Lithographic printing plate precursor

通过在光聚合物印刷版涂层中使用pH敏感着色剂和热敏成色IR染料,解决了印出图像对比度低和不稳定的问题,实现了在加工和储存期间保持高对比度的效果,确保印刷 Quality and correctness of image rendering.

CN118973822APending Publication Date: 2024-11-15AGFA OFFSET BV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380032420.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-07
Filing Date
2023-01-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The printed image obtained after exposure by existing photopolymer printing plates is characterized by a low contrast between exposed and non-exposed areas and gradually decreasing over time, making it difficult to maintain stability during processing and storage, affecting printing quality and image rendering. .

Method used

Using a coating containing a pH-sensitive colorant and a thermosensitive color-forming IR dye, high contrast printed images are formed by IR radiation and heating, and remain stable or enhanced during processing and storage.

Benefits of technology

The printed images maintaining high contrast during processing and storage ensures image clarity and color rendering accuracy, and facilitates image quality evaluation and press settings adjustment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005070011700000091
    Figure BDA0005070011700000091
  • Figure BDA0005070011700000121
    Figure BDA0005070011700000121
  • Figure BDA0005070011700000141
    Figure BDA0005070011700000141
Patent Text Reader

Abstract

Disclosed is a lithographic printing plate precursor comprising a support and a coating comprising: a photopolymerizable layer comprising a polymerizable compound, an initiator, and a pH sensitive colorant precursor, and a protective overcoat layer provided on the photopolymerizable layer, the protective overcoat layer comprising a heat sensitive color forming IR dye, the heat-sensitive color-forming IR dye forms a printed image upon exposure to heat and / or light, which remains stable or increases during storage of the precursor in a bright or dark environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a novel lithographic printing plate precursor. Background Art

[0002] Lithographic printing generally involves the use of a so-called printing master, such as a printing plate mounted on a rotary printing press cylinder. The master carries a lithographic image on its surface, and the print is obtained by applying ink to the image and then transferring the ink from the master to a receiving material (which is generally paper). In conventional lithographic printing, ink and an aqueous fountain solution (also called a dampening solution) are supplied to a lithographic image consisting of oleophilic (or hydrophobic, i.e., ink-accepting, water-repelling) areas and hydrophilic (or oleophobic, i.e., water-accepting, ink-repelling) areas. In so-called waterless offset lithography, the lithographic image consists of ink-accepting and ink-resistant (ink-repelling) areas, and during waterless offset lithography, only ink is supplied to the master.

[0003] Lithographic printing masters are usually obtained by image-wise exposure and processing of a radiation-sensitive layer on a lithographic support. Imaging and processing make the so-called lithographic printing plate precursor a printing plate or master. Generally, the radiation-sensitive coating is image-wise exposed to heat or light-triggered (physico)chemical processes such as ablation, polymerization, insolubilization by crosslinking of polymers or by agglomeration of particles of thermoplastic polymer latex, by destroying intermolecular interactions or by increasing the permeability of the development barrier layer. Although some printing plate precursors are able to produce a lithographic image immediately after exposure, the most popular lithographic printing plate precursors require wet processing because exposure causes a solubility difference or dissolution rate difference in the developer between the exposed and non-exposed areas of the coating. In positive-working lithographic printing plate precursors, the exposed areas of the coating dissolve in the developer and the non-exposed areas remain resistant to the developer. In negative-working lithographic printing plate precursors, the non-exposed areas of the coating dissolve in the developer while the exposed areas remain resistant to the developer. Most lithographic printing plate precursors contain a hydrophobic coating on a hydrophilic support, so that the areas that remain resistant to the developer define the ink-receptive areas of the plate, and thus the printing areas, while in the non-printing areas the hydrophilic support is revealed by dissolution of the coating in the developer.

[0004] Photopolymer printing plates rely on a working mechanism whereby the coating - which generally comprises a free-radically polymerizable compound - hardens upon exposure. "Hardening" means that the coating becomes insoluble or non-dispersible in a developer, and may be achieved by polymerization and / or crosslinking of the photosensitive coating upon exposure to light. Photopolymer printing plate precursors may be sensitive to blue, green or red light (i.e., wavelengths in the range of 450nm-750nm), to violet light (i.e., wavelengths in the range of 350nm-450nm), or to infrared light (i.e., wavelengths in the range of 750nm-1500nm). Optionally, the exposure step is followed by a heating step to enhance or accelerate the polymerization and / or crosslinking reaction.

[0005] Typically, a top layer or protective overcoat on the imageable layer is required to act as an oxygen barrier in order to provide the desired sensitivity to the plate. The protective overcoat generally comprises a water-soluble or water-swellable polymer, such as polyvinyl alcohol. In addition to acting as an oxygen barrier, the protective overcoat should preferably be easily removable during processing and sufficiently transparent to actinic radiation (e.g., 300-450 nm, or 450-750 nm, or 750-1500 nm).

[0006] The classical workflow of a photopolymer printing plate first involves an exposure step of the photopolymer printing plate precursor in a violet or infrared plate-making machine, followed by an optional preheating step, a washing step of the protective outer coating, an alkaline development step, and a rinsing and gumming step. In the past few years, there has been a significant move towards simplifying the workflow, wherein the preheating step and / or the washing step are eliminated, and wherein the processing and gumming steps are carried out in a single step, or wherein processing is carried out with a neutral gum and then gumming in a second step. Alternatively, on-machine processing has become very popular, wherein the printing plate is mounted on a printing press, and the coating is developed by interaction with fountain solution and ink supplied to the printing plate during the operation of the printing press. During the first operation of the printing press, the non-image area is removed from the carrier, and thereby the non-printing area of ​​the printing plate is defined.

[0007] In order to be able to assess the image quality of a lithographic printing plate before it is mounted on a printing press, such as image resolution and detail rendering (usually measured with an optical densitometer), lithographic printing plate precursors often contain a colorant, such as a dye or pigment, in a coating. After processing, this colorant provides a contrast between the image area containing the colorant and the hydrophilic support from which the coating has been removed, which enables the end user to assess the image quality and / or determine whether the precursor has been exposed to light. Furthermore, in addition to allowing an assessment of the image quality, a high contrast between the image and the hydrophilic support is required in order to obtain a good image registration (alignment) of different printing plates in multicolor printing in order to ensure image sharpness (resolution) and correct rendering of the colors in the rendered image.

[0008] However, it is not possible to inspect and authenticate a printing plate including colorants before processing the exposed printing plate. A solution has been provided in the art, for example by including components into the coating which, when exposed, form a so-called "printed image", i.e. an image visible before processing.

[0009] Coloring agents that provide contrast obtained by so-called leuco dyes that change color when pH, temperature, UV etc. change have been widely used in the art.Leuco dye technology relates to the change between two chemical forms, one of which is substantially colorless. If the color change is caused by, for example, pH or temperature, it is converted into reversible. Irreversible changes are based on redox reactions. For example, in US 7,402,374, US 7,425,406 and US 7,462,440, the coloring agents that provide contrast obtained by becoming colored leuco dyes in the presence of a thermal acid generator are described.

[0010] Thermochromic dye technology involves designing IR dyes containing thermally cleavable groups to obtain a color shift when exposed to heat and / or light. This technology provides enhanced lithographic contrast by increasing the concentration of thermochromic dyes or the exposure energy. The thermosensitive lithographic printing plate precursor disclosed in EP 925 916 includes an IR dye that converts IR radiation into heat and changes color when IR irradiated. In these prior art materials, the IR dyes also show lateral absorption in the visible wavelength range in addition to strong absorption in the IR wavelength range.

[0011] One problem associated with prior art materials is that the printed image obtained after exposure is often characterized by a relatively low contrast between exposed and non-exposed areas, and that this contrast often fades away over time when the exposed printing plate is not immediately used for a printing job. In other words, the contrast obtained often decreases during processing and / or storage. It is therefore difficult or even impossible to measure the dot gain before processing and / or printing in order to adjust the press settings based on the obtained dot size.

[0012] In summary, there remains a need for photopolymer printing plate coating formulations that provide stable contrast between image and non-image areas not only after processing steps, but also before processing steps, and that are designed for both direct on-press and off-press development. Summary of the invention

[0013] It is therefore an object of the present invention to provide a printing plate based on photopolymerization which is characterized by a high image contrast between image and non-image areas (support) of the printing plate after processing and at the same time by an excellent print-out image when imaging before processing, which remains stable or even intensifies during handling and / or storage.

[0014] This object is achieved by a printing plate precursor as defined in claim 1, preferred embodiments of which are defined in the dependent claims. A particular feature of the invention is that the printing plate precursor comprises a coating comprising a pH-sensitive colorant precursor in a photopolymerizable layer and a thermosensitive color-forming IR dye in a protective overcoat layer. The thermosensitive color-forming IR dye is capable of inducing a CIE 1976 color difference ΔE1 of 2.0 or more (preferably 3 or more, more preferably 4 or more, most preferably 5 or more) upon IR radiation and / or heating, and the pH-sensitive colorant precursor is capable of forming a CIE 1976 color difference ΔE2 of 12.0 or more, more preferably 15.0 or more, most preferably 18 or more when treated with a liquid having a pH of about 4 or less.

[0015] The color difference ΔE1 between the exposed (image) area and the non-exposed (non-image) area of ​​the coating and the color difference ΔE2 between the image area and the support are calculated from their L*a*b* values. Even at low energy densities, for example, between 70-190 mJ / m 2 More preferably, between 75-150 mJ / m 2 Between 80-120 mJ / m 2 When the coatings of the present invention are exposed to light, a printed image characterized by a CIE 1976 color difference ΔE1 of 2 or greater is also formed.

[0016] The CIE 1976 color coordinates L*, a* and b* discussed herein are part of the well-known CIE (Commission Internationale de l'Eclairage e) system of tristimulus color coordinates, which also includes the color coordinate system defined as C* = [(a) 2 +(b) 2 ] 1 / 2 The CIE 1976 color system is described, for example, in "Colorimetry, CIE 116-1995: Industrial Colour Difference Evaluation" or "Measuring Colour", RWG Hunt, 2nd edition, edited in 1992 by Ellis Horwood Limited, England.

[0017] The CIE L*a*b* values ​​discussed and reported herein were measured according to ASTM E308-85 method.

[0018] Surprisingly, it has been found that the printed image formed upon heat and / or light exposure of the coating (comprising a specific combination of a pH-sensitive colorant precursor and a thermosensitive color-forming IR dye) remains stable or even enhanced after storage, i.e. when the printing plate is not immediately used for processing and / or printing. Storage of the printing plate includes, for example, storing the printing plate under light, such as office light conditions, or storing the printing plate in a dark environment; for example, storing for, for example, 8 hours or more after the heat and / or light exposure step, up to one day after the heat and / or light exposure step, and even up to several days, such as 2, 3, 4 or 5 days, or one week to several weeks (several two weeks) after the heat and / or light exposure step.

[0019] Therefore, in order to ensure image sharpness (resolution) and correct rendering of colors in the presented image, it is convenient to measure the printing plate linearization on the printing plate precursor of the present invention after imaging and off-press processing rather than on the printing paper, which is not only time consuming but also disadvantageous in terms of ink, paper and printing chemical consumption.

[0020] Other features, elements, steps, characteristics and advantages of the present invention will become more apparent from the following detailed description of preferred embodiments of the present invention. Specific embodiments of the present invention are also defined in the dependent claims. DETAILED DESCRIPTION

[0021] Lithographic printing plate precursors

[0022] The lithographic printing plate precursor according to the invention is negative-working, i.e. after exposure and development, the non-exposed areas of the coating are removed from the support and define hydrophilic (non-printing or non-image) areas, while the exposed coating is not removed from the support and defines oleophilic (printing or image) areas. The hydrophilic areas are defined by a support having a hydrophilic surface or provided with a hydrophilic layer. The hydrophobic areas are defined by the coating, which hardens upon exposure, optionally followed by a heating step. Areas with hydrophilic properties mean areas with a higher affinity for aqueous solutions than for oleophilic inks; areas with hydrophobic properties mean areas with a higher affinity for oleophilic inks than for aqueous solutions.

[0023] "Hardening" means that the coating becomes insoluble or non-dispersible in the developer and can be achieved by polymerization and / or crosslinking of the photosensitive coating during an exposure step, optionally followed by a heating step to enhance or accelerate the polymerization and / or crosslinking reaction. In this optional heating step, hereinafter also referred to as "preheating", the printing plate precursor is preferably heated at a temperature of about 80° C. to 150° C. and preferably during a residence time of about 5 seconds to 1 minute.

[0024] The coating comprises a top layer - also referred to herein as a protective overcoat - and at least one layer comprising a photopolymerizable composition, also referred to as a "photopolymerizable layer". The coating thickness of the photopolymerizable layer is preferably in the range of 0.2 to 5.0 g / m 2 In the range of 0.4-3.0 g / m 2 Between, most preferably between 0.6-2.2g / m 2 between.

[0025] A protective overcoat layer is provided on top of the photopolymerizable layer.The coating may further comprise other layers, such as intermediate layers between the support and the photopolymerizable layer and / or between the top layer and the photopolymerizable layer, adhesion improving layers and / or other layers.

[0026] The lithographic printing plate precursors of the present invention are characterized by strong color development of the image area after processing with a developer having a pH of about 4 or below 4. In addition, the lithographic printing plate precursors provide a sharp printout image immediately after the exposure step, which remains substantially stable during handling and / or storage. The printout image is visible due to the contrast of the image, which is defined as the difference between the optical density of the exposed area and the non-exposed area.

[0027] The contrast between image (exposed) areas and non-image (non-exposed) areas is preferably as high as possible and enables the end user to distinguish between different color selections and to check image quality defects on the printing plate precursor such as scratches, pinholes, wear marks, and to control dot gain by measuring and subsequently adjusting the press settings based on the obtained dot size.

[0028] The printing plate of the invention is characterized in that it can be exposed at low energy densities, i.e. below 190 mJ / m 2 ; preferably at 70mJ / m 2 -150 mJ / m 2 More preferably, between 75mJ / m 2 -120mJ / m 2 and most preferably a maximum of 80 mJ / m 2 .

[0029] definition

[0030] The term hydrocarbyl in this context refers to an optionally substituted aliphatic or aromatic hydrocarbyl. An optionally substituted aliphatic hydrocarbyl preferably refers to an alkyl, cycloalkyl, alkenyl, cycloalkenyl or alkynyl group; suitable groups thereof are described below. An optionally substituted aromatic hydrocarbyl preferably refers to a hetero(aryl) group; suitable hetero(aryl) groups - i.e. suitable aryl or heteroaryl groups - are described below.

[0031] The term "alkyl" means in this context all possible variations for each number of carbon atoms in the alkyl group, i.e. methyl, ethyl, for 3 carbon atoms: n-propyl and isopropyl; for 4 carbon atoms: n-butyl, isobutyl and tert-butyl; for 5 carbon atoms: n-pentyl, 1,1-dimethyl-propyl, 2,2-dimethylpropyl and 2-methyl-butyl, etc. Examples of suitable alkyl groups are methyl, ethyl, n-propyl, isopropyl, n-butyl, 1-isobutyl, 2-isobutyl and tert-butyl, n-pentyl, n-hexyl, chloromethyl, trichloromethyl, isopropyl, isobutyl, isopentyl, neopentyl, 1-methylbutyl and isohexyl, 1,1-dimethyl-propyl, 2,2-dimethylpropyl and 2-methyl-butyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl and methylcyclohexyl. Preferably, the alkyl group is C 1 -C 6 -alkyl.

[0032] Suitable alkenyl groups are preferably C 2 -C 6 -alkenyl, such as ethenyl, n-propenyl, n-butenyl, n-pentenyl, n-hexenyl, isopropenyl, isobutenyl, isopentenyl, neopentenyl, 1-methylbutenyl, isohexenyl, cyclopentenyl, cyclohexenyl and methylcyclohexenyl.

[0033] Suitable alkynyl groups are preferably C 2 -C 6 -alkynyl; Suitable aralkyl groups are preferably those comprising one, two, three or more C 1 -C 6 - phenyl or naphthyl alkyl;

[0034] Suitable alkaryl groups are preferably C 2- or C 3-containing aryl groups (preferably phenyl or naphthyl). 1 -C 6 -alkyl.

[0035] The cyclic group or cyclic structure includes at least one ring structure and may be a monocyclic or polycyclic group, and a polycyclic group means one or more rings fused together.

[0036] Examples of suitable aryl groups can be represented by, for example, optionally substituted phenyl, benzyl, tolyl or o-, m- or p-xylyl, optionally substituted naphthyl, anthracenyl, phenanthryl and / or combinations thereof. Heteroaryl is preferably a monocyclic or polycyclic aromatic ring comprising carbon atoms and one or more heteroatoms in the ring structure, preferably 1-4 heteroatoms independently selected from nitrogen, oxygen, selenium and sulfur. Preferred examples thereof include optionally substituted furyl, pyridyl, pyrimidyl, pyrazolyl, imidazolyl, oxazolyl, isoxazolyl, thienyl, tetrazolyl, thiazolyl, (1,2,3) triazolyl, (1,2,4) triazolyl, thiadiazolyl, thiofenyl and / or combinations thereof.

[0037] Examples of aralkyl groups preferably include one, two, three or more C 1 -C 6 -alkyl, phenyl or naphthyl.

[0038] Examples of the alkaryl group are preferably C aryl including phenyl or naphthyl. 7 -C 20 -alkyl.

[0039] Halogen is selected from fluorine, chlorine, bromine or iodine.

[0040] Suitable polyalkylene oxide groups preferably contain a plurality of alkylene oxide repeating units of the formula -CnH2n-O-, wherein n is preferably an integer in the range of 2-5. Preferred alkylene oxide repeating units are generally ethylene oxide, propylene oxide or a mixture thereof. Partial -CnH2n- may include straight or branched chains, and may also be substituted. The number of repeating units in the polyalkylene oxide group is preferably in the range of 2-10 units, more preferably between 2-5 units, and preferably less than 100, more preferably less than 60.

[0041] The term "substituted" in, for example, a substituted alkyl group means that the alkyl group may be substituted with atoms other than the atoms normally present in such groups (i.e., carbon and hydrogen). For example, a substituted alkyl group may include a halogen atom or a thiol group. An unsubstituted alkyl group contains only carbon and hydrogen atoms.

[0042] The optional substituents are preferably selected from hydroxy, -F, -Cl, -Br, -I, -OH, -SH, -CN, -NO 2 , alkyl (such as methyl or ethyl), alkoxy (such as methoxy or ethoxy), aryloxy, carboxylic acid or its alkyl ester, sulfonic acid or its alkyl ester, phosphonic acid or its alkyl ester, phosphate or ester (such as alkyl ester, such as methyl or ethyl ester), thioalkyl, thioaryl, thioheteroaryl, -SH, thioether (such as thioalkyl or thioaryl), ketone, aldehyde, sulfoxide, sulfone, sulfonate, sulfonamide, amino, vinyl, alkenyl, alkynyl, cycloalkyl, alkaryl, aralkyl, aryl, heteroaryl or heteroalicyclic group and / or combinations thereof.

[0043] The term printed image refers to the image that becomes visible after imaging but before processing.

[0044] Top layer or protective outer covering

[0045] The coating includes a top layer or protective overcoat, which preferably acts as an oxygen barrier. Low molecular weight species present in air may degrade or even inhibit image formation, and therefore a protective overcoat is applied to the coating. The protective overcoat should preferably be easily removable during development, adhere well to the photopolymerizable layer or optional other layers of the coating, and should preferably not inhibit light transmission during exposure. A protective overcoat is provided on top of the photopolymerizable layer.

[0046] The protective overcoat comprises a thermosensitive color-forming IR dye - i.e. an infrared absorbing compound capable of forming a colored compound, whereby a printout image is formed when exposed to infrared light and / or heat. The thermosensitive color-forming IR dye is preferably a thermochromic infrared absorbing dye, also referred to herein as a thermochromic IR dye. The thermochromic IR dye preferably has a major absorption in the infrared wavelength range of the electromagnetic spectrum - i.e. a wavelength range between about 750nm-1500nm - and preferably has no substantial light absorption in the visible wavelength range of the electromagnetic spectrum - i.e. a wavelength range between 390nm-700nm. The thermosensitive color-forming IR dye preferably comprises at least one thermally cleavable group, which is converted into a group that is a stronger electron donor by a chemical reaction induced by exposure to IR radiation or heat. Therefore, the exposed thermochromic IR dye preferably absorbs substantially more light in the visible wavelength range of the electromagnetic spectrum, or in other words, the thermochromic dye preferably undergoes a blue shift, whereby a visible image is formed, also referred to as a printout image. The formation of such a printout image is significantly different from a process in which a compound changes from a substantially colorless compound to a light-colored to colored compound. These compounds generally change absorption from the UV wavelength range of the electromagnetic spectrum to the visible wavelength range of the electromagnetic spectrum, ie these compounds generally have a bathochromic shift.Compared with the above-described color forming methods of thermosensitive color-forming IR dyes, the contrast of the printed image obtained by this method is much weaker.

[0047] The contrast of the printed image can be defined as the difference between the optical density of the exposed areas and the optical density of the unexposed areas, and is preferably as high as possible.

[0048] The concentration of the thermochromic IR dye may be 0.1% wt - 20.0% wt, more preferably 0.5% wt - 15.0% wt, most preferably 1.0% wt - 10.0% wt, relative to the total dry weight of the coating.

[0049] The thermosensitive color-forming IR dye is preferably represented by the following formula I, II or III:

[0050]

[0051] in

[0052] Ar 1 ,Ar 2 and Ar3 independently represent an optionally substituted aromatic hydrocarbon group or an aromatic hydrocarbon group having an optionally substituted cyclic benzene ring;

[0053] W 1 and W 2 independently represents a sulfur atom, an oxygen atom, NR¨, wherein R¨ represents an optionally substituted alkyl group, NH or -CM 10 M 11 Group, where M 10 and M 11 is independently an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group, or wherein M 10 and M 11 Together contain the necessary atoms to form a cyclic structure, preferably a 5- or 6-membered ring;

[0054] W 3 represents a sulfur atom or -C(A 3 )=C(A 4 )-group,

[0055] W 4 represents a sulfur atom or -C(A 7 )=C(A 8 )-group,

[0056] M 1 and M 2 M independently represents hydrogen, an optionally substituted aliphatic hydrocarbon group or the necessary atoms together to form an optionally substituted cyclic structure, preferably 1 and M 2 Together they comprise the necessary atoms to form an optionally substituted cyclic structure, which may comprise an optionally substituted cyclic benzene ring, which is preferably a 5- or 6-membered ring, more preferably a 5-membered ring, most preferably a 5-membered ring having a cyclic structure of 5 carbon atoms;

[0057] M 3 and M 4 independently represent an optionally substituted aliphatic hydrocarbon group;

[0058] M 5 、M 6 、M 7 and M 8 、M 16 and M 17 independently represent hydrogen, halogen or an optionally substituted aliphatic hydrocarbon group,

[0059] A 1 -A 8 independently represent hydrogen, a halogen atom, an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group, or wherein A 1 and A2 , A 3 and A 4 , A 5 and A 6 or A 7 and A 8 Each of which together contain the necessary atoms to form a cyclic structure, preferably a 5- or 6-membered ring;

[0060] M 12 and M 13 and M 14 and M 15 independently represents an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group, or wherein said M 14 、M 15 , A 5 or A 7 Two of the M together contain the necessary atoms to form at least one cyclic structure, preferably a 5- or 6-membered ring; the M 12 、M 13 , A 2 or A 4 Two of the together contain the necessary atoms to form at least one cyclic structure, preferably a 5- or 6-membered ring;

[0061] M 9 is converted into the M 9 A group that is a stronger electron donor; and said conversion provides an increase in the integrated light absorption of said dye between 350-700 nm;

[0062] and optionally one or more counterions to obtain a neutrally charged compound.

[0063] Thermochromic IR dyes can be neutral, anionic or cationic dyes, depending on the type of substituents and the number of each substituent. In a preferred embodiment, the dye of formula I, II or III contains at least one anionic or acidic group, such as -CO 2 H, -CONHSO 2 R h 、-SO 2 NHCOR i 、-SO 2 NHSO 2 R j ,-PO 3 H 2 ,-OPO 3 H 2 、-OSO 3 H, -S-SO 3 H or -SO 3 H group or its corresponding salt, wherein Rh , R i and R j is independently aryl or alkyl, preferably methyl, and wherein the salt is preferably an alkali metal salt or an ammonium salt, including a mono- or di- or tri- or tetra-alkylammonium salt. These anions or acid groups may be present in Ar 1 ,Ar 2 or Ar 3 On an aromatic hydrocarbon group or cyclic benzene ring, or on M 3 、M 4 or M 12 -M 15 On the aliphatic hydrocarbon group, or on M 12 -M 15 The other substituents may be selected from halogen atoms, cyano groups, sulfone groups, carbonyl groups or carboxylate groups.

[0064] In another preferred embodiment, M 3 、M 4 or M 12 -M 15 At least one of the following is substituted at the terminal end by at least one of these groups, more preferably by -CO 2 H, -CONHSO 2 -Me, -SO 2 NHCO-Me, -SO 2 NHSO 2 -Me, -PO 3 H 2 or -SO 3 H group or its corresponding salt, wherein Me represents a methyl group.

[0065] In a preferred embodiment, the thermosensitive color-forming IR dye is represented by the above formula I, II or III, including M represented by one of the following groups: 9 :

[0066] -(N=CR 17 )a-NR 5 -CO-R 4 ,

[0067] -(N=CR 17 )b-NR 5 -SO 2 -R 6 ,

[0068] -(N=CR 17 )c-NR 11 -SO-R 12 ,

[0069] -SO 2 -NR 15R 16 and

[0070] -S-CH 2 -CR 7 (H) 1-d (R 8 ) d -NR 9 -COOR 18 ,

[0071] in

[0072] a, b, c and d are independently 0 or 1;

[0073] R 17 represents hydrogen, an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group, or wherein R 17 and R 5 or R 17 and R 11 together contain the necessary atoms to form a ring structure;

[0074] R 4 Indicates -OR 10 、-NR 13 R 14 or -CF 3 ;

[0075] Where R 10 represents an optionally substituted (hetero)aryl group or an optionally branched aliphatic hydrocarbon group;

[0076] R 13 and R 14 independently represent hydrogen, an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group, or wherein R 13 and R 14 together contain the necessary atoms to form a ring structure;

[0077] R 6 represents an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group, -OR 10 、-NR 13 R 14 or -CF 3 ;

[0078] R 5 represents hydrogen, an optionally substituted aliphatic hydrocarbon group, SO 3- Group, -COOR 18 or an optionally substituted (hetero)aryl group, or wherein R 5 With R 10 , R 13 and R 14 At least one of them together contain the necessary atoms to form a ring structure;

[0079] R 11 , R 15 and R 16 independently represent hydrogen, an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group, or wherein R 15 and R 16 together contain the necessary atoms to form a ring structure;

[0080] R 12 represents an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group;

[0081] R 7 and R 9 independently represent hydrogen or an optionally substituted aliphatic hydrocarbon group;

[0082] R 8 Indicates -COO- or -COOR 8’ , where R 8’ represents hydrogen, an alkali metal cation, an ammonium ion or a mono-, di-, tri- or tetra-alkylammonium ion;

[0083] R 18 represents an optionally substituted (hetero)aryl group or an α-branched aliphatic hydrocarbon group.

[0084] Suitable examples of thermosensitive colour-forming IR dyes for use in the present invention are described in EP 1 910 082, pages 4-8, IRD-001 to IRD-101.

[0085] In a highly preferred embodiment, the thermosensitive color-forming IR dye is represented by the following formula IV

[0086]

[0087] Among them, Ar 1 ,Ar 2 , W 1 , W 2 and M 1 -M 9 As defined above.

[0088] Most preferably, the thermosensitive color-forming IR dye is represented by Formula IV, wherein

[0089] Ar 1 and Ar 2 independently represents an optionally substituted aryl group; optionally forming a ring with an optionally substituted benzene ring,

[0090] W 1 and W 2 Indicates -C(CH 3 ) 2 ;

[0091] M 1 and M 2 together contain the necessary atoms to form an optionally substituted 5-membered ring which may comprise an optionally substituted cyclic benzene ring;

[0092] M 3 and M 4 independently represent an optionally substituted aliphatic hydrocarbon group,

[0093] M 5 、M 6 、M 7 and M 8 represents hydrogen;

[0094] M 9 express

[0095] -NR 5 -CO-R 4

[0096] -NR 5 -SO 2 -R 6

[0097] -NR 11 -SO-R 12

[0098] -SO 2 -NR 15 R 16

[0099] Where R 4 , R 5 , R 6 , R 11 , R 12 , R 15 and R 16 As defined above;

[0100] and optionally one or more counterions to obtain a neutral compound. Preferably the IR dye contains at least one anionic group or an acid group, such as -CO 2 H, -CONHSO 2 R h 、-SO 2 NHCOR i 、-SO 2 NHSO 2 R j ,-PO 3 H 2 ,-OPO 3 H 2 、-OSO 3 H, -SO 3H or -S-SO 3 H group or its corresponding salt, wherein R h , R i and R j is independently aryl or alkyl. More preferably, M 3 or M 4 At least one of the aliphatic hydrocarbon groups is substituted at a terminal with at least one of the anionic groups or acid groups.

[0101] In a highly preferred embodiment, the thermosensitive color-forming IR dye is represented by Formula IV, wherein

[0102] Ar 1 and Ar 2 independently represent optionally substituted aryl;

[0103] W 1 and W 2 Indicates -C(CH 3 ) 2 ;

[0104] M 1 and M 2 together contain the necessary atoms to form an optionally substituted 5-membered ring, the optionally substituted 5-membered ring may contain an optionally substituted cyclic benzene ring;

[0105] M 3 and M 4 independently represent an optionally substituted aliphatic hydrocarbon group,

[0106] M 5 、M 6 、M 7 and M 8 represents hydrogen;

[0107] M 9 express

[0108] -NR 5 -CO-R 4

[0109] -NR 5 -SO 2 -R 6

[0110] in

[0111] R 4 For-OR 10 , where R 10 is an optionally branched aliphatic hydrocarbon group;

[0112] R 5 represents hydrogen, an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group,

[0113] R 6 represents an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group; and

[0114] Optionally one or more counterions are present to obtain a neutrally charged compound.

[0115] Preferably, the IR dye contains at least one anionic group or acid group, such as -CO 2 H, -CONHSO 2 R h 、-SO 2 NHCOR i 、-SO 2 NHSO 2 R j ,-PO 3 H 2 ,-OPO 3 H 2 、-OSO 3 H, -SO 3 H or -S-SO 3 H group or its corresponding salt, wherein R h , R i and R j is independently aryl or alkyl. More preferably, M 3 or M 4 At least one of the aliphatic hydrocarbon groups is substituted at the terminal by at least one of the anionic groups or acid groups. The salt is preferably an alkali metal salt or an ammonium salt, including a mono- or di- or tri- or tetra-alkylammonium salt.

[0116] Optional counterions to obtain electrically neutral compounds may be selected, for example, from halogens, sulfonates, perfluorosulfonates, toluenesulfonates, tetrafluoroborate, hexafluorophosphate, arylborates, arylsulfonates; or cations such as alkali metal salts or ammonium salts, including mono- or di- or tri- or tetra-alkylammonium salts.

[0117] Particularly preferred thermosensitive color-forming IR dyes are represented by one of the following formulas V-XII:

[0118]

[0119] in

[0120] R represents hydrogen or optionally substituted alkyl, such as optionally substituted methyl, ethyl, propyl or butyl;

[0121] X - represents a halogen, a sulfonate, a perfluorosulfonate, a toluenesulfonate, a tetrafluoroborate, a hexafluorophosphate, an arylborate or an arylsulfonate; and

[0122] R 3 , R3’ independently represents an optionally substituted alkyl group, preferably methyl or ethyl; or an ether group, preferably -CH 2 -CH 2 -O-CH 3 ;

[0123]

[0124] in

[0125] M + =Li + 、Na + , K + NH 4 + 、R'R”R”'NH + , wherein R', R", R'" independently represent hydrogen, optionally substituted alkyl or aryl;

[0126]

[0127] The above-mentioned thermochromic IR dyes can also be coupled to each other or to other IR dyes to form IR dye dimers or oligomers. In addition to the covalent coupling between two or more thermochromic IR dyes, supramolecular complexes comprising two or more thermochromic IR dyes can also be formed by ionic interactions. For example, a dimer consisting of two different IR dyes can be formed by the interaction between cationic and anionic IR dyes, as described in, for example, WO / 2004069938 and EP 1 466728. IR dyes can also be ionically bonded to polymers, as described, for example, in EP 1582346, in which IR dyes containing 2-4 sulfonate groups are ionically bonded to polymers containing covalently attached ammonium, phosphonium and sulfonium groups.

[0128] Supramolecular complexes comprising two or more thermochromic IR dyes can also be formed through hydrogen bonding or dipole-dipole interactions.

[0129] The protective outer cover may further include a binder. A preferred binder that can be used for the protective outer cover is polyvinyl alcohol. The polyvinyl alcohol preferably has a degree of hydrolysis in the range of 74 mol% to 99 mol%, more preferably in the range of 80-98%. The weight average molecular weight of the polyvinyl alcohol can be measured by the viscosity of a 4% by weight aqueous solution at 20°C, as defined in DIN 53015, and the viscosity value is preferably in the range of 2-26, more preferably in the range of 2-15, and most preferably in the range of 2-10.

[0130] The protective outer coating may comprise a halogenated polymer, which is preferably a hydrophobic polymer, i.e., insoluble or non-swellable in water at about neutral pH. The binder may be used in the protective outer coating in the form of a dispersion; i.e., an emulsion or a suspension. The amount of halogenated binder in the protective outer coating may be between 30 wt% and 96 wt%, more preferably between 40 wt% and 90 wt%, and most preferably between 50 wt% and 85 wt%. The halogenated binder preferably comprises between 60 wt% and 95 wt% of monomer units derived from a vinylidene monomer, such as vinylidene fluoride, vinylidene chloride, vinylidene bromide and / or vinylidene iodide.

[0131] The protective outer coating may optionally include other ingredients, such as inorganic or organic acids, matting agents, surfactants such as anionic surfactants, for example sodium alkyl sulfates or sodium alkyl sulfonates; amphoteric surfactants, for example alkylaminocarboxylates and alkylaminodicarboxylates; nonionic surfactants, for example polyoxyethylene alkylphenyl ethers, (co)polymers containing siloxane and / or perfluoroalkyl units and / or oligo(alkylene oxide) units; fillers; (organic) waxes; alkoxylated alkylenediamines, as disclosed, for example, in EP 1 085 380 (paragraphs

[0021] and

[0022] ); glycerol; inorganic particles; pigments or wetting agents, as disclosed in EP 2 916 171.

[0132] The coating thickness of the protective outer layer is 0.10-1.75g / m 2 Between, preferably between 0.20-1.30g / m 2 More preferably, between 0.25-1.0 g / m 2 Between and most preferably between 0.30-0.80 g / m 2 In a more preferred embodiment of the present invention, the coating thickness of the protective outer coating is between 0.25 and 1.75 g / m 2 and comprising polyvinyl alcohol having a degree of hydrolysis in the range of 74 mol% to 99 mol% and a viscosity value in the range of 3 to 26 as defined above.

[0133] Hydrophilic polymers in the protective overcoat may lead to a problematic viscosity increase of printing press chemicals such as fountain solution and / or developer solution.Thus, the thickness of the protective overcoat should preferably not be too high; for example above the ranges given above.

[0134] Colorant Precursors

[0135] The photopolymerizable layer of the lithographic printing plate precursor comprises one or more colorant precursors. Colorant precursors are compounds that can change from substantially colorless or light-colored to colored when the pH changes. The pH change required for this color change is preferably obtained upon exposure and can be enhanced by applying a liquid having a pH of about 4 or below to the coating, preferably in an off-press development step.

[0136] The reaction process can be represented as follows:

[0137] Leuco dye + acid → colored dye

[0138] Preferred leuco dyes that form color upon treatment with a liquid having a pH of about 4 or less and / or are preferably used in combination with an acid generator include phthalide-type and benzopyrrolidone-type leuco dyes, such as triarylmethanephthalide, diarylmethanephthalide, monoarylmethanephthalide, heterocyclic-substituted phthalide, alkenyl-substituted phthalide, bridged phthalide (e.g., spirofluorenephthalide and spirobenzoanthraphthalide), and bisphthalide; fluoran leuco dyes, such as fluorescein, rhodamine, and p-aminophenol.

[0139] Particularly preferred colorant precursors are leuco dyes such as heterocyclic substituted phthalides, alkenyl substituted phthalides, bridged phthalides (eg spirofluorenephthalide and spirobenzoanthraphthalide) and bisphthalide; and fluoran leuco dyes such as fluorescein, rhodamine and rhodol.

[0140] The most preferred leuco dyes are the fluoran leuco dyes, such as fluorescein, rhodamine and rhodol.

[0141] More information on leuco dyes can be found, for example, in Chemistry and Applications of Leuco Dyes, Ramaiah Muthyala, Plenum Press, 1997.

[0142] The leuco dye is preferably 0.01-0.1 g / m 2 The amount is preferably 0.02-0.08 g / m 2 The amount is preferably 0.025-0.05 g / m 2 An amount of is present in the protective outer covering.

[0143] The liquid having a pH of about 4 or below is preferably a gum solution and is described in more detail below.

[0144] The photopolymerizable layer preferably comprises an acid generator. All known light and thermal acid generators can be used. They can optionally be combined with photosensitive dyes. Light and thermal acid generators are widely used, for example, in conventional photoresist materials. More information can be obtained, for example, in "Encyclopaedia of polymer science", 4th edition, Wiley or "Industrial Photoinitiators, A Technical Guide", CRC Press 2010.

[0145] Preferred classes of photo- and thermal-acid generators are iodonium salts, sulfonium salts, ferrocenium salts, sulfonyl oximes, halomethyl triazines, halomethyl aryl sulfones, α-haloacetophenones, sulfonates, tert-butyl esters, allyl-substituted phenols, tert-butyl carbonates, sulfates, phosphates, and phosphonates.

[0146] Polymerizable compounds

[0147] The photopolymerizable layer of the lithographic printing plate precursor further comprises a polymerizable compound, such as a polymerizable monomer or oligomer comprising at least one terminal olefinic group, hereinafter also referred to as a “free radical polymerizable monomer.” Polymerization comprises linking the free radical polymerizable monomers together.

[0148] Suitable free-radically polymerizable monomers are disclosed in EP 2 916 171 at

[0042] and

[0050] .

[0149] Initiator

[0150] The photopolymerizable layer of the lithographic printing plate precursor further comprises one or more photoinitiators. According to the present invention, any free radical initiator capable of generating free radicals when directly exposed or in the presence of a sensitizer is a suitable initiator, also referred to herein as a photoinitiator. Suitable examples of photoinitiators include onium salts, compounds containing carbon-halogen bonds (such as [1,3,5] triazines with trihalomethyl groups), organic peroxides, aromatic ketones, thio compounds, azo polymerization initiators, azide compounds, ketoxime esters, hexaaryl diimidazoles, metallocenes, active ester compounds, boric acid esters and quinone diazides. Among them, iodonium and / or sulfonium salts are particularly preferred in view of storage stability.

[0151] More specific suitable free radical initiators include, for example, derivatives of acetophenone (such as 2,2-dimethoxy-2-phenylacetophenone and 2-methyl-1-[4-(methylthio)phenyl-2-morpholinopropan-1-one); benzophenone; benzil; ketocoumarin (such as 3-benzoyl-7-methoxycoumarin and 7-methoxycoumarin); xanthone; thioxanthone; benzoin or alkyl-substituted anthraquinone; onium salts (such as diaryliodonium hexafluoroantimonate, diaryliodonium trifluoromethanesulfonate, hexafluoroantimonate (4-(2-hydroxytetradecyloxy) hexafluorophosphate, triarylsulfonium p-toluenesulfonate, (3-phenylpropan-2-onyl)triarylphosphonium hexafluoroantimonate, and N-ethoxy(2-methyl)pyridinium hexafluorophosphate, as well as onium salts described in U.S. Pat. Nos. 5,955,238, 6,037,098, and 5,629,354); borates (such as tetrabutylammonium triphenyl(n-butyl)borate, tetraethylammonium triphenyl(n-butyl)borate, diphenyliodonium tetraphenylborate, diphenyliodonium tetraphenylborate (wherein the iodonium salt substituted with a group comprising at least six carbon atoms), diphenyliodonium tetraphenylborate (wherein one of the iodonium salt phenyl groups is substituted with a branched alkyl group comprising at least three carbon atoms) and triphenylsulfonium triphenyl(n-butyl)borate, and borates as described in U.S. Pat. Nos. 6,232,038 and 6,218,076); haloalkyl-substituted s-triazines (such as 2,4-bis(trichloromethyl)-6-(p-methoxy-phenylvinyl)-s-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxy-naphthalene- 1-yl)-s-triazine, 2,4-bis(trichloromethyl)-6-piperonyl-s-triazine and 2,4-bis(trichloromethyl)-6-[(4-ethoxy-vinyloxy)-phenyl-1-yl]-s-triazine and s-triazines as described in U.S. Pat. Nos. 5,955,238, 6,037,098, 6,010,824 and 5,629,354); and titanocene (bis(etha.9-2,4-cyclopentadien-1-yl)bis[2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium). Onium salts, borates and s-triazines are preferred free radical initiators. Diaryliodonium salts and triarylsulfonium salts are preferred onium salts. Triarylalkylborates are preferred borates. Trichloromethyl-substituted s-triazines are preferred s-triazines. These initiators may have an optional substituent and may be used alone or in combination.

[0152] Optionally substituted trihaloalkyl sulfones are particularly preferred initiators, wherein halogen independently represents fluorine, bromine, chlorine or iodine and sulfone is a compound containing a sulfonyl functional group attached to two carbon atoms. Tribromomethylphenyl sulfone is the most preferred initiator. More details about this initiator can be found in paragraphs

[0029] to

[0040] of WO2019 / 179995.

[0153] The amount of photoinitiator is generally in the range of 0.05-30% by weight, preferably 0.1-15% by weight, most preferably 0.2-10% by weight, relative to the total dry weight of the components in the photopolymerizable composition.

[0154] Very high sensitivity can be achieved by using a fluorescent brightener as a combination of sensitizer and polymerization initiator.

[0155] The photopolymerizable layer may also include a coinitiator. Typically, a coinitiator is used in combination with a free radical initiator. Suitable coinitiators for photopolymer coatings are disclosed in US 6,410,205, US 5,049,479, EP 1079 276, EP 1369 232, EP 1 369 231, EP 1 341 040, US 2003 / 0124460, EP 1 241 002, EP 1 288 720 and in reference books including the following cited references: Chemistry & Technology UV & EB formulation for coatings, inks & paints - Volume 3 - Photoinitiators for Free Radical and Cationic Polymerisation, edited by KK Dietliker–PKT Oldring - 1991 - ISBN 0 947798161. Specific coinitiators may be present in the photopolymerizable layer to further increase the sensitivity, as described in EP 107 792. Preferred coinitiators are disclosed in EP 2 916 171

[0051] .

[0156] Very high sensitivity can be obtained by including a sensitizer (such as a fluorescent whitening agent) in the coating. Suitable examples of fluorescent whitening agents as sensitizers are described in WO 2005 / 109103, page 24, line 20 to page 39. Useful sensitizers can be selected from the sensitizing dyes disclosed in US 6,410,205, US 5,049,479, EP 1 079 276, EP 1 369 232, EP 1 369 231, EP 1 341 040, US 2003 / 0124460, EP 1 241 002 and EP 1 288 720.

[0157] As described in EP 107 792, specific coinitiators may be present in the photopolymerizable layer to further increase the sensitivity. Preferred coinitiators are sulfur compounds, especially mercaptans, such as 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, 2-mercaptobenzimidazole, 4-methyl-3-propyl-1,2,4-triazol-5-thione, 4-methyl-3-n-heptyl-1,2,4-triazol-5-thione, 4-phenyl-3-n-heptyl-1,2,4-triazol-5-thione, 4-phenyl-3,5-dimercapto .... , 2,4-triazole, 4-n-decyl-3,5-dimercapto-1,2,4-triazole, 5-phenyl-2-mercapto-1,3,4-oxadiazole, 5-methylthio-1,3,4-thiadiazoline-2-thione, 5-hexylthio-1,3,4-thiadiazoline-2-thione, mercaptophenyltetrazolyl, pentaerythritol mercaptopropionate, butyric acid-3-mercaptoneopentane tetrayl ester, pentaerythritol tetrakis (thioglycolate). Other preferred coinitiators are polythiols as disclosed in WO 2006 / 048443 and WO2006 / 048445. These polythiols can be used in combination with the above-mentioned thiols (e.g., 2-mercaptobenzothiazole).

[0158] The photopolymerizable layer may optionally include an infrared light absorbing dye as a sensitizer, absorbing light between 750nm-1300nm, preferably between 780nm-1200nm, more preferably between 800nm-1100nm. Particularly preferred sensitizers are the heptamethine cyanine dyes disclosed in paragraphs

[0030] to

[0032] of EP 1 359 008.

[0159] Other ingredients

[0160] The photopolymerizable layer preferably includes a binder. The binder can be selected from a wide range of organic polymers. Compositions of different binders can also be used. Useful binders are described in WO2005 / 111727, page 17, line 21 to page 19, line 30, paragraph

[0013] of EP 1 043 627, and WO2005 / 029187, page 16, line 26 to page 18, line 11. Granular polymers are also suitable, including homopolymers or copolymers prepared from monomers such as ethylene, styrene, vinyl chloride, methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, acrylonitrile, vinyl carbazole, acrylates or methacrylates or mixtures thereof.

[0161] Thermo-reactive polymer particles may be included in the coating, the thermo-reactive polymer particles including thermo-reactive groups such as ethylenically unsaturated groups, cationically polymerizable groups, isocyanate groups, epoxy groups, vinyloxy groups, and functional groups having active hydrogen atoms, carboxyl groups, hydroxyl groups, amino groups, or acid anhydrides.

[0162] The average particle size of the polymer granules is preferably 0.01 mm to 3.0 mm. Particulate polymers in the form of microcapsules, microgels or reactive microgels are suitable, as disclosed in EP 1 132 200, EP 1 724 112, US 2004 / 106060.

[0163] The photopolymerizable layer may also contain particles which increase the resistance of the coating to manual or mechanical damage. The particles may be inorganic particles, organic particles or fillers, such as described in, for example, US 7,108,956. More details of suitable spacer particles are described in

[0053] to

[0056] of EP 2 916 171.

[0164] The photopolymerizable layer may also contain inhibitors. Specific inhibitors for photopolymer coatings are disclosed in US Pat. No. 6,410,205, EP 1 288 720 and EP 1 749 240.

[0165] The photopolymerizable layer may further comprise an adhesion promoting compound. The adhesion promoting compound is a compound that can interact with the carrier, preferably having an olefinic unsaturated bond that can be addition polymerized and a compound that can interact with the carrier's functional group. Under "interaction" it is understood to be a physical and / or chemical reaction or process of each type, whereby a bond is formed between the functional group and the carrier, which can be a covalent bond, an ionic bond, a complex bond, a coordination bond or a hydrogen bond, and can be formed by an adsorption process, a chemical reaction, an acid-base reaction, a complex formation reaction or a chelating group or a ligand reaction. The adhesion promoting compound described in EP 2 916 171

[0058] is a suitable example.

[0166] Various surfactants may be added to the photopolymerizable layer to allow or enhance the developability of the precursor; especially development with a gum solution. Both polymeric and small molecule surfactants (e.g. nonionic surfactants) are preferred. Further details are described in EP 2 916 171

[0059] .

[0167] Carrier

[0168] The lithographic printing plate used in the present invention comprises a support having a hydrophilic surface or provided with a hydrophilic layer. The support is preferably a grained and anodized aluminum support well known in the art. Suitable supports are disclosed, for example, in EP 1 843 203 (paragraphs

[0066] to

[0075] ). The surface roughness obtained after the graining step is often expressed as the arithmetic mean center line roughness Ra (ISO 4287 / 1 or DIN 4762) and can vary between 0.05-1.5 μm. The aluminum support of the present invention preferably has an Ra value of less than 0.45 μm, more preferably less than 0.40 μm and most preferably less than 0.30 μm. The lower limit of the Ra value is preferably about 0.1 μm. More details about the preferred Ra values ​​of the grained and anodized aluminum support surface are described in EP 1 356 926. By anodizing the aluminum support, Al 2 O 3 layer and anode weight (g / m formed on the aluminum surface 2 Al 2 O 3 ) in 1-8g / m 2 The anode weight is preferably ≥ 3 g / m 2 , more preferably ≥3.5g / m 2 and most preferably ≥4.0 g / m 2 .

[0169] The granulated and anodized aluminum support may be subjected to a so-called post-anodization treatment, for example treatment with polyvinylphosphonic acid or a derivative thereof, treatment with polyacrylic acid, treatment with potassium fluorozirconate or potassium phosphate, treatment with an alkali metal silicate or a combination thereof. Alternatively, the support may be treated with an adhesion promoting compound, such as those described in

[0010] of EP 1 788 434 and WO 2013 / 182328. However, for precursors optimized for use without a preheating step, it is preferred to use a granulated and anodized aluminum support without any post-anodization treatment.

[0170] Besides aluminium supports, it is also possible to use plastic supports, for example polyester supports, which are provided with one or more hydrophilic layers, as disclosed, for example, in EP 1 025 992 .

[0171] A lithographic printing plate precursor may be prepared by (i) applying a coating as described above on a support and (ii) drying the precursor.

[0172] Exposure Steps

[0173] The printing plate precursor is preferably image-wise exposed by a laser emitting IR light. Preferably, the image-wise exposing step is performed off-machine in a plate-making machine, i.e. an exposure device suitable for image-wise exposing the precursor with a laser, such as a laser diode emitting about 830 nm or a Nd YAG laser emitting about 1060 nm, or by conventional exposure in contact with a mask. In a preferred embodiment of the invention, the precursor is image-wise exposed by a laser emitting IR light.

[0174] Preheating Steps

[0175] After the exposure step, the precursor may be preheated in a preheating unit, preferably at a temperature of about 80° C. to 150° C. and preferably during a residence time of about 5 seconds to 1 minute. The preheating unit may comprise a heating element, preferably an IR lamp, a UV lamp, heated air or a heated roller. Such a preheating step may be used for a printing plate precursor comprising a photopolymerizable composition to enhance or accelerate the polymerization and / or crosslinking reaction.

[0176] Development Steps

[0177] Following the exposure step or the preheating step (when present), the printing plate precursor may be processed (developed). Before developing the imaged precursor, a pre-rinsing step may be performed, in particular for negative-working lithographic printing precursors having a protective oxygen barrier or topcoat. This pre-rinsing step may be performed in a separate device or by manually rinsing the imaged precursor with water, or the pre-rinsing step may be performed in a washing unit integrated in a processor for developing the imaged precursor. The washing liquid is preferably water, more preferably tap water. More details about the washing step are described in

[0026] of EP 1 788 434.

[0178] During the development step, the non-exposed areas of the image-recording layer are at least partially removed without substantially removing the exposed areas. The processing liquid (also called developer) can be applied to the printing plate by hand or in an automated processing device, for example by rubbing with an impregnated pad, by dipping, immersing, coating, spin coating, spraying, pouring. The treatment with the processing liquid can be combined with mechanical rubbing (for example by a rotating brush). During the development step, any water-soluble protective layer present is preferably also removed. The development is preferably carried out in an automated processing unit at a temperature between 20-40° C.

[0179] In a highly preferred embodiment, the processing steps described above are replaced by machining, whereby the imaged precursor is mounted on a printing press and machined by rotating the plate cylinder while feeding fountain solution and / or ink to the coating of the precursor to remove unexposed areas from the support. In a preferred embodiment, only fountain solution is supplied to the printing plate during start-up of the printing press. After a number of rotations of the plate cylinder, preferably less than 50 and most preferably less than 5 rotations, the ink supply is also switched on. In an alternative embodiment, the supply of fountain solution and ink may be started simultaneously, or only ink may be supplied during a number of rotations before the fountain solution supply is switched on.

[0180] The processing steps can also be performed by combining the above-described embodiments, for example combining development with a processing fluid with on-press development by applying ink and / or fountain solution.

[0181] Processing fluid

[0182] Most preferably, the processing liquid is a gum solution, whereby the non-exposed areas of the photopolymerizable layer are removed from the support during the development step. At the same time, the printing plate is gummed, i.e. in a single step. Development with a gum solution has the additional benefit that, due to the residual gum in the non-exposed areas on the printing plate, an additional gumming step can be omitted to protect the support surface in the non-printing areas. Thus, the precursor is processed and gummed in a single step, which involves a less complex development device than a development device comprising a developer tank, a rinsing section and a gumming section. The gumming section may comprise at least one gumming unit or may comprise two or more gumming units. These gumming units may have the configuration of a cascade system, i.e. when a gum replenisher is added to the second gumming unit or when the gum solution in the second gumming unit is used only once, i.e. when the precursor is developed in the second gumming unit using only the starting gum solution by preferably a spray or jet technique, the gum solution used for the second gumming unit and present in the second tank overflows from the second tank to the first tank. More details about this gum development are described in EP1 788 444. The gum solution is generally an aqueous liquid comprising one or more surface protective compounds which are capable of protecting the lithographic image of the printing plate from contamination, for example by oxidation, fingerprints, fat, oil or dust, or damage, for example by scratches during handling of the printing plate. Suitable examples of such surface protective compounds are film-forming hydrophilic polymers or surfactants. The layer remaining on the printing plate after treatment with the gum solution preferably comprises 0.005-20 g / m 2 More preferably, between 0.010-10 g / m 2 Between, most preferably between 0.020-5g / m 2. More details on the surface protective compounds in the gum solution can be found in WO 2007 / 057348, page 9, line 3 to page 11, line 6. Since the developed printing plate precursor is developed and gummed in one step, no post-treatment of the processed printing plate is required. However, after the gumming step, a finishing gum can be applied.

[0183] The glue solution preferably has a pH between 1.5-10, more preferably between 2-9 and most preferably between 2.5-7. Suitable glue solutions are described in, for example,

[0008] to

[0022] of EP 1342568 and in WO2005 / 111727. In the present invention, the pH of the glue solution is preferably about 4 or lower than 4, more preferably 3 or lower than 3 and most preferably 2 or lower than 2. The glue solution may further comprise an inorganic salt, an anionic surfactant, a wetting agent, a chelate compound, a preservative compound, a defoaming compound and / or an ink receptor and / or a combination thereof. More details about these additional ingredients are described in WO 2007 / 057348 page 11, line 22 to page 14, line 19.

[0184] The processing fluid may be an alkaline developer or a solvent-based developer. Suitable alkaline developers have been described in US2005 / 0162505. Alkaline developers are aqueous solutions having a pH of at least 11, more generally at least 12, preferably 12-14. Alkaline developers generally contain an alkaline agent to obtain a high pH value, which may be an inorganic or organic alkaline agent. The developer may contain anionic, nonionic and amphoteric surfactants (up to 3% based on the total composition weight); biocides (antimicrobial and / or antifungal agents), defoamers or chelating agents (such as alkaline gluconates) and thickeners (water-soluble or water-dispersible polyols, such as glycerol or polyethylene glycol).

[0185] If the processing liquid is an alkaline solution and / or the pH is greater than 4, it is necessary to additionally treat the processed printing plate with a liquid having a pH of about 4 or below 4. The liquid may contain, for example, at least one non-polymeric acid or a polyfunctional acid and / or a salt thereof, such as a compound comprising carboxylic acid and / or carboxylate groups. The polyfunctional compound is preferably an aliphatic or aromatic organic polyfunctional compound. In the context of the present invention, non-polymeric means that the compound does not comprise more than two repeating units.

[0186] Drying and baking steps

[0187] After the processing step, the printing plate can be dried in a drying unit. In a preferred embodiment, the printing plate is dried by heating the printing plate in a drying unit which can contain at least one heating element selected from IR lamps, UV lamps, heated metal rollers or heated air.

[0188] After drying, the printing plate can optionally be heated in a baking unit. More details about heating in a baking unit can be found in WO 2007 / 057348, page 44, line 26 to page 45, line 20.

[0189] The printing plate thus obtained can be used for conventional so-called wet offset printing, in which ink and an aqueous fountain solution are supplied to the printing plate. Another suitable printing method uses a so-called single-fluid ink without a fountain solution. Suitable single-fluid inks have been described in US 4,045,232, US 4,981,517 and US 6,140,392. In a most preferred embodiment, as described in WO 00 / 32705, the single-fluid ink comprises an ink phase (also called a hydrophobic or oleophilic phase) and a polyol phase.

[0190] Example

[0191] Preparation of comparative printing plate precursors and printing plate precursors of the present invention.

[0192] Preparation of aluminum support S-01

[0193] A 0.3 mm thick aluminum foil was degreased by spraying with an aqueous solution containing 26 g / l NaOH at 65°C for 2 seconds and rinsing with demineralized water for 1.5 seconds. 2 At a current density of 15 g / l HCl, 15 g / l SO 4 2- ions and 5g / l Al 3+ The foil was electrochemically grained for 10 seconds using alternating current in an aqueous solution of ions. Afterwards, the foil was then decontaminated by etching with an aqueous solution containing 5.5 g / l NaOH at 36°C for 2 seconds and rinsed with demineralized water for 2 seconds. The foil was then heated at a temperature of 50°C and 17 A / dm 2 The sample was subjected to anodization in an aqueous solution containing 145 g / l sulfuric acid at a current density of 1.50 Å for 15 seconds, then washed with demineralized water for 11 seconds and dried at 120° C. for 5 seconds.

[0194] The carrier thus obtained is characterized by a surface roughness Ra of 0.35-0.4 μm (measured with interferometer NT1100) and an oxide weight of 3.0 g / m 2 .

[0195] Photopolymerizable layer

[0196] Printing plate precursors PPP-01 to PPP-05, inventive printing plates PPP-06 to PPP-17 were prepared by first coating the photosensitive composition as defined in Table 1 onto the above support S-01. The components were dissolved in a mixture of 35% by volume of MEK and 65% by volume of Dowanol PM (1-methoxy-2-propanol, commercially available from DOW CHEMICAL Company). The coating solution was applied at a wet coating thickness of 30 μm and then dried in a circulation oven at 120° C. for 1 minute.

[0197] Table 1: Composition of photosensitive layers PL-01 to PL-08

[0198]

[0199] (1) FST 510 is the reaction product of 1 mole of 2,2,4-trimethylhexamethylene diisocyanate and 2 moles of hydroxyethyl methacrylate, commercially available from AZ Electronics as an 82 wt.% solution in MEK;

[0200] (2) CN 104 is an epoxy acrylate oligomer commercially available from Arkema;

[0201] (3) Ini-01 is 4-hydroxyphenyl-tribromomethyl-sulfone; Ini-02 is bis(4-tert-butylphenyl)iodonium tetraphenylborate;

[0202] (4) IR-01 is an infrared absorbing dye represented by the following structure:

[0203]

[0204] (5) Black XV is 6-diethylamino-3-methyl-2-(2,4-dimethylphenylamino)fluoran and GN-169 is 3-[2,2-bis(1-ethyl-2-metghyl-1H-indol-3-yl)vinyl]-3-[4-(diethylamino)phenyl]phthalide, both color-forming compounds are commercially available from Mitsui Chemicals Europe GmbH. LBC-51 is 3-(4-dimethylamino)-3-(1-butyl-2-methyl-indol-3-yl)-6-dimethylaminophthalide as a color-forming compound, which is commercially available from Shangai Thermand Pressure sensitive Export and Import;

[0205] (6) Ruco coating EC4811 is a nonionic aliphatic polyether polyurethane commercially available from Rudolf GmbH;

[0206] (7) SLEC BL10 is poly(vinyl butyral-co-vinyl acetate-co-vinyl alcohol), commercially available from Sekisui Chemical Co., Ltd.;

[0207] (8) Tegoglide 410 is a polyether siloxane copolymer commercially available from Evonik Resource Efficiency GmbH;

[0208] (9) JPA 528 is polyethylene glycol monomethacrylate acid phosphate, commercially available from Johoku Chemical Co., Ltd.;

[0209] (10) Belclene 400 is a phosphine-based polycarboxylic acid commercially available from BWA Water Additives UK Ltd.;

[0210] (11) Aerosil 150 is a hydrophilic fumed silica commercially available from Evonik Resource Efficiency GmbH.

[0211] Protective outer covering

[0212] On top of the photosensitive layer, an aqueous solution (40 μm wet film) with the composition as defined in Table 2 was coated on the printing plate precursor and dried at 110° C. for 2 minutes.

[0213] Table 2: Composition of protective outer covering

[0214]

[0215] (1) Mowiol 4-88™ is a partially hydrolyzed polyvinyl alcohol commercially available from Kuraray;

[0216] (2) Mowiol 4-98™ and Mowiol 28-99 are fully hydrolyzed polyvinyl alcohols commercially available from Kuraray;

[0217] (3) Diofan A050 is a polyvinylidene chloride latex commercially available from Solvay;

[0218] (4) Acticide LA1206™ is a biocide commercially available from Thor;

[0219] (5) Lutensol A8™ is a surfactant commercially available from BASF.

[0220] (6) Luviskol K30™ is a polyvinylpyrrolidone homopolymer commercially available from BASF.

[0221] (7) IR-02 is an infrared absorbing dye having the following formula:

[0222]

[0223] Imaging

[0224] At 130mJ / cm 2 The obtained printing plate precursors PPP-01 to PPP-17 were imaged at 2400 dpi using a High Power Creo 40W TE38 Thermal Platesetter™ (200 lpi Agfa Balanced Screening (ABS)) commercially available from Kodak and equipped with an 830 nm IR laser diode at an energy density of 1.5 Å.

[0225] result

[0226] ΔE measurement

[0227] Laboratory measurements were made with a GretagMacBeth SpectroEye reflectance spectrophotometer with the following settings: D50 (illuminant), 2° (observer), no filter; commercially available from GretagMacBeth. The total color difference ΔE is a single value that takes into account the differences between the L, a* and b* values ​​for the image and non-image areas:

[0228]

[0229] The higher the total color difference ΔE, the better the contrast obtained. The color difference between exposed and non-exposed areas is defined herein as ΔE1, and the color difference between the image area and the support after processing is defined herein as ΔE2.

[0230] Stability of printed images

[0231] The stability of the printed images (obtained after the above exposure steps) of the printing plate precursors PPP-01 to PPP-17 was evaluated by determining the total color difference ΔE1 before and after exposing the printing plate precursors to ordinary white office light (800 lux) for 8 hours and after storing the printing plates under dark conditions for 40 hours. The obtained ΔE1 measurements are summarized in the following Tables 3, 4 and 5.

[0232] Table 3: ΔE1 results obtained for comparative printing plate precursors PPP-01 to PPP-05

[0233]

[0234] *ΔE1: color difference between exposed and non-exposed areas;

[0235] **: See above.

[0236] Table 4: ΔE1 results obtained for the inventive printing plate precursors PPP-06 to PPP-15

[0237]

[0238]

[0239] *ΔE1: color difference between exposed and non-exposed areas;

[0240] **: See above.

[0241] Table 5: ΔE1 results obtained for comparative printing plate precursors PPP-16 and PPP-17

[0242]

[0243] *ΔE1: color difference between exposed and non-exposed areas;

[0244] **: See above.

[0245] The results summarized in Tables 3-5 show that after 40 h in a dark environment (comparative printing plates PP-01, PP-03 and PP-05) and / or after 8 h exposure to office light (comparative printing plates PP-02 and PP-04), the ΔE1 of the comparative printing plates PP-01 to PP-05 decreased by 50% or more; and after 40 h in a dark environment, the ΔE1 of the inventive printing plates PP-06 to PP-015 decreased by only 25% or less;

[0246] Off-machine processing

[0247] After the exposure step, the printing plate precursors PPP-01 to PPP-17 were subjected to manual washing of the non-image areas with an acidic liquid. The acidic liquid used was RC795A, a storage gel commercially available from Agfa, with a pH of 1.6.

[0248] Subsequently, the total color difference ΔE2 between the image area and the support was determined and the results are summarized in Tables 6, 7 and 8 below.

[0249] Table 6: ΔE2 results obtained for comparative printing plates PP-01 to PP-05

[0250]

[0251]

[0252] *ΔE2: Color difference between the image area and the carrier after processing.

[0253] Table 7: ΔE2 results obtained for inventive printing plates PP-06 to PP-15

[0254]

[0255] *ΔE2: Color difference between the image area and the carrier after processing.

[0256] Table 8: ΔE2 results obtained for comparative printing plates PP-16 and PP-17

[0257]

[0258] *ΔE2: Color difference between the image area and the carrier after processing.

[0259] The results in Tables 6-8 show that for all printing plates PP-01 to PP-15, which include a pH-sensitive coupler in the photosensitive layer, the color difference ΔE2 between the image area and the support is at least 15. Comparative printing plates PP-16 and PP-17, which do not contain a pH-sensitive coupler in the photosensitive layer, have a ΔE2 value of only 5.

Claims

1. A negative-working lithographic printing plate precursor comprising a support and a coating comprising: a photopolymerizable layer comprising a polymerizable compound and a photoinitiator, and a protective overcoat provided on the photopolymerizable layer; Features The photopolymerizable layer includes a pH-sensitive colorant precursor capable of forming a CIE 1976 color difference ΔE2 of 12.0 or more when treated with a liquid having a pH of about 4 or less, and the protective overcoat includes a thermosensitive color-forming IR dye capable of inducing a CIE 1976 color difference ΔE1 of 2.0 or more when heated and / or IR irradiated.

2. A printing plate precursor according to claim 1, wherein the thermosensitive colour-forming IR dye comprises a thermally cleavable group which upon exposure to heat and / or IR radiation is converted into a group which is a more powerful electron donor.

3. A printing plate precursor according to claim 1 or 2, wherein the thermosensitive color-forming IR dye is an infrared absorbing dye, which has a main absorption in the infrared wavelength range of the electromagnetic spectrum before exposure to heat and / or IR radiation, and absorbs substantially more light in the visible wavelength range of the electromagnetic spectrum after exposure to heat and / or IR radiation.

4. The printing plate precursor according to claims 1-3, wherein the thermosensitive color-forming IR dye is represented by the following formula IV in Ar 1 and Ar 2 independently represent an optionally substituted aromatic hydrocarbon group or an aromatic hydrocarbon group having an optionally substituted cyclic benzene ring; W 1 and W 2 independently represents a sulfur atom, an oxygen atom, NR¨, wherein R¨ represents an optionally substituted alkyl group, NH or -CM 10 M 11 Group, where M 10 and M 11 is independently an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group, or wherein M 10 and M 11 Together contain the necessary atoms to form a cyclic structure, preferably a 5- or 6-membered ring; M 3 and M 4 independently represent an optionally substituted aliphatic hydrocarbon group; M 5 、M 6 、M 7 and M 8 independently represent hydrogen, halogen or an optionally substituted aliphatic hydrocarbon group, M 1 and M 2 together contain the necessary atoms to form an optionally substituted 5-membered ring which may comprise an optionally substituted cyclic benzene ring; M 9 Represents one of the following groups: -(N=CR 17 )a-NR 5 -CO-R 4 , -(N=CR 17 )b-NR 5 -SO2-R 6 , -(N=CR 17 )c-NR 11 -SO-R 12 , -SO2-NR 15 R 16 and -S-CH2-CR 7 (H) 1-d (R 8 ) d -NR 9 -COOR 18 , in a, b, c and d are independently 0 or 1; R 17 represents hydrogen, an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group, or wherein R 17 and R 5 or R 17 and R 11 together contain the necessary atoms to form a ring structure; R 4 Indicates -OR 10 、-NR 13 R 14 or -CF3; Where R 10 represents an optionally substituted (hetero)aryl group or an optionally branched aliphatic hydrocarbon group; R 13 and R 14 independently represent hydrogen, an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group, or wherein R 13 and R 14 together contain the necessary atoms to form a ring structure; R 6 represents an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group, -OR 10 、-NR 13 R 14 or -CF3; R 5 represents hydrogen, an optionally substituted aliphatic hydrocarbon group, SO3 - Group, -COOR 18 or an optionally substituted (hetero)aryl group, or wherein R 5With R 10 , R 13 and R 14 At least one of them together contain the necessary atoms to form a ring structure; R 11 , R 15 and R 16 independently represent hydrogen, an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group, or wherein R 15 and R 16 together contain the necessary atoms to form a ring structure; R 12 represents an optionally substituted aliphatic hydrocarbon group or an optionally substituted (hetero)aryl group; R 7 and R 9 independently represent hydrogen or an optionally substituted aliphatic hydrocarbon group; R 8 Indicates -COO- or -COOR 8’ , where R 8’ represents hydrogen, an alkali metal cation, an ammonium ion or a mono-, di-, tri- or tetra-alkylammonium ion.

5. A printing plate precursor according to any one of the preceding claims, wherein the pH sensitive colorant precursor is selected from phthalide-type and phthalidone-type leuco dyes, and fluoran leuco dyes.

6. A printing plate precursor according to any one of the preceding claims, wherein the photopolymerizable layer further comprises an acid generator.

7. A printing plate precursor according to any one of the preceding claims, wherein the photoinitiator is selected from optionally substituted trihaloalkyl sulfones or onium salts.

8. A method for preparing a negative working lithographic printing plate precursor comprising the following steps: - applying a coating as defined in claims 1 to 7 to a carrier, - Drying the precursor.

9. A method for preparing a negative-working lithographic printing plate, comprising the steps of: - image-wise exposing a lithographic printing plate precursor as defined in claims 1 to 7, - optionally subjecting the lithographic printing plate precursor to heating; - developing the exposed printing plate precursor with a liquid having a pH of about 4 or below, thereby removing the coating from the support in the non-image areas.

10. A method for preparing a negative-working lithographic printing plate, comprising the steps of: - image-wise exposing a lithographic printing plate as defined in claims 1 to 7; - optionally subjecting the lithographic printing plate precursor to heating; - developing the printing plate precursor by mounting the precursor on a plate cylinder of a lithographic printing press and rotating the plate cylinder while feeding dampening fluid and / or ink to the precursor, thereby removing the non-exposed areas of the coating from the support.

Citation Information

Patent Citations

  • A lithographic printing plate precursor

    CN111867839A

  • Lithographic printing plate precursor and color-forming composition

    CN112770910A

  • A lithographic printing plate precursor

    WO2021259648A1