Electrode material comprising iron-doped sodium, lithium, manganese and metal tunnel-type oxides, electrode comprising said electrode material and use thereof in electrochemistry
By developing electrochemically active materials for lithium to replace iron-doped sodium, manganese and metal tunnel oxides, combined with electronic conductive materials and other components, the problem of high cost of positive electrode materials in the prior art is solved, and high energy density and Low-cost electrochemical battery performance.
Patent Information
- Application Number
- CN202380031975.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-07
- Filing Date
- 2023-04-06
- Publication Date
- 2024-11-15
AI Technical Summary
The high production cost of the cathode materials of existing lithium-ion batteries and all-solid state batteries, especially the high price of cobalt, limits the market application of these batteries, especially in large-scale and high-energy-density energy storage systems, resulting in low-cost and high-cost The demand for new cathode materials with capacity and high voltage has increased.
Develop an electrochemically active material containing a tunnel oxide of lithium substituted iron-doped sodium, manganese and at least one metal element, with the specific chemical formula NaaLibFecMndMeO2, wherein a, b, c, d are in a specific numerical range , M is selected from the group consisting of metals such as manganese, titanium, vanadium, nickel, etc., and combined with electronic conductive materials, adhesives and additives, electrode materials are prepared for electrochemical batteries.
By replacing iron-doped sodium, manganese and metal tunnel-type oxides with lithium, the electrochemical performance of electrochemical cells is significantly improved, the average operating voltage and energy density is improved, the production cost is reduced, and lithium ions and all-solid state is met Market demand for batteries.
Smart Images

Figure CN118974962A_ABST
Abstract
Description
[0001] Related Applications
[0002] This application claims priority under applicable law to U.S. Provisional Patent Application No. 63 / 362,616, filed on April 7, 2022, the contents of which are incorporated herein by reference in their entirety for all purposes. Technical Field
[0003] The present application generally relates to the field of electrochemically active materials and their use in electrochemical applications. More particularly, the present application relates to electrode materials comprising tunnel oxides of sodium, magnesium and at least one metal partially substituted with lithium as electrochemically active materials, electrodes comprising them, methods for their manufacture and their use in electrochemical cells. Background Art
[0004] Currently, commercial cathode materials used in lithium-ion batteries (LIBs) and so-called all-solid-state batteries, such as LiCoO 2 、LiNi 0.33 Mn 0.33 Co 0.33 O 2 (NMC 111), LiNi 0.6 Mn 0.2 Co 0.2 O 2 (NMC 622) and LiNi 0.8 Mn 0.1 Co 0.1 O 2 One of the main disadvantages of (NMC 811) is their high production cost. The raw materials used in the manufacture of cathode materials are becoming increasingly important in the overall cost of a battery pack, which could pose a problem for the growth of the market share of LIBs and so-called all-solid-state batteries. For example, the weighted average price of cobalt could limit the future application of LIBs and all-solid-state batteries. Therefore, cathode materials with reduced cobalt content and cobalt-free cathode materials are of great interest, especially in large-scale and high-energy-density energy storage systems. For example, lithium iron phosphate (LiFePO 4 LFP (LFP) has attracted great attention due to its cost-effectiveness. However, the energy density of LFP battery packs has not been improved enough to meet the needs of the electric vehicle market.
[0005] Therefore, there remains a need to develop new electrode materials that do not include one or more disadvantages of conventional commercial cathode materials. For example, there is a need to develop new low-cost, high-capacity, high-voltage cathode materials for LIBs and so-called all-solid-state batteries. Summary of the invention
[0006] According to one aspect, the present technology relates to an electrochemically active material comprising a tunnel-type oxide of sodium, manganese and at least one metal element doped with lithium-substituted iron, the oxide having a formula of Na a Li b Fe c Mn d M e O 2 , wherein a is a number such that 0<a<0.22; b is a number such that 0.18<b<0.40 and such that a+b is 0.38<a+b<0.62; c is a number such that 0<c≤0.40; d is a number such that 0.44≤d<1; e is a number such that c+d+e=1; and M is selected from manganese (Mn), titanium (Ti), vanadium (V), nickel (Ni), cobalt (Co), chromium (Cr), molybdenum (Mo), zirconium (Zr), tin (Sn), ruthenium (Ru), other similar metals and a combination of at least two thereof.
[0007] According to one example, M is selected from manganese (Mn), titanium (Ti), vanadium (V), nickel (Ni), cobalt (Co), chromium (Cr), molybdenum (Mo), zirconium (Zr), ruthenium (Ru), other similar metals and a combination of at least two thereof. According to a related example, M is titanium (Ti).
[0008] According to another example, a is a number such that 0.01<a<0.22, or 0.02<a<0.22, or 0.03<a<0.22, or 0.04<a<0.22, or 0.05<a<0.22, or 0.06<a<0.22, or 0.07<a<0.22, or 0.08≤a≤0.21. According to a related example, a is a number such that 0.08≤a≤0.21.
[0009] According to another example, b is a number such that 0.19<b<0.40, or 0.20≤b<0.40, or 0.20≤b<0.39, or 0.20≤b≤0.38. According to a related example, b is a number such that 0.20≤b≤0.38.
[0010] According to another example, c is a number such that 0.05<c≤0.40, or 0.10<c≤0.40, or 0.15<c≤0.40, or 0.20<c≤0.40, or 0.25<c≤0.40, or 0.30≤c≤0.40. According to a related example, c is a number such that 0.30≤c≤0.40.
[0011] According to another example, d is a number such that 0.44≤d<1, or 0.44≤d<0.95, or 0.44≤d<0.90, or 0.44≤d<0.85, or 0.44≤d<0.80, or 0.44≤d<0.75, or 0.44≤d<0.70, or 0.44≤d<0.65, or 0.44≤d<0.60, or 0.44≤d≤0.55. According to a related example, d is a number such that 0.44≤d≤0.55.
[0012] According to another example, the lithium-substituted iron-doped tunnel oxide of sodium, manganese and at least one metal is selected from Na 0.10 Li 0.33 Fe 0.34 Mn 0.44 Ti 0.22 O 2 、Na 0.08 Li 0.38 Fe 0.30 Mn 0.55 Ti 0.15 O 2 、Na 0.20 Li 0.24 Fe 0.34 Mn 0.55 Ti 0.11 O 2 、Na 0.21 Li 0.20 Fe 0.40 Mn 0.50 Ti 0.10 O 2 、Na 0.10 Li 0.40 Fe 0.08 Mn 0.81 Ti 0.11 O 2 and Na 0.10 Li 0.40 Fe 0.11 Mn 0.78 Ti 0.11 O 2 .
[0013] According to another aspect, the present technology relates to an electrode material comprising an electrochemically active material as defined herein.
[0014] According to one embodiment, the electrode material further comprises an electronically conductive material. According to one example, the electronically conductive material is selected from carbon black, acetylene black, graphite, graphene, carbon fiber, carbon nanofiber, carbon nanotube, and a combination of at least two thereof. According to a related example, the electronically conductive material comprises carbon black. For example, the carbon black is Super P TM Carbon or KetjenTM Carbon. According to another related example, the electronically conductive material comprises carbon fiber. For example, the carbon fiber is vapor grown carbon fiber (VGCF).
[0015] According to another embodiment, the electrode material further comprises a binder. According to an example, the binder is selected from a polyether polymer binder, a fluorinated polymer and a water-soluble binder. According to a related example, the binder is a fluorinated polymer. For example, the fluorinated polymer is polyvinylidene fluoride (PVDF).
[0016] According to another embodiment, the electrode material further comprises an additive. According to one example, the additive is selected from ion conductors, inorganic particles, glass particles, ceramic particles, salts and other similar additives.
[0017] According to another aspect, the present technology relates to an electrode comprising an electrode material as defined herein on a current collector.
[0018] According to one embodiment, the electrode is a cathode.
[0019] According to another aspect, the present technology relates to an electrochemical cell comprising a negative electrode, a positive electrode, and an electrolyte, wherein the positive electrode is as defined herein.
[0020] According to one embodiment, the negative electrode comprises an alkali metal, an alloy containing an alkali metal, or a pre-lithiated electrochemically active material. According to one example, the negative electrode comprises metallic lithium or an alloy containing metallic lithium. According to a related example, the negative electrode comprises metallic lithium.
[0021] According to another embodiment, the electrolyte is a glass or ceramic electrolyte.
[0022] According to another embodiment, the electrolyte is a liquid electrolyte comprising a salt in a solvent.
[0023] According to another embodiment, the electrolyte is a gel electrolyte comprising a salt and optionally a solvating polymer in a solvent.
[0024] According to another embodiment, the electrolyte is a solid polymer electrolyte comprising a salt in a solvated polymer.
[0025] According to one embodiment, the salt is a lithium salt. For example, the lithium salt is selected from lithium hexafluorophosphate (LiPF 6 ), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), 2-trifluoromethyl-4,5-dicyanoimidazole lithium (LiTDI), 4,5-dicyano-1,2,3-triazole lithium (LiDCTA), lithium bis(pentafluoroethylsulfonyl)imide (LiBETI), lithium tetrafluoroborate (LiBF4 ), lithium bis(oxalate)borate (LiBOB), lithium nitrate (LiNO 3 ), lithium chloride (LiCl), lithium bromide (LiBr), lithium fluoride (LiF), lithium perchlorate (LiClO 4 ) lithium hexafluoroarsenate (LiAsF 6 ), lithium trifluoromethanesulfonate (LiSO 3 CF 3 )(LiTf), fluoroalkyl lithium phosphate Li[PF 3 (CF 2 CF 3 ) 3 ](LiFAP), lithium tetrakis(trifluoroacetoxy)borate Li[B(OCOCF 3 ) 4 ](LiTFAB), Lithium Bis(1,2-Benzenediol(2-)-O,O')borate[B(C 6 O 2 ) 2 ](LiBBB) and a combination of at least two thereof. According to a related embodiment, the lithium salt is lithium hexafluorophosphate (LiPF 6 ).
[0026] According to another aspect, the present technology relates to a battery comprising at least one electrochemical cell as defined herein.
[0027] According to one embodiment, the battery is selected from the group consisting of lithium batteries, lithium ion batteries, sodium batteries, sodium ion batteries, potassium batteries, potassium ion batteries, magnesium batteries and magnesium ion batteries. According to one example, the battery is a lithium battery or a lithium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 is the formula Na as described in Example 1(d) 0.08 Li 0.36 MnO 2 X-ray diffraction patterns of tunnel-type sodium, lithium and manganese oxide powders
[0029] Figure 2 is the formula Na as described in Example 1(d) 0.10 Li 0.33 Fe 0.34 Mn 0.44 Ti 0.22 O 2 X-ray diffraction patterns of tunnel-type sodium, lithium, iron, manganese and titanium oxide powders.
[0030] Figure 3 is the formula Na as described in Example 1(d) 0.08 Li0.38 Fe 0.30 Mn 0.55 Ti 0.15 O 2 X-ray diffraction patterns of tunnel-type sodium, lithium, iron, manganese and titanium oxide powders.
[0031] Figure 4 is the formula Na as described in Example 1(d) 0.20 Li 0.24 Fe 0.34 Mn 0.55 Ti 0.11 O 2 X-ray diffraction patterns of tunnel-type sodium, lithium, iron, manganese and titanium oxide powders.
[0032] Figure 5 is the formula Na as described in Example 1(d) 0.21 Li 0.20 Fe 0.40 Mn 0.50 Ti 0.10 O 2 X-ray diffraction patterns of tunnel-type sodium, lithium, iron, manganese and titanium oxide powders.
[0033] Figure 6 The charge and discharge curves obtained for Cell 1 as described in Example 2(b) are presented, and (1) is recorded from 2.0 V to 4.8 V vs. Li + / Li at a cycle rate of 0.1C; and (2) recorded at 2.0V to 4.6Vvs.Li + The curve between / Li shows the results of the second discharge and charge cycle.
[0034] Figure 7 The results obtained for Cell 2 as described in Example 2(b) and at 2.0 V to 4.6 V vs. Li + The charge and discharge curves recorded between 1.5 and 2.5A at a cycle rate of 0.1 C. Shown are the results of the second discharge and charge cycle.
[0035] Figure 8 The results obtained for Cell 3 as described in Example 2(b) and at 2.0 V to 4.6 V vs. Li + The charge and discharge curves recorded between 1.5 and 2.5A at a cycle rate of 0.1 C. Shown are the results of the second discharge and charge cycle.
[0036] Fig. 9 The results obtained for Cell 4 as described in Example 2(b) and at 2.0 V to 4.8 V vs. Li +Charge and discharge curves recorded between 1.5V and 1.5V at a cycling rate of 0.1 C. Shown are the results of the second (1) and fifth (2) charge / discharge cycles.
[0037] Fig.10 The results obtained for Cell 5 as described in Example 2(b) and at 2.5 V to 4.8 V vs. Li + Charge and discharge curves recorded between 1.5V and 1.5V at a cycle rate of 0.1C. Shown are the results of the second charge / discharge cycle.
[0038] Fig.11 The results obtained for Cell 6 as described in Example 2(b) are presented: (a) at 2.0 V to 4.8 V vs. Li + (a) charge and discharge curves recorded at a cycling rate of 0.1 C between Li / Li; and (b) a graph showing capacity vs. cycle number.
[0039] Fig.12 The results obtained for Cell 7 as described in Example 2(b) are presented: (a) at 2.0 V to 4.8 V vs. Li + (a) charge and discharge curves recorded at a cycling rate of 0.1 C between Li / Li; and (b) a graph showing capacity vs. cycle number. DETAILED DESCRIPTION
[0040] All technical and scientific terms and expressions used herein have the same definitions as commonly understood by one of ordinary skill in the art. Nevertheless, definitions of some terms and expressions used are provided below.
[0041] When the term "about" is used herein, it means approximately, around, or in the vicinity. For example, when the term "about" is used with respect to a value, it modifies the value to vary by 10% above and below the nominal value. This term can also take into account, for example, experimental error of the measuring device or rounding.
[0042] When a numerical interval is mentioned in this application, unless otherwise stated, the lower limit and upper limit of the interval are always included in the definition. When a numerical interval is mentioned in this application, all intermediate intervals and sub-intervals and individual values included in these numerical intervals are also included in the definition.
[0043] When the article "a" is used in this application to introduce an element, it does not mean "only one", but "one or more". Of course, when the specification indicates that a specific step, component, element or feature "may" or "can" be included, the specific step, component, element or feature does not need to be included in every embodiment.
[0044] The present technology generally relates to electrochemically active materials, methods of making them, and their use in electrochemical cells. More particularly, the present technology relates to an electrochemically active material comprising a tunnel oxide of sodium, manganese, and at least one metal element doped with lithium-substituted iron.
[0045] According to one example, the metal element of the tunnel oxide of sodium, manganese and at least one metal element doped with lithium substituted iron can be a transition metal, a post-transition metal, a metalloid, an alkali metal other than lithium or sodium, an alkaline earth metal, or a combination thereof when compatible. For example, the metal can be a transition metal or a post-transition metal selected from manganese (Mn), titanium (Ti), vanadium (V), nickel (Ni), cobalt (Co), chromium (Cr), molybdenum (Mo), zirconium (Zr), tin (Sn), ruthenium (Ru) and other similar metal elements, or a combination thereof when compatible.
[0046] According to another example, the electrochemically active material comprises a tunnel oxide of sodium, manganese and at least one metal element doped with lithium-substituted iron, the oxide having a formula of Na a Li b Fe c Mn d M e O 2 , wherein a is a number such that 0<a<0.22; b is a number such that 0.18<b<0.40 and such that a+b is 0.38<a+b<0.62; c is a number such that 0<c≤0.40; d is a number such that 0.44≤d<1; e is a number such that c+d+e=1; and M is selected from manganese (Mn), titanium (Ti), vanadium (V), nickel (Ni), cobalt (Co), chromium (Cr), molybdenum (Mo), zirconium (Zr), tin (Sn), ruthenium (Ru) and other similar metal elements, or their combinations when compatible.
[0047] It is to be understood that when the metal element (M) is manganese (Mn), the tunnel-type oxide of sodium, manganese and at least one metal element doped with lithium-substituted iron includes manganese having at least two different oxidation states.
[0048] According to some examples, the metal element (M) is a transition metal selected from manganese (Mn), titanium (Ti), vanadium (V), nickel (Ni), cobalt (Co), chromium (Cr), molybdenum (Mo), zirconium (Zr), ruthenium (Ru) and other similar transition metals, or a combination thereof when compatible. According to some related examples, the metal element is titanium (Ti).
[0049] According to some examples, a is a number such that 0.01 < a < 0.22, or 0.02 < a < 0.22, or 0.03 < a < 0.22, or 0.04 < a < 0.22, or 0.05 < a < 0.22, or 0.06 < a < 0.22, or 0.07 < a < 0.22, or 0.08 ≤ a ≤ 0.21. According to some related examples, a is a number such that 0.08 ≤ a ≤ 0.21.
[0050] According to some examples, b is such that a+b is 0.38<a+b<0.61, or 0.38<a+b<0.60, or 0.38<a+b<0.59, or 0.38<a+b<0.58, or 0.38<a+b<0.57, or 0.38<a+b<0.56, or 0.38<a+b<0.55, or 0.38<a+b<0.54, or 0.38<a+b<0.53, or 0.38<a+b<0.52, or 0.38<a+b<0.51, or 0.38<a+b<0.50, or 0.38<a+b<0.49, or 0.38<a+b<0.48, or 0.38<a+b<0.47, or 0.39<a+b<0.47, or 0.40<a+b<0.47. According to some related examples, b is a number such that a+b is 0.40<a+b<0.47. For example, b can be a number such that 0.19<b<0.40, or 0.20≤b<0.40, or 0.20≤b<0.39, or 0.20≤b≤0.38. According to some related examples, b is a number such that 0.20≤b≤0.38.
[0051] According to some examples, c is a number such that 0.05<c≤0.40, or 0.10<c≤0.40, or 0.15<c≤0.40, or 0.20<c≤0.40, or 0.25<c≤0.40, or 0.30≤c≤0.40. According to some related examples, c is a number such that 0.30≤c≤0.40.
[0052] According to some examples, d is a number such that 0.44≤d<1, or 0.44≤d<0.95, or 0.44≤d<0.90, or 0.44≤d<0.85, or 0.44≤d<0.80, or 0.44≤d<0.75, or 0.44≤d<0.70, or 0.44≤d<0.65, or 0.44≤d<0.60, or 0.44≤d≤0.55. According to some related examples, d is a number such that 0.44≤d≤0.55.
[0053] Non-limiting examples of tunnel oxides of sodium, manganese and at least one metal element doped with lithium-substituted iron include Na 0.10 Li 0.33 Fe 0.34Mn 0.44 Ti 0.22 O 2 、Na 0.08 Li 0.38 Fe 0.30 Mn 0.55 Ti 0.15 O 2 、Na 0.20 Li 0.24 Fe 0.34 Mn 0.55 Ti 0.11 O 2 、Na 0.21 Li 0.20 Fe 0.40 Mn 0.50 Ti 0.10 O 2 、Na 0.10 Li 0.40 Fe 0.08 Mn 0.81 Ti 0.11 O 2 and Na 0.10 Li 0.40 Fe 0.11 Mn 0.78 Ti 0.11 O 2 .
[0054] According to another example, the electrochemically active material may further include at least one doping element that may be included in a smaller amount, for example to adjust or optimize its electrochemical properties. For example, the electrochemically active material may be doped by partially replacing the metal element with at least one other element. For example, the electrochemically active material may be slightly doped with at least one doping element selected from transition metals (e.g., iron (Fe), cobalt (Co), nickel (Ni), manganese (Mn), titanium (Ti), chromium (Cr), copper (Cu), vanadium (V), zinc (Zn) and / or yttrium (Y)), post-transition metals (e.g., Al), alkaline earth metals (e.g., Mg) and / or metalloids (e.g., Sb).
[0055] According to another example, the electrochemically active material may be in the form of particles (eg, microparticles and / or nanoparticles), which may be freshly formed and may additionally include a coating material. The coating material may be an electronically conductive material, such as a carbon coating.
[0056] For example, partial replacement of sodium ions by lithium ions can significantly improve the electrochemical performance of an electrochemical cell containing the present electrochemically active material.
[0057] According to some examples, partial replacement of sodium ions by lithium ions in a tunnel oxide of sodium, manganese and at least one metal element doped with iron by lithium can significantly improve the electrochemical properties of the electrochemically active material. Without wishing to be bound by theory, partial replacement of sodium ions by lithium ions can stabilize the structure of the electrochemically active material based on the tunnel oxide of sodium, manganese and at least one metal element doped with iron, and thus significantly improve its electrochemical performance. For example, the electrochemical properties of the electrochemically active material can be adjusted by changing the degree of lithium substitution.
[0058] According to some examples, iron ion doped lithium-substituted sodium, manganese and at least one metal element tunnel oxide can also significantly improve the electrochemical properties of the electrochemically active material. For example, partial substitution of manganese by iron ions can significantly increase the average operating voltage of the electrochemically active material. For example, the electrochemical properties of the electrochemically active material can be adjusted by changing the iron substitution degree.
[0059] According to some examples, cation doping of transition metals or post-transition metals (such as those described above) to lithium-substituted iron-doped sodium, manganese, and at least one metal element tunnel oxides can also significantly improve the electrochemical properties of electrochemically active materials. For example, partial replacement of manganese by titanium can significantly improve the electrochemical properties of electrochemically active materials. For example, the electrochemical properties of electrochemically active materials can be adjusted by changing the composition of the transition metal or the post-transition metal in the lithium-substituted iron-doped sodium, manganese, and at least one metal element tunnel oxide.
[0060] The present technology also relates to a method of making an electrochemically active material as defined herein, the method comprising the steps of:
[0061] (i) preparing a tunnel-type oxide of sodium, manganese and at least one metal element doped with iron; and
[0062] (ii) partially replacing sodium ions of the iron-doped tunnel oxide of sodium, manganese and at least one metal element with lithium ions to obtain an electrochemically active material.
[0063] According to one example, the iron-doped tunnel oxide of sodium, manganese and at least one metal element prepared in step (i) has a formula of Na a Fe c Mn d M e O 2, wherein a is a number such that 0.38<a<0.62; c is a number such that 0<c≤0.40; d is a number such that 0.44≤d<1; e is a number such that c+d+e=1; and M is selected from manganese (Mn), titanium (Ti), vanadium (V), nickel (Ni), cobalt (Co), chromium (Cr), molybdenum (Mo), zirconium (Zr), tin (Sn), ruthenium (Ru) and other similar metals, or combinations thereof when compatible.
[0064] According to some examples, the metal element (M) is a transition metal selected from manganese (Mn), titanium (Ti), vanadium (V), nickel (Ni), cobalt (Co), chromium (Cr), molybdenum (Mo), zirconium (Zr), ruthenium (Ru) and other similar transition metals, or a combination thereof when compatible. According to some related examples, the metal element is titanium (Ti).
[0065] According to some examples, a is a number such that 0.38<a<0.62, or 0.38<a<0.60, or 0.38<a<0.58, or 0.38<a<0.56, or 0.38<a<0.54, or 0.38<a<0.52, or 0.38<a<0.50, or 0.38<a<0.48, or 0.38<a≤0.46, or 0.40<a≤0.46, or 0.41≤a≤0.46. According to some related examples, a is a number such that 0.41≤a≤0.46.
[0066] Non-limiting examples of iron-doped tunnel oxides of sodium, manganese, and at least one metal element include Na 0.44 Fe 0.34 Mn 0.44 Ti 0.22 O 2 、Na 0.43 Fe 0.34 Mn 0.44 Ti 0.22 O 2 、Na 0.44 Fe 0.30 Mn 0.55 Ti 0.15 O 2 、Na 0.46 Fe 0.30 Mn 0.55 Ti 0.15 O 2 、Na 0.44 Fe 0.34 Mn 0.55 Ti 0.11 O 2 、Na 0.44 Fe 0.40 Mn 0.50 Ti 0.10 O2 、Na 0.41 Fe 0.40 Mn 0.50 Ti 0.10 O 2 、Na 0.50 Fe 0.08 Mn 0.81 Ti 0.11 O 2 and Na 0.50 Fe 0.11 Mn 0.78 Ti 0.11 O 2 .
[0067] According to an example, the tunnel oxide of iron doped sodium, manganese and at least one metal element can be prepared by a solid state synthesis technique or by a wet synthesis technique. For example, the wet synthesis technique can be a sol-gel method.
[0068] According to some examples, iron-doped tunnel oxides of sodium, manganese and at least one metal element can be prepared by a solid-state synthesis method. The solid-state synthesis method may involve mixing and grinding appropriate precursors (metal oxides or metal carbonates) in selected amounts to obtain iron-doped tunnel oxides of sodium, manganese and at least one metal element with a desired stoichiometry. The mixing and grinding steps may be performed sequentially, simultaneously or partially overlapping each other in time.
[0069] According to some examples, the mixing and grinding steps are carried out simultaneously. All compatible mixing and grinding methods are designed. For example, the solid precursor can be mixed and ground manually or by any compatible mechanical method (such as mechanical grinding). The solid-state synthesis method can also include heating the mixed and ground precursor to obtain the desired iron-doped sodium, manganese and tunnel-type oxides of at least one metal element. The heating step can be carried out at a temperature and duration sufficient to obtain a powder of iron-doped sodium, manganese and tunnel-type oxides of at least one metal element. The heating step can be carried out, for example, in a furnace at a temperature between about 800° C. and about 1000° C. (including limits). The heating step can be carried out for a time of, for example, about 3 hours to about 24 hours, including upper and lower limits. The heating step can be carried out under any suitable conditions to obtain the desired powder of iron-doped sodium, manganese and tunnel-type oxides of at least one metal element. For example, the heating step can be carried out under air or oxygen atmosphere, but any other compatible atmosphere is designed.
[0070] According to some examples, the tunnel oxide of sodium, manganese and at least one metal element doped with iron can be prepared by wet chemical synthesis, such as sol-gel method. The sol-gel method can be carried out in an aqueous medium using an inorganic salt precursor and a chelating agent. For example, the inorganic salt precursor can be a metal carbonate, acetate, oxalate or alkoxide precursor, and the chelating agent can be an organic acid such as citric acid. The sol-gel method can include dissolving an appropriate amount of an inorganic salt precursor in water and the molar ratio of (Na+Mn): chelating agent is about 10. For example, the dissolving step can be carried out under stirring. The solution thus obtained can then be heated to a temperature and duration sufficient to form a sol-gel precursor under stirring. For example, the solution can then be heated to a temperature of about 80°C until a sol-gel precursor is formed. The sol-gel precursor thus obtained can then be calcined at a temperature and duration sufficient to decompose organic and inorganic contents. For example, the sol-gel precursor can then be calcined in a furnace at a temperature of about 400°C for about 6 hours. The powder thus obtained can then be ground and calcined at a temperature and time sufficient to obtain the desired powder of iron-doped tunnel-type oxide of sodium, manganese and at least one metal element. For example, the calcination step can be carried out in a furnace at a temperature of about 900° C. for about 9 hours. The calcination step can be carried out under any suitable conditions to obtain the desired powder of iron-doped tunnel-type oxide of sodium, manganese and at least one metal element. For example, the calcination step can be carried out under an air or oxygen atmosphere, but any other compatible atmosphere is contemplated.
[0071] According to some examples, partial replacement of sodium ions by lithium ions may be performed by a one-step or two-step ion exchange process. The ion exchange reaction may be performed by mixing the powder of the tunnel oxide of sodium, manganese and at least one metal element doped with iron prepared in step (i) with an excess of a lithium salt or a lithium salt composition. The lithium salt composition may be lithium nitrate (LiNO 3 ) and lithium chloride (LiCl) or lithium hydroxide (LiOH), such as a mixture of LiNO in a molar ratio of about 2:1 3 :LiCl or LiOH mixture. For example, the powder prepared in step (i) can be mixed with a lithium salt or a lithium salt composition in a molar excess of up to 20 times. The mixture can then be heated at a temperature and duration sufficient to obtain an electrochemically active material, i.e., a tunnel oxide of sodium, manganese and at least one metal element doped with lithium replacing iron in the desired stoichiometric amount. For example, the mixture can be heated to a temperature between about 240°C and about 400°C, heated once for about 4 hours to about 15 hours, or heated twice for about 2 hours to about 10 hours.
[0072] The present technology also relates to an electrode material comprising an electrochemically active material as defined herein or an electrochemically active material prepared by a method as defined herein.
[0073] According to one example, the electrode material as defined herein may further include an electronically conductive material. Non-limiting examples of electronically conductive materials include carbon sources, such as carbon black (e.g., Ketjen TM Carbon and Super P TM Carbon), acetylene black (such as Shawinigan carbon and Denka TM Carbon black), graphite, graphene, carbon fiber (such as vapor grown carbon fiber (VGCF)), carbon nanofibers, carbon nanotubes (CNTs), and combinations of at least two thereof. According to a related variation, the electronically conductive material is selected from Ketjen TM Carbon, Super P TM Carbon, VGCF and a combination of at least two thereof. According to a related embodiment, the electronically conductive material is a mixture of VGCF and carbon black.
[0074] According to another example, the electrode material as defined herein may further include a binder. For example, the binder can be selected based on its compatibility with the various elements of the electrochemical cell. Any known compatible binder is considered. For example, the binder can be a polyether polymer binder, a fluorinated polymer and a water-soluble binder. According to an example, the binder is a fluorinated polymer, such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE). According to another example, the binder is a water-soluble binder, such as styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber (NBR), hydrogenated NBR (HNBR), epichlorohydrin rubber (CHR) or acrylate rubber (ACM), and optionally includes a thickener, such as carboxymethyl cellulose (CMC), or an acidic polymer, such as poly (acrylic acid) (PAA), poly (methyl methacrylate) (PMMA) or a combination thereof. According to another example, the binder is an optionally cross-linked polyether polymer binder. For example, the polyether polymer binder is linear, branched and / or crosslinked and is based on poly(ethylene oxide) (PEO), poly(propylene oxide) (PPO) or a combination of the two (e.g. as an EO / PO copolymer), and optionally includes crosslinkable units. According to a related variant, the binder is polyvinylidene fluoride (PVDF).
[0075] According to another example, the electrode material as defined herein may further optionally include at least one additional additive, such as an ion conductor, an inorganic particle, a glass or ceramic particle, a nanoceramic (e.g., alumina (Al 2 O 3 ), titanium dioxide (TiO 2 ), silicon dioxide (SiO 2) and other similar compounds), salts (e.g., lithium salts) and other similar additives. For example, the additional additive can be an ionic conductor selected from crystalline and / or amorphous forms of NASICON, LISICON, sulfo-LISICON, garnet, sulfide, sulfur halide, phosphate, thiophosphate, and a combination of at least two thereof.
[0076] According to another aspect, the present technology relates to an electrode comprising an electrode material as defined herein on a current collector (e.g., aluminum or copper foil). The electrode may also be a self-supporting electrode. According to a related example, the electrode is a positive electrode.
[0077] According to another aspect, the present technology is directed to an electrochemical cell comprising a negative electrode, a positive electrode, and an electrolyte, wherein the positive electrode is as defined herein.
[0078] According to one example, the negative electrode (counter electrode) includes an electrochemically active material selected from all known compatible electrochemically active materials. For example, the electrochemically active material of the negative electrode can be selected based on its electrochemical compatibility with the various elements of the electrochemical cell as defined herein. Non-limiting examples of electrochemically active negative electrode materials include alkali metals, alkali metal alloys, and pre-lithiated electrochemically active materials. According to a related example, the electrochemically active material of the negative electrode can be a metallic lithium film or an alloy including metallic lithium.
[0079] According to another example, the electrolyte can be selected based on its compatibility with the various elements of the electrochemical cell. Any type of compatible electrolyte is contemplated. For example, the electrolyte can be a liquid electrolyte containing a salt in a solvent. The electrolyte can also be a gel electrolyte containing a salt in a solvent and an optional solvating polymer. The electrolyte can also be a solid polymer electrolyte containing a salt in a solvating polymer. The electrolyte can also be a glass or ceramic electrolyte.
[0080] If present in the electrolyte, the salt may be an ionic salt, such as a lithium salt. Non-limiting examples of lithium salts include lithium hexafluorophosphate (LiPF 6 ), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), 2-trifluoromethyl-4,5-dicyanoimidazole lithium (LiTDI), 4,5-dicyano-1,2,3-triazole lithium (LiDCTA), lithium bis(pentafluoroethylsulfonyl)imide (LiBETI), lithium tetrafluoroborate (LiBF 4 ), lithium bis(oxalate)borate (LiBOB), lithium nitrate (LiNO 3 ), lithium chloride (LiCl), lithium bromide (LiBr), lithium fluoride (LiF), lithium perchlorate (LiClO 4 ) lithium hexafluoroarsenate (LiAsF 6 ), lithium trifluoromethanesulfonate (LiSO3 CF 3 )(LiTf), fluoroalkyl lithium phosphate Li[PF 3 (CF 2 CF 3 ) 3 ](LiFAP), lithium tetrakis(trifluoroacetoxy)borate Li[B(OCOCF 3 ) 4 ](LiTFAB), Lithium Bis(1,2-Benzenediol(2-)-O,O')borate[B(C 6 O 2 ) 2 ](LiBBB) and a combination of at least two thereof. According to a related embodiment, the lithium salt is lithium hexafluorophosphate (LiPF 6 ).
[0081] If present in the electrolyte, the solvent is preferably a non-aqueous solvent. Non-limiting examples of non-aqueous solvents include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), and vinylene carbonate (VC); acyclic carbonates such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dipropyl carbonate (DPC); lactones such as γ-butyrolactone (γ-BL) and γ-valerolactone (γ-VL); acyclic ethers such as 1,2-dimethoxyethane (DME), 1,2- Diethoxyethane (DEE), ethoxymethoxyethane (EME), trimethoxymethane, tetraethylene glycol dimethyl ether or tetraethylene glycol dimethyl ether (TEGDME) and ethyl monoethylene glycol dimethyl ether; cyclic ethers such as tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane and dioxolane derivatives; and other solvents such as dimethyl sulfoxide, formamide, acetamide, dimethylformamide, acetonitrile, propionitrile, nitromethane, triesters of phosphate, cyclopentane, methyl cyclopentane, propylene carbonate derivatives and mixtures thereof. According to some related examples, the non-aqueous solvent is a mixture of at least two carbonates, such as a mixture of ethylene carbonate and ethyl methyl carbonate (EC / EMC). According to a related example, the electrolyte is a liquid electrolyte and comprises LiPF in an EC / EMC mixture ([3:7] volume ratio) with 5% fluoroethylene carbonate (FEC). 6 .
[0082] According to some examples, the electrolyte is a liquid electrolyte, and the electrode material comprises an electrochemically active material as defined herein or an electrochemically active material prepared by a method as defined herein, PVDF as a binder, and a Ketjen TM Carbon, Super P TM Electronically conductive materials of carbon and VGCF.
[0083] According to some examples, the electrolyte is a gel electrolyte or a gel polymer electrolyte. The gel polymer electrolyte may include, for example, a polymer precursor, a salt (e.g., a salt as previously defined), a solvent (e.g., a solvent as previously defined), and, if necessary, a polymerization and / or crosslinking initiator. Non-limiting examples of gel electrolytes include, but are not limited to, gel electrolytes described in PCT patent applications with publication numbers WO2009 / 111860 (Zaghib et al.) and WO2004 / 068610 (Zaghib et al.).
[0084] According to some examples, a liquid electrolyte or gel electrolyte as previously defined may also be impregnated into the separator. Examples of separators include, but are not limited to, Whatman TM Diaphragms such as glass fiber GF filters.
[0085] According to some examples, the electrolyte is a solid polymer electrolyte including a salt in a solvent polymer. For example, the solid polymer electrolyte can be selected from all known solid polymer electrolytes and can be selected based on its compatibility with various elements of the electrochemical cell. For example, the solid polymer electrolyte is selected based on its compatibility with lithium. The solid polymer electrolyte can generally include one or more optionally cross-linked solid polar polymers and salts (e.g., salts as previously defined). Polyether polymers can be used, such as those based on PEO, but several other compatible polymers are also known for preparing solid polymer electrolytes and are also considered for use. The polymer can be cross-linked. Examples of such polymers include branched polymers, such as star polymers or comb polymers, such as those described in U.S. Patent Publication No. 7,897,674B2 (Zaghib et al.) (US'674).
[0086] According to some examples, the solid polymer electrolyte may include a block copolymer consisting of at least one lithium ion solvating segment and optionally at least one crosslinkable segment. Preferably, the lithium ion solvating segment is selected from a homopolymer or copolymer having a repeating unit of formula I:
[0087]
[0088] in,
[0089] R is selected from hydrogen atom, C 1 -C 10 Alkyl or -(CH 2 -OR a R b ) group;
[0090] R a Yes (CH 2 -CH 2 -O) y ;
[0091] R b Selected from hydrogen atoms and C 1 -C 10 alkyl;
[0092] x is an integer selected from the range of 10 to 200,000; and
[0093] y is an integer selected from the range of 0 to 10.
[0094] According to another example, the cross-linkable segment may be a polymer segment including at least one functional group that can be multi-dimensionally cross-linked by irradiation or heat treatment.
[0095] According to some embodiments, the electrolyte includes LiPF 6 and a solid polymer electrolyte of a PEO-based solvating polymer. According to some examples, the electrolyte is a solid polymer electrolyte as previously defined, and the electrode material comprises an electrochemically active material as defined herein or an electrochemically active material prepared by a method as defined herein, and is selected from Ketjen TM Carbon, Super P TM Electronically conductive materials of carbon and VGCFs.
[0096] In instances where the electrolyte is a solid polymer electrolyte, the electrode material may, for example, include about 80 wt % to about 90 wt % electrochemically active material, about 1 wt % to about 5 wt % electronically conductive material, and about 5 wt % to about 19 wt % solid polymer electrolyte.
[0097] According to some examples, the electrolyte is a glass or ceramic electrolyte. For example, the glass or ceramic electrolyte may include a crystalline ion-conducting ceramic or an amorphous ion-conducting ceramic, an amorphous ion-conducting glass, or an ion-conducting glass-ceramic. Non-limiting examples of glass or ceramic electrolytes include site-deficient perovskite electrolytes, garnet electrolytes, NASICON glass-ceramic electrolytes, LISICON electrolytes, lithium-stabilized sodium ions (Na + ) Conductive Alumina (Al 2 O 3 ) and other similar glass or ceramic electrolytes.
[0098] According to some examples, the electrolyte may also optionally include at least one additional additive, such as an ion-conducting material, an inorganic particle, a glass or a ceramic particle, such as a nanoceramic (e.g., alumina (Al 2 O 3 ), titanium dioxide (TiO 2 ), silicon dioxide (SiO 2) and similar compounds), and other such additives. For example, the additional additives can be selected from crystalline and / or amorphous forms of NASICON, LISICON, thio-LISICON, garnet, sulfide, sulfur halide, phosphate, thiophosphate and combinations thereof. According to one example, the additional additives can be substantially dispersed in the electrolyte. The additional additives can also be present in a separate layer.
[0099] The technology also relates to a battery comprising at least one electrochemical cell as defined herein. For example, the battery may be a lithium battery or lithium ion battery, a sodium battery or sodium ion battery, a magnesium battery or magnesium ion battery, or a potassium battery or potassium ion battery. According to a related variant, the battery is a lithium battery or lithium ion battery. According to another related variant, the battery is a sodium battery or sodium ion battery.
[0100] Example
[0101] The following examples are for illustration only and should not be construed as further limiting the scope of the invention as intended.These examples are better understood with reference to the accompanying drawings.
[0102] Unless otherwise stated, all numerical values used herein representing component amount, preparation conditions, concentration, property, etc. should be understood to be modified by the term "about" in all cases. At least, each numerical parameter should be interpreted according to the reported significant digits and by applying common rounding techniques. Therefore, unless otherwise stated, the numerical parameters given in this specification are approximate values that can vary with the desired properties. Although the numerical range and parameters that define the scope of the embodiment are in fact approximate values, the numerical values given in the following examples are reported as accurately as possible. However, any numerical value inherently contains a certain error caused by the variation in experiments, test measurements, statistical analysis, etc.
[0103] Example 1: Synthesis of electrochemically active materials
[0104] a) Solid-state synthesis of iron-doped tunnel oxides of sodium, manganese and at least one metal element
[0105] A tunnel oxide of iron-doped sodium, manganese and at least one metal element having the following chemical formula was synthesized by a simple solid-state reaction: Na 0.44 Mn 0.55 Ti 0.10 O 2 、Na 0.43 Fe 0.34 Mn 0.44 Ti 0.22 O 2 、Na 0.46 Fe 0.30 Mn 0.55 Ti0.15 O 2 、Na 0.44 Fe 0.34 Mn 0.55 Ti 0.11 O 2 、Na 0.41 Fe 0.40 Mn 0.50 Ti 0.10 O 2 、Na 0.50 Fe 0.08 Mn 0.81 Ti 0.11 O 2 and Na 0.50 Fe 0.11 Mn 0.78 Ti 0.11 O 2 . The respective precursors sodium carbonate (Na 2 CO 3 ), manganese(III) oxide (Mn 2 O 3 ), iron(III) oxide (Fe 2 O 3 ) and titanium dioxide (TiO 2 ) are weighed to obtain the desired stoichiometry. The samples are prepared by grinding and mixing the precursor powders. The ground and mixed precursor powders are then placed in a furnace and heated to a temperature between about 700° C. and about 1000° C. for 2 to 24 hours in an air or oxygen atmosphere.
[0106] b) Wet chemical synthesis of tunnel oxides of iron doped with sodium, manganese and at least one metal element
[0107] Alternatively, a tunnel oxide of iron-doped sodium, manganese and at least one metal element having the following chemical formula is also prepared using a sol-gel method: Na 0.44 Mn 0.55 Ti 0.10 O 2 、Na 0.43 Fe 0.34 Mn 0.44 Ti 0.22 O 2 、Na 0.46 Fe 0.30 Mn 0.55 Ti 0.15 O 2 、Na 0.44 Fe 0.34 Mn 0.55 Ti 0.11 O 2 、Na 0.41 Fe 0.40 Mn0.50 Ti 0.10 O 2 、Na 0.50 Fe 0.08 Mn 0.81 Ti 0.11 O 2 and Na 0.50 Fe 0.11 Mn 0.78 Ti 0.11 O 2 . Use citric acid (C 6 H 8 O 7 ) as a chelating agent to synthesize sol-gel powder. 2 CO 3 ), manganese(III) acetate ((CH 3 CO 2 ) 2 Mn), iron(II) oxalate and titanium(C 16 H 36 O 4 Ti 2 ) (all from Sigma-Aldrich, ≥99.99%) were weighed to obtain the desired stoichiometry and mixed with C under magnetic stirring. 6 H 8 O 7 Together with (Na+Mn) / C 6 H 8 O 7 = 10 in distilled water. The solution thus obtained is then heated to a temperature of about 80° C. under stirring until a transparent sol-gel precursor is obtained.
[0108] The sol-gel precursor thus obtained is then calcined in a furnace at a temperature of about 400° C. for about 6 hours to decompose the organic and inorganic contents (including anionic salts and C 6 H 8 O 7 ).
[0109] Finally, the powder thus obtained was ground in a mortar and calcined in a furnace in an air or oxygen atmosphere at a temperature of about 900° C. for about 9 hours to obtain the final sol-gel powder Na 0.44 Mn 0.55 Ti 0.10 O 2 、Na 0.43 Fe 0.34 Mn 0.44 Ti 0.22 O 2 、Na 0.46 Fe 0.30 Mn0.55 Ti 0.15 O 2 、Na 0.44 Fe 0.34 Mn 0.55 Ti 0.11 O 2 、Na 0.41 Fe 0.40 Mn 0.50 Ti 0.10 O 2 、Na 0.50 Fe 0.08 Mn 0.81 Ti 0.11 O 2 and Na 0.50 Fe 0.11 Mn 0.78 Ti 0.11 O 2 .
[0110] c) Synthesis of tunnel oxides of sodium, lithium, manganese and at least one metal element doped with iron
[0111] A tunnel oxide of sodium, lithium, manganese and at least one metal element doped with iron having the following chemical formula is prepared by partially replacing sodium ions with lithium ions using a one-step or two-step ion exchange method: Na 0.10 Li 0.33 Fe 0.34 Mn 0.44 Ti 0.22 O 2 、Na 0.08 Li 0.38 Fe 0.30 Mn 0.55 Ti 0.15 O 2 、Na 0.20 Li 0.24 Fe 0.34 Mn 0.55 Ti 0.11 O 2 、Na 0.21 Li 0.20 Fe 0.40 Mn 0.50 Ti 0.10 O 2 、Na 0.10 Li 0.40 Fe 0.08 Mn 0.81 Ti 0.11 O 2 and Na 0.10 Li 0.40 Fe 0.11 Mn 0.78 Ti0.11 O 2 .
[0112] The powders prepared in Examples 1(a) and 1(b) were mixed with 20-fold molar excess of lithium nitrate (LiNO 3 ) and lithium chloride (LiCl) or lithium hydroxide (LiOH) lithium eutectic salt composition (LiNO 3 :LiCl or LiOH = 1:1 molar ratio) to carry out ion exchange reaction. The mixture is then heated to a temperature between about 120° C. and about 400° C., and heated once for about 0.5 hour to about 10 hours, or heated twice for about 0.25 hour to about 5 hours to obtain the desired stoichiometry.
[0113] Finally, for comparison, the formula Na 0.08 Li 0.36 MnO 2 The tunnel oxide of sodium, lithium, manganese and at least one metal element. The formula Na as described in PCT Patent Application Publication No. WO2021 / 195778 (Wang et al.) is used. 0.44 MnO 2 This material is obtained by the ion exchange reaction of the tunnel-type sodium and manganese oxides of this embodiment.
[0114] d) X-ray diffraction (XRD) of the sample
[0115] The atomic and molecular structures of the electrochemically active materials were studied by X-ray diffraction of powders of iron-doped tunnel oxides of sodium, lithium, manganese and at least one metal element as prepared in Example 1(c). Figures 1 to 5 The tunneling Na 0.08 Li 0.36 MnO 2 、Na 0.10 Li 0.33 Fe 0.34 Mn 0.44 Ti 0.22 O 2 、Na 0.08 Li 0.38 Fe 0.30 Mn 0.55 Ti 0.15 O 2 、Na 0.20 Li 0.24 Fe 0.34 Mn 0.55 Ti 0.11 O 2 and Na 0.21 Li 0.20 Fe 0.40 Mn 0.50Ti 0.10 O 2 X-ray diffraction pattern of powder.
[0116] Example 2: Electrochemical properties
[0117] a) Electrochemical cell configuration
[0118] The electrochemical properties of the electrochemically active materials prepared in Example 1(c) were investigated. All cells were assembled in 2032-type button cell housings having the components shown in Table 1 and a negative electrode comprising a metallic lithium film on an aluminum current collector. All cells were tested with Whatman TM Glass fiber GF filter paper membrane assembly, the membrane is made of LiPF 6 A 1 M solution in a non-aqueous solvent mixture of EC / EMC ([3:7] volume ratio) and 5% FEC was used as the liquid electrolyte for impregnation. The electronically conductive material was Ketjen TM Carbon and SuperP TM A mixture of carbon ([1:1] weight ratio).
[0119] Table 1. Electrochemical cell configuration
[0120]
[0121] b) Electrochemical behavior
[0122] This example illustrates the electrochemical behavior of the electrochemical cell as described in Example 2(a).
[0123] Figure 6 Two charge and discharge curves of a comparative battery (Battery 1) are presented. (1) At about 2.0 V to about 4.8 V vs. Li + / Li at a cycle rate of 0.1C, and (2) between about 2.0V and about 4.6V vs.Li + / Li, charging and discharging were performed. Charging and discharging were performed at a temperature of about 25°C. Results for the second discharge and charge cycle are shown.
[0124] Figure 7 A second charge and discharge curve for battery 2 is presented. At about 2.0 V to about 4.8 V vs. Li + / Li was charged and discharged at a cycle rate of 0.1 C. The charging and discharging was performed at a temperature of about 25°C.
[0125] Figure 8 The charge and discharge curves of battery 3 are presented. At about 2.0V to about 4.8V vs. Li + / Li were charged and discharged at a cycle rate of 0.1 C. The charging and discharging were performed at a temperature of about 25°C. The results for the second discharge and charge cycle are shown.
[0126] Fig. 9 The charge and discharge curves of battery 4 are presented. At about 2.0 V to about 4.8 V vs. Li + / Li were charged and discharged at a cycle rate of 0.1 C. The charging and discharging were performed at a temperature of about 25°C. The results for the second (1) and fifth (2) charge and discharge cycles are shown.
[0127] Fig.10 The charge and discharge curves of battery 5 are presented. At about 2.0V to about 4.8V vs. Li + / Li were charged and discharged at a cycle rate of 0.1 C. The charging and discharging were performed at a temperature of about 25°C. The results for the second discharge and charge cycle are shown.
[0128] Fig.11 (a) shows the charge and discharge curves of battery 6. At about 2.0V to about 4.8V vs. Li + / Li was charged and discharged at a cycle rate of 0.1 C. The charging and discharging was performed at a temperature of about 25°C. Fig.11 (b) is a graph showing the capacity obtained for battery 6 vs. number of cycles.
[0129] Fig.12 (a) shows the charge and discharge curves of battery 7. At about 2.0V to about 4.8V vs. Li + / Li was charged and discharged at a cycle rate of 0.1 C. The charging and discharging was performed at a temperature of about 25°C. Fig.12 (b) is a graph showing the capacity obtained for battery 7 vs. the number of cycles.
[0130] The capacity, voltage and specific energy of batteries 1 to 5 are shown in Table 2.
[0131] Table 2. Capacity, voltage, and specific energy provided by the electrochemical cells in Table 1.
[0132]
[0133] As can be observed in Table 2, the presence of iron ions significantly increases the average working potential of the electrochemically active material. Table 2 also shows that the electrochemical properties of the electrochemically active material can be significantly improved by partial replacement of sodium ions by lithium ions and / or partial replacement of manganese ions by titanium ions.
[0134] Many modifications may be made to any of the embodiments described above without departing from the scope of the invention as intended.The references, patents or scientific literature mentioned in this application are hereby incorporated by reference in their entirety for all purposes.
Claims
1. An electrochemically active material comprising a tunnel-type oxide of sodium, manganese and at least one metal element doped with lithium-substituted iron, the oxide having the formula Na a Li b Fe c Mn d M e O2, wherein a is a number such that 0<a<0.22; b is a number such that 0.18<b<0.40 and such that a+b is 0.38<a+b<0.62; c is a number such that 0<c≤0.40; d is a number such that 0.44≤d<1; e is a number such that c+d+e=1; and M is selected from manganese (Mn), titanium (Ti), vanadium (V), nickel (Ni), cobalt (Co), chromium (Cr), molybdenum (Mo), zirconium (Zr), tin (Sn), ruthenium (Ru), other similar metals and a combination of at least two thereof.
2. The electrochemically active material of claim 1, wherein M is selected from manganese (Mn), titanium (Ti), vanadium (V), nickel (Ni), cobalt (Co), chromium (Cr), molybdenum (Mo), zirconium (Zr), ruthenium (Ru), other similar metals, and a combination of at least two thereof.
3. The electrochemically active material according to claim 1 or 2, wherein M is titanium (Ti).
4. The electrochemically active material according to any one of claims 1 to 3, wherein a is a number such that 0.01<a<0.22, or 0.02<a<0.22, or 0.03<a<0.22, or 0.04<a<0.22, or 0.05<a<0.22, or 0.06<a<0.22, or 0.07<a<0.22, or 0.08≤a≤0.
21. 5 . The electrochemically active material according to claim 4 , wherein a is a number such that 0.08≦a≦0.
21.
6. The electrochemically active material according to any one of claims 1 to 5, wherein b is a number such that 0.19<b<0.40, or 0.20≤b<0.40, or 0.20≤b<0.39, or 0.20≤b≤0.
38.
7. The electrochemically active material according to claim 6, wherein b is a number such that 0.20≤b≤0.
38.
8. The electrochemically active material according to any one of claims 1 to 7, wherein c is a number such that 0.05<c≤0.40, or 0.10<c≤0.40, or 0.15<c≤0.40, or 0.20<c≤0.40, or 0.25<c≤0.40, or 0.30≤c≤0.
40.
9. The electrochemically active material according to claim 8, wherein c is a number such that 0.30≤c≤0.
40.
10. The electrochemically active material according to any one of claims 1 to 9, wherein d is a number such that 0.44≤d<1, or 0.44≤d<0.95, or 0.44≤d<0.90, or 0.44≤d<0.85, or 0.44≤d<0.80, or 0.44≤d<0.75, or 0.44≤d<0.70, or 0.44≤d<0.65, or 0.44≤d<0.60, or 0.44≤d≤0.
55.
11. The electrochemically active material according to claim 10, wherein d is a number such that 0.44≤d≤0.
55.
12. The electrochemically active material according to any one of claims 1 to 11, wherein the tunnel oxide of sodium, manganese and at least one metal element doped with lithium-substituted iron is selected from Na 0.10 Li 0.33 Fe 0.34 Mn 0.44 Ti 0.22 O2、Na 0.08 Li 0.38 Fe 0.30 Mn 0.55 Ti 0.15 O2、Na 0.20 Li 0.24 Fe 0.34 Mn 0.55 Ti 0.11 O2、Na 0.21 Li 0.20 Fe 0.40 Mn 0.50 Ti 0.10 O2、Na 0.10 Li 0.40 Fe 0.08 Mn 0.81 Ti 0.11 O2 and Na 0.10 Li 0.40 Fe 0.11 Mn 0.78 Ti 0.11 O2.
13. An electrode material comprising the electrochemically active material according to any one of claims 1 to 12. The electrode material according to claim 13 , further comprising an electronically conductive material.
15. The electrode material according to claim 14, wherein the electronically conductive material is selected from the group consisting of carbon black, acetylene black, graphite, graphene, carbon fiber, carbon nanofiber, carbon nanotube, and a combination of at least two thereof.
16. The electrode material of claim 15, wherein the electronically conductive material comprises carbon black.
17. The electrode material according to claim 16, wherein the carbon black is Super P TM carbon.
18. The electrode material according to claim 16, wherein the carbon black is Ketjen TM carbon.
19. The electrode material of claim 15, wherein the electronically conductive material comprises carbon fibers.
20. The electrode material according to claim 19, wherein the carbon fiber is vapor grown carbon fiber (VGCF).
21. The electrode material according to any one of claims 13 to 20, further comprising a binder.
22. The electrode material according to claim 21, wherein the binder is selected from the group consisting of polyether polymers, fluorine-containing polymers and water-soluble binders.
23. The electrode material of claim 22, wherein the binder is a fluoropolymer.
24. The electrode material of claim 23, wherein the fluorine-containing polymer is polyvinylidene fluoride (PVDF).
25. The electrode material according to any one of claims 13 to 24, further comprising an additive.
26. The electrode material according to claim 25, wherein the additive is selected from ion conductors, inorganic particles, glass particles, ceramic particles, salts and other similar additives.
27. An electrode comprising the electrode material according to any one of claims 13 to 26 on a current collector.
28. The electrode according to claim 27, which is a positive electrode.
29. An electrochemical cell comprising a negative electrode, a positive electrode and an electrolyte, wherein the positive electrode is according to claim 27 or 28.
30. The electrochemical cell of claim 29, wherein the negative electrode comprises an alkali metal, an alloy containing an alkali metal, or a pre-lithiated electrochemically active material.
31. The electrochemical cell of claim 30, wherein the negative electrode comprises metallic lithium or an alloy containing metallic lithium.
32. The electrochemical cell of claim 31 , wherein the negative electrode comprises metallic lithium.
33. The electrochemical cell of any one of claims 29 to 32, wherein the electrolyte is a glass or ceramic electrolyte.
34. An electrochemical cell according to any one of claims 29 to 32, wherein the electrolyte is a liquid electrolyte comprising a salt in a solvent.
35. An electrochemical cell according to any one of claims 29 to 32, wherein the electrolyte is a gel electrolyte comprising a salt and optionally a solvating polymer in a solvent.
36. An electrochemical cell according to any one of claims 29 to 32, wherein the electrolyte is a solid polymer electrolyte comprising a salt in a solvated polymer.
37. The electrochemical cell of any one of claims 34 to 36, wherein the salt is a lithium salt.
38. The electrochemical cell of claim 37, wherein the lithium salt is selected from the group consisting of lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), 2-trifluoromethyl-4,5-dicyanoimidazole lithium (LiTDI), 4,5-dicyano-1,2,3-triazole lithium (LiDCTA), lithium bis(pentafluoroethylsulfonyl)imide (LiBETI), lithium tetrafluoroborate (LiBF4), lithium bis(oxalato)borate (LiBOB), lithium nitrate (LiNO3), lithium chloride Lithium (LiCl), lithium bromide (LiBr), lithium fluoride (LiF), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiSO3CF3) (LiTf), lithium fluoroalkyl phosphate Li[PF3(CF2CF3)3] (LiFAP), lithium tetrakis(trifluoroacetoxy)borate Li[B(OCOCF3)4] (LiTFAB), lithium bis(1,2-benzenediol(2-)-O,O')borate [B(C6O2)2] (LiBBB) and a combination of at least two thereof.
39. The electrochemical cell of claim 38, wherein the lithium salt is lithium hexafluorophosphate (LiPF6).
40. A battery comprising at least one electrochemical cell according to any one of claims 29 to 39.
41. The battery of claim 40, wherein the battery is selected from the group consisting of a lithium battery, a lithium ion battery, a sodium battery, a sodium ion battery, a potassium battery, a potassium ion battery, a magnesium battery, and a magnesium ion battery.
42. A battery according to claim 40 or 41, wherein the battery is a lithium battery or a lithium ion battery.