove surface, it is advantageous to direct the direction indicated by the tip of the electrode toward the groove surface 2. The direction indicated by the tip of the electrode changes greatly depending on the supply angle of the welding wire supplied from the power supply electrode tip at the front end of the welding torch. In this regard, with respect to the supply angle φ of each welding wire 3b, 4b supplied from the power supply electrode tips 3a, 4a of the first electrode 3 and the second electrode 4 to the bottom groove, the direction toward the outside, that is, the direction approaching the groove surface 2 is set as positive, and the direction narrowing toward the inside is set as negative. When the supply angle φ of the welding wire 3b, 4b supplied from the power supply electrode tips 3a, 4a at the front end of the welding torch to the bottom groove is lower than 0° relative to the vertical line, that is, when the tips of the welding wires 3b, 4b of the first electrode 3 and the second electrode 4 are close, the current flows into a path with a smaller resistance. As a result, the arc climbs up in the welding wire as the electrode (arc climbing), and it becomes difficult to maintain the melting of the target groove surface 2, especially the bottom. On the other hand, if the supply angle φ of the welding wire supplied from the power supply electrode tip at the front end of the welding torch to the bottom groove exceeds 15° relative to the vertical line, the arc is excessively directed toward the groove surface 2 and the weld bead shape becomes convex, and the melting of the arc in the welding after the first layer 21 becomes insufficient and welding defects are easily generated. Therefore, it is preferred that the supply angle φ of the welding wire 3b, 4b of the first electrode 3 and the second electrode 4 to each bottom groove is in the range of 0 to 15° relative to the vertical line. More preferably, it is in the range of 5 to 12°. It should be noted that the supply angle φ of the welding wire 3b, 4b of the first electrode 3 and the second electrode 4 to each bottom groove is the same as the inclination of the power supply electrode tip 3a, 4a, especially the front end of the power supply electrode tip, so the supply angle of the welding wire can be controlled by the inclination of the front end of the power supply electrode tip.
[0089] Distance d between the side end of the tip of the welding wire supplied from the first electrode and the second electrode and the groove surface of the thick steel plate: 0.5 to 3.0 mm
[0090] If the distance between the side end of the front end of the welding wire 3b, 4b at the bottom groove and the groove surface 2 of the thick steel plate 1 is less than 0.5 mm, the arc is generated between the upper part of the welding wire and the groove surface 2, and the groove surface 2 at the bottom of the thick steel plate cannot be efficiently melted. On the other hand, if it exceeds 3.0 mm, the arc is far away from the groove surface 2, and the groove surface 2 cannot be efficiently melted. Therefore, it is preferred that the distance d between the side end of the front end of the welding wire 3b, 4b and the groove surface 2 of the thick steel plate 1 is set in the range of 0.5 to 3.0 mm. It is more preferably in the range of 0.5 to 2.0 mm, and even more preferably in the range of 0.5 to 1.0 mm. The so-called "side end of the front end of the welding wire" here refers to the side end on the side close to the groove surface 2 of the thick steel plate 1 that is to be melted by each electrode 3, 4.
[0091] · Radius of curvature R of the welding wire fed to the power supply electrode tips of the first and second electrodes: 150 to 300 mm
[0092] In the present embodiment, in order to control the supply angle φ of the welding wire 3b, 4b supplied from the power supply electrode tips 3a, 4a at the front end of the welding torch of the first electrode 3 and the second electrode 4, the power supply electrode tips 3a, 4a with bent front ends are used. At this time, since the welding wire 3b, 4b passes through the power supply electrode tips 3a, 4a with bent front ends, it is preferable to bend the welding wire 3b, 4b in advance using a so-called three-point roller or the like in order to make it pass more smoothly.
[0093] When the curvature radius R of the welding wire 3b, 4b is less than 150 mm, the feeding resistance of the welding wire becomes large, the welding wire 3b, 4b cannot be fed stably, and it becomes difficult to maintain the arc. On the other hand, if the curvature radius R of the welding wire 3b, 4b exceeds 300 mm, there is no effect on reducing the feeding resistance of the welding wire when the front end of the power supply electrode tip 3a, 4a is bent, so the welding wire 3b, 4b cannot be fed stably, and it becomes difficult to maintain the arc. Based on this situation, it is preferred that the curvature radius R of the welding wire 3b, 4b fed to the power supply electrode tip 3a, 4a of the first electrode 3 and the second electrode 4 is in the range of 150 to 300 mm. More preferably, it is in the range of 175 to 275 mm.
[0094] · Electrodes after the third electrode: placed at the center of the groove behind the first and second electrodes
[0095] If the weld stack height H exceeds the bottom groove gap G, that is, H / G exceeds 1, the risk of high-temperature cracking increases. In order to avoid this, it is effective to arrange the electrodes after the third electrode 5 at the center of the groove behind the first electrode 3 and the second electrode 4 relative to the welding direction WD. In addition, thereby, it is further possible to reduce the number of stacking, which can greatly reduce the risk of stacking defects in multi-layer welding. It should be noted that the polarity after the third electrode 5 is not particularly limited, and it can also be any of the negative connection of the welding wire (positive polarity) and the positive connection of the welding wire (reverse polarity). It should be noted that the so-called "center of the groove" allows the range on both sides of 10% of the groove gap G relative to the center line 81 of the groove when viewed from above.
[0096] ·Shielding gas: A mixed gas containing more than 60% by volume of CO2 gas
[0097] Since the amount of oxygen in the weld metal is greatly affected by the composition of the shielding gas, in this embodiment, as the shielding gas used in the gas shielded arc welding, a mixed gas containing 60% by volume or more of CO2 gas and the balance being an inert gas such as Ar is preferably used. It should be noted that the CO2 gas is more preferably 100% by volume. It should be noted that in this embodiment, it is preferred to increase the oxygen concentration in the weld metal that controls the flow of the molten metal of the weld metal so that the forced convection of the weld metal is from the center to the outside, thereby stably deepening the melting depth p at the bottom of the thick steel plate in the groove.
[0098] It should be noted that the conditions other than the above do not need to be particularly limited and can be carried out according to conventional methods. For example, the welding current can be set in the range of 280 to 360 A, the welding voltage that increases with the current can be set in the range of 32 to 37 V, the welding speed can be set in the range of 30 to 90 cm / min, the wire protrusion length can be set in the range of 15 to 30 mm, and the welding heat input per pass can be set in the range of 10 to 50 kJ / cm.
[0099] [Welding equipment]
[0100] Next, a preferred welding device (hereinafter referred to as the present device) used in the present embodiment will be described.
[0101] This device is a welding device for narrow groove gas shielded arc welding, which is used to join thick steel plates with a thickness of 22 mm or more by multi-layer welding of narrow grooves using the multi-electrode gas shielded welding method with more than three electrodes involved in the above-mentioned embodiment. The so-called "narrow groove" here is Figure 1 The groove angle θ shown is a V groove (θ>0°) or an I groove (θ=0°) with a groove angle θ of 25° or less, and the bottom groove gap G is in the range of 7 to 18 mm.
[0102] Figure 42 shows an outline of the structure of this device in the case of four electrodes. Figure 4 (a) is a stereogram, Figure 4 (b) is the main view, Figure 4 (c) is a top view.
[0103] The welding device 100 of the present device comprises: a welding table or a welding trolley (not shown); a plurality of electrodes 3 to 6 having more than three electrodes; a plurality of welding power sources 9 to 12 for supplying welding power to the plurality of electrodes 3 to 6; power supply electrode heads 3a to 6a provided at the front ends of the welding torches of the plurality of electrodes 3 to 6; a plurality of welding wire supply units (not shown) for respectively feeding welding wires 3b to 6b to the plurality of electrodes 3 to 6; and a shielding gas supply unit (not shown) for supplying shielding gas.
[0104] In the welding device 100, one of the first electrode 3 and the second electrode 4 among the plurality of electrodes is connected in a manner that the welding wire is negatively connected (positive polarity) and the other is positively connected (reverse polarity). In addition, the power supply electrode tips 3a to 6a are configured to supply welding wires 3b to 6b in the range of 1.0 to 1.6 mm. In addition, the first electrode 3 and the second electrode 4 are arranged at positions along predetermined parallel welding lines 8, 8, and the distance between the first electrode 3 and the second electrode 4 is within the range of 5 to 16 mm in terms of the distance a between the tips of the welding wires 3b and 4b supplied from the power supply electrode tips 3a and 4a provided at the front ends of the welding torches of the electrodes. In addition, the angle α formed by the straight line connecting the tips of the welding wires 3b and 4b supplied from the power supply electrode tips 3a and 4a provided at the front ends of the welding torches of the first electrode 3 and the second electrode 4 and the orthogonal direction of the welding line 8 is 60 degrees or less. In the welding device 100, the electrodes after the third electrode 5 are arranged so that the distance between the electrodes after the second electrode 4 is in the range of 10 to 100 mm in terms of the distance from the respective adjacent preceding electrodes. For example, the third electrode 5, which is the subsequent electrode, is arranged so that the distance b between the second electrode 4 and the third electrode 5 is in the range of 10 to 100 mm in terms of the distance between the front ends of the welding wires 4b and 5b supplied from the welding electrode tips 4a and 5a arranged at the front ends of the welding torches of the respective electrodes 4 and 5. The arrangement of the electrodes after the third electrode 5 is similar. The fourth electrode 6 is arranged so that the distance c between the third electrode 5 and the fourth electrode 6 is in the range of 10 to 100 mm.
[0105] In the welding device 100 of the present device, three or more electrodes are arranged as electrodes on a welding table or a welding carriage in a narrow groove of a predetermined shape formed by a thick steel plate 1 as a material to be welded and a backing material 7. Figure 44 electrodes are shown in the figure, which are the first electrode 3, the second electrode 4, the third electrode 5 and the fourth electrode 6. Each electrode is connected to a welding power source 9, 10, 11, and 12, and is supplied with welding power. It should be noted that the first electrode 3 and the second electrode 4 are connected in such a way that one is negatively connected to the welding wire (positive polarity) and the other is positively connected to the welding wire (reverse polarity). The polarity of the electrodes after the third electrode 5 is not particularly limited, and can be set to positive polarity or reverse polarity.
[0106] At the front end of the welding torch of each electrode 3, 4, 5, 6, a power supply electrode tip 3a, 4a, 5a, 6a is provided, respectively, and welding current is supplied to the welding wire 3b, 4b, 5b, 6b via each power supply electrode tip 3a, 4a, 5a, 6a. In addition, in the welding device 100 involved in the present device, there is a welding wire supply unit (not shown) and a shielding gas supply unit (not shown) for supplying welding wire 3b, 4b, 5b, 6b to each welding torch (electrode). In addition, there may also be a common moving unit (not shown) that can move the electrode or welding table at a specified speed. In addition, both the welding wire supply unit and the shielding gas supply unit are suitable for using common units.
[0107] It should be noted that the power supply electrode tips 3a and 4a provided at the front ends of the welding torches of the first electrode 3 and the second electrode 4 are preferably inclined outwardly at the front ends in the range of 0 to 15° relative to the vertical line. As a result, the melting depth p of the groove surface 2 can be stably deepened at the groove bottom. In addition, if the welding wire supply unit for supplying welding wires to the first electrode 3 and the second electrode 4 is configured to be able to feed welding wires 3b and 4b bent with a curvature radius R in the range of 150 to 300 mm, it becomes easy to set the supply angle φ of the welding wires 3b and 4b from the above-mentioned power supply electrode tips 3a and 4a to the range of 0 to 15°.
[0108] It should be noted that in Figure 4 (c) shows only the tip positions of the welding wires 3b, 4b, 5b, 6b of the electrodes 3, 4, 5, 6, and other structures are omitted.
[0109] In addition, it is preferred that the electrodes after the third electrode 5 are arranged at the center of the groove behind the first electrode 3 and the second electrode 4 with respect to the welding direction WD. This can suppress the occurrence of high temperature cracking. It should be noted that the "center of the groove" allows the range on both sides of 10% of the groove gap G relative to the center line 81 of the groove when viewed from above.
[0110] Hereinafter, the present invention will be further described based on examples.
[0111] Example
[0112] For various thick steel plates 1 of steel type (grade) and plate thickness shown in Table 1, groove processing was performed by gas cutting to obtain groove shapes shown in Table 2. It should be noted that no finishing such as grinding was performed on the groove surface 2. For the groove surface 2 after processing, the surface properties of the groove surface 2 were measured using a laser displacement meter, and the maximum concave depth was obtained and shown in Table 2.
[0113] [Table 1]
[0114]
[0115] [Table 2]
[0116]
[0117] The thick steel plate 1 with the groove shape shown in Table 2 sets the length in the welding direction WD to 500 mm. In addition, a welding wire corresponding to the steel type (grade) shown in Table 1 is used as the first layer welding 21, and narrow groove gas shielded arc welding is performed under the welding conditions shown in Tables 3 and 4. Next, multi-layer welding after the second layer welding 22 is performed to obtain a narrow groove gas shielded arc welding joint with a welding length of 500 mm. It should be noted that the welding conditions after the second layer welding 22 are set to be the same as those of the first layer welding 21. When using electrodes after the third electrode 5, the electrodes are all arranged at the center of the groove behind the first electrode 3 and the second electrode 4 relative to the welding direction WD.
[0118] The obtained welded joint is cut into 5 sections along the length direction, as shown in Figure 3 As shown in Table 4, the bottom melting width W is measured for each section. For each section, the length corresponding to the bottom groove gap G is subtracted from the obtained melting width W, and the obtained value is divided by 2, and the obtained value is set as the melting depth in the section. Then, the average value of the five sections is calculated and set as the bottom melting depth p of the welded joint. The obtained results are shown in Table 4. In addition, when observing the section, the presence or absence of high temperature cracking is also investigated and shown in Table 4.
[0119] In addition, the obtained welded joints were subjected to ultrasonic flaw detection tests to evaluate the presence or absence of welding defects. It should be noted that the case where no defects were detected was marked as ◎, the case where only the detected defects were qualified defects with a length of 3 mm or less was marked as ○, and the case where the length of the detected defects exceeded 3 mm was marked as ×. The obtained results are recorded in Table 4.
[0120] [Table 3]
[0121]
[0122] [Table 4]
[0123]
[0124] In the examples of the invention, multi-electrode welding with more than 3 electrodes was used to perform multi-layer welding of narrow grooves, and the bottom melting depth p showed more than 1.5 mm, and no high-temperature cracking occurred. In addition, there was no problem of welding defects without trimming the groove surface 2. Therefore, a sound narrow groove gas shielded arc welding joint was formed, and the welding construction efficiency was also improved. On the other hand, in the comparative examples, at least one of the conditions deviated from the scope of the present invention, and as a result, the bottom melting depth p was less than 1.5 mm, or high-temperature cracking was confirmed, or unacceptable welding defects were detected, and a sound narrow groove gas shielded arc welding joint could not be obtained.
[0125] Description of Reference Numerals
[0126] 1 Thick steel plate
[0127] 2 Bevel surface
[0128] 31st electrode
[0129] 3a, 4a, 5a, 6a power supply electrode head
[0130] 3b, 4b, 5b, 6b welding wire
[0131] 4 Second electrode
[0132] 5Third electrode
[0133] 6 4th electrode
[0134] 7 Backing material
[0135] 8 Welding line
[0136] 9, 10, 11, 12 welding power supply
[0137] 20 Molten Pool
[0138] 21First floor (welding)
[0139] 22 2 layers (welding)
[0140] 81 Center line of groove
[0141] a (distance between the 1st and 2nd electrodes)
[0142] b (distance between the 2nd and 3rd electrodes)
[0143] c (distance between the 3rd and 4th electrodes)
[0144] d (distance between welding wire and groove surface)
[0145] G (bottom) groove clearance
[0146] W(bottom) melting width
[0147] WD welding direction
[0148] θ Groove angle
Claims
1. A narrow groove gas shielded arc welding method, wherein: The groove angle θ is set to 25° or less, the bottom groove gap G is set to 7 to 18 mm, and thick steel plates with a plate thickness t of 22 mm or more are joined by multi-layer welding with narrow grooves. Wherein, the multi-layer welding is set as multi-electrode welding with more than 3 electrodes, The first electrode and the second electrode of the plurality of electrodes are arranged at positions along predetermined parallel welding lines, and One of the first electrode and the second electrode is set to positive polarity and the other is set to reverse polarity, Furthermore, the distance a between the front ends of the welding wires supplied from the power supply electrode tips provided at the front ends of the welding torches of the first electrode and the second electrode is set to a range of 5 to 16 mm, and the angle α formed by the straight line connecting the front ends of the welding wires of the first electrode and the second electrode and the direction orthogonal to the welding line is set to a range of 60° or less, Furthermore, the diameter of the welding wire used in all electrodes of the multi-electrode is set to a range of 1.0 to 1.6 mm. The distance between the electrodes after the second electrode in the multi-electrode is set to a range of 10 to 100 mm, Furthermore, the supply angle φ of each welding wire supplied from the power supply electrode tips of the first electrode and the second electrode to the bottom groove is optionally set to a range of 0 to 15° relative to a perpendicular line of the bottom groove, Furthermore, the distance d between the side end of the front end of the welding wire supplied from the first electrode and the second electrode and the groove surface of the thick steel plate is optionally set to a range of 0.5 to 3.0 mm, The total amount of deposited metal per unit time of all electrodes is set to 200 g / min or more, and the fusion depth p at the bottom of the thick steel plate in a direction perpendicular to the weld line is set to 1.5 mm or more.
2. The narrow groove gas shielded arc welding method according to claim 1, wherein: The electrodes after the third electrode are arranged at the center of the groove behind the first electrode and the second electrode.
3. The narrow groove gas shielded arc welding method according to claim 1 or 2, wherein: A welding wire bent with a curvature radius in the range of 150 to 300 mm is fed to the power supply electrode tips of the first electrode and the second electrode.
4. The narrow groove gas shielded arc welding method according to claim 1 or 2, wherein: A mixed gas containing 60% by volume or more of CO 2 gas is used as the shielding gas used in the multi-layer welding.
5. A welding device for narrow groove gas shielded arc welding, which is a welding device for narrow groove gas shielded arc welding of thick steel plates for performing multi-layer welding of narrow grooves on thick steel plates with a plate thickness t of 22 mm or more, wherein the narrow groove is a groove with a groove angle θ of less than 25° and a bottom groove gap G in the range of 7 to 18 mm, in, The narrow groove gas shielded arc welding device comprises: a plurality of electrodes with more than three electrodes; a plurality of welding power supplies for supplying welding power to the plurality of electrodes; a power supply electrode head arranged at the front end of the welding torch of the plurality of electrodes; a plurality of welding wire supply units for respectively feeding welding wire to the plurality of electrodes; and a shielding gas supply unit for supplying shielding gas; and a welding table or a welding trolley, Furthermore, among the plurality of electrodes, one of the first electrode and the second electrode is connected in a manner of setting the positive polarity and the other of the first electrode and the second electrode to a reverse polarity. The power supply electrode tip is configured to supply welding wire in the range of 1.0 to 1.6 mm. The first electrode and the second electrode are arranged at positions along a predetermined parallel welding line, and the distance between the first electrode and the second electrode is within a range of 5 to 16 mm as measured by the distance a between the tips of the welding wires supplied from the power supply electrode tips provided at the tips of the welding torches of the electrodes, and further, the first electrode and the second electrode are arranged in such a manner that an angle α formed by a straight line connecting the tips of the welding wires supplied from the power supply electrode tips provided at the tips of the welding torches of the first electrode and the second electrode and a direction orthogonal to the welding line is less than 60°, Furthermore, the electrodes after the third electrode are arranged so that the distance between the electrodes after the second electrode is in the range of 10 to 100 mm in terms of the distance from the respective adjacent preceding electrodes. Optionally, the power supply electrode tip disposed at the front end of the welding torch of the first electrode and the second electrode has an inclination at the front end thereof in the range of 0 to 15° relative to a vertical line.
6. The welding device for narrow groove gas shielded arc welding according to claim 5, wherein: The electrodes after the third electrode are arranged at the center of the groove behind the first electrode and the second electrode.
7. The welding device for narrow groove gas shielded arc welding according to claim 5 or 6, wherein: The welding wire supply unit is configured to be able to feed a welding wire bent with a curvature radius in a range of 150 to 300 mm.
8. The welding device for narrow groove gas shielded arc welding according to claim 5 or 6, wherein: The shielding gas supply unit is configured to supply a mixed gas containing 60% by volume or more of CO 2 gas as the shielding gas.