Separator, method for manufacturing same, electrode assembly including same, method for manufacturing same, and lithium secondary battery including same
By using a mixture of nonwoven fabric substrates and fibers of different diameters and inorganic particles in the lithium secondary battery separator, the problem of heat shrinkage and ignition of the separator at high temperature is solved, and the hardness and insulation of the battery cell are improved.
Patent Information
- Application Number
- CN202380030701.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-12-11
- Filing Date
- 2023-12-15
- Publication Date
- 2024-11-15
AI Technical Summary
Existing lithium secondary battery separators may cause heat shrinkage and internal short circuits at high temperatures, increasing the risk of ignition, and making it difficult to ensure both insulation and adhesion.
A mixture of a nonwoven fabric substrate with small-diameter fibers and large-diameter fibers is used, and the pores are filled with inorganic particles to adjust the melting point of the fibers and the particle size of the particles to improve the insulation and adhesion of the separator.
The partition is in close contact with the electrodes through lamination or hot pressing processes, ensuring stable hardness and shape of the battery cell, reducing the risk of ignition, and improving the battery's heat resistance and insulation performance.
Smart Images

Figure BDA0005061477240000191
Abstract
Description
Technical Field
[0001] The present disclosure relates to a separator, a manufacturing method thereof, an electrode assembly including the same, a manufacturing method thereof, and a lithium secondary battery including the same.
[0002] This application is based on and claims the benefit of priority of Korean Patent Application No. 10-2023-0025333 filed on February 24, 2023, in the Korean Intellectual Property Office, and Korean Patent Application No. 10-2023-0179147 filed on December 11, 2023, in the Korean Intellectual Property Office, the disclosures of which are incorporated herein by reference in their entirety. Background Art
[0003] In recent years, there has been a growing interest in energy storage technology. As the field of application expands to include mobile phones, cameras, notebook PCs, and even electric vehicles, more efforts are being made to research and develop electrochemical devices. In this regard, electrochemical devices are one of the most prominent areas, and the development of secondary batteries such as lithium secondary batteries that can be charged and discharged has become a focus of attention.
[0004] For the separator constituting such a battery, its basic requirement is to separate the positive electrode and the negative electrode and electrically insulate them, while increasing the permeability of ions such as lithium ions based on high porosity, thereby increasing ion conductivity. The substrate commonly used for the separator is a porous polyolefin film made of a polyolefin-based material such as polyethylene (PE) and polypropylene (PP) that is conducive to pore formation and has excellent chemical resistance, mechanical properties and thermal properties.
[0005] However, due to the material properties and manufacturing process of the porous polyolefin membrane (particularly the manufacturing process involving stretching), the separator may thermally shrink at high temperatures, causing internal short circuits and melting of the polymer separator substrate during thermal runaway. Therefore, the risk of fire increases. Summary of the invention
[0006] Technical issues
[0007] According to one aspect, the present disclosure provides a separator having improved insulation and adhesion to an electrode while having a nonwoven fabric substrate and inorganic particles filled to be positioned in pores thereof.
[0008] According to another aspect, the present disclosure provides an electrode assembly including the disclosed separator and a method of manufacturing the same.
[0009] According to still another aspect, the present disclosure provides a lithium secondary battery having an electrode assembly using the disclosed separator.
[0010] It is obvious that the objects and advantages of the present disclosure can be achieved by the means or methods described in the claims and their combinations.
[0011] Technical Solution
[0012] One aspect of the present disclosure provides a separator according to the following embodiments.
[0013] The first embodiment relates to a separator, which includes: a non-woven fabric substrate, which is formed by mixing first fibers having an average diameter of about 10 μm or more and second fibers having an average diameter of about 1 μm or less; and inorganic particles, which are positioned in pores formed between the first fibers and the second fibers of the non-woven fabric substrate, wherein the melting point of the first fibers is about 150° C. or less, and the D50 of the inorganic particles is about 400 nm or less.
[0014] The second embodiment is directed to the separator according to the first embodiment, wherein a mixing weight ratio of the first fibers to the second fibers is about 1:9 to 9:1.
[0015] The third embodiment is directed to the separator according to the first embodiment or the second embodiment, wherein the average diameter of the first fibers is about 10 μm to 30 μm, and the average diameter of the second fibers is about 0.1 μm to 1 μm.
[0016] A fourth embodiment is directed to the separator according to any one of the first to third embodiments, wherein D50 of the inorganic particles is about 30 nm to 400 nm.
[0017] A fifth embodiment is directed to the separator according to any one of the first to fourth embodiments, wherein the melting point of the first fiber is about 50°C to 120°C.
[0018] The sixth embodiment is directed to the separator according to any one of the first to fifth embodiments, wherein the first fibers are formed of one or more polymers selected from the group consisting of polyamide, polyester, thermoplastic polyurethane, and ethylene-vinyl acetate copolymer.
[0019] A seventh embodiment is directed to the separator according to any one of the first to sixth embodiments, wherein the melting point of the second fiber is about 200° C. or higher.
[0020] An eighth embodiment relates to a separator according to any one of the first to seventh embodiments, wherein the second fiber is formed by one or more polymers selected from the group consisting of polyethylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene ether, polyphenylene sulfide and polyethylenenaphthalene.
[0021] A ninth embodiment is directed to the separator according to any one of the first to eighth embodiments, wherein the thickness of the separator is about 10 μm to 30 μm.
[0022] The tenth embodiment is directed to the separator according to any one of the first to ninth embodiments, wherein the nonwoven fabric substrate has a unit weight of about 5 g / m 2 Up to 30g / m 2 , and the weight per unit area of the inorganic particles is about 10 g / m 2 Up to 50g / m 2 .
[0023] An eleventh embodiment is directed to the separator according to any one of the first to tenth embodiments, wherein the separator has a permeability of about 1 sec / 100 cm3 to 300 sec / 100 cm3.
[0024] The twelfth embodiment is directed to the separator according to any one of the first to eleventh embodiments, wherein the inorganic particles are coated with a binder polymer on at least a portion of a surface thereof.
[0025] Another aspect of the present disclosure provides a method of preparing a separator of a lithium secondary battery according to the following embodiments.
[0026] A thirteenth embodiment relates to a method for preparing a separator for a lithium secondary battery, the method comprising: forming a nonwoven fabric substrate from a mixture of first fibers and second fibers having different predetermined diameter ranges; and arranging inorganic particles in holes formed between the first fibers and the second fibers, wherein the average diameter of the first fibers is adjusted to about 10 μm or greater, the average diameter of the second fibers is adjusted to about 1 μm or less, the first fibers are fibers having a melting point of about 150° C. or less, and the D50 of the inorganic particles is controlled to be about 400 nm or less.
[0027] A fourteenth embodiment is directed to a method according to the thirteenth embodiment, wherein the first fibers are formed from one or more polymers selected from the group consisting of polyamides, polyesters, thermoplastic polyurethanes, and ethylene vinyl acetate copolymers.
[0028] A fifteenth embodiment is directed to the method according to the thirteenth embodiment or the fourteenth embodiment, wherein the second fiber is a fiber having a melting point of about 200° C. or higher.
[0029] A sixteenth embodiment is directed to a method according to any one of the thirteenth to fifteenth embodiments, wherein the second fiber is formed of one or more polymers selected from the group consisting of polyethylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, and polyethylene naphthalene.
[0030] Still another aspect of the present disclosure provides an electrode assembly according to the following embodiments.
[0031] The seventeenth embodiment is directed to an electrode assembly including: a positive electrode; a negative electrode; and the separator of any one of the first to twelfth embodiments disposed between the positive electrode and the negative electrode.
[0032] Still another aspect of the present disclosure provides a method of manufacturing an electrode assembly according to the following embodiments.
[0033] The eighteenth embodiment relates to a method for manufacturing an electrode assembly, which includes: preparing the separator of any one of the first to twelfth embodiments; and inserting the separator between the positive electrode and the negative electrode, followed by heating and pressurizing at a temperature range of about -80°C to +30°C based on the melting point of the first fiber.
[0034] Still another aspect of the present disclosure provides a lithium secondary battery according to the following embodiments.
[0035] A nineteenth embodiment is directed to a lithium secondary battery, including: the electrode assembly of the seventeenth embodiment.
[0036] Beneficial Effects
[0037] According to the present disclosure, a nonwoven fabric substrate is formed by a mixture of fibers having different predetermined diameter ranges, and the melting point of fibers having a large diameter and the average particle size of inorganic particles filled to be positioned in the pores of the nonwoven fabric substrate are controlled at the same time, so that adhesion and insulation to the electrode can be ensured at the same time.
[0038] Therefore, when the separator of the present disclosure is combined with the electrode and assembled into an electrode structure, for example, via a lamination or hot pressing process, the hardness (robustness) of the battery cell is maintained even after electrolyte injection. This is because the electrode interface and the separator are firmly attached, inhibiting the battery cell from bending and / or twisting.
[0039] The effects of each constituent element of the present disclosure will be described in more detail below. DETAILED DESCRIPTION
[0040] Hereinafter, the present disclosure will be described in detail. In the following detailed description, reference is made to the accompanying drawings that form a part thereof. The exemplary embodiments described in the detailed description, the accompanying drawings, and the claims are not intended to be limiting. Other embodiments may be utilized and other changes may be made without departing from the spirit or scope of the subject matter presented herein.
[0041] Throughout the specification, unless particularly described to the contrary, when it is mentioned that a component “includes” or “is provided with” a certain component, this means that other components are not excluded, but are included or further provided with the other components.
[0042] As used herein, a feature of having pores means that the object includes a plurality of pores, and gaseous and / or liquid fluids can pass from one side of the object to the other due to a structure in which the pores are connected to each other.
[0043] Generally, in order to increase the battery capacity, the battery is produced in the form of a stack of overlapping multiple unit cells. For example, in a roll-to-roll process, the battery is manufactured by contacting a pre-made separator with electrodes such as a positive electrode and a negative electrode, and the process is repeated to continuously produce the battery. Therefore, in the continuous manufacturing process of the battery, the adhesion between the separator and the electrode is an important factor, and therefore, when compared with a conventional separator, the disclosed separator has excellent adhesion to the electrode.
[0044] If the contact between the separator and the electrode is available, the lithium secondary battery can be manufactured by an assembly process such as lamination and hot pressing. In this case, there are advantages that the electrode interface and the separator are in close contact, and the hardness of the battery cell is ensured even in the case of electrolyte injection. In particular, as the size of the battery cell increases, when the electrode and the separator are not combined, there is a risk that the alignment of the stacked separator and the electrode may be misaligned, and there is a problem that the battery is bent or twisted even after the battery is manufactured.
[0045] In the art, a separator is used in a form in which porous polyolefin is coated with an inorganic material to improve heat resistance, but it has disadvantages such as polyolefin used as a base material is highly flammable, thereby increasing the risk of fire.
[0046] The present disclosure discloses a separator that includes a nonwoven fabric substrate made of heat-resistant fibers such as polyethylene terephthalate as a substrate material for the separator, and heat resistance is enhanced by filling inorganic particles in pores formed between the fibers. The separator is a building-like structure made of steel bars (corresponding to the fibers constituting the nonwoven fabric) as a basic frame and filled with concrete containing gravel or sand (corresponding to the inorganic particles).
[0047] Such a nonwoven fabric substrate has the advantages of a relatively simple manufacturing process and low manufacturing cost, but when the pores are too large, it may be difficult to ensure sufficient insulation using only inorganic particles positioned in the pores.
[0048] At the same time, since the separator of the present disclosure is assembled into an electrode structure by attaching to the electrode via a lamination or hot pressing process, the electrode interface and the separator are in close contact to maintain hardness such as structural integrity even after electrolyte injection, for example, the shape and size of the battery cell. In particular, if the electrode and the separator are not in close contact, there is a risk that the arrangement of the stacked separators and electrodes may be distorted as the size of the battery increases and the battery becomes larger and longer, and / or the battery may become bent or twisted even after the battery cell is manufactured. Therefore, even when the separator is filled with inorganic particles in the pores of the non-woven fabric substrate, the present disclosure ensures adhesion to the electrode.
[0049] In this specification, the separator has a porous feature including a large number of pores, and serves as a porous ion-conductive barrier that allows ions to pass therethrough while preventing electrical contact between a negative electrode and a positive electrode in an electrochemical device.
[0050] As used herein, "nonwoven fabric" refers to a fabric formed by entanglement of fibers with each other, rather than a fabric woven by warp yarns and weft yarns using a loom or a knitted fabric using a knitting machine.
[0051] The present disclosure provides a separator comprising: a nonwoven fabric substrate formed by mixing first fibers having an average diameter of about 10 μm or more and second fibers having an average diameter of about 1 μm or less; and inorganic particles positioned in pores formed between the first fibers and the second fibers of the nonwoven fabric substrate, wherein the melting point of the first fibers is about 150° C. or less, and the D50 of the inorganic particles is about 400 nm or less.
[0052] [Nonwoven fabric substrate]
[0053] When a conventional nonwoven fabric is coated with ceramic, the nonwoven fabric does not have adhesiveness and therefore cannot be introduced into the lamination process. However, since the nonwoven fabric of the present disclosure has adhesiveness, the electrode and the separator can be attached to each other using a method such as hot melting without forming a separate adhesive layer.
[0054] The nonwoven fabric substrate of the present disclosure is formed from a mixture of first fibers and second fibers having different average diameters.
[0055] The average diameter of the first fibers is about 10 μm or more. For example, the average diameter of the first fibers may be about 10 μm to 30 μm, or 10 μm to 20 μm, or about 12 μm to 17 μm.
[0056] The first fibers having such a large average diameter increase the surface roughness of the nonwoven fabric, so that the first fibers are exposed in large quantities on the surface of the nonwoven fabric substrate. This makes it easier to contact the electrode. This is also conducive to filling the pores of the nonwoven fabric substrate with inorganic particles.
[0057] When the average diameter of the first fibers is less than 10 μm, the surface roughness of the nonwoven fabric decreases, and the exposure ratio of the inorganic particles and the second fibers on the surface of the nonwoven fabric increases. Therefore, there is a problem that the exposure ratio of the first fibers on the surface of the nonwoven fabric substrate decreases.
[0058] The first fiber has a melting point of about 150°C or less, such as about 50°C to 120°C, or about 60°C to 100°C, or about 70°C to 100°C, or about 80°C to 95°C.
[0059] When the separator of the present disclosure is heated and pressurized to be attached to the electrode via a lamination or hot pressing process, the first fiber having the above-mentioned melting point range partially flows by, for example, melting, and is attached to the electrode interface. Therefore, the separator is bonded to the electrode and closely attached to each other, so that the hardness of the battery cell is maintained even after the electrolyte is injected, and the bending or distortion of the battery cell is suppressed. In addition, during the thermal runaway of the battery, the first fiber may melt and provide a shutoff function to the separator to close the pores.
[0060] When the melting point of the first fiber exceeds 150°C, it is difficult for the first fiber to flow without affecting the electrode when heated for thermal bonding. In addition, during thermal runaway of the battery, the shutdown temperature of the separator becomes too high, making it difficult to suppress ignition of the battery.
[0061] The first fibers may be formed from one or more polymers selected from the group consisting of polyamide, polyester, thermoplastic polyurethane (TPU), and ethylene vinyl acetate copolymer.
[0062] Examples of polyamides include synthetic products prepared by reacting a linear diacid, such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, hexadecanedioic acid, heneicosanediol, phellogenic acid, or equisetolic acid, or a mixture of two or more of these compounds. acid); the aromatic diacid is for example phthalic acid, isophthalic acid, terephthalic acid, bibenzoic acid, or 2,6-naphthalene dicarboxylic acid; the lactam is for example β-propiolactam, γ-butyrolactam, δ-valerolactam, or ε-caprolactam; the diamine is for example methylenediamine, ethylenediamine, 1,3-diaminopropane, putrescine, cadaverine, hexamethylenediamine, 1,2-diaminopropane, 1,4-diazacycloheptane, PPD (p-phenylenediamine), 1,4-diazacycloheptane, o-xylene diamine, m-xylene diamine, p-xylene diamine, o-phenylene diamine, m-phenylene diamine, p-phenylene diamine, dimethyl-4-phenylene diamine, 4,4'-diaminobiphenyl, or 1,8-diaminonaphthalene.
[0063] Examples of polyesters include synthetic products prepared from terephthalic acid or isophthalic acid and 1,4-butadiene, in which the melting point can be adjusted by adding tackifying resins, plasticizing oils, or both, or mixtures of two or more of these compounds.
[0064] Examples of the ethylene-vinyl acetate copolymer include an ethylene-vinyl acetate-based compound including vinyl acetate in an amount of about 18 parts by weight or more and less than 40 parts by weight, or a mixture of two or more thereof.
[0065] The second fibers are mixed with the first fibers to form a nonwoven fabric substrate.
[0066] In the present specification, the term “mixed” should be construed to include a state in which the first fibers and the second fibers are uniformly mixed, and a state in which the first fibers and the second fibers are non-uniformly mixed such that they are not separated from each other and form separate layers.
[0067] The average diameter of the second fiber is about 1 μm or less. For example, the average diameter of the second fiber can be about 0.1 μm to 1 μm, or about 0.5 μm to 1 μm, or about 0.6 μm to 0.8 μm. In this way, the second fiber with an average diameter less than the first fiber helps to ensure the insulation of the separator by controlling the hole size and deviation of the nonwoven fabric substrate to a small range. In addition, the second fiber suppresses the separation phenomenon of the inorganic particles positioned in the hole of the nonwoven fabric substrate. In addition, the second fiber suppresses the thickness of the nonwoven fabric substrate to become too thick to ensure insulation.
[0068] When the average diameter of the second fibers exceeds 1 μm, the above functions of the second fibers may be deteriorated. In this regard, the mixing weight ratio of the first fibers to the second fibers may be about 1:9 to 9:1, for example, about 2:8 to 8:2, or about 3:7 to 7:3.
[0069] Similar to the first fibers, the second fibers may have a melting point of about 150° C. or less. The second fibers having such a melting point range further improve the adhesion of the separator to the electrode. In addition, the shutdown function of the separator is further enhanced.
[0070] Meanwhile, the melting point of the second fiber may be about 200° C. or higher. When the second fiber having such a high melting point is used, even when the first fiber is completely melted due to the thermal runaway of the battery, the shape of the separator is maintained due to the second fiber, thereby improving heat resistance. The second fiber having a high melting point may be formed of one or more polymers selected from the group consisting of polyethylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, and polyethylene naphthalene, but is not limited thereto.
[0071] Considering the functions of the first fiber and the second fiber, the weight per unit area of the nonwoven fabric substrate may be about 5 g / m 2 Up to 30g / m 2 , for example about 8g / m 2 Up to 25g / m 2 , but not limited to this.
[0072] [Inorganic particles]
[0073] The pores formed between the fibers of the nonwoven fabric substrate are filled with inorganic particles. Even when the nonwoven fabric substrate melts during thermal runaway of the battery, the inorganic particles help prevent the explosion of the battery by preventing direct contact between the positive electrode and the negative electrode. The inorganic particles also help improve the insulation of the separator.
[0074] The average particle size (D50) of the inorganic particles is about 400 nm or less, for example, D50 is about 30 nm to 400 nm, about 50 nm to 350 nm, about 65 nm to 300 nm, or about 70 nm to 290 nm.
[0075] In this specification, the term "D50" means the particle size at the 50% point of the cumulative distribution of particle volume according to the particle size. D50 can be measured using a laser diffraction method. For example, the powder to be measured is dispersed in a dispersion medium and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Malvern MASTERSIZER 3000) to measure the difference in the diffraction pattern according to the particle size when the particle passes through the laser beam, thereby calculating the particle size distribution. D50 can be measured by calculating the particle size at the 50% point of the cumulative distribution of particle volume according to the particle size in the measuring device.
[0076] When the D50 of the inorganic particles exceeds 400 nm, the insulation of the separator may be reduced, and the ratio of the surface exposed to the separator may increase, thereby reducing the adhesive strength of the separator. In this regard, the unit area weight of the inorganic particles in the separator may be about 10 g / m 2 Up to 50g / m 2 , for example about 12 g / m 2 Up to 40g / m 2 , or about 15g / m 2 Up to 30g / m 2 , but not limited to this.
[0077] The inorganic particles are not particularly limited as long as they are electrochemically stable. That is, the inorganic particles that can be used in the present disclosure are not particularly limited as long as they are within the operating voltage range of the electrochemical device to which they are applied (e.g., based on Li / Li + , 0V to 5V) without undergoing oxidation and / or reduction reaction. In particular, the use of inorganic particles with a high dielectric constant can help increase the dissociation of electrolyte salts such as lithium salts in liquid electrolytes, thereby improving the ionic conductivity of the electrolyte.
[0078] For the above reasons, the inorganic particles may include high dielectric constant inorganic particles having a dielectric constant of about 5 or more, or about 10 or more. Non-limiting examples of inorganic particles having a dielectric constant of 5 or more include any inorganic particle selected from the group consisting of BaTiO3, Pb(Zr x ,Ti 1-x )O3(PZT, where 0 <x<1)、Pb 1-x La x Zr 1-y Ti y O3(PLZT, where 0 <x<1,0<y<1)、(1-x)Pb(Mg 1 / 3 Nb 2 / 3 ) 3-xPbTiO3 (PMN-PT, where 0 < x < 1), hafnium dioxide (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, boehmite, Al(OH)3, AlOOH, SiC, TiO2, or a mixture of two or more thereof.
[0079] In addition, inorganic particles having lithium ion transfer ability (i.e., inorganic particles containing the element lithium but not storing lithium and having the ability to transfer lithium ions) can be used as the inorganic particles. Non-limiting examples of inorganic particles having lithium ion transfer ability include lithium phosphate (Li3PO4); lithium titanate (Li x Ti y (PO4)3, 0 < x < 2, 0 < y < 3); lithium aluminum titanate (Li x Al y Ti z (PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3); (LiAlTiP) x O y series glass (0 < x < 4, 0 < y < 13), such as 14Li2O-9Al2O3-38TiO2-39P2O5; lithium lanthanum titanate (Li x La y TiO3, 0 < x < 2, 0 < y < 3); lithium germanium thiophosphate (Li x Ge y P z S w ., 0 < x < 4, 0 < y < 1, 0 < z < 1, w < 5), such as Li 3.25 Ge 0.25 P 0.75 S4; lithium nitride (Li x N y ., 0 < x < 4, 0 < y < 2), such as Li3N; SiS2 series glass (Li x Si y S z ., 0 < x < 3, 0 < y < 2, 0 < z < 4), such as Li3PO4-Li2S-SiS2; P2S5 series glass (Li x P y S z ., 0 < x < 3, 0 < y < 3, 0 < z < 7), such as LiI-Li2S-P2S5; or a mixture of two or more thereof.
[0080] Inorganic particles can be coated with binder polymer on at least a portion of its surface.Binder polymer coated on the surface allows inorganic particles to be attached to the fiber of nonwoven fabric, thereby suppressing the separation phenomenon of inorganic particles.The limiting examples of binder include polyvinylidene fluoride, polyvinylidene fluoride-copolymerization-hexafluoropropylene, polyvinylidene fluoride-copolymerization-trichloroethylene, polyvinylidene fluoride-copolymerization-chlorotrifluoroethylene, polymethyl methacrylate, polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl acetate, ethylene vinyl acetate copolymer (polyethylene-copolymerization-vinyl acetate), polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethyl cellulose, acrylonitrile-styrene-butadiene copolymer, polyimide or a mixture of both or more thereof.
[0081] Except when the first fiber or the second fiber is interposed therebetween, the inorganic particles may be positioned to substantially contact each other. In this case, when a coating of a binder polymer is formed on the surface of the inorganic particles, the binder polymer may connect and fix the inorganic particles so that the inorganic particles remain bonded to each other.
[0082] Therefore, according to one embodiment of the present disclosure, a method for preparing a separator of a lithium secondary battery includes: forming a nonwoven fabric substrate from a mixture of first fibers and second fibers having different predetermined diameter ranges; and arranging inorganic particles in holes formed between the first fibers and the second fibers. The average diameter of the first fibers is adjusted to about 10 μm or more, the average diameter of the second fibers is adjusted to about 1 μm or less, the first fibers are fibers having a melting point of about 150° C. or less, and the D50 of the inorganic particles is controlled to about 400 nm or less.
[0083] [Separator]
[0084] The permeability of the separator provided with the above-mentioned nonwoven fabric substrate and inorganic particles can be about 1 sec / 100 cubic centimeter to 300 sec / 100 cubic centimeter, for example, about 100 sec / 100 cubic centimeter to 300 sec / 100 cubic centimeter, about 140 sec / 100 cubic centimeter to 300 sec / 100 cubic centimeter, or about 150 sec / 100 cubic centimeter to 290 sec / 100 cubic centimeter.
[0085] In this specification, the term "permeability" refers to the time for 100 cubic centimeters of air to pass through an object to be measured for permeability, such as a separator, and the unit can be seconds / 100 cubic centimeters. Permeability can be used interchangeably with transmittance and is usually expressed as a Gurely value. In a specific embodiment of the present disclosure, permeability is measured according to JIS P8117.
[0086] In addition, the separator may have a thickness of about 10 μm to 30 μm, for example, about 15 μm to 30 μm, or about 20 μm to 25 μm, but is not limited thereto.
[0087] [Electrode assembly]
[0088] The electrode assembly is formed of a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode.
[0089] Hereinafter, the configuration of the electrode assembly and the method of manufacturing the above-mentioned separator will be described in more detail.
[0090] The positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector.
[0091] In the positive electrode, the positive electrode collector is not particularly limited as long as it is conductive without causing chemical changes in the battery, and examples thereof include stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium or silver. In addition, the thickness of the positive electrode collector may be about 3 μm to 500 μm, and fine irregularities may be formed on the surface of the positive electrode collector to increase the adhesion of the positive electrode active material. For example, the positive electrode collector may be used in various forms such as films, sheets, foils, nets, porous bodies, foams, and nonwovens.
[0092] The positive electrode active material layer may include a known positive electrode active material, a conductive material, and a binder.
[0093] The positive electrode active material includes layered compounds such as lithium cobalt oxide (LiCoO2) and lithium nickel oxide (LiNiO2), or compounds substituted by one or more transition metal elements; lithium manganese oxides such as Li 1+x Mn 2-x O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3 and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5 and Cu2V2O7; 1-x M x Ni-site lithium nickel oxide represented by O2 (wherein M is Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x is 0.01 to 0.3); 2-x M x Lithium manganese composite oxide represented by Li2Mn3MO8 (wherein M is Co, Ni, Fe, Cr, Zn or Ta, and x is 0.01 to 0.1) or Li2Mn3MO8 (wherein M is Fe, Co, Ni, Cu or Zn); LiMn2O4 in which some of the Li in the formula is replaced by alkaline earth metal ions; disulfide compounds; Fe2(MoO4)3, but not limited to these.
[0094] The conductive material is used to impart conductivity to the electrode and can be used without particular limitation as long as it has electronic conductivity without causing chemical changes in the battery to be constructed. Examples include graphite, such as natural or artificial graphite; carbon-based materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powders or metal fibers, such as copper, nickel, aluminum, and silver; conductive whiskers, such as zinc oxide and potassium titanate; conductive metal oxides, such as titanium oxide; conductive polymers, such as polyphenylene derivatives. These can be used alone or in mixtures of two or more thereof. The conductive material may be generally included in an amount of about 1% by weight to 30% by weight, based on the total weight of the positive electrode active material layer.
[0095] Binder is used to enhance the adhesion between positive active material particles and the adhesion between positive active material and positive current collector. Its specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-copolymer-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluorinated rubber or its various copolymers. These can be used alone or in a mixture of two or more thereof. Based on the gross weight of the positive active material layer, the binder can be included in an amount of about 1 weight % to 30 weight %.
[0096] The positive electrode can be manufactured according to a conventional positive electrode manufacturing method. For example, the positive electrode can be manufactured by applying a composition for forming a positive electrode active material layer on a positive electrode current collector, followed by drying and rolling. The composition includes, for example, a positive electrode active material and an optional binder and a conductive material. At this time, the types and contents of the positive electrode active material, the binder and the conductive material are as described above.
[0097] The solvent may be a solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropanol, N-methylpyrrolidone (NMP), acetone, or water, which may be used alone or as a mixture of two or more thereof. Considering the thickness of the slurry and the manufacturing yield, the amount of solvent used is sufficient to dissolve or disperse the positive electrode active material, the conductive material, and the binder, and provide a viscosity that can exhibit good thickness uniformity when subsequently applied to positive electrode production.
[0098] Alternatively, the positive electrode may be manufactured by casting a composition for forming a positive electrode active material layer on a separate support and then laminating a film obtained by peeling from the support on a positive electrode current collector.
[0099] The negative electrode includes a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.
[0100] The negative electrode current collector is a highly conductive material that does not cause chemical changes in the battery, for example, and examples thereof include copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper, or stainless steel surface-treated with carbon, nickel, titanium or silver, and aluminum-cadmium alloys. In addition, the thickness of the negative electrode current collector may be about 3 μm to 500 μm, and similar to the positive electrode current collector, fine irregularities may be formed on the surface of the negative electrode current collector to enhance the binding force of the negative electrode active material. For example, the negative electrode current collector may be used in various forms (e.g., films, sheets, foils, nets, porous bodies, foams, and nonwovens).
[0101] In addition to the negative electrode active material, the negative electrode active material layer optionally contains a binder and a conductive material. The negative electrode active material layer can be prepared by, for example, applying a composition for forming a negative electrode active material layer containing a negative electrode active material and optional binders and coating materials on a negative electrode current collector and drying the composition for forming a negative electrode active material layer, or casting the negative electrode forming composition on a separate support, and then laminating the film obtained by peeling off the support to the negative electrode current collector.
[0102] The negative electrode active material may be any compound capable of reversibly intercalating and deintercalating lithium. Examples include carbon-based materials such as artificial graphite, natural graphite, graphitized carbon fibers, and amorphous carbon; metal compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; metal oxides capable of doping and dedoping lithium, such as SiO β (0<β<2), SnO2, vanadium oxide, lithium vanadium oxide; or a composite material comprising the above metal compound and a carbon-based material, such as a Si-C composite material or a Sn-C composite material, and these can be used alone or as a mixture of two or more thereof. In addition, a metallic lithium film can be used as a negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon can be used as carbon materials. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include amorphous, plate-like, in-plane, spherical or fibrous natural or artificial graphite, crystalline graphite (Kish graphite), pyrolytic carbon, carbon fiber based on mesophase pitch, mesophase carbon microbeads (meso-carbonmicrobeads), mesophase pitch, high-temperature calcined carbon such as coke derived from petroleum or coal tar pitch.
[0103] The binder and conductive material may be the same as those previously described for the positive electrode.
[0104] The separator may be manufactured by immersing a nonwoven fabric substrate formed by mixing the first and second fibers having different average diameters as described above in a slurry containing inorganic particles, or applying such a slurry to the nonwoven fabric substrate and then drying it.
[0105] The nonwoven fabric substrate is formed, for example, by mixing a first fiber and a second fiber having different average diameters, and can be manufactured by spinning the first fiber and the second fiber through a spinning confinement in which a nozzle for spinning the first fiber and a nozzle for spinning the second fiber are arranged to intersect. The nonwoven fabric substrate can be a spunbond nonwoven fabric manufactured using a spunbond device or a meltblown nonwoven fabric manufactured using a meltblown device, but is not limited thereto.
[0106] The slurry containing inorganic particles can be prepared by dispersing the inorganic particles in an aqueous dispersion medium such as water, or an oil-based dispersion medium such as acetone, and further dispersing a particulate binder polymer in the dispersion medium, or further dissolving a binder polymer soluble in the dispersion medium if necessary. When additional binder polymer is added, the binder polymer forms a coating on the surface of the inorganic particles.
[0107] According to the manufacturing method of the electrode assembly according to one aspect of the present disclosure, the electrode assembly can be manufactured by inserting the separator prepared by the above method between the positive electrode and the negative electrode, followed by heating and pressurizing. At this time, the suitable heating temperature can vary according to the glass transition temperature (Tg) and melting point (Tm) of the first fiber, and based on the melting point of the first fiber, the suitable heating temperature can be a temperature of -80°C to +30°C, particularly a temperature of -50°C to +10°C, more particularly a temperature of -30°C to +10°C, and most particularly a temperature of 0°C to +10°C.
[0108] That is, when the separator of the present disclosure is heated and pressurized to the above-mentioned temperature range via a lamination or hot pressing process, a portion of the first fiber of the separator flows and attaches to the electrode, thereby ensuring good adhesion between the electrode interface and the separator, maintaining the hardness of the battery cell even after electrolyte injection, and inhibiting the shape of the battery cell from bending or twisting.
[0109] Meanwhile, a lithium secondary battery according to one aspect of the present disclosure includes the electrode structure as described above.
[0110] The lithium secondary battery includes the above-mentioned electrode structure and an electrolyte. Examples of the electrolyte used in the present disclosure include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited thereto.
[0111] For example, the electrolyte may include an organic solvent and a lithium salt.
[0112] The organic solvent can be used without particular limitation, as long as it can be used as a medium for the migration of ions participating in the electrochemical reaction of the battery. Examples of organic solvents include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone and ε-caprolactone; ether-based solvents such as dibutyl ether and tetrahydrofuran; ketone-based solvents such as cyclohexanone; aromatic hydrocarbon-based solvents such as benzene and fluorobenzene; carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC) and propylene carbonate (PC); alcohol-based solvents such as ethanol and isopropanol; nitriles such as R-CN (wherein R is a linear, branched or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; cyclopentane. Among these, carbonate-based solvents can be used, and a mixture of cyclic carbonates (e.g., ethylene carbonate or propylene carbonate) with high ion conductivity and high dielectric constant that can improve the charge and discharge performance of the battery and a linear carbonate-based compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) with low viscosity can also be used. In this case, excellent electrolyte performance can be obtained by mixing cyclic carbonates and chain carbonates in a volume ratio of about 1:1 to about 1:9.
[0113] The lithium salt can be any compound that can provide the lithium ions used in the lithium secondary battery without particular limitation. Examples of lithium salts include LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, LiB(C2O4)2. The concentration of the lithium salt can be used in the range of about 0.1M to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, which can show good electrolyte performance and can effectively transport lithium ions.
[0114] For the purpose of improving the life characteristics of the battery, suppressing the reduction of the battery capacity, and improving the discharge capacity of the battery, in addition to the above electrolyte components, the electrolyte may also contain one or more additives, such as halogenated alkylene carbonate-based compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, N-glyme, hexanetriamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted Oxazolidinone, N,N-substituted imidazoline, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride. In this case, the additive may be included in an amount of about 0.1 wt % to 5 wt % based on the total weight of the electrolyte.
[0115] The lithium secondary cell or battery according to the present disclosure may be used in the fields of portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0116] Hereinafter, the embodiments of the present disclosure will be described in detail so that those skilled in the art can easily implement the present disclosure. However, the present disclosure can be implemented in many different forms and is not limited to the embodiments described herein.
[0117] Example 1
[0118] First, a high-porosity nonwoven fabric is prepared in which a first fiber having a melting point of 150°C or less and a second fiber having a melting point of 200°C or more are mixed. The nonwoven fabric is spun simultaneously using different nozzles so that the first fiber and the second fiber exist separately. The first fiber having a low melting point melts and is used to combine the electrode and the separator, while the second fiber having a high melting point does not melt at high temperature and is used as a support.
[0119] In this embodiment, the first fiber and the second fiber are melt-spun through a spinneret in which the spinning nozzles have different diameters and are arranged to intersect, thereby preparing a melt-blown nonwoven fabric substrate (porosity 62%) formed by mixing the first fiber having an average diameter of 12 μm and a melting point of 80° C. of a polyester (Chemtexa D1531E) polymer and the second fiber having an average diameter of 0.7 μm and a melting point of 260° C. of a polyethylene terephthalate polymer. In the prepared nonwoven fabric substrate, the mixing weight ratio of the first fiber and the second fiber is 5:5, and the unit area weight of the nonwoven fabric substrate is 10.7 g / m 2 .
[0120] Next, a slurry for coating is prepared. Since inorganic particles alone cannot exist in a bound state in a nonwoven fabric, a polymer binder is added to the slurry so that the inorganic particles are retained in a bound state in the nonwoven fabric. In the case of a slurry for coating, the binder and the inorganic particles are added to a solvent and shaken vigorously using, for example, a shaker to ensure that the inorganic particles and the binder are uniformly dispersed in the solution.
[0121] In this example, 20 g of AlOOH (Nabaltec, D50 290 nm), 0.74 g of polyacrylic acid dispersant solution (solid content 42%) and 20 g of 0.5 mm beads for dispersion were added to 31.1 g of a 95:5 mixture of water and ethanol, and stirred for 2 hours with a paint shaker to prepare an inorganic particle dispersion. Then, 1.04 g of an acrylic polymer (CSB130, Toyoink, Inc.) dispersed in water at 40 wt % was added as a binder component to the inorganic particle dispersion, and shaken to prepare a coating slurry.
[0122] Next, the slurry thus prepared is impregnated onto the nonwoven fabric substrate prepared by the above method using an impregnation method, and then dried to prepare a separator. For this purpose, the coating slurry is placed in a sufficiently large container to fully impregnate the nonwoven fabric, thereby impregnating the nonwoven fabric. A separator in which the pores of the nonwoven fabric are filled with inorganic particles and a binder is prepared by an impregnation process in which the nonwoven fabric is impregnated in a container containing the coating slurry and then taken out of the container.
[0123] The thickness of the prepared separator was 21.2 μm, and the unit area weight of the inorganic particles in the separator was 25.3 g / m 2 , the permeability of the separator is 159 seconds / 100 cubic centimeters.
[0124] Examples 2 to 7
[0125] A separator is prepared as in Example 1, except that the polymer type and melting point of the first fiber and the second fiber, the average diameter, the mixing weight ratio of the first fiber and the second fiber, the porosity and unit area weight of the non-woven fabric substrate, the thickness of the separator, the unit area weight of the inorganic particles, and the permeability are changed according to Table 1.
[0126] Comparative Examples 1 to 7
[0127] A separator is prepared as in Example 1, except that the polymer type and melting point of the first fiber and the second fiber, the average diameter, the mixing weight ratio of the first fiber and the second fiber, the porosity and unit area weight of the non-woven fabric substrate, the thickness of the separator, the unit area weight of the inorganic particles, and the permeability are changed according to Table 1.
[0128] <Average fiber diameter>
[0129] In this specification, the average diameter of the fibers is defined as measured as follows.
[0130] Nonwoven fabric sample is fixed to the support for SEM measurement using carbon tape.Then, use ion sputtering instrument to carry out Pt coating 60 seconds to the surface.Use FE-SEM (Hitachi S-4800) instrument to measure the sample through Pt coating under 10kV condition.Use software, in the × 500 image observed with FE-SEM, the diameter of a fiber bundle is measured at more than 10 points, and the fiber diameter is calculated by averaging the measured value.
[0131] <Measurement of Melting Point of Fiber>
[0132] In this specification, the melting point of the fiber is defined as measured as follows.
[0133] The "melting point" of the first fiber and the second fiber constituting the nonwoven fabric is measured by differential scanning calorimetry (DSC) as a temperature at which a peak appears due to endothermic absorption at a certain temperature when the temperature is increased from -30°C to 200°C at a constant rate of 10°C / min.
[0134] <Measurement of D50 of Inorganic Particles>
[0135] In this specification, D50 of the inorganic particles is defined according to measurement using a laser diffraction particle size measuring device.
[0136] For example, the D50 of the inorganic particles is measured using a Malvern MASTERSIZER 3000 laser diffraction particle size measuring device.
[0137] <Weight per unit area of nonwoven fabric and inorganic particles>
[0138] In the present specification, the weight per unit area of the nonwoven fabric and the inorganic particles is defined as measured as follows.
[0139] The weight per unit area of nonwoven fabric is 2 The weight per unit area of the inorganic particles in the separator is measured for the prepared nonwoven fabric, and is obtained by measuring the weight per unit area of the separator and then subtracting the weight per unit area of the nonwoven fabric used.
[0140] <Permeability of Separator>
[0141] In this specification, the permeability of a separator is defined as measured as follows.
[0142] The permeability of the separator is measured according to JIS P8117.
[0143] <Evaluation of Adhesion and Insulation Properties of Separator>
[0144] Evaluation of adhesion
[0145] The negative electrode slurry was prepared by mixing natural graphite, carbon black, carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) with water in a weight ratio of 96:1:2:2. The negative electrode slurry was coated on a copper foil (Cu-foil) with a capacity of 3.55 mAh / g to form a thin electrode plate, dried at 135°C for 3 hours or more, and then pressed to prepare a negative electrode.
[0146] The prepared negative electrode was cut into a size of 25mm×100mm. The separators prepared in the embodiments and comparative examples were cut into a size of 25mm×100mm. Each separator and the negative electrode were overlapped and sandwiched between 100μm PET films and then combined using a flat press. At this time, the conditions of the flat press were heated and pressed at 70°C and a pressure of 600kgf for 20 seconds. The combined separator and the negative electrode were attached to the slide glass using a double-sided tape. The end of the adhesive side of the separator (10mm or less from the end of the adhesive side) was peeled off and attached in the longitudinal direction using a 25mm×100mm PET film and a single-sided adhesive tape. Thereafter, the slide glass was mounted on the lower holder of the UTM instrument (LLOYD Instrument LF Plus), and the PET film attached to the separator was then mounted on the upper holder of the UTM instrument. Then, the force required to peel off the negative electrode and the porous coating opposite to the negative electrode was measured by applying force at 180° at a measuring speed of 300mm / min.
[0147] Evaluation of insulation breakdown voltage
[0148] The separator samples prepared in the examples and comparative examples were placed between aluminum fixtures (upper fixture diameter 30 mm, lower fixture 50×100 mm), and the voltage when short circuit occurred was measured using a Hi-pot tester. At this time, the measurement conditions were set to DC, 0.5 mA current and 100 V / sec voltage rise (up to 3 kV).
[0149] Table 1
[0150]
[0151] As shown in Tables 1 and 2, Comparative Example 1 using the nonwoven fabric made of only the first fiber had poor insulation and it was difficult to control the thickness.
[0152] Comparative Example 2 using the nonwoven fabric made of only the second fiber, Comparative Examples 3 and 5 using small diameter fibers as the first fiber, and Comparative Example 7 using polypropylene (PP) fibers having a high melting point as the first fiber had low adhesiveness.
[0153] Comparative Example 4 using inorganic particles having a large D50 as inorganic particles and Comparative Example 6 using large-diameter fibers as second fibers had poor insulation properties.
Claims
1. A separator, comprising: A nonwoven fabric substrate formed by mixing first fibers having an average diameter of 10 μm or more and second fibers having an average diameter of 1 μm or less; and Inorganic particles positioned in pores formed between the first fibers and the second fibers of the nonwoven fabric substrate, The melting point of the first fiber is 150° C. or lower, and the D50 of the inorganic particles is 400 nm or less. 2 . The separator according to claim 1 , wherein a mixing weight ratio of the first fibers to the second fibers is 1:9 to 9:
1. 3 . The separator according to claim 1 , wherein an average diameter of the first fibers is 10 μm to 30 μm, and an average diameter of the second fibers is 0.1 μm to 1 μm. The separator according to claim 1 , wherein D50 of the inorganic particles is 30 nm to 400 nm. The separator according to claim 1 , wherein the first fibers have a melting point of 50° C. to 120° C.
6. The separator of claim 1, wherein the first fibers are formed of one or more polymers selected from the group consisting of polyamide, polyester, thermoplastic polyurethane, and ethylene vinyl acetate copolymer. The separator according to claim 1 , wherein the second fiber has a melting point of 200° C. or higher.
8. The separator according to claim 7, wherein the second fibers are formed of one or more polymers selected from the group consisting of polyethylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, and polyethylene naphthalene. 9 . The separator according to claim 1 , wherein a thickness of the separator is 10 μm to 30 μm.
10. The separator according to claim 1, wherein the nonwoven fabric substrate has a unit area weight of 5 g / m 2 Up to 30g / m 2 , and the weight per unit area of the inorganic particles is 10 g / m 2 Up to 50g / m 2 . 11 . The separator according to claim 1 , wherein the separator has a permeability of 1 sec / 100 cm 3 to 300 sec / 100 cm 3 . 12 . The separator according to claim 1 , wherein the inorganic particles are coated with a binder polymer on at least a portion of a surface thereof.
13. A method for preparing a separator for a lithium secondary battery, the method comprising: forming a nonwoven fabric substrate from a mixture of first fibers and second fibers having different predetermined diameter ranges; as well as providing inorganic particles in the pores formed between the first fibers and the second fibers, wherein the average diameter of the first fibers is adjusted to 10 μm or more, and the average diameter of the second fibers is adjusted to 1 μm or less, and A fiber material having a melting point of 150° C. or less is used as the first fiber, and the D50 of the inorganic particles is controlled to be less than 400 nm.
14. The method of claim 13, wherein the first fibers are formed from one or more polymers selected from the group consisting of polyamides, polyesters, thermoplastic polyurethanes, and ethylene vinyl acetate copolymers.
15. The method according to claim 14, wherein the second fiber is a fiber having a melting point of 200°C or higher.
16. The method of claim 15, wherein the second fiber is formed from one or more polymers selected from the group consisting of polyethylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, and polyethylene naphthalene.
17. An electrode assembly comprising: positive electrode; negative electrode; as well as The separator according to any one of claims 1 to 12 provided between the positive electrode and the negative electrode.
18. A method for manufacturing an electrode assembly, the method comprising: Prepare a separator according to any one of claims 1 to 12; as well as The separator is inserted between the positive electrode and the negative electrode, followed by heating and pressurizing at a temperature range of -80°C to +30°C based on the melting point of the first fiber.
19. A lithium secondary battery comprising the electrode assembly according to claim 17.