Composite membrane material as well as preparation method and application thereof

By designing composite membrane materials, combining the structural parameters of the inner and outer membranes and the addition of nanoparticles, the shortcomings of the existing MABR membrane materials in oxygen mass transfer efficiency and microbial membrane hanging effect are solved, and efficient wastewater treatment is achieved.

CN118976386APending Publication Date: 2024-11-19CHINA THREE GORGES CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411053077.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing MABR film materials have shortcomings in oxygen mass transfer efficiency and microbial membrane hanging effect. The hydrophobic microporous membrane has high oxygen mass transfer efficiency but poor microbial membrane hanging effect, low oxygen mass transfer efficiency of hydrophilic dense membrane and good microbial membrane hanging effect , but it is difficult to meet the needs of complex sewage treatment.

Method used

Composite membrane materials are used, including inner membrane and outer membrane. The inner membrane has an inner diameter of 300-450 μm, a porosity of 0.1-0.5 μm, a porosity of 45%-80%, an outer membrane thickness of no more than 5 μm, and a porosity of 30%- 60%, the surface contact angle is less than 70°, and magnetic nanoparticles, hydrophilic silane solvents and polyalkyl siloxane solvents are added to the outer membrane to form a high oxygen mass transfer efficiency and easy microbial hanging through a specific preparation method. Film material.

Benefits of technology

It achieves high oxygen mass transfer efficiency and good microbial membrane hanging effect, improves the sewage treatment efficiency and stability of the MABR system, avoids the problem of blockage of oxygen flux, and enhances the bioaffinity and mechanical properties of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976386A_ABST
    Figure CN118976386A_ABST
Patent Text Reader

Abstract

The invention provides a composite membrane material as well as a preparation method and application thereof. The invention provides a composite membrane material which comprises an inner membrane and an outer membrane, the inner diameter of the inner membrane is 300-450 [mu] m, the thickness is not more than 100 [mu] m, the aperture is 0.1-0.5 [mu] m, and the porosity is 45-80%; the thickness of the outer film is not larger than 5 microns, the porosity is 30%-60%, the surface contact angle is smaller than 70 degrees, and the roughness is 50-140 nm. The composite membrane material disclosed by the invention has the characteristics of high oxygen mass transfer efficiency and easiness in biofilm formation of microorganisms.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of filtration membranes, and in particular to a composite membrane material and a preparation method and application thereof. Background Art

[0002] Membrane Aeration Biofilm Reactor (MABR) is an emerging low-carbon technology for sewage and wastewater treatment. In the MABR system, the microbial membrane is attached to the surface of the oxygen-permeable hollow fiber MABR membrane. When the sewage flows around the membrane, the pollutants enter the microbial membrane under the action of concentration gradient and microbial adsorption. In the microbial membrane, through the metabolism and proliferation of microorganisms, the pollutants are converted into inorganic substances or fixed in the microorganisms, thereby achieving water purification.

[0003] In the MABR system, the MABR membrane, as the core part of the system, not only needs to have good oxygen mass transfer efficiency, but also needs to be easy for microorganisms to form biofilms. At present, the commonly used MABR membrane materials are hydrophobic microporous membranes, hydrophilic dense membranes and composite membranes. Hydrophobic microporous membranes have high oxygen mass transfer efficiency because oxygen molecules are transferred through the micropores inside them, but their surface is hydrophobic, resulting in poor microbial biofilm effect. In addition, during the long-term use of hydrophobic microporous membranes, solutions and impurities are easy to enter the micropores, causing blockage, which has a great impact on oxygen flux; the surface of hydrophilic dense membranes is hydrophilic, so it is conducive to microbial biofilm formation, but oxygen diffuses through the membrane through molecules, and the oxygen mass transfer efficiency is poor; composite membranes are a thin dense layer covering the surface of hydrophobic microporous membranes. The composite membranes combine the performance of hydrophobic microporous membranes and dense membranes. While ensuring oxygen mass transfer efficiency, they also have microbial biofilm effect. However, with the increasing difficulty of sewage treatment, higher requirements are also put forward for the oxygen mass transfer efficiency and microbial biofilm effect of MABR membrane materials. Summary of the invention

[0004] The invention provides a composite membrane material, which has the advantages of high oxygen mass transfer efficiency and easy microbial biofilm formation.

[0005] The invention also provides a preparation method and application of the composite membrane material.

[0006] A first aspect of the present invention provides a composite membrane material, which comprises an inner membrane and an outer membrane;

[0007] The inner membrane has an inner diameter of 300 to 450 μm, a thickness of no more than 100 μm, a pore size of 0.1 to 0.5 μm, and a porosity of 45% to 80%;

[0008] The thickness of the outer film is not higher than 5 μm, the porosity is 30% to 60%, the surface contact angle is less than 70°, and the roughness is 50 to 140 nm.

[0009] According to the above composite film material, wherein the outer film comprises magnetic nanoparticles, a hydrophilic silane solvent and a polyalkylsiloxane solvent.

[0010] According to the above-mentioned composite film material, the mass ratio of the magnetic nanoparticles, the hydrophilic silane solvent and the polyalkylsiloxane solvent is (1-20): (5-18): (20-40).

[0011] According to the above composite film material, the average particle size of the magnetic nanoparticles is 20 to 100 nm.

[0012] According to the above-mentioned composite film material, the magnetic nanoparticles include at least one of Fe3O4 nanoparticles, Fe2O3 nanoparticles, and Fe2O3-Al2O3 composite nanoparticles.

[0013] According to the above composite membrane material, wherein the inner membrane is one of polyvinylidene fluoride membrane, polyethylene membrane, polytetrafluoroethylene membrane and polypropylene membrane.

[0014] According to the above composite membrane material, wherein the hydrophilic silane solvent includes one or two of Y-aminopropyltrimethoxysilane and methyltrimethoxysilane;

[0015] And / or, the polyalkylsiloxane solvent includes one or both of polymethylsiloxane and polydimethylsiloxane.

[0016] A second aspect of the present invention provides a method for preparing a composite membrane material, comprising the following steps:

[0017] At a pH of 8 to 9, the magnetic nanoparticle solution, the polyalkylsiloxane solvent and the cosolvent are mixed in a mass ratio of (12% to 30%): (60% to 80%): (1% to 8%) to obtain a coating solution, wherein the mass concentration of the magnetic nanoparticle solution is 5% to 10%;

[0018] The inner membrane is placed in the coating solution, soaked for 3 to 8 minutes, then taken out and subjected to curing treatment.

[0019] According to the above preparation method, before placing the inner membrane in the coating solution, the inner membrane is also immersed in an organic solvent for 3 to 5 minutes, then washed in clean water for 3 to 5 minutes, and dried to remove the residual moisture in the inner membrane.

[0020] A third aspect of the present invention provides a MABR system, which includes the above-mentioned composite membrane material or the composite membrane material obtained according to the above-mentioned preparation method.

[0021] The composite membrane material of the invention comprises an inner membrane and an outer membrane. By controlling the performance parameters of the inner and outer membranes, the composite membrane material has the characteristics of high oxygen mass transfer efficiency and easy microbial biofilm formation. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0023] Figure 1 It is a schematic cross-sectional view of a composite membrane material provided in one embodiment of the present invention. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] A first aspect of the present invention provides a composite membrane material, which comprises an inner membrane and an outer membrane;

[0026] The inner membrane has an inner diameter of 300 to 450 μm, a thickness of no more than 100 μm, a pore size of 0.1 to 0.5 μm, and a porosity of 45% to 80%;

[0027] The thickness of the outer film is not higher than 5 μm, the porosity is 30% to 60%, the surface contact angle is less than 70°, and the roughness is 50 to 140 nm.

[0028] The composite membrane material of the present invention is used for water purification, and its cross-sectional schematic diagram is as follows Figure 1 As shown, the inner membrane is a hollow fiber membrane, oxygen / air is input from one end of the inner membrane and output from the other end; the outer membrane is attached to the inner membrane, forming the composite membrane material of the present invention. When the composite membrane material is placed in a polluted water body, microorganisms will attach to the outer membrane to form a microbial membrane. The oxygen / air input from one end of the inner membrane penetrates into the outer membrane through the pores of the inner membrane and supplies the microorganisms on the outer membrane.

[0029] The inner diameter of the inner membrane is 300-450 μm. When it is higher than 450 μm, there are the following adverse effects: (1) Reduced oxygen transfer efficiency: The surface area of ​​the membrane filaments is relatively small, resulting in a weakened oxygen transfer capacity per unit area, affecting the effective utilization rate of oxygen in the MABR system and reducing the biological treatment efficiency. (2) Reduced biofilm surface area: Thicker inner membrane filaments will result in a thicker overall membrane diameter, a smaller membrane surface area, and a reduced attachment area of ​​the biofilm on its surface. The biofilm is a key component in the MABR system, and the reduction in its attachment area will affect the efficiency and stability of wastewater treatment. (3) Reduced load-bearing capacity: Thicker membrane filaments may not be strong or stable enough to withstand the required biological load or operating conditions (such as water pressure, mechanical stress, etc.), which may cause damage to the membrane or shorten its life. When it is lower than 300 μm, there are the following adverse effects: (1) Reduced mechanical strength: Too thin a membrane filament diameter means that the thickness of the overall membrane material is also reduced accordingly, thereby reducing the mechanical strength and durability of the membrane, which will increase the risk of damage or rupture of the membrane during operation. (2) Reduced gas transfer efficiency: Too thin membrane filaments may limit the speed and efficiency of air or oxygen passing through the membrane, thereby reducing the gas transfer efficiency in the MABR system and affecting the efficiency and stability of the biological process. (3) Increased manufacturing costs: Too thin membrane filaments usually require a higher precision manufacturing process and more complex assembly and installation techniques, which may increase the manufacturing cost of the membrane and the overall cost of the system.

[0030] The thickness of the inner membrane is not higher than 100 μm. When it is higher than 100 μm, the thickness is too large and affects the mass transfer efficiency of oxygen / air from the inner membrane to the outer membrane.

[0031] The pore size of the inner membrane is 0.1-0.5 μm, and the porosity is 45%-80%, which ensures that the inner membrane has pores of appropriate size so that oxygen / air can penetrate into the outer membrane through the pores of the inner membrane;

[0032] The thickness of the outer membrane is not higher than 5 μm. When it is higher than 5 μm, it will affect the mass transfer efficiency of oxygen / air from the outer membrane to the microbial membrane.

[0033] The porosity of the outer membrane is 30% to 60%, which ensures that oxygen / air from the inner membrane can penetrate into the outer membrane while preventing impurities in the water from entering the pores of the outer membrane and causing blockage.

[0034] The contact angle of the outer membrane surface is less than 70°; the roughness of the outer membrane is 50-140nm. When it is greater than 140nm, it has the following effects: (1) Increased biofilm attachment: Although a rougher surface provides more surface area and microstructure, this may increase the adhesion capacity of biofilms and microorganisms. This will lead to premature formation of biofilms and excessive biofilm thickness, reducing gas transfer efficiency and wastewater treatment efficiency. (2) Increased resistance: A rougher surface will increase the friction resistance of water flowing through the membrane, thereby increasing energy consumption. This will increase the operating cost of the system and may require more energy to maintain the required water flow rate.

[0035] When the roughness is less than 50nm, the following effects occur: (1) Difficulty in microbial attachment: Too smooth a membrane surface is difficult to provide sufficient surface area and structure to support effective microbial attachment and biofilm formation. (2) Decreased reactor performance: When the membrane surface roughness is less than 50nm, microbial attachment to the membrane surface is insufficient, reducing the reactor's treatment efficiency and capacity, especially under long-term operation and high-load conditions.

[0036] The composite membrane material of the present invention ensures that oxygen / air can penetrate smoothly from the inner membrane to the outer membrane by controlling the thickness and porosity of the inner and outer membranes. At the same time, the surface contact angle of the outer membrane is less than 70°, which is hydrophilic and has a specific roughness, which is conducive to the attachment of microorganisms to the outer membrane. Therefore, the composite membrane material has the characteristics of high oxygen mass transfer efficiency and easy microbial biofilm formation.

[0037] In a specific embodiment, the inner membrane is one of polyvinylidene fluoride membrane (PVDF), polyethylene membrane (PE), polytetrafluoroethylene membrane (PTFE), and polypropylene membrane (PP).

[0038] Preferably, the inner membrane is one of a polyvinylidene fluoride membrane (PVDF) and a polytetrafluoroethylene membrane (PTFE).

[0039] In a specific embodiment, the outer film includes magnetic nanoparticles, a hydrophilic silane solvent and a polyalkylsiloxane solvent.

[0040] The magnetic nanoparticles in the present invention are nano-scale particles, generally composed of a magnetic core composed of metal oxide and a high molecular polymer shell wrapped outside the magnetic core, and the average particle size is 20-100nm.

[0041] When the outer membrane includes magnetic nanoparticles, hydrophilic silane solvents and polyalkylsiloxane solvents, the outer membrane can meet the above conditions. In addition, when the outer membrane includes magnetic nanoparticles, the bioaffinity of the outer membrane is further increased. The inventors speculate that this may be due to the magnetic nanoparticles having magnetic properties, special electrical properties and biocompatibility.

[0042] In a specific embodiment, the magnetic nanoparticles include at least one of Fe3O4 nanoparticles, Fe2O3 nanoparticles, and Fe2O3-Al2O3 composite nanoparticles.

[0043] Preferably, the magnetic nanoparticles include Fe3O4 nanoparticles.

[0044] In a specific embodiment, the average particle size of the magnetic nanoparticles is 20 to 100 nm.

[0045] Magnetic nanoparticles smaller than 20nm are prone to agglomeration, resulting in poor loading effect; magnetic nanoparticles larger than 100nm may affect the pore size and permeability of the composite membrane material, thereby affecting the oxygen mass transfer effect.

[0046] Furthermore, the magnetic nanoparticles are spherical.

[0047] The spherical magnetic nanoparticles, whose concave-convex structures formed on the membrane surface, provide more attachment sites and surface energy, which helps microorganisms form a more stable and uniform biofilm on the membrane surface. This can not only increase the amount of biological attachment of the biofilm, but also improve the stability and activity of biological attachment; at the same time, spherical magnetic nanoparticles usually have a very uniform shape and size distribution, which makes it easier to control during the preparation process, which is conducive to improving the stability and consistency of the outer membrane material. In addition, spherical nanoparticles have a higher specific surface area and a larger surface energy, which is more biocompatible than non-spherical nanoparticles, which helps to enhance the biofilm effect on the surface of the nanoparticle membrane.

[0048] In a specific embodiment, the hydrophilic silane solvent includes one or both of Y-aminopropyltrimethoxysilane and methyltrimethoxysilane;

[0049] The polyalkylsiloxane solvent includes one or both of polymethylsiloxane (PMS) and polydimethylsiloxane (PDMS).

[0050] The silicon-oxygen bonds of the hydrophilic silane solvents have a strong binding force with the magnetic nanoparticles, and are used to improve the adhesion and durability between the hydrophilic silane solvents and the magnetic nanoparticles, as well as the compatibility with the inner membrane.

[0051] Polyalkylsiloxane solvents have a structure in which multiple alkyl groups are connected to silicon-oxygen bonds. They are used to improve the water resistance of the outer film coating, enhance the wear resistance, and enhance the adhesion of magnetic nanomaterials in the outer film material, so that the magnetic nanoparticles can be more stably integrated in the outer film organic matrix. At the same time, polyalkylsiloxane can be used as a protective agent, coated on the surface of the inner film to form a protective film to prevent corrosion, pollution and oxidation.

[0052] Furthermore, the hydrophilic silane solvent includes γ-aminopropyltrimethoxysilane.

[0053] Furthermore, in a specific embodiment, the mass ratio of the magnetic nanoparticles, the hydrophilic silane solvent and the polyalkylsiloxane solvent is (1-20): (5-18): (20-40).

[0054] The outer film and the inner film can have appropriate adhesion to prevent the outer film from falling off; at the same time, the outer film can have certain mechanical properties and adhesion of magnetic nanoparticles to prevent the composite membrane material from breaking and the magnetic nanoparticles from falling off, and will not affect the efficient oxygen mass transfer performance of the inner film itself.

[0055] The second aspect of the present invention provides a method for preparing the above-mentioned composite membrane material, comprising the following steps:

[0056] At a pH of 8 to 9, the magnetic nanoparticle solution, the polyalkylsiloxane solvent and the cosolvent are mixed in a mass ratio of (12% to 30%): (60% to 80%): (1% to 8%) to obtain a coating solution, wherein the mass concentration of the magnetic nanoparticle solution is 5% to 10%;

[0057] The inner membrane is placed in the coating solution, soaked for 3 to 8 minutes, then taken out and subjected to curing treatment.

[0058] In a specific embodiment, the above method comprises the following steps:

[0059] Step 1: At a pH of 8 to 9, the magnetic nanoparticle solution, polyalkylsiloxane solvent and co-solvent are mixed in a mass ratio of (12% to 30%): (60% to 80%): (1% to 8%) to obtain a coating solution, wherein the mass concentration of the magnetic nanoparticle solution is 5% to 10%.

[0060] The magnetic nanoparticles are dispersed in a hydrophilic silane solvent to prepare a magnetic nanoparticle solution with a mass concentration of 5% to 10%.

[0061] In order to evenly disperse the magnetic nanoparticles in the solution, magnetic stirring, ultrasound and the like can be used.

[0062] At a pH of 8 to 9, the magnetic nanoparticle solution, polyalkylsiloxane solvent and co-solvent are uniformly mixed in a mass ratio of (12% to 30%): (60% to 80%): (1% to 8%) to obtain a coating solution.

[0063] Similarly, in order to mix the above three solutions evenly, heating, magnetic stirring and ultrasound can be used.

[0064] Furthermore, the heating temperature is 30-60°C; the ultrasonic intensity is 100-350W / cm 2 , ultrasonic frequency is 20-30kHz; magnetic stirring speed is 60-120r / min, and stirring time is 6h-12h.

[0065] The co-solvent of the present invention is a conventional organic solvent in the art, such as alcohols, ethers, esters, ketones, and aromatic hydrocarbons.

[0066] Step 2: placing the inner membrane in the coating solution, soaking for 3 to 8 minutes, then taking it out and performing a curing treatment.

[0067] The inner membrane is immersed in the coating solution for 3-8 minutes, then pulled up, and then cured to obtain a composite membrane material.

[0068] The curing method of the present invention can be one or both of heat treatment and ultraviolet irradiation. The curing process can improve the stability and durability of the outer film and reduce the risk of the outer film falling off and being contaminated.

[0069] By controlling the immersion time of the inner membrane in the coating solution, the thickness of the outer membrane can be controlled to ensure that the magnetic nanoparticles can be firmly attached to the surface of the inner membrane. At the same time, the outer membrane cannot be too thick to avoid adverse effects on the gas transmission and water diffusion properties of the outer membrane.

[0070] In a specific embodiment, before placing the inner membrane in the coating solution, the inner membrane is also immersed in an organic solvent for 3 to 5 minutes, then washed in clean water for 3 to 5 minutes, and dried to remove the residual moisture in the inner membrane.

[0071] The above-mentioned organic solvent is a conventional organic solvent in the art, such as acetone, ethanol, isopropanol, toluene, etc.

[0072] The above treatment of the inner film can remove impurities in the inner film, ensure the cleanliness, smoothness and dryness of the inner film surface, provide a good basis for coating the outer film, improve the coating effect, and ensure the uniformity, adhesion and stability of the outer film.

[0073] It is understandable that, depending on the content of impurities in the inner membrane and the difficulty of removing them, the above treatment can be repeated on the inner membrane.

[0074] The third aspect of the present invention provides a MABR system, comprising the above-mentioned composite membrane material or the composite membrane material obtained according to the above-mentioned preparation method.

[0075] The solution provided by the present invention is further described below in conjunction with specific embodiments.

[0076] Example 1

[0077] The method for preparing the composite membrane material of this embodiment comprises the following steps:

[0078] (1) A PVDF membrane is used as the inner membrane of the composite membrane material. The inner diameter of the PVDF membrane is 360 μm, the inner membrane thickness is 80 μm, the pore size is 0.35 μm, and the porosity is 64%.

[0079] The PVDF inner membrane was immersed in acetone for 3 minutes, then washed in clean water for 3 minutes, and repeated twice. The residual water on the surface of the PVDF inner membrane was removed by vacuum drying to obtain a pretreated PVDF inner membrane.

[0080] (2) A solution of magnetic Fe3O4 nanoparticles with a mass concentration of 10% was prepared, the solvent was γ-aminopropyltrimethoxysilane, and the average particle size of the magnetic Fe3O4 nanoparticles was 40 nm.

[0081] At a pH of 8 to 9, a solution of magnetic Fe304 nanoparticles, a PMS solvent and a co-solvent ethanol are uniformly mixed in a mass ratio of 28%:70%:2% to obtain a coating solution.

[0082] (3) The pretreated PVDF inner membrane is immersed in the coating solution, and then pulled after immersion for 5 minutes, and then heat-treated to form an outer membrane on the surface of the PVDF inner membrane, wherein the magnetic F e3 The mass ratio of O4 nanoparticles, γ-aminopropyltrimethoxysilane and PMS solvent is 1:9:25, and the composite membrane material of this embodiment is obtained.

[0083] Example 2

[0084] The method for preparing the composite membrane material of this embodiment comprises the following steps:

[0085] (1) A PTFE membrane is used as the inner membrane of the composite membrane material. The inner diameter of the PTFE membrane is 380 μm, the thickness is 70 μm, the pore size is 0.5 μm, and the porosity is 70%.

[0086] The PTFE inner membrane was immersed in toluene for 4 minutes, and then washed in clean water for 4 minutes, and this process was repeated twice. The residual water on the surface of the PTFE inner membrane was removed by vacuum drying to obtain a pretreated PTFE inner membrane.

[0087] (2) Preparation of magnetic F with a mass concentration of 6% e3 A solution of O4 nanoparticles, the solvent is methyltrimethoxysilane, magnetic F e3 The average particle size of O4 nanoparticles is 50 nm.

[0088] At a pH of 8 to 9, a solution of magnetic Fe304 nanoparticles, a PDMS solvent and a co-solvent ether were uniformly mixed in a mass ratio of 30%:65%:5% to obtain a coating solution.

[0089] (3) The pretreated PTFE inner membrane is immersed in the coating solution, and then pulled up after immersion for 6 minutes, and then subjected to UV treatment to form an outer membrane on the surface of the PVDF inner membrane, wherein the mass ratio of magnetic Fe3O4 nanoparticles, methyltrimethoxysilane and PDMS solvent is 1:16:36, thereby obtaining the composite membrane material of this embodiment.

[0090] Example 3

[0091] The method for preparing the composite membrane material of this embodiment comprises the following steps:

[0092] (1) A PTFE membrane is used as the inner membrane of the composite membrane material. The inner diameter of the PTFE membrane is 450 μm, the thickness is 80 μm, the pore size is 0.45 μm, and the porosity is 75%.

[0093] The PTFE inner membrane was immersed in isopropanol for 3 minutes, and then washed in clean water for 2 minutes, and the process was repeated once. The residual water on the surface of the PTFE inner membrane was removed by vacuum drying to obtain a pretreated PTFE inner membrane.

[0094] (2) A solution of magnetic Fe3O4 nanoparticles with a mass concentration of 8% was prepared, the solvent was Y-aminopropyltrimethoxysilane, and the average particle size of the magnetic Fe3O4 nanoparticles was 60 nm.

[0095] At a pH of 8 to 9, a solution of magnetic Fe304 nanoparticles, a PMS solvent and a co-solvent acetone were uniformly mixed in a mass ratio of 28%:67%:5% to obtain a coating solution.

[0096] (3) The pretreated PTFE inner membrane is immersed in the coating solution for 3-8 minutes, then pulled up and subjected to UV treatment to form an outer membrane on the surface of the PVDF inner membrane, wherein the mass ratio of magnetic Fe3O4 nanoparticles, γ-aminopropyltrimethoxysilane and PMS solvent is 1:12:30, thereby obtaining the composite membrane material of this embodiment.

[0097] Example 4

[0098] This embodiment is basically consistent with Embodiment 3, except that in step (2), the magnetic Fe3O4 nanoparticles are replaced by magnetic Fe2O3 nanoparticles.

[0099] Example 5

[0100] This embodiment is basically consistent with Embodiment 3, except that in step (2), the magnetic Fe3O4 nanoparticles are replaced by magnetic Fe2O3-Al2O3 composite nanoparticles.

[0101] Comparative Example 1

[0102] The preparation method of the composite membrane material in this comparative example comprises the following steps:

[0103] (1) A PVDF membrane is used as the inner membrane of the composite membrane material. The inner diameter of the PVDF membrane is 200 μm, the thickness is 100 μm, the pore size is 0.1 μm, and the porosity is 45%.

[0104] The PVDF inner membrane was immersed in acetone for 3 minutes, then washed in clean water for 3 minutes, and repeated twice. The residual water on the surface of the PVDF inner membrane was removed by vacuum drying to obtain a pretreated PVDF inner membrane.

[0105] (2) At a pH of 8, γ-aminopropyltrimethoxysilane solvent, PMS solvent and ethanol were uniformly mixed in a mass ratio of 28%:70%:2% to obtain a coating solution.

[0106] (3) The pretreated PVDF inner membrane is immersed in a coating solution, and then pulled up after immersion for 5 minutes, and then heat-treated to obtain a composite membrane material.

[0107] Comparative Example 2

[0108] The preparation method of the composite membrane material in this comparative example comprises the following steps:

[0109] (1) A PTFE membrane is used as the inner membrane of the composite membrane material. The inner diameter of the PTFE membrane is 250 μm, the thickness is 120 μm, the pore size is 0.6 μm, and the porosity is 40%.

[0110] The PTFE inner membrane was immersed in toluene for 2 minutes, and then washed in clean water for 3 minutes, and the process was repeated once. The residual water on the surface of the PTFE inner membrane was removed by vacuum drying to obtain a pretreated PTFE inner membrane.

[0111] (2) A solution of magnetic Fe3O4 nanoparticles with a mass concentration of 6% was prepared, the solvent was Y-aminopropyltrimethoxysilane, and the average particle size of the magnetic Fe3O4 nanoparticles was 50 nm.

[0112] At a pH of 8 to 9, a solution of magnetic Fe304 nanoparticles, a PDMS solvent and diethyl ether were uniformly mixed in a mass ratio of 15%:80%:5% to obtain a coating solution.

[0113] The pretreated PTFE inner membrane is immersed in the coating solution, and then pulled after immersion for 5 minutes, and then heat-treated to obtain a composite membrane material.

[0114] Comparative Example 3

[0115] The membrane material of this comparative example only includes the PTFE membrane in Example 3.

[0116] Comparative Example 4

[0117] This comparative example is basically consistent with Example 3, except that a PTFE membrane is used as the inner membrane of the composite membrane material, the inner diameter of the PTFE membrane is 250 μm, the thickness is 100 μm, the pore size is 0.4 μm, and the porosity is 45%.

[0118] Comparative Example 5

[0119] This comparative example is basically consistent with Example 3, except that the mass concentration of the solution of magnetic Fe3O4 nanoparticles is 2%; when preparing the coating solution, the mass ratio of the solution of magnetic Fe3O4 nanoparticles, PMS solvent and co-solvent is 2:17:1.

[0120] Experimental example

[0121] The porosity, surface roughness, contact angle, oxygen transfer performance, number of days for microbial film attachment, membrane surface loading, nitrification reaction rate and outer membrane thickness of the composite membrane materials prepared in the examples and comparative examples were tested. The test results are shown in Table 1.

[0122] Porosity test method: A method for measuring surface roughness based on scanning probe technology using an atomic force microscope (AFM). In the experiment, during the surface scanning process, AFM obtains surface topography information through the interaction force between the probe and the membrane surface, thereby obtaining the surface roughness.

[0123] Surface roughness test method: Atomic force microscopy (AFM) was used to measure the surface roughness.

[0124] Contact angle test method: Use a contact angle meter to measure the contact angle between distilled water or ultrapure water drops when they reach equilibrium on the surface of the film sample, and determine the wetting tension of the film by converting the contact angle and wetting tension. Analyze the contours of liquid and solid samples by the principle of optical appearance projection. When the liquid forms droplets on the film surface and reaches equilibrium, the angle between the tangent line of the gas-liquid-solid interface and the solid-liquid boundary line is the intersection point of the gas-liquid-solid three-phase, which is the tangent line of the gas-liquid interface.

[0125] Test method for oxygen transfer performance: Calculate according to the following formula.

[0126]

[0127]

[0128] Where OTE is the oxygen transfer efficiency, that is, the proportion of oxygen in the air supplied to the MABR membrane module transferred to the biofilm, %;

[0129] O 2,inis the percentage of oxygen in the air entering the MABR membrane cavity, and the constant value is 20.9%;

[0130] O 2,out is the percentage of oxygen in the tail gas of the MABR membrane module, %;

[0131] F V is the volume loss coefficient;

[0132] OTR is oxygen transfer rate, g O2 / m 2 / h;

[0133] Q air is the air flow rate, L / h;

[0134] 32 is the relative molecular mass of oxygen;

[0135] 22.4 is the standard molar volume constant of the gas;

[0136] S bf is the MABR biofilm area, m 2 .

[0137] Test method for days of biofilm attachment: Due to the obstruction of water flow by hollow fiber membrane, the mixed liquid (sludge) first quickly forms a thicker microbial film on the outer surface of the entire membrane assembly. With the flushing of water flow and the full mixing of reaction, the microorganisms are dispersed to the membrane surface of the entire membrane assembly (reversible attachment), and the excess sludge is suspended in the water and eventually overflows the reactor. With the mixing and flushing of water flow, the microorganisms increase in value, the overly thick biofilm falls off, the loose biofilm tends to be dense, and the uniformly distributed biofilm formed in the early stage of biofilm attachment is an irreversibly attached biofilm. Continue to operate and observe the removal effect of the reactor on pollutants and the color change of the biofilm. As the attached biofilm gradually becomes dense, the color changes from brown to gray and finally to brown. The thickness of the biofilm also becomes uniform with the flushing of water flow and its own increase in value, the pollutant removal ability is gradually enhanced, and the biological community unique to the biofilm is gradually formed. The biofilm attachment test phase is completed.

[0138] The test method of outer film thickness is to measure the film thickness by observing the inclined cross-section morphology of the composite film through a scanning electron microscope. Usually, the focused ion beam cutting technology is used to first cut the sample into an inclined cross-section, and then the film morphology and thickness on the cross-section are observed through a scanning electron microscope.

[0139] Test method for membrane surface loading: Take a composite membrane material with a length of L and an outer diameter of D without attached microbial membrane, dry it at 105°C for 2 hours, and weigh it, marking it as G1;

[0140] The surface area of ​​the membrane material at this length is A = L × D × π;

[0141] After the microbial film was attached, the composite film material of the same length was taken and dried at 105 °C for 2 h and then weighed and marked as G2;

[0142] Membrane surface loading = (G2-G1) / A.

[0143] Test method for nitrification reaction rate:

[0144]

[0145] NHx,inf——ammonia nitrogen concentration entering the MABR reaction unit, mg / L;

[0146] NHx,eff——ammonia nitrogen concentration outflowing from MABR reaction unit, mg / L;

[0147] A——MABR membrane area;

[0148] Qinf——flow rate through the MABR reaction unit, m3 / d;

[0149] NR——MABR nitrification reaction rate, g N / m2 / d.

[0150]

[0151] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A composite membrane material, characterized in that: Includes inner and outer membranes; The inner membrane has an inner diameter of 300 to 450 μm, a thickness of no more than 100 μm, a pore size of 0.1 to 0.5 μm, and a porosity of 45% to 80%; The thickness of the outer film is not higher than 5 μm, the porosity is 30% to 60%, the surface contact angle is less than 70°, and the roughness is 50 to 140 nm.

2. The composite membrane material according to claim 1, characterized in that: The outer film comprises magnetic nanoparticles, a hydrophilic silane solvent and a polyalkylsiloxane solvent.

3. The composite membrane material according to claim 2, characterized in that: The mass ratio of the magnetic nanoparticles, the hydrophilic silane solvent and the polyalkylsiloxane solvent is (1-20): (5-18): (20-40).

4. The composite membrane material according to claim 2 or 3, characterized in that: The average particle size of the magnetic nanoparticles is 20-100 nm.

5. The composite membrane material according to any one of claims 2 to 4, characterized in that: The magnetic nanoparticles include at least one of Fe3O4 nanoparticles, Fe2O3 nanoparticles, and Fe2O3-Al2O3 composite nanoparticles.

6. The composite membrane material according to any one of claims 1 to 5, characterized in that: The inner film is one of polyvinylidene fluoride film, polyethylene film, polytetrafluoroethylene film and polypropylene film.

7. The composite membrane material according to any one of claims 2 to 6, characterized in that: The hydrophilic silane solvent includes one or two of γ-aminopropyltrimethoxysilane and methyltrimethoxysilane; And / or, the polyalkylsiloxane solvent includes one or both of polymethylsiloxane and polydimethylsiloxane.

8. A method for preparing a composite membrane material according to any one of claims 1 to 7, characterized in that: The steps include: At a pH of 8 to 9, the magnetic nanoparticle solution, the polyalkylsiloxane solvent and the cosolvent are mixed in a mass ratio of (12% to 30%): (60% to 80%): (1% to 8%) to obtain a coating solution, wherein the mass concentration of the magnetic nanoparticle solution is 5% to 10%; The inner membrane is placed in the coating solution, soaked for 3 to 8 minutes, then taken out and subjected to curing treatment.

9. The preparation method according to claim 8, characterized in that: Before placing the inner membrane in the coating solution, the inner membrane is immersed in an organic solvent for 3 to 5 minutes, then washed in clean water for 3 to 5 minutes, and dried to remove the residual moisture in the inner membrane.

10. A MABR system, characterized in that: The invention comprises the composite membrane material according to any one of claims 1 to 7 or the composite membrane material obtained by the preparation method according to claim 8 or 9.